Method for preparing high nickel matte by mixing low nickel matte into high nickel material
Through the Ausmelt furnace smelting and converter blowing process of mixing low nickel matte with high nickel materials, the problems of high energy consumption and low output in the smelting of high nickel matte are solved, achieving efficient production of high nickel matte and reducing production costs and carbon emissions.
Patent Information
- Application Number
- CN202410865391.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-01
- Publication Date
- 2024-10-25
AI Technical Summary
The existing high nickel matte smelting process has the problems of high comprehensive energy consumption per unit of high nickel matte, high production cost per unit of high nickel matte, and low output of high nickel matte.
Using the method of mixing low matte nickel into high nickel materials, through the Ausmelt furnace smelting and converter blowing process of nickel concentrate, combined with the heat treatment of quartz stone solvent, air and oxygen, multiple sedimentation separation and water quenching are carried out, and finally in The holding furnace performs water quenching and casting to produce high nickel matte products with high nickel content.
It significantly reduces the comprehensive energy consumption and production cost of high nickel matte, while increasing the output of high nickel matte, reducing carbon emissions, and has environmental protection and economic advantages.
Smart Images

Figure CN118835100A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of nickel smelting, and in particular relates to a method for preparing high-nickel matte by mixing low-nickel matte into high-nickel material. Background Art
[0002] In recent years, with the vigorous development of new energy vehicles, the market demand for power batteries has increased sharply, and the market demand for electrolytic nickel and nickel sulfate has increased significantly, thus promoting the development of the high-grade nickel matte industry. The market demand for high-grade nickel matte is also mainly driven by the following factors: first, the rapid development of the stainless steel industry, stainless steel accounts for the largest proportion of the demand for high-grade nickel matte; second, the demand for high-grade nickel matte in traditional fields such as electroplating and alloys is stable. It can be seen that the high-grade nickel matte market has a good development prospect.
[0003] The global nickel ores are divided into nickel sulfide ore and laterite nickel ore, both of which can be used to smelt high-grade nickel matte. Among them, the high-grade nickel matte process of nickel sulfide ore is mainly the nickel sulfide ore pyrometallurgy, and the process of smelting high-grade nickel matte from nickel sulfide ore pyrometallurgy is mainly electric furnace smelting and flash smelting. Low-grade nickel matte is first obtained through electric furnace smelting and flash smelting, and then high-grade nickel matte is obtained through converter blowing. However, both processes have the problems of high comprehensive energy consumption per unit of high-grade nickel matte, high production cost per unit of high-grade nickel matte, and low output of high-grade nickel matte. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a method for preparing high-nickel matte which can reduce the comprehensive energy consumption per unit of high-nickel matte, the production cost per unit of high-nickel matte, and increase the output of high-nickel matte.
[0005] In order to solve the above technical problems, the present invention provides a method for preparing high nickel matte by mixing low nickel matte into high nickel material, and the technical solution is as follows:
[0006] (I) Smelting of nickel concentrate
[0007] After being batched, the nickel concentrate is transported to the Ausmelt furnace together with the quartz solvent. Air, oxygen and pulverized coal fuel are sprayed into the Ausmelt furnace through a spray gun to provide heat, so that the nickel concentrate and the quartz solvent form a melt in the Ausmelt furnace. The Ausmelt furnace produces high-temperature liquid low-matte nickel A and Ausmelt slag with a nickel content of about 0.3%, where the nickel content is the mass percentage of the nickel element. The mixture of high-temperature liquid low-matte nickel A and Ausmelt slag flows into the settling electric furnace, where it is separated by sedimentation to obtain high-temperature liquid low-matte nickel B with a nickel content of 30% to 35% and high-temperature slag A. The high-temperature slag A is quenched with water to obtain waste slag. The smelting flue gas generated during the smelting process passes through a waste heat boiler and an electric dust collector, and then the flue gas is used to make acid to obtain sulfuric acid.
[0008] (II) Converter blowing with high nickel materials
[0009] When the water content of the high-nickel material is greater than or equal to 0.5%, the high-nickel material is first fed into the converter, and then the high-temperature liquid low-nickel matte B obtained in the above steps is fed into the converter for blowing. After blowing for a period of time, cold material is added according to the furnace temperature. Matte bun lumps, converter splashes, and blowing smoke lumps can all be used as cold materials. The nickel content of the cold material is less than 1%. After adding the cold material, the blowing and heating are continued, and then quartz stone solvent is added according to the slag type. Finally, high-temperature liquid high-nickel matte, smelting flue gas and converter slag are obtained. The converter slag is returned to the sedimentation furnace, and high-temperature slag B is obtained by sedimentation and separation in the sedimentation furnace. After the high-temperature slag B is quenched with water, waste slag is obtained, and the high-temperature liquid high-nickel matte is fed into the insulation furnace for water quenching and casting of anode plates. Finally, three products, water-quenched high-nickel matte, nickel anode plates, and large blocks of high-nickel matte are produced. The smelting flue gas passes through a waste heat boiler and an electric dust collector, and then flue gas acid is produced to obtain sulfuric acid.
[0010] When the water content of the high-nickel material is less than 0.5%, the high-nickel material is first fed into the converter, and then the high-temperature liquid low-nickel matte B obtained in the above steps is fed into the converter for refining; or the high-temperature liquid low-nickel matte B obtained in the above steps is first fed into the converter, and then the high-nickel material is fed into the converter during the refining process of the converter. After the high-nickel material and the high-temperature liquid low-nickel matte B are blown in the converter for a period of time, a quartz stone solvent is added according to the slag type, and finally high-temperature liquid high-nickel matte, smelting flue gas and converter slag are obtained. The converter slag is returned to the sedimentation furnace, and the high-temperature slag B is obtained by sedimentation and separation in the sedimentation furnace. After the high-temperature slag B is quenched with water, the waste slag is obtained. The high-temperature liquid high-nickel matte is fed into the insulation furnace for water quenching and casting of anode plates. Finally, three products are produced: water-quenched high-nickel matte, nickel anode plates, and large blocks of high-nickel matte. The smelting flue gas is passed through a waste heat boiler and an electric dust collector for flue gas acid production to obtain sulfuric acid.
[0011] The high-nickel material contains 50% to 72% nickel.
[0012] When the water content of the high-nickel material is greater than or equal to 0.5%, the mass of the high-nickel material is 6% to 9% of the mass of the high-temperature liquid low-nickel matte B fed into the converter.
[0013] When the water content of the high-nickel material is less than 0.5%, the mass of the high-nickel material is 10% to 15% of the mass of the high-temperature liquid low-nickel matte B fed into the converter.
[0014] The nickel content of the high nickel matte is 55% to 65%.
[0015] Through the above-mentioned design scheme, the present invention can bring the following beneficial effects: compared with the existing process, the preparation process adds high-nickel material as one of the converter raw materials into the converter, while ensuring the appropriate furnace temperature and good slag shape of the converter blowing, it increases the output of high-nickel matte products of the smelter, and at the same time can greatly reduce the comprehensive energy consumption of producing unit high-nickel matte, thereby greatly reducing carbon emissions, which is beneficial to environmental protection and reduces the production cost of high-nickel matte. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments.
[0017] Figure 1 This is a flow chart of the method for preparing high-grade nickel matte in an embodiment of the present invention. DETAILED DESCRIPTION
[0018] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the following is a further detailed description of a method for preparing high nickel matte by mixing low nickel matte with high nickel material in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and do not constitute a limitation of the present invention.
[0019] Example 1
[0020] (I) Smelting of nickel concentrate
[0021] After being batched, the nickel concentrate is transported to the Ausmelt furnace together with the quartz solvent. Air, oxygen and pulverized coal fuel are sprayed into the Ausmelt furnace through a spray gun to provide heat, so that the nickel concentrate and the quartz solvent form a melt in the Ausmelt furnace. The Ausmelt furnace produces high-temperature liquid low-matte nickel A and Ausmelt slag with a nickel content of 0.28%. The mixture of high-temperature liquid low-matte nickel A and Ausmelt slag continuously flows into the settling furnace, and is separated by sedimentation in the settling furnace to obtain high-temperature slag A and high-temperature liquid low-matte nickel B with a nickel content of 30.51%. The high-temperature slag A is quenched with water to obtain waste slag. The smelting flue gas generated in the smelting process passes through a waste heat boiler and an electric dust collector, and then the flue gas is used to make acid to obtain sulfuric acid.
[0022] (II) Converter blowing with high nickel materials
[0023] The high-temperature liquid low-nickel matte B obtained in the above steps is fed into the converter, and then in the process of blowing the converter, a high-nickel material with a nickel content of 71.96% and a water content of 0.32% is fed into the converter. After blowing in the converter, high-temperature liquid high-nickel matte, smelting flue gas and converter slag are obtained. The converter slag is returned to the settling furnace, and is separated and settled in the settling furnace to obtain high-temperature slag B. The high-temperature slag B is quenched with water to obtain waste slag. The high-temperature liquid high-nickel matte is fed into a holding furnace for water quenching and casting of anode plates. Finally, three products, namely water-quenched high-nickel matte, nickel anode plates and large blocks of high-nickel matte, all of which have a nickel content of 61.48%, are produced. The smelting flue gas passes through a waste heat boiler and an electric dust collector, and then is used to make acid from the flue gas to obtain sulfuric acid.
[0024] A comparison of the yields of high nickel matte obtained by using the method of preparing high nickel matte by mixing low nickel matte into high nickel material according to the present invention and the process of preparing high nickel matte by the traditional nickel sulfide ore pyrometallurgical method is shown in Tables 1 and 2.
[0025] Table 1
[0026]
[0027] Table 2
[0028]
[0029] Table 3 shows a comparison of the unit energy consumption of preparing high nickel matte by mixing low nickel matte with high nickel material according to the present invention and preparing high nickel matte by conventional nickel sulfide ore pyrometallurgy.
[0030] Table 3
[0031]
[0032] The energy consumption limit levels per unit product for nickel smelting in GB 25323-2023 “Energy consumption limits per unit product for non-ferrous and heavy metal smelting enterprises” are shown in Table 4.
[0033] Table 4 Unit is kilograms of standard coal per ton
[0034]
[0035]
[0036] Example 2
[0037] (I) Smelting of nickel concentrate
[0038] After being batched, the nickel concentrate is transported to the Ausmelt furnace together with the quartz solvent. Air, oxygen and pulverized coal fuel are sprayed into the Ausmelt furnace through a spray gun to provide heat, so that the nickel concentrate and the quartz solvent form a melt in the Ausmelt furnace. The Ausmelt furnace produces high-temperature liquid low-matte nickel A and Ausmelt slag with a nickel content of 0.31%. The mixture of high-temperature liquid low-matte nickel A and Ausmelt slag continuously flows into the settling furnace, and is separated by sedimentation in the settling furnace to obtain high-temperature slag A and high-temperature liquid low-matte nickel B with a nickel content of 30.51%. The high-temperature slag A is quenched with water to obtain waste slag. The smelting flue gas generated in the smelting process passes through a waste heat boiler and an electric dust collector, and then the flue gas is used to make acid to obtain sulfuric acid.
[0039] (II) Converter blowing with high nickel materials
[0040] First, a high-nickel material with a nickel content of 69.83% and a water content of 0.73% is fed into the converter, and then the high-temperature liquid low-nickel matte B obtained in the above steps is fed into the converter for blowing. After blowing for a period of time, cold material is added according to the furnace temperature, and the nickel content of the cold material is 0.85%. After adding the cold material, the blowing and heating are continued, and then a quartz stone solvent is added according to the slag type. Finally, high-temperature liquid high-nickel matte, smelting flue gas and converter slag are obtained. The converter slag is returned to the sedimentation furnace, and high-temperature slag B is obtained by sedimentation and separation in the sedimentation furnace. After the high-temperature slag B is quenched with water, waste slag is obtained, and the high-temperature liquid high-nickel matte is fed into a holding furnace for water quenching and casting of anode plates. Finally, three products, water-quenched high-nickel matte, nickel anode plates, and large blocks of high-nickel matte, each with a nickel content of 60.48% are produced. The smelting flue gas passes through a waste heat boiler and an electric dust collector, and then flue gas acid is produced to obtain sulfuric acid.
[0041] The comparison of the output of high nickel matte obtained by mixing low nickel matte into high nickel material using the method of the present invention and the conventional process for preparing high nickel matte is shown in Tables 5 and 6.
[0042] Table 5
[0043]
[0044] Table 6
[0045]
[0046] Table 7 shows a comparison of unit energy consumption of the method for preparing high nickel matte by mixing low nickel matte into high nickel material according to the present invention and the method for preparing high nickel matte by the traditional process for preparing high nickel matte.
[0047] Table 7
[0048]
[0049] It can be seen from the data in Tables 1, 2, 5 and 6 that, compared with the traditional process of preparing high nickel matte using nickel sulfide ore, the method of preparing high nickel matte by mixing low nickel matte with high nickel material according to the present invention significantly improves the conversion rate of preparing high nickel matte from low nickel matte, and the output of high nickel matte is greatly increased.
[0050] It can be seen from the data in Tables 3, 4 and 7 that, compared with the traditional process of preparing high nickel matte using nickel sulfide ore, the method of preparing high nickel matte by mixing low nickel matte into high nickel material according to the present invention is a three-level energy consumption method, and the method of preparing high nickel matte by mixing low nickel matte into high nickel material according to the present invention is a two-level energy consumption method, and the comprehensive energy consumption per unit product of the high nickel matte process is greatly reduced.
Claims
1. A method for preparing high nickel matte by mixing low nickel matte into high nickel material, characterized in that: The preparation method is as follows, (I) Smelting of nickel concentrate After being batched, the nickel concentrate is transported to the Ausmelt furnace together with the quartz solvent. Air, oxygen and pulverized coal fuel are sprayed into the Ausmelt furnace through a spray gun to provide heat, so that the nickel concentrate and the quartz solvent form a melt in the Ausmelt furnace. The Ausmelt furnace produces high-temperature liquid low-matte nickel A and Ausmelt slag. The mixture of high-temperature liquid low-matte nickel A and Ausmelt slag flows into the sedimentation furnace, and is separated by sedimentation in the sedimentation furnace to obtain low-matte nickel B and high-temperature slag A. The high-temperature slag A is quenched with water to obtain waste slag. The smelting flue gas generated in the smelting process is passed through a waste heat boiler and an electric dust collector, and then the flue gas is used for acid production to obtain sulfuric acid. (II) Converter blowing with high nickel matte material When the water content of the high-nickel material is greater than or equal to 0.5%, the high-nickel material, cold material, quartz stone solvent, and the high-temperature liquid low-nickel matte B obtained in the above steps are sent to the converter for blowing, and finally high-temperature liquid high-nickel matte, smelting flue gas and converter slag are obtained. The converter slag is returned to the sedimentation furnace, and is separated and precipitated in the sedimentation furnace to obtain high-temperature slag B. After the high-temperature slag B is quenched with water, waste slag is obtained. The high-temperature liquid high-nickel matte is sent to the insulation furnace for water quenching and casting anode plates. Finally, three products, water-quenched high-nickel matte, nickel anode plates, and high-nickel matte blocks, are produced. The smelting flue gas passes through a waste heat boiler and an electric dust collector, and then the flue gas is used for acid production to obtain sulfuric acid. When the water content of the high-nickel material is less than 0.5%, the high-nickel material, quartz stone solvent and the high-temperature liquid low-nickel matte B obtained in the above steps are sent to the converter for blowing, and finally high-temperature liquid high-nickel matte, smelting flue gas and converter slag are obtained. The converter slag is returned to the sedimentation furnace, and sedimented and separated in the sedimentation furnace to obtain high-temperature slag B. After the high-temperature slag B is quenched with water, waste slag is obtained, and the high-temperature liquid high-nickel matte is sent to the insulation furnace for water quenching and casting anode plates. Finally, three products, water-quenched high-nickel matte, nickel anode plates and high-nickel matte blocks, are produced. The smelting flue gas passes through a waste heat boiler and an electric dust collector, and then the flue gas is used to make acid to obtain sulfuric acid.
2. The method for preparing high nickel matte by mixing low nickel matte into high nickel material according to claim 1, characterized in that: When the water content of the high-nickel material is greater than or equal to 0.5%, the mass of the high-nickel material is 6% to 9% of the mass of the low-nickel matte fed into the converter.
3. The method for preparing high nickel matte by mixing low nickel matte into high nickel material according to claim 1, characterized in that: When the water content of the high-nickel material is less than 0.5%, the mass of the high-nickel material is 10% to 15% of the mass of the low-nickel matte fed into the converter.
4. The method for preparing high nickel matte by mixing low nickel matte into high nickel material according to claim 1, characterized in that: When the water content of high-nickel material is greater than or equal to 0.5%, the high-nickel material is first sent to the converter, and then the high-temperature liquid low-nickel matte B is sent to the converter for blowing. After blowing for a period of time, cold material is added according to the furnace temperature. After adding the cold material, the temperature is continued to be blown and raised, and then the quartz stone solvent is added according to the slag type.
5. The method for preparing high nickel matte by mixing low nickel matte into high nickel material according to claim 1, characterized in that: When the water content of high-nickel material is less than 0.5%, the high-nickel material is first sent to the converter, and then the high-temperature liquid low-nickel matte B is sent to the converter for blowing. After blowing for a period of time, quartz stone solvent is added according to the slag type.
6. The method for preparing high nickel matte by mixing low nickel matte into high nickel material according to claim 1, characterized in that: When the water content of high-nickel material is less than 0.5%, high-temperature liquid low-nickel matte B is first fed into the converter, and then the high-nickel material is fed into the converter during the blowing process. After blowing for a period of time, quartz stone solvent is added according to the slag type.