High-conductivity corrosion-resistant composite coating and preparation method thereof

Through DC-coupled AC cathode turret technology and magnetron sputtering technology, the metal coating structure is optimized, which solves the corrosion problem of metal coatings in acidic solutions and electrochemical environments in the existing technology, and achieves high conductivity and corrosion resistance. The combination of sex is suitable for industrial production.

CN118835210AActive Publication Date: 2024-10-25HEFEI UNIV OF TECH

Patent Information

Application Number
CN202410886884.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-10-25
Estimated Expiration
2044-07-03

AI Technical Summary

Technical Problem

Existing metal coatings are prone to corrosion in acidic solutions and electrochemical environments, resulting in reduced conductivity and short service life. The production process is complex and the cost is high, which limits industrial application.

Method used

DC-coupled AC cathode turret technology is used for plasma nitriding treatment to form a nitrided layer, and a metal nitride intermediate layer and doped TAC layer are prepared by magnetron sputtering, and the coating structure is optimized to improve conductivity and corrosion resistance. sex.

Benefits of technology

It achieves a combination of high conductivity and corrosion resistance, reduces coating thickness and production costs, improves the anti-corrosion performance and service life of the metal substrate, and is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118835210A_ABST
    Figure CN118835210A_ABST
Patent Text Reader

Abstract

The invention discloses a high-conductivity corrosion-resistant composite coating and a preparation method thereof, and the preparation method comprises the following steps: pretreating the surface of a metal matrix, then clamping the metal matrix in a vacuum chamber of a coating machine, baking and exhausting in a vacuum state, cleaning with an ion beam, and then nitriding to form a nitriding layer with the thickness of 0.1-1 mu m on the surface of the metal matrix; sequentially depositing pure metal and nitride of the pure metal to form a base layer with the total thickness of 0.02-0.5 mu m; sequentially depositing two kinds of metal and nitrides of the two kinds of metal to form an intermediate layer with the total thickness of 0.02-1.5 microns; and then depositing a metal-doped TAC layer with the thickness of 0.03-1 [mu] m to obtain the composite coating with the total thickness of 0.17-3.5 [mu] m. Element doping modification and a multi-layer composite structure are adopted, the compactness of the coating is improved, meanwhile, the excellent performance of the metal nitride and the amorphous carbon layer is exerted, and the obtained coating is small in thickness and good in corrosion resistance and conductivity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of material surface treatment, and in particular to a high-conductivity, corrosion-resistant composite coating and a preparation method thereof. Background Art

[0002] Metals and their alloys play an important role in the industrial field. However, factors such as solutions and currents in the working environment can corrode metal materials, causing the failure of various properties of metal materials, thereby causing huge economic losses, catastrophic accidents, energy waste and environmental pollution. For example: In the field of new energy, the energy conversion efficiency and service life of batteries are important performance indicators. Metal materials have become the preferred materials for important battery accessories such as plates and collectors due to their good processability, mechanical properties and conductivity. However, in the acidic solution of the battery and the electrochemical working environment, metal accessories are extremely susceptible to corrosion, which will damage the functional structure of the metal accessories. The metal ions produced by corrosion will also reduce the energy conversion efficiency and service life of the battery. In the 3C field, due to the complex and changeable working environment of electronic products, their metal accessories are often corroded by various solutions, which will reduce their conductivity, and then cause electrostatic discharge and electromagnetic interference, which will cause electronic products to malfunction at the least, and insulation breakdown, explosion and other accidents at the worst.

[0003] As a result, a large number of coating technologies for surface modification and protection of metal materials have emerged, such as metal nitride coatings CrN, TiN, NbN, etc. and amorphous carbon coatings (DLC). These methods effectively improve the electrochemical corrosion resistance and interface conductivity of metal materials. However, metal nitride coatings often have a very obvious columnar crystal structure, and the gaps between the columnar crystals can easily become channels for corrosive ions, which have a poor protective effect on the substrate. Amorphous carbon coatings have defects such as hydrophilicity, poor toughness, and large internal stress, which limit the advantages of its corrosion resistance. In order to avoid the above situation, the thickness of the coating structure design is often above 500nm, and the problems of low production process efficiency and unbalanced overall performance have led to an increase in production costs and production delivery cycles, which is not conducive to industrial production and the actual application of products.

[0004] A Chinese patent application document with publication number CN115911436A discloses a process for preparing a carbon-based composite coating for a metal bipolar plate of a PEM fuel cell, comprising the following steps: baking and degassing the surface of the bipolar plate to be plated, ion cleaning and activation, preparing an ion-diffused layer, depositing a metal base layer, depositing a metal nitride layer, depositing a DLC layer, and depositing a Ta-C layer in sequence under a vacuum state. It combines ion nitriding / carburizing, magnetron sputtering MS, plasma enhanced chemical vapor deposition PECVD, and pure ion plating PIC to prepare a carbon-based composite coating on a metal bipolar plate, which can improve the corrosion resistance and bonding strength of the bipolar plate and extend its service life. However, the coating is still relatively thick, the coating deposition time is long, and there are many composite processes, which is not conducive to industrial production. Summary of the invention

[0005] The technical problem to be solved by the present invention is how to effectively improve the electrical conductivity and corrosion resistance of the metal coating.

[0006] The present invention solves the above technical problems through the following technical means:

[0007] A method for preparing a highly conductive and corrosion-resistant composite coating comprises the following steps:

[0008] S1. Pre-treat the surface of the metal substrate, then clamp it in the vacuum chamber of the coating machine, and bake and exhaust it under vacuum;

[0009] S2, performing ion beam cleaning on the metal substrate after baking exhaust;

[0010] S3, performing nitriding treatment on the metal substrate after ion beam cleaning to form a nitriding layer on the surface of the metal substrate; wherein the thickness of the nitriding layer is 0.1-1 μm;

[0011] S4, depositing pure metal and the nitride of the above metal on the surface of the metal substrate treated by S3 in sequence to form a base layer; wherein the total thickness of the base layer is 0.02-0.5 μm;

[0012] S5, depositing two metals and nitrides of the two metals on the surface of the base layer formed in S4 in sequence to form an intermediate layer; wherein the total thickness of the intermediate layer is 0.02-1.5 μm;

[0013] S6. Depositing a metal-doped TAC layer on the surface of the intermediate layer formed in S5 to obtain the highly conductive and corrosion-resistant composite coating, wherein the thickness of the metal-doped TAC layer is 0.03-1 μm, and the total thickness of the obtained composite coating is 0.17-3.5 μm.

[0014] Preferably, in S1, pre-treating the surface of the metal substrate comprises the following steps: in a dust-free environment, washing the metal substrate with detergent and deionized water in sequence, and then placing the metal substrate in anhydrous ethanol for ultrasonic cleaning; after the cleaning is completed, placing the metal substrate in a 70-90° C. depassivation film solution and soaking it for 20-40 minutes; placing the metal substrate in deionized water for ultrasonic cleaning again, and then air-drying it with nitrogen; during the baking exhaust process, evacuating the metal substrate to 1×10 -2 Pa, the baking temperature is 200-350°C, and the time is 30-120min; in S2, the following steps are specifically included: vacuuming to 7×10 -3 Pa and maintain the temperature at 200-350°C, start the turntable to rotate at a uniform speed, then fill with argon, the argon partial pressure is 0.2-0.8Pa, then turn on the ion source power supply and the turntable bias power supply, the ion source voltage is 200-1200V, the current is 0.5-2A, the turntable bias is 500-2000V, the bias current is 0.5-2A, the bias duty cycle is set to 50-80%, and the metal substrate surface is evenly cleaned for 20-180 minutes.

[0015] Preferably, in S3, the following steps are specifically included: after ion beam cleaning, turn off the argon gas, maintain the temperature at 200-350°C, keep the rotating frame rotating at a constant speed, and evacuate to 7×10 -3 Pa, nitrogen is introduced to maintain the nitrogen partial pressure between 5-20Pa; then nitriding treatment is carried out. During the nitriding treatment, two sets of power supplies, DC power supply and AC power supply, are used. The AC rotary frame bias is 1200-2000V, the DC rotary frame voltage is 900-1500V, the AC rotary frame bias current is 3-7A, the DC rotary frame bias current is 3-7A, and the nitriding time is 30-120min to form a nitriding layer on the surface of the metal substrate.

[0016] Preferably, in S4, the pure metal includes one metal or two metals; the one metal is one of Ti, Cr, Nb, Zr, and Ta; the two metals are one of Ni and Cr, or Al and Cr; the metal nitride is one of TiN, CrN, NbN, ZrN, TaN, NiCrN, and AlCrN; in S5, the deposited two metals are one of Cr and Mo, or Zr and Mo; the metal nitride is one of CrMoN and ZrMoN; in S6, the doped metal is one or more of Ti, Cr, and Zr.

[0017] Preferably, in S4, the following steps are specifically included: turning off the nitrogen, turning off the bias of the rotating frame, maintaining the temperature at 200-350°C, keeping the rotating frame rotating at a constant speed, and evacuating to 2×10 -3Pa, fill with argon gas, the argon partial pressure is 0.1-3Pa, start magnetron sputtering of metal to form a metal base layer, set the sputtering power to 2-10KW, the turret bias to 100-300V, the turret bias duty cycle to 50-80%, the sputtering time to 5-40min, and complete the sputtering of the metal base layer; then introduce nitrogen gas to maintain the gas pressure at 0.1-3Pa, start magnetron sputtering of metal nitride to form a metal nitride base layer, set the sputtering power to 2-10KW, the turret bias to 100-300V, the turret bias duty cycle to 50-80%, the sputtering time to 5-120min, and complete the sputtering of the metal nitride base layer to form a base layer.

[0018] Preferably, in S5, the following steps are specifically included: turning off the nitrogen, turning off the bias of the rotating frame, maintaining the temperature at 200-350°C, keeping the rotating frame rotating at a constant speed, and evacuating to 2×10 -3 Pa, fill with argon gas, the argon partial pressure is 0.1-3Pa, start co-sputtering of two metals to form a metal intermediate layer, set the metal target sputtering power to 1-10KW, the turret bias to 100-300V, the turret bias duty cycle to 50-80%, the sputtering time to 10-60min, and complete the co-sputtering of the metal intermediate layer; then introduce nitrogen gas to maintain the gas pressure at 0.1-3Pa, set the metal target sputtering power to 1-10KW, the turret bias to 100-300V, the turret bias duty cycle to 50-80%, the sputtering time to 10-120min, and complete the sputtering of the metal nitride intermediate layer.

[0019] Preferably, in S6, the following steps are specifically included: turning off the nitrogen and argon gas, turning off the sputtering system and the heating system, waiting for the temperature to drop below 120° C., turning on the multi-arc ion plating system, and evacuating to 3×10 -4 Below Pa, multi-arc ion plating begins, with carbon target arc current of 50-150A, metal target arc current of 50-150A, turret bias of 100-2000V, and time of 5-60min.

[0020] Preferably, S5 further includes repeatedly depositing two metals and nitrides of the two metals to form n intermediate layers; wherein n is less than or equal to 50.

[0021] Preferably, in S4, pure metal is deposited to form a metal base layer, the thickness of the metal base layer is 0.01-0.3 μm, and metal nitride is deposited to form a metal nitride base layer, the thickness of the metal nitride base layer is 0.01-0.3 μm; in S5, two metals are deposited to form a metal intermediate layer, the thickness of the metal intermediate layer is 0.01-0.5 μm; two metal nitrides are deposited to form a metal nitride intermediate layer, the thickness of the metal nitride intermediate layer is 0.01-1 μm.

[0022] Preferably, in S1, the metal matrix is ​​one of stainless steel, aluminum and aluminum alloys, titanium and titanium alloys, nickel and nickel alloys, copper and copper alloys or carbon steel.

[0023] Preferably, the thickness of the nitriding layer is 0.1 μm; the total thickness of the primer layer is 0.02-0.04 μm; the total thickness of the intermediate layer is 0.02-0.06 μm; the thickness of the metal-doped TAC layer is 0.03-0.04 μm, and the total thickness of the obtained composite coating is 0.17-0.22 μm.

[0024] The present invention also provides a high-conductivity and corrosion-resistant composite coating, which is prepared by adopting the preparation method of the high-conductivity and corrosion-resistant composite coating.

[0025] The advantages of the present invention are:

[0026] In the preparation method of the high-conductivity, corrosion-resistant composite coating of the present invention, first, a DC-coupled AC cathode rotatable rack technology (i.e., dual-power nitriding, two different types of power supplies are selected to simultaneously power the rotatable rack. The present invention selects a combination of AC pulse and DC pulse power supplies) is used to carry out plasma nitriding treatment, which can optimize the surface morphology and structure of the metal substrate and achieve the first-level corrosion protection of the metal substrate. Compared with the traditional plasma nitriding treatment, the DC-coupled AC cathode rotatable rack technology has better nitriding uniformity and higher efficiency. The base layer is prepared by magnetron sputtering technology to ensure good bonding between the conductive corrosion-resistant layer and the substrate. Then, the metal nitride intermediate layer prepared by co-sputtering of Mo and Cr or Zr can eliminate the columnar crystal structure originally existing in CrN or ZrN, so that the grain size of the coating is reduced and has a denser structure, and the co-sputtered product MoN 2 It has good electrical conductivity, effectively optimizes the structural defects of metal nitrides, and while ensuring high electrical conductivity, the dense structure can effectively prevent corrosion ions from contacting the metal matrix, thereby achieving the second level of protection. TAC, as the hardest amorphous carbon, has good corrosion resistance, but because it contains a large amount of diamond-like structures, it has a large internal stress, which may cause film failure and peeling. TAC coatings modified by single or co-doping of Cr, Zr, and Ti will produce nanophases such as CrC, ZrC, and TiC. These phases have good hydrophobicity and electrical conductivity, which are conducive to the removal of corrosive solutions, and can effectively reduce the internal stress of the coating, maintain the dense structure of amorphous carbon, and prevent the generation of defects and other diffusion channels of corrosion ions, thereby achieving the third level of protection. The method of the present invention adopts element doping modification and multi-layer composite structure, which can improve the density of the coating while giving play to the excellent performance of the metal nitride and the amorphous carbon layer, so that the obtained coating is thin in thickness, corrosion-resistant, and conductive. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a schematic flow chart of a method for preparing a highly conductive and corrosion-resistant composite coating provided in Example 1 of the present invention;

[0028] Figure 2 A schematic diagram of the structure of a highly conductive, corrosion-resistant composite coating provided in Example 2 of the present invention;

[0029] Figure 3 It is an assembly relationship diagram of the power supply used in the nitriding process of the embodiment of the present invention;

[0030] Figure 2 Description of main symbols:

[0031] 1. Metal substrate after nitriding; 1-1. Metal substrate; 1-2. Nitriding layer; 2. Base layer; 2-1. Metal base layer; 2-2. Metal nitride base layer; 3. Intermediate layer; 3-1. Metal intermediate layer; 3-2. Metal nitride intermediate layer; 4. Metal-doped TAC layer.

[0032] Figure 3 Description of main symbols:

[0033] 1. AC cathode plate; 2. DC cathode plate; 3. DC cathode conductive support rod; 4. AC cathode conductive support rod; 5. DC cathode connector; 6. AC cathode connector; 7. Insulating sleeve.

[0034] Figure 4 This is a test diagram of acid corrosion current density of the coatings prepared in Example 1 of the present invention and Comparative Example 1. DETAILED DESCRIPTION

[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Unless otherwise specified, the test materials and reagents used in the following examples can be obtained from commercial sources.

[0037] If no specific techniques or conditions are specified in the examples, they can be carried out according to the techniques or conditions described in the literature in the art or according to the product instructions.

[0038] In the embodiments and comparative examples, the DC coupled AC cathode rotating frame technology used in the nitriding process specifically uses two sets of AC and DC power supplies for nitriding treatment, and the assembly relationship thereof is as follows: Figure 3As shown, 1 is an AC cathode plate; 2 is a DC cathode plate; 3 is a DC cathode conductive support rod; 4 is an AC cathode conductive support rod; 5 is a DC cathode connector; 6 is an AC cathode connector; 7 is an insulating sleeve; the AC cathode plate 1 is connected to the AC cathode conductive support rod 4, the negative pole of the AC pulse power supply is connected to the AC cathode connector 6, and the positive pole of the power supply is connected to the vacuum chamber of the coating machine; the DC cathode plate 2 is connected to the DC cathode conductive support rod 3, the negative pole of the DC pulse power supply is connected to the DC cathode connector 5, and the positive pole of the power supply is connected to the vacuum chamber of the coating machine; the two sets of cathode plates are parallel to each other, and the two sets of cathode systems are insulated from each other by the insulating sleeve 7.

[0039] The depassivation film solution is a HNO 3 and HF mixed solution, where HNO 3 The volume fraction of is 8%, and the volume fraction of HF is 2%.

[0040] Example 1

[0041] Combination Figure 1 , a flow chart of a method for preparing a highly conductive and corrosion-resistant composite coating, wherein the highly conductive and corrosion-resistant composite coating is prepared on the surface of stainless steel (metal substrate), that is, ion nitriding, deposition of a base layer, deposition of an intermediate layer, and deposition of a metal-doped TAC layer are sequentially performed on the surface of the stainless steel, specifically comprising the following steps:

[0042] S1. In a dust-free environment, pre-treat the surface of the metal substrate; then clamp the metal substrate in the vacuum chamber of the coating machine and bake and exhaust it under vacuum, which specifically includes the following steps: in a dust-free environment, wash the metal substrate to be coated with detergent and deionized water in turn, and then put it into anhydrous ethanol for ultrasonic cleaning; after the cleaning is completed, put the metal substrate into a 70°C depassivation film solution and soak it for 30 minutes; put the metal substrate into deionized water for ultrasonic cleaning again, and then put it into a nitrogen cabinet for nitrogen air drying, and the pre-treatment is completed; clamp the pre-treated metal substrate into the rotating rack of the vacuum chamber of the coating machine, and evacuate to 1×10 -2 Pa, start the heating system to heat the temperature in the cavity to 250℃ and bake for 60 minutes.

[0043] S2, ion beam cleaning the baked metal substrate, specifically including the following steps: vacuuming to 7×10 -3 Pa and maintain the temperature at 250℃, start the turntable and rotate it at a uniform speed, then fill it with argon, the argon partial pressure is 0.4Pa, and then turn on the ion source power supply and the turntable bias power supply, the ion source voltage is 800V, the current is 1A, the turntable bias is 1000V, the bias current is 1A, the bias duty cycle is set to 70%, and the metal substrate surface is evenly cleaned for 30 minutes.

[0044] S3, filling the vacuum chamber with nitrogen to perform nitriding treatment on the metal substrate, specifically including the following steps: after ion beam cleaning, turn off the argon gas, maintain the temperature at 250 ° C, keep the rotating frame rotating at a constant speed, and evacuate to 7×10 -3 Pa, nitrogen is introduced to maintain the nitrogen partial pressure at 15Pa; DC coupled AC cathode rack technology is used to carry out nitriding. The bias current is turned on, the AC rack bias is 2000V, the DC rack voltage is 1500V, the AC rack bias current is 3A, the DC rack bias current is 3A, and the ion nitriding time is 30min. A 0.1μm thick nitriding layer is formed on the surface of the metal substrate.

[0045] S4, depositing pure metal and its metal nitride on the surface of the nitrided metal substrate to form a base layer, the metal is Cr; the metal nitride is CrN; the specific deposition steps of the base layer are: turn off the nitrogen, turn off the bias of the rotating frame, maintain the temperature at 250 ° C, keep the rotating frame rotating at a constant speed, and evacuate to 2×10 -3 Pa, fill with argon gas, and the argon partial pressure is 0.2Pa. Start magnetron sputtering Cr to form a metal base layer, set the sputtering power to 5KW, the turret bias to 180V, the turret bias duty cycle to 75%, the sputtering time to 5min, and complete the sputtering of the metal base layer. Then introduce nitrogen gas to maintain the gas pressure at 0.5Pa, set the sputtering power to 6KW, the turret bias to 180V, the turret bias duty cycle to 75%, the sputtering time to 10min, and complete the sputtering of the metal nitride base layer. Form a (10nm thick Cr + 10nm thick CrN) base layer on the surface of the nitrided layer.

[0046] S5, depositing two metals and their metal nitrides on the surface of the base layer to form an intermediate layer; the metals are Cr and Mo; the metal nitride is CrMoN; the specific deposition steps of the intermediate layer are: turn off the nitrogen, turn off the bias of the rotating frame, maintain the temperature at 250°C, keep the rotating frame rotating at a constant speed, and evacuate to 2×10 -3 Pa, fill with argon gas, and the argon partial pressure is 0.2Pa. Start to co-sputter Cr and Mo, set the Cr target sputtering power to 6KW, the Mo target sputtering power to 6KW, the turret bias to 180V, the turret bias duty cycle to 75%, the sputtering time to 10min, and complete the co-sputtering of the metal intermediate layer. Then introduce nitrogen to maintain the gas pressure at 0.5Pa, set the Cr target sputtering power to 6KW, the Mo target sputtering power to 6KW, the turret bias to 180V, the turret bias duty cycle to 75%, the sputtering time to 15min, and complete the sputtering of the metal nitride intermediate layer. Form an intermediate layer (10nm thick CrMo + 10nm thick CrMoN) on the surface of the base layer.

[0047] S6, depositing a metal-doped TAC layer on the surface of the intermediate layer, wherein the doped metal element of the metal-doped TAC layer is Cr, and the specific deposition steps of the metal-doped TAC layer are as follows: turning off the nitrogen and argon gas, turning off the sputtering system and the heating system, waiting for the temperature to drop to 60° C., turning on the multi-arc ion plating system, and evacuating to 3×10 -4 Pa or less. Start multi-arc ion plating, with carbon target arc current of 60A, Cr target arc current of 70A, turret bias of 300V, and time of 5min. Complete the deposition of metal-doped TAC layer with a thickness of 30nm.

[0048] Example 2

[0049] Combination Figure 2 , a schematic diagram of the structure of a highly conductive and corrosion-resistant composite coating, wherein a highly conductive and corrosion-resistant composite coating is prepared on the surface of a stainless steel (metal substrate) 1-1, that is, ion nitriding is sequentially performed on the surface of the stainless steel 1-1 to form a nitrided metal substrate 1, a base layer 2 is deposited, an intermediate layer 3 is deposited, and a metal-doped TAC layer 4 is deposited, specifically comprising the following steps:

[0050] S1. In a dust-free environment, pre-treat the surface of the stainless steel substrate 1-1; then clamp the stainless steel substrate 1-1 in the vacuum chamber of the coating machine and bake and exhaust it under vacuum; specifically, the following steps are included: in a dust-free environment, wash the stainless steel substrate 1-1 to be coated with detergent and deionized water in turn, and then put it into anhydrous ethanol for ultrasonic cleaning; after the cleaning is completed, put the stainless steel substrate 1-1 into a 70°C depassivation film solution and soak it for 30 minutes; put the stainless steel substrate 1-1 into deionized water for ultrasonic cleaning again, and then put it into a nitrogen cabinet for nitrogen air drying, and the pre-treatment is completed; clamp the pre-treated stainless steel substrate 1-1 into the rotating rack of the vacuum chamber of the coating machine, and evacuate to 1×10 -2 Pa, start the heating system to heat the temperature in the cavity to 250℃ and bake for 60 minutes.

[0051] S2, ion beam cleaning the baked stainless steel substrate 1-1, specifically comprising the following steps: vacuuming to 7×10 -3 Pa and maintain the temperature at 250°C, start the turntable and rotate it at a uniform speed, then fill it with argon, the argon partial pressure is 0.4Pa, and then turn on the ion source power supply and the turntable bias power supply, the ion source voltage is 800V, the current is 1A, the turntable bias is 1000V, the bias current is 1A, and the bias duty cycle is set to 70%, and the surface of the stainless steel substrate 1-1 is evenly cleaned for 30 minutes.

[0052] S3, filling nitrogen into the vacuum chamber to perform nitriding treatment on the stainless steel substrate 1-1, specifically including the following steps: after ion beam cleaning, turning off the argon gas, maintaining the temperature at 250°C, maintaining the rotating frame to rotate at a constant speed, and evacuating to 7×10 -3 Pa, nitrogen is introduced to maintain the nitrogen partial pressure at 15Pa; DC coupled AC cathode rotary rack technology is used to carry out nitriding. The bias current is turned on, the AC rotary rack bias is 2000V, the DC rotary rack voltage is 1500V, the AC rotary rack bias current is 3A, the DC rotary rack bias current is 3A, and the ion nitriding time is 30min. A 0.1μm thick nitriding layer 1-2 is formed on the surface of the stainless steel substrate 1-1 to obtain the nitrided stainless steel substrate 1.

[0053] S4, depositing pure metal and its metal nitride on the surface of the nitrided stainless steel substrate 1 to form a base layer 2; the metal is Cr; the metal nitride is CrN; the specific deposition steps of the base layer 2 are: turn off the nitrogen, turn off the bias of the rotating frame, maintain the temperature at 250°C, keep the rotating frame rotating at a constant speed, and evacuate to 2×10 -3 Pa, fill with argon gas, and the argon partial pressure is 0.3Pa. Start magnetron sputtering Cr to form metal base layer 2-1, set the sputtering power to 5KW, the turret bias to 180V, the turret bias duty cycle to 75%, the sputtering time to 5min, and complete the sputtering of metal base layer 2-1. Then introduce nitrogen gas to maintain the gas pressure at 0.6Pa, set the sputtering power to 6KW, the turret bias to 180V, the turret bias duty cycle to 75%, the sputtering time to 10min, and complete the sputtering of metal nitride base layer 2-2. Form a (10nm thick Cr + 10nm thick CrN) base layer 2 on the surface of the nitriding layer 1-2.

[0054] S5, deposit two metals and their metal nitrides on the surface of the base layer 2 to form an intermediate layer 3; the metals are Cr and Mo; the metal nitride is CrMoN; the intermediate layer 3 includes three periodic coatings. The specific deposition steps of the intermediate layer 3 are: turn off the nitrogen, turn off the bias of the rotating frame, maintain the temperature at 250°C, keep the rotating frame rotating at a constant speed, and evacuate to 2×10 -3Pa, fill with argon gas, and the argon partial pressure is 0.3Pa. Start to co-sputter Cr and Mo to form metal intermediate layer 3-1, set the Cr target sputtering power to 6KW, the Mo target sputtering power to 6KW, the turret bias to 180V, the turret bias duty cycle to 75%, the sputtering time to 10min, and complete the co-sputtering of metal intermediate layer 3-1. Then introduce nitrogen gas to maintain the gas pressure at 0.6Pa, set the Cr target sputtering power to 6KW, the Mo target sputtering power to 6KW, the turret bias to 180V, the turret bias duty cycle to 75%, the sputtering time to 15min, and complete the sputtering of metal nitride intermediate layer 3-2. Repeat the steps of depositing metal intermediate layer 3-1 and metal nitride intermediate layer 3-2 3 times. Form (10nm thick CrMo + 10nm thick CrMoN) × 3 intermediate layers 3 on the surface of the base layer 2.

[0055] S6, depositing a metal-doped TAC layer 4 on the surface of the intermediate layer 3; the doped metal element of the metal-doped TAC layer 4 is selected as Cr, and the specific deposition steps of the metal-doped TAC layer 4 are as follows: turn off the nitrogen and argon gas, turn off the sputtering system and the heating system, wait until the temperature drops to 60°C, turn on the multi-arc ion plating system, and evacuate to 3×10 -4 The multi-arc ion plating was started, with the carbon target arc current of 60A, the Cr target arc current of 70A, the turret bias of 300V, and the time of 5min. The deposition of the metal-doped TAC layer 4 was completed, with a thickness of 30nm.

[0056] Example 3

[0057] A titanium alloy is selected as a metal matrix, that is, ion nitriding, a base layer deposition, an intermediate layer deposition, and a metal-doped TAC layer deposition are sequentially performed on the surface of the titanium alloy, specifically including the following steps:

[0058] S1. In a dust-free environment, pre-treat the surface of the titanium alloy substrate; then clamp the titanium alloy substrate in the vacuum chamber of the coating machine and bake and exhaust it under vacuum, which specifically includes the following steps: in a dust-free environment, wash the titanium alloy substrate to be coated with detergent and deionized water in turn, and then put it into anhydrous ethanol for ultrasonic cleaning; after the cleaning is completed, put the titanium alloy substrate into a 70°C depassivation film solution and soak it for 20 minutes; put the titanium alloy substrate into deionized water for ultrasonic cleaning again, and then put it into a nitrogen cabinet for nitrogen air drying, and the pre-treatment is completed; clamp the pre-treated titanium alloy substrate into the rotating rack of the vacuum chamber of the coating machine, and evacuate to 1×10 -2 Pa, start the heating system to heat the temperature in the cavity to 300℃ and bake for 60 minutes.

[0059] S2, ion beam cleaning the baked titanium alloy substrate, specifically including the following steps: vacuuming to 7×10 -3 Pa and maintain the temperature at 300℃, start the turntable and rotate it at a uniform speed, then fill it with argon, the argon partial pressure is 0.3Pa, and then turn on the ion source power supply and the turntable bias power supply, the ion source voltage is 600V, the current is 1A, the turntable bias is 1500V, the bias current is 0.5A, and the bias duty cycle is set to 65%, and the surface of the titanium alloy substrate is evenly cleaned for 40 minutes.

[0060] S3, filling the vacuum chamber with nitrogen to perform nitriding treatment on the titanium alloy substrate, specifically including the following steps: after ion beam cleaning, turn off the argon gas, maintain the temperature at 300 ° C, keep the rotating frame rotating at a constant speed, and evacuate to 7×10 -3 Pa, nitrogen is introduced to maintain the nitrogen partial pressure at 13Pa; DC coupled AC cathode rotary rack technology is used for nitriding. The bias current is turned on, the AC rotary rack bias is 1600V, the DC rotary rack voltage is 1200V, the AC rotary rack bias current is 3.5A, the DC rotary rack bias current is 3.5A, and the ion nitriding time is 40min. A 0.1μm thick nitriding layer is formed on the surface of the titanium alloy substrate.

[0061] S4, depositing pure metal and its metal nitride on the surface of the titanium alloy substrate after nitriding to form a base layer, the metal is Ti; the metal nitride is TiN; the specific deposition steps of the base layer are: turn off the nitrogen, turn off the bias of the rotating frame, maintain the temperature at 300 ° C, keep the rotating frame rotating at a constant speed, and evacuate to 2×10 -3 Pa, fill with argon gas, and the argon partial pressure is 0.3Pa. Start magnetron sputtering Ti to form a metal base layer, set the sputtering power to 5KW, the turret bias to 220V, the turret bias duty cycle to 65%, the sputtering time to 10min, and complete the sputtering of the metal base layer. Then introduce nitrogen to maintain the gas pressure at 0.6Pa, set the sputtering power to 5KW, the turret bias to 220V, the turret bias duty cycle to 65%, and the sputtering time to 15min. Form a (10nm thick Ti + 10nm thick TiN) base layer on the surface of the nitriding layer.

[0062] S5, depositing two metals and their metal nitrides on the surface of the base layer to form an intermediate layer; the metals are Zr and Mo; the metal nitride is ZrMoN; the intermediate layer includes three periodic coatings, each periodic coating is composed of a metal intermediate layer and a metal nitride intermediate layer, and the specific deposition steps of the intermediate layer are: turn off the nitrogen, turn off the bias of the rotating frame, maintain the temperature at 300°C, keep the rotating frame rotating at a constant speed, and evacuate to 2×10 -3Pa, fill with argon gas, and the argon partial pressure is 0.3Pa. Start to co-sputter Zr and Mo to form a metal intermediate layer, set the Zr target sputtering power to 6KW, the Mo target sputtering power to 6KW, the turret bias to 220V, the turret bias duty cycle to 65%, the sputtering time to 10min, and complete the co-sputtering of the metal intermediate layer. Then introduce nitrogen to maintain the gas pressure at 0.7Pa, set the Zr target sputtering power to 6KW, the Mo target sputtering power to 6KW, the turret bias to 220V, the turret bias duty cycle to 65%, the sputtering time to 15min, and complete the sputtering of the metal nitride intermediate layer. Repeat the steps of depositing the metal intermediate layer and the metal nitride intermediate layer 3 times. Form (10nm thick ZrMo + 10nm thick ZrMoN) × 3 intermediate layers on the surface of the base layer.

[0063] S6, depositing a metal-doped TAC layer on the surface of the intermediate layer, wherein the doped metal element of the metal-doped TAC layer is Ti, and the specific deposition steps of the metal-doped TAC layer are as follows: turning off the nitrogen and argon gas, turning off the sputtering system and the heating system, waiting for the temperature to drop to 80° C., turning on the multi-arc ion plating system, and evacuating to 3×10 -4 Pa or less. Start multi-arc ion plating, carbon target arc current is 60A, Ti target arc current is 60A, turret bias is 350V, time is 7min. Complete the deposition of metal-doped TAC layer with a thickness of 30nm.

[0064] Example 4

[0065] A highly conductive and corrosion-resistant composite coating is prepared on the surface of stainless steel (metal substrate), that is, ion nitriding, deposition of a base layer, deposition of an intermediate layer, and deposition of a metal-doped TAC layer are sequentially performed on the surface of the stainless steel, specifically including the following steps:

[0066] S1. In a dust-free environment, pre-treat the surface of the metal substrate; then clamp the metal substrate in the vacuum chamber of the coating machine and bake and exhaust it under vacuum, which specifically includes the following steps: in a dust-free environment, wash the metal substrate to be coated with detergent and deionized water in turn, and then put it into anhydrous ethanol for ultrasonic cleaning; after the cleaning is completed, put the metal substrate into a 70°C depassivation film solution and soak it for 30 minutes; put the metal substrate into deionized water for ultrasonic cleaning again, and then put it into a nitrogen cabinet for nitrogen air drying, and the pre-treatment is completed; clamp the pre-treated metal substrate into the rotating rack of the vacuum chamber of the coating machine, and evacuate to 1×10 -2 Pa, start the heating system to heat the temperature in the cavity to 250℃ and bake for 60 minutes.

[0067] S2, ion beam cleaning the baked metal substrate, specifically including the following steps: vacuuming to 7×10 -3Pa and maintain the temperature at 250℃, start the turntable and rotate it at a uniform speed, then fill it with argon, the argon partial pressure is 0.4Pa, and then turn on the ion source power supply and the turntable bias power supply, the ion source voltage is 800V, the current is 1A, the turntable bias is 1000V, the bias current is 1A, the bias duty cycle is set to 70%, and the metal substrate surface is evenly cleaned for 30 minutes.

[0068] S3, filling the vacuum chamber with nitrogen to perform nitriding treatment on the metal substrate, specifically including the following steps: after ion beam cleaning, turn off the argon gas, maintain the temperature at 250 ° C, keep the rotating frame rotating at a constant speed, and evacuate to 7×10 -3 Pa, nitrogen is introduced to maintain the nitrogen partial pressure at 15Pa; DC coupled AC cathode rack technology is used to carry out nitriding. The bias current is turned on, the AC rack bias is 2000V, the DC rack voltage is 1500V, the AC rack bias current is 3A, the DC rack bias current is 3A, and the ion nitriding time is 30min. A 0.1μm thick nitriding layer is formed on the surface of the metal substrate.

[0069] S4, depositing pure metal and its metal nitride on the surface of the nitrided metal substrate to form a base layer. The metal is Cr; the metal nitride is CrN; the specific deposition steps of the base layer are: turn off the nitrogen, turn off the bias of the rotating frame, maintain the temperature at 250°C, keep the rotating frame rotating at a constant speed, and evacuate to 2×10 -3 Pa, fill with argon gas, and the argon partial pressure is 0.5Pa. Start magnetron sputtering Cr to form a metal base layer, set the sputtering power to 5KW, the turret bias to 180V, the turret bias duty cycle to 75%, the sputtering time to 10min, and complete the sputtering of the metal base layer. Then introduce nitrogen gas to maintain the gas pressure at 0.7Pa, set the sputtering power to 6KW, the turret bias to 180V, the turret bias duty cycle to 75%, the sputtering time to 23min, and complete the sputtering of the metal nitride base layer. Form a (20nm thick Cr + 20nm thick CrN) base layer on the surface of the nitrided layer.

[0070] S5. Deposit two metals and their metal nitrides on the surface of the base layer to form an intermediate layer. The metals are Cr and Mo; the metal nitride is CrMoN; the specific deposition steps of the intermediate layer are: turn off the nitrogen, turn off the bias of the rotating frame, maintain the temperature at 250°C, keep the rotating frame rotating at a constant speed, and evacuate to 2×10 -3Pa, fill with argon gas, and the argon partial pressure is 0.5Pa. Start to co-sputter Cr and Mo to form a metal intermediate layer, set the Cr target sputtering power to 6KW, the Mo target sputtering power to 6KW, the turret bias to 180V, the turret bias duty cycle to 75%, the sputtering time to 20min, and complete the co-sputtering of the metal intermediate layer. Then introduce nitrogen to maintain the gas pressure at 0.7Pa, set the Cr target sputtering power to 6KW, the Mo target sputtering power to 6KW, the turret bias to 180V, the turret bias duty cycle to 75%, the sputtering time to 30min, and complete the sputtering of the metal nitride intermediate layer. Form an intermediate layer (20nm thick CrMo + 20nm thick CrMoN) on the surface of the base layer.

[0071] S6, depositing a metal-doped TAC layer on the surface of the intermediate layer. The metal-doped TAC layer is doped with Cr and Ti. The specific deposition steps of the metal-doped TAC layer are as follows: turn off the nitrogen and argon gas, turn off the sputtering system and the heating system, wait until the temperature drops to 60°C, turn on the multi-arc ion plating system, and evacuate to 3×10 -4 Pa or less. Start multi-arc ion plating, with carbon target arc current of 60A, CrTi composite target arc current of 80A, turret bias of 300V, and time of 10min. Complete the deposition of metal-doped TAC layer with a thickness of 40nm.

[0072] Comparative Example 1

[0073] Compared with Example 1, the difference is that the intermediate layer is not doped with Mo, and specifically includes the following steps:

[0074] S1. In a dust-free environment, pre-treat the surface of the metal substrate; then clamp the metal substrate in the vacuum chamber of the coating machine and bake and exhaust it under vacuum, which specifically includes the following steps: in a dust-free environment, wash the metal substrate to be coated with detergent and deionized water in turn, and then put it into anhydrous ethanol for ultrasonic cleaning; after the cleaning is completed, put the metal substrate into a 70°C depassivation film solution and soak it for 30 minutes; put the metal substrate into deionized water for ultrasonic cleaning again, and then put it into a nitrogen cabinet for nitrogen air drying, and the pre-treatment is completed; clamp the pre-treated metal substrate into the rotating rack of the vacuum chamber of the coating machine, and evacuate to 1×10 -2 Pa, start the heating system to heat the temperature in the cavity to 250℃ and bake for 60 minutes.

[0075] S2, ion beam cleaning the baked metal substrate, specifically including the following steps: vacuuming to 7×10 -3Pa and maintain the temperature at 250℃, start the turntable and rotate it at a uniform speed, then fill it with argon, the argon partial pressure is 0.4Pa, and then turn on the ion source power supply and the turntable bias power supply, the ion source voltage is 800V, the current is 1A, the turntable bias is 1000V, the bias current is 1A, the bias duty cycle is set to 70%, and the metal substrate surface is evenly cleaned for 30 minutes.

[0076] S3, filling the vacuum chamber with nitrogen to perform nitriding treatment on the metal substrate, specifically including the following steps: after ion beam cleaning, turn off the argon gas, maintain the temperature at 250 ° C, keep the rotating frame rotating at a constant speed, and evacuate to 7×10 -3 Pa, nitrogen is introduced to maintain the nitrogen partial pressure at 15Pa; DC coupled AC cathode rack technology is used to carry out nitriding. The bias current is turned on, the AC rack bias is 2000V, the DC rack voltage is 1500V, the AC rack bias current is 3A, the DC rack bias current is 3A, and the ion nitriding time is 30min. A 0.1μm thick nitriding layer is formed on the surface of the metal substrate.

[0077] S4, depositing pure metal and its metal nitride on the surface of the nitrided metal substrate to form a base layer, the metal is Cr; the metal nitride is CrN; the specific deposition steps of the base layer are: turn off the nitrogen, turn off the bias of the rotating frame, maintain the temperature at 250 ° C, keep the rotating frame rotating at a constant speed, and evacuate to 2×10 -3 Pa, fill with argon gas, and the argon partial pressure is 0.2Pa. Start magnetron sputtering Cr to form a metal base layer, set the sputtering power to 5KW, the turret bias to 180V, the turret bias duty cycle to 75%, the sputtering time to 5min, and complete the sputtering of the metal base layer. Then introduce nitrogen gas to maintain the gas pressure at 0.5Pa, set the sputtering power to 6KW, the turret bias to 180V, the turret bias duty cycle to 75%, the sputtering time to 10min, and complete the sputtering of the metal nitride base layer. Form a (10nm thick Cr + 10nm thick CrN) base layer on the surface of the nitrided layer.

[0078] S5, depositing a metal and its metal nitride on the surface of the base layer to form an intermediate layer; the metal is Cr; the metal nitride is CrN; the specific steps of depositing the intermediate layer are: turning off the nitrogen, turning off the bias of the rotating frame, maintaining the temperature at 250°C, keeping the rotating frame rotating at a constant speed, and evacuating to 2×10 -3Pa, fill with argon gas, and the argon partial pressure is 0.2Pa. Start sputtering Cr, set the Cr target sputtering power to 6KW, the turret bias to 180V, the turret bias duty cycle to 75%, the sputtering time to 4min, and complete the sputtering of the metal intermediate layer. Then introduce nitrogen gas to maintain the gas pressure at 0.5Pa, set the Cr target sputtering power to 6KW, the turret bias to 180V, the turret bias duty cycle to 75%, the sputtering time to 9min, and complete the sputtering of the metal nitride intermediate layer. Form a (10nm thick Cr + 10nm thick CrN) intermediate layer on the surface of the base layer.

[0079] S6, depositing a metal-doped TAC layer on the surface of the intermediate layer, wherein the doped metal element of the metal-doped TAC layer is Cr, and the specific deposition steps of the metal-doped TAC layer are as follows: turning off the nitrogen and argon gas, turning off the sputtering system and the heating system, waiting for the temperature to drop to 60° C., turning on the multi-arc ion plating system, and evacuating to 3×10 -4 Pa or less. Start multi-arc ion plating, carbon target arc current is 60A, Cr target arc current is 70A, turntable bias is 300V, time is 5min. Complete the deposition of metal-doped TAC layer with a thickness of 30nm.

[0080] Effect detection

[0081] The above examples and comparative examples were tested using the following method:

[0082] Corrosion resistance: in neutral salt solution and acid solution (0.5MH 2 SO 4 +5ppm HF) was used for electrochemical corrosion test, and the potentiodynamic polarization curve was tested using a three-electrode system. The corrosion current density was deduced from the Tafel curve. The lower the corrosion current density, the better the corrosion resistance.

[0083] Conductivity: The interfacial contact resistance between the sample and the conductive carbon paper is tested by the voltammetry method. The sample is placed between two sheets of Toray conductive carbon paper and supported by a copper plate on the outermost side. During the test, the copper plate is uniformly pressurized to 1.4 MPa using a pressure device. The smaller the contact resistance, the better the conductivity.

[0084] Hydrophobicity: The optical contact measuring instrument and the optical analysis software that comes with the equipment measure the water contact angle. The larger the water contact angle, the better the hydrophobicity, the less likely the corrosive solution will adhere, and the better the corrosion resistance.

[0085] Table 1

[0086]

[0087] From the above Table 1 and Figure 4As a result, we can see that the present invention achieves high conductivity and corrosion resistance modification of the metal substrate surface with an ultra-thin coating. The ultra-thin coating can save a lot of production costs and production cycles in industrial production, and has practical prospects for industrial application.

[0088] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a highly conductive and corrosion-resistant composite coating, characterized in that: The following steps are involved: S1. Pre-treat the surface of the metal substrate, then clamp it in the vacuum chamber of the coating machine, and bake and exhaust it under vacuum; S2, performing ion beam cleaning on the metal substrate after baking exhaust; S3, performing nitriding treatment on the metal substrate after ion beam cleaning to form a nitriding layer on the surface of the metal substrate; wherein the thickness of the nitriding layer is 0.1-1 μm; S4, depositing pure metal and the nitride of the above metal on the surface of the metal substrate treated by S3 in sequence to form a base layer; wherein the total thickness of the base layer is 0.02-0.5 μm; S5, depositing two metals and nitrides of the two metals on the surface of the base layer formed in S4 in sequence to form an intermediate layer; wherein the total thickness of the intermediate layer is 0.02-1.5 μm; S6. Depositing a metal-doped TAC layer on the surface of the intermediate layer formed in S5 to obtain the highly conductive and corrosion-resistant composite coating, wherein the thickness of the metal-doped TAC layer is 0.03-1 μm, and the total thickness of the obtained composite coating is 0.17-3.5 μm.

2. The method for preparing a highly conductive and corrosion-resistant composite coating according to claim 1, characterized in that: In S1, the metal substrate surface is pre-treated, including the following steps: in a dust-free environment, the metal substrate is cleaned with detergent and deionized water in turn, and then ultrasonically cleaned in anhydrous ethanol; after cleaning, the metal substrate is placed in a depassivation film solution at 70-90° C. and soaked for 20-40 minutes; the metal substrate is ultrasonically cleaned in deionized water again, and then air-dried with nitrogen; during the baking exhaust process, the metal substrate is vacuumed to 1×10 -2 Pa, the baking temperature is 200-350°C, and the time is 30-120min; in S2, the following steps are specifically included: vacuuming to 7×10 -3 Pa and maintain the temperature at 200-350°C, start the turntable to rotate at a uniform speed, then fill with argon, the argon partial pressure is 0.2-0.8Pa, then turn on the ion source power supply and the turntable bias power supply, the ion source voltage is 200-1200V, the current is 0.5-2A, the turntable bias is 500-2000V, the bias current is 0.5-2A, the bias duty cycle is set to 50-80%, and the metal substrate surface is evenly cleaned for 20-180 minutes.

3. The method for preparing a highly conductive and corrosion-resistant composite coating according to claim 1, characterized in that: In S3, the following steps are specifically included: after ion beam cleaning, turn off the argon gas, maintain the temperature at 200-350°C, keep the rotating frame rotating at a constant speed, and evacuate to 7×10 -3 Pa, nitrogen is introduced to maintain the nitrogen partial pressure between 5-20Pa; then nitriding treatment is carried out. During the nitriding treatment, two sets of power supplies, DC power supply and AC power supply, are used. The AC rotary frame bias is 1200-2000V, the DC rotary frame voltage is 900-1500V, the AC rotary frame bias current is 3-7A, the DC rotary frame bias current is 3-7A, and the nitriding time is 30-120min to form a nitriding layer on the surface of the metal substrate.

4. The method for preparing a highly conductive and corrosion-resistant composite coating according to claim 1, characterized in that: In S4, the pure metal includes one metal or two metals; the one metal is one of Ti, Cr, Nb, Zr, and Ta; the two metals are one of Ni and Cr, or Al and Cr; the metal nitride is one of TiN, CrN, NbN, ZrN, TaN, NiCrN, and AlCrN; in S5, the deposited two metals are one of Cr and Mo, or Zr and Mo; the metal nitride is one of CrMoN and ZrMoN; in S6, the doped metal is one or more of Ti, Cr, and Zr.

5. The method for preparing a highly conductive and corrosion-resistant composite coating according to claim 1, characterized in that: In S4, the following steps are specifically included: turning off the nitrogen, turning off the bias voltage of the rotating frame, maintaining the temperature at 200-350°C, keeping the rotating frame rotating at a constant speed, and evacuating to 2×10 -3 Pa, fill with argon gas, the argon partial pressure is 0.1-3Pa, start magnetron sputtering of metal to form a metal base layer, set the sputtering power to 2-10KW, the turret bias to 100-300V, the turret bias duty cycle to 50-80%, the sputtering time to 5-40min, and complete the sputtering of the metal base layer; then introduce nitrogen gas to maintain the gas pressure at 0.1-3Pa, start magnetron sputtering of metal nitride to form a metal nitride base layer, set the sputtering power to 2-10KW, the turret bias to 100-300V, the turret bias duty cycle to 50-80%, the sputtering time to 5-120min, and complete the sputtering of the metal nitride base layer to form a base layer.

6. The method for preparing a highly conductive and corrosion-resistant composite coating according to claim 1, characterized in that: In S5, the following steps are specifically included: turning off the nitrogen, turning off the bias voltage of the rotating frame, maintaining the temperature at 200-350°C, keeping the rotating frame rotating at a constant speed, and evacuating the vacuum to 2×10 -3 Pa, fill with argon gas, the argon partial pressure is 0.1-3Pa, start co-sputtering of two metals to form a metal intermediate layer, set the metal target sputtering power to 1-10KW, the turret bias to 100-300V, the turret bias duty cycle to 50-80%, the sputtering time to 10-60min, and complete the co-sputtering of the metal intermediate layer; then introduce nitrogen gas to maintain the gas pressure at 0.1-3Pa, set the metal target sputtering power to 1-10KW, the turret bias to 100-300V, the turret bias duty cycle to 50-80%, the sputtering time to 10-120min, and complete the sputtering of the metal nitride intermediate layer.

7. The method for preparing a highly conductive and corrosion-resistant composite coating according to claim 1, characterized in that: In S6, the following steps are specifically included: turning off the nitrogen and argon gas, turning off the sputtering system and the heating system, waiting for the temperature to drop below 120°C, turning on the multi-arc ion plating system, and evacuating to 3×10 -4 Below Pa, multi-arc ion plating begins, with carbon target arc current of 50-150A, metal target arc current of 50-150A, turret bias of 100-2000V, and time of 5-60min.

8. The method for preparing a highly conductive and corrosion-resistant composite coating according to claim 1, characterized in that: S5 further includes repeatedly depositing two metals and nitrides of the two metals to form n intermediate layers; wherein n is less than or equal to 50.

9. The method for preparing a highly conductive and corrosion-resistant composite coating according to any one of claims 1 to 8, characterized in that: In S4, pure metal is deposited to form a metal base layer, the thickness of the metal base layer is 0.01-0.3μm, and metal nitride is deposited to form a metal nitride base layer, the thickness of the metal nitride base layer is 0.01-0.3μm; in S5, two metals are deposited to form a metal middle layer, the thickness of the metal middle layer is 0.01-0.5μm; two metal nitrides are deposited to form a metal nitride middle layer, the thickness of the metal nitride middle layer is 0.01-1μm.

10. A highly conductive and corrosion-resistant composite coating, characterized in that: The high-conductivity, corrosion-resistant composite coating is prepared by the preparation method of any one of claims 1 to 9.

Citation Information

Patent Citations

  • Multilayer multi-component compound hard PVD (Physical Vapor Deposition) plating layer on surface of piston ring, piston ring and preparation process

    CN103789725A

  • Mo metal doped composite diamond-like coating titanium alloy artificial bone joint and manufacturing method thereof

    CN103920185A

  • Preparation method of CrSiBCN nanocomposite film

    CN107988577A

  • Cr-doped ta-C conductive corrosion-resistant carbon-based thin film as well as preparation method and application thereof

    CN115044869A

  • Corrosion-resistant conductive coating as well as preparation method and application thereof

    CN116145080A

Cited By

  • High-density strong-insulation super-thick carbon-doped ceramic coating and preparation method thereof

    CN119615079A