Preparation method and application of fluorine-doped transition metal oxide hydrogen precipitation electrocatalyst

By using the fluorine-doped transition metal oxide BaCo0.4Fe0.4Zr0.1Y0.1O3-δ-0.5αFα as a hydrogen evolution electrocatalyst, the problem of scarcity and high cost of precious metal catalysts is solved, and high-efficiency hydrogen evolution performance and large-scale production are achieved. applicability, reducing the overpotential of the electrode and simplifying the preparation process.

CN118835271AActive Publication Date: 2024-10-25SOUTH CHINA UNIV OF TECH
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410861617.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-25
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

Existing hydrogen evolution catalysts mainly rely on precious metals, resulting in scarcity of raw materials, high prices, and difficulty in large-scale application. Impurities in hydrogen obtained through fossil fuel cracking are difficult to completely remove, increasing production costs and equipment damage risks.

Method used

The fluorine-doped transition metal oxide BaCo0.4Fe0.4Zr0.1Y0.1O3-δ-0.5αFα is used as the hydrogen evolution electrocatalyst. By regulating and activating the transition metal oxide lattice oxygen activity, the catalytic activity is improved, and through a simple preparation method A hydrogen evolution electrode suitable for large-scale production was prepared.

Benefits of technology

It achieves efficient hydrogen evolution performance, reduces the overpotential of the electrode, simplifies the preparation process, is suitable for large-scale production, and provides flexible electrode shapes and sizes, with universal applicability and efficient performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118835271A_ABST
    Figure CN118835271A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a fluorine-doped transition metal oxide hydrogen precipitation electrocatalyst. The chemical formula of the fluorine-doped transition metal oxide hydrogen precipitation electrocatalyst is BaCo < 0.4 > Fe < 0.4 > Zr < 0.1 > Y < 0.1 > O < 3-delta-0. 5 alpha > F < alpha >. The F element in the BaCo < 0.4 > Fe < 0.4 > Zr < 0.1 > Y < 0.1 > O < 3-delta-0. 5 alpha > F < alpha > electrocatalyst provided by the invention has higher electronegativity and is easier to capture electrons of oxygen sites, so that lattice oxygen is activated, formation of oxygen vacancies in the catalyst is promoted, active sites for hydrogen precipitation are increased, the catalytic activity of the catalyst is improved, and the overpotential of BaCo < 0.4 > Fe < 0.4 > Zr < 0.1 > Y < 0.1 > O < 2.925-deltaF < 0.15 > under 10mA / cm < 2 > is reduced by 71mV compared with that of BaCo < 0.4 > Fe < 0.4 > Zr < 0.1 > Y < 0.1 > O < 3-delta-0. 5 > F < 0.15 >.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of electrocatalytic materials, and in particular relates to a preparation method and application of a fluorine-doped transition metal oxide hydrogen evolution electrocatalyst. Background Art

[0002] At present, hydrogen, as the energy carrier with the highest energy density, has attracted much attention among many new energy raw materials. Hydrogen energy not only has high energy density, is clean and pollution-free, but also has a wide range of sources, and has broad prospects in the field of new energy development. At present, a major source of hydrogen is the cracking of fossil fuels such as petroleum. Its main disadvantages include limited raw materials, serious energy consumption in the preparation process, and low purity of the produced hydrogen. The biggest disadvantage is that the hydrogen obtained by cracking fossil fuels still contains impurities such as S and P, which need to be further desulfurized through subsequent complex processes, which not only increases the production cost, but also incomplete desulfurization can easily poison catalysts such as Pt in the hydrogen energy use device. The most ideal way to prepare hydrogen is to produce hydrogen through water electrolysis. On the one hand, the raw materials are simple and easy to obtain, and can be used on a large scale to convert scattered energy such as solar energy and wind energy into hydrogen energy for storage. On the other hand, the prepared hydrogen is pure, does not require further desulfurization, and the process is simple.

[0003] At present, the catalysts used for hydrogen evolution reaction are mainly precious metals and precious metal alloys, such as Pt and Pt alloys. However, the raw materials of this kind of precious metal-based catalysts are scarce, expensive, and easily poisoned, making them difficult to use on a large scale in practical applications. In recent years, many researchers have been committed to developing catalysts that do not contain precious metal elements. Among them, transition metal oxides have the advantages of low price and excellent performance and are considered to have great potential to compete with precious metals and become the preferred commercial catalyst for the next generation of HER. Summary of the invention

[0004] In order to overcome the deficiencies of the prior art, the present invention aims to provide a method for preparing and using a fluorine-doped transition metal oxide hydrogen evolution electrocatalyst.

[0005] The present invention firstly provides an electrocatalyst for hydrogen evolution reaction by regulating and activating the lattice oxygen activity of transition metal oxide by fluorine doping.

[0006] Another object of the present invention is to provide a method for preparing the above-mentioned hydrogen evolution electrocatalyst.

[0007] Another object of the present invention is to provide a hydrogen evolution electrode prepared by the above hydrogen evolution electrocatalyst.

[0008] The purpose of the present invention is achieved by at least one of the following technical solutions:

[0009] A fluorine-doped transition metal oxide hydrogen evolution electrocatalyst with the chemical formula BaCo0.4 Fe 0.4 Zr 0.1 Y 0.1 O 3-δ-0.5α F α , where δ is the oxygen defect stoichiometry, δ ranges from 0<δ<2, α is the F doping amount, α ranges from 0.01≤α≤0.5.

[0010] Preferably, the value range of α is 0.1≤α≤0.3.

[0011] The method for preparing the fluorine-doped transition metal oxide hydrogen evolution electrocatalyst comprises the following steps:

[0012] (1) mixing barium oxide, cobalt oxide, iron oxide, zirconium oxide, yttrium oxide, and yttrium fluoride powders according to a stoichiometric ratio, adding anhydrous ethanol to obtain a mixed solution, and then ball milling the mixed solution;

[0013] (2) heating the mixed solution after ball milling until the anhydrous ethanol is completely volatilized to obtain a mixed powder;

[0014] (3) grinding the mixed powder and calcining it at high temperature;

[0015] (4) ball milling the calcined powder to obtain a fluorine-doped transition metal oxide hydrogen evolution electrocatalyst.

[0016] Preferably, the volume ratio of liquid to solid in the mixed solution described in step (1) is 2:1 to 3:1;

[0017] Preferably, the ball milling time in step (1) is 5-15 hours;

[0018] Preferably, the rotation speed of the ball mill in step (1) is 800-1500 rpm;

[0019] Preferably, the heating in step (2) is performed under an infrared lamp; the heating temperature is 60-80°C.

[0020] Preferably, the calcination temperature in step (3) is 1000-1200°C;

[0021] Preferably, the calcination time in step (3) is 8-12 hours.

[0022] Preferably, the ball milling time in step (4) is 18-30 hours;

[0023] Preferably, the rotation speed of the ball mill in step (4) is 800-1500 rpm.

[0024] A hydrogen evolution electrode comprises the above-mentioned fluorine-doped transition metal oxide hydrogen evolution electrocatalyst (catalytically active material).

[0025] A method for preparing a hydrogen evolution electrode comprises the following steps:

[0026] (a) dispersing the fluorine-doped transition metal oxide hydrogen evolution electrocatalyst in a mixed solution of isopropanol, water and perfluorosulfonic acid resin, and subjecting the mixture to ultrasonic treatment to obtain a catalyst suspension;

[0027] (b) coating the catalyst suspension obtained in step (a) on the surface of carbon paper and drying at room temperature to obtain a hydrogen evolution electrode.

[0028] Preferably, the concentration of the fluorine-doped transition metal oxide hydrogen evolution electrocatalyst in the catalyst suspension in step (a) is 5 to 20 mg / mL; more preferably 10 mg / mL.

[0029] Preferably, the volume percentages of isopropanol, water and perfluorosulfonic acid resin calculated as 5 wt % of the dispersion in the mixed solution in step (a) are 10-80%, 10-80% and 5-20%;

[0030] Preferably, the ultrasonic treatment time in step (a) is 1 to 5 hours;

[0031] Preferably, the catalyst suspension in step (b) is coated on the carbon paper surface with a single-sided loading of 1 to 5 mg / cm 2 ;

[0032] Preferably, in step (b), both sides of the carbon paper surface are coated;

[0033] Preferably, the time of room temperature drying in step (b) is 6 to 36 hours.

[0034] A hydrogen evolution electrode is prepared by the above preparation method.

[0035] Application of the fluorine-doped transition metal oxide hydrogen evolution electrocatalyst or the hydrogen evolution electrode or the hydrogen evolution electrode prepared by the preparation method in hydrogen evolution reaction.

[0036] The principle of the present invention is: BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 3-δ-0.5α F α The F element in BaCo has a higher electronegativity and is more likely to capture electrons from oxygen sites, thereby activating lattice oxygen and promoting the formation of BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1O 3-δ-0.5α F α The formation of oxygen vacancies in the material increases the active sites for hydrogen evolution and improves the catalytic activity of the catalyst.

[0037] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0038] (1) BaCo provided by the present invention 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 3-δ-0.5α F α The electrocatalyst is synthesized by solid phase method, the preparation process is simple, and it is suitable for large-scale production.

[0039] (2) The carbon paper current collector used in the present invention can be prepared into electrodes of any shape and size, and has strong applicability in practical applications.

[0040] (3) The strategy of F doping to regulate the electrocatalytic activity of transition metal oxides proposed in the present invention is also applicable to other transition metal oxides. Various transition metal compound catalysts can be easily prepared according to needs, and are universal.

[0041] (4) BaCo provided by the present invention 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 3-δ-0.5α F α The catalyst has high efficiency in hydrogen evolution. 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 2.925-δ F 0.15 At 10mA / cm 2 Lower overpotential than BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 3-δ Reduced by 71mV. BRIEF DESCRIPTION OF THE DRAWINGS

[0042] Figure 1 The linear sweep voltammetry curves obtained in the comparative example and embodiment 1 are shown in FIG.

[0043] Figure 2 1 is the X-ray diffraction pattern of the electrocatalyst obtained in the comparative example and example 1.

[0044] Figure 3 The XPS O1s spectra of the electrocatalysts obtained in the comparative example and example 1.

[0045] Figure 4 The linear sweep voltammetry curves obtained in the comparative example and example 2 are shown in FIG.

[0046] Figure 5 The linear sweep voltammetry curves obtained in the comparative example and embodiment 3 are shown in FIG. DETAILED DESCRIPTION

[0047] The specific implementation of the present invention is further described below in conjunction with the accompanying drawings and examples, but the implementation and protection of the present invention are not limited thereto. It should be noted that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art. If the manufacturer of the reagents or instruments used is not indicated, they are deemed to be conventional products that can be purchased commercially.

[0048] Comparative Example:

[0049] This comparative example provides a hydrogen evolution electrocatalyst BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 3-δ , the preparation method comprises the following steps:

[0050] 1. Mix barium oxide, cobalt oxide, iron oxide, zirconium oxide, and yttrium oxide powders according to a stoichiometric ratio, and add anhydrous ethanol to obtain a mixed solution, in which the volume ratio of liquid to solid in the mixed solution is 2: 1. Then the mixed solution is ball-milled for 10 hours at a ball-milling speed of 1200 rpm.

[0051] 2. The mixed solution after ball milling is placed under an infrared lamp and heated at 70°C until the anhydrous ethanol is completely evaporated to obtain a mixed powder.

[0052] 3. After grinding the above mixed powder, put it into a muffle furnace for high-temperature calcination at a temperature of 1200°C and a calcination time of 10 hours.

[0053] 4. The calcined powder was ball-milled for 24 h at a speed of 1200 rpm to obtain BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 3-δ Electrocatalyst.

[0054] The X-ray diffraction pattern of the electrocatalyst obtained in the comparative example is as follows Figure 2 , XPS O1s spectrum as Figure 3 .

[0055] In addition, this comparative example provides a hydrogen evolution electrode, and the preparation method comprises the following steps:

[0056] 1. Catalytically active material BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 3-δ Dispersed in a mixed solution of isopropanol, ultrapure water and perfluorosulfonic acid resin, the concentration of the catalytically active material is 10 mg / mL, and the volume percentages of isopropanol, ultrapure water and perfluorosulfonic acid resin (calculated based on a 5wt% dispersion) are 45%, 45% and 10%. The mixed solution is then subjected to ultrasonic treatment for 2 hours to obtain a catalyst suspension.

[0057] 2. Apply the obtained catalyst suspension on the surface of carbon paper (double-sided coating), with a single-sided loading of 2 mg / cm 2 The mixture was dried at room temperature for 24 hours to obtain a hydrogen evolution electrode.

[0058] In this comparative example, the obtained hydrogen evolution electrode was tested for its catalytic activity. Test conditions: a standard three-electrode system was used as the test system, the obtained catalyst material was used as the working electrode, saturated Ag / AgCl was used as the reference electrode, a graphite rod was used as the counter electrode, and 1 mol L -1 The KOH solution was used as the electrolyte and the test instrument was Shanghai Chenhua 660E electrochemical workstation. The linear sweep voltammetric curve was tested at room temperature of 25°C. The obtained linear sweep voltammetric curve is shown in Figure 1 shown.

[0059] Embodiment 1:

[0060] This embodiment provides a hydrogen evolution electrocatalyst BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 2.95-δ F 0.1 , the preparation method comprises the following steps:

[0061] 1. Mix barium oxide, cobalt oxide, iron oxide, zirconium oxide, yttrium oxide, and yttrium fluoride powders according to a stoichiometric ratio, and add anhydrous ethanol to obtain a mixed solution, in which the volume ratio of liquid to solid in the mixed solution is 2: 1. Then the mixed solution is ball-milled for 10 hours at a ball-milling speed of 1200 rpm.

[0062] 2. The mixed solution after ball milling is placed under an infrared lamp and heated at 70°C until the anhydrous ethanol is completely evaporated to obtain a mixed powder.

[0063] 3. After grinding the above mixed powder, put it into a muffle furnace for high-temperature calcination at a temperature of 1200°C and a calcination time of 10 hours.

[0064] 4. The calcined powder was ball-milled for 24 h at a speed of 1200 rpm to obtain BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 2.95-δ F 0.1 Electrocatalyst.

[0065] The X-ray diffraction pattern of the electrocatalyst obtained in Example 1 is as follows: Figure 2 , XPS O1s spectrum as Figure 3 .

[0066] In addition, this embodiment provides a hydrogen evolution electrode, and the preparation method includes the following steps:

[0067] 1. Catalytically active material BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 2.95-δ F 0.1 Dispersed in a mixed solution of isopropanol, ultrapure water and perfluorosulfonic acid resin, the concentration of the catalytically active material is 10 mg / mL, and the volume percentages of isopropanol, ultrapure water and perfluorosulfonic acid resin (calculated based on a 5wt% dispersion) are 45%, 45% and 10%. The mixed solution is then subjected to ultrasonic treatment for 2 hours to obtain a catalyst suspension.

[0068] 2. Apply the obtained catalyst suspension on the surface of carbon paper (double-sided coating), with a single-sided loading of 2 mg / cm 2 The mixture was dried at room temperature for 24 hours to obtain a hydrogen evolution electrode.

[0069] In this example, the obtained hydrogen evolution electrode was tested for its catalytic activity. Test conditions: a standard three-electrode system was used as the test system, the obtained catalyst material was used as the working electrode, saturated Ag / AgCl was used as the reference electrode, a graphite rod was used as the counter electrode, and 1 mol L -1 The KOH solution was used as the electrolyte and the test instrument was Shanghai Chenhua 660E electrochemical workstation. The linear sweep voltammetric curve was tested at room temperature of 25°C. The obtained linear sweep voltammetric curve is shown in Figure 1 shown.

[0070] Embodiment 2:

[0071] This embodiment provides a hydrogen evolution electrocatalyst BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 2.925-δ F 0.15, the preparation method comprises the following steps:

[0072] 1. Mix barium oxide, cobalt oxide, iron oxide, zirconium oxide, yttrium oxide, and yttrium fluoride powders according to a stoichiometric ratio, and add anhydrous ethanol to obtain a mixed solution, in which the volume ratio of liquid to solid in the mixed solution is 2: 1. Then the mixed solution is ball-milled for 12 hours at a ball-milling speed of 1000 rpm.

[0073] 2. The mixed solution after ball milling is placed under an infrared lamp and heated at 70°C until the anhydrous ethanol is completely evaporated to obtain a mixed powder.

[0074] 3. After grinding the above mixed powder, put it into a muffle furnace for high-temperature calcination at a temperature of 1100°C and a calcination time of 12 hours.

[0075] 4. The calcined powder was ball-milled for 30 h at a speed of 1000 rpm to obtain BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 2.925-δ F 0.15 Electrocatalyst.

[0076] In addition, this embodiment provides a hydrogen evolution electrode, and the preparation method includes the following steps:

[0077] 1. Catalytically active material BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 2.925-δ F 0.15 Dispersed in a mixed solution of isopropanol, ultrapure water and perfluorosulfonic acid resin, the concentration of the catalytically active material is 10 mg / mL, and the volume percentages of isopropanol, ultrapure water and perfluorosulfonic acid resin (calculated based on a 5wt% dispersion) are 45%, 45% and 10%. The mixed solution is then subjected to ultrasonic treatment for 2 hours to obtain a catalyst suspension.

[0078] 2. Apply the obtained catalyst suspension on the surface of carbon paper (double-sided coating), with a single-sided loading of 2 mg / cm 2 The mixture was dried at room temperature for 24 hours to obtain a hydrogen evolution electrode.

[0079] In this example, the obtained hydrogen evolution electrode was tested for its catalytic activity. Test conditions: a standard three-electrode system was used as the test system, the obtained catalyst material was used as the working electrode, saturated Ag / AgCl was used as the reference electrode, a graphite rod was used as the counter electrode, and 1 mol L -1The KOH solution was used as the electrolyte and the test instrument was Shanghai Chenhua 660E electrochemical workstation. The linear sweep voltammetric curve was tested at room temperature of 25°C. The obtained linear sweep voltammetric curve is shown in Figure 4 shown.

[0080] Embodiment 3:

[0081] This embodiment provides a hydrogen evolution electrocatalyst BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 2.85-δ F 0.3 , the preparation method comprises the following steps:

[0082] 1. Mix barium oxide, cobalt oxide, iron oxide, zirconium oxide, yttrium oxide, and yttrium fluoride powders according to a stoichiometric ratio, and add anhydrous ethanol to obtain a mixed solution, in which the volume ratio of liquid to solid in the mixed solution is 2: 1. Then the mixed solution is ball-milled for 12 hours at a ball-milling speed of 1200 rpm.

[0083] 2. The mixed solution after ball milling is placed under an infrared lamp and heated at 70°C until the anhydrous ethanol is completely evaporated to obtain a mixed powder.

[0084] 3. Grind the above mixed powder and put it into a muffle furnace for high-temperature calcination at a temperature of 1200°C for 8 hours.

[0085] 4. The calcined powder was ball-milled for 20 h at a speed of 1500 rpm to obtain BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 2.85-δ F 0.3 Electrocatalyst.

[0086] In addition, this embodiment provides a hydrogen evolution electrode, and the preparation method includes the following steps:

[0087] 1. Catalytically active material BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 2.85-δ F 0.3 Dispersed in a mixed solution of isopropanol, ultrapure water and perfluorosulfonic acid resin, the concentration of the catalytically active material is 10 mg / mL, and the volume percentages of isopropanol, ultrapure water and perfluorosulfonic acid resin (calculated based on a 5wt% dispersion) are 45%, 45% and 10%. The mixed solution is then subjected to ultrasonic treatment for 2 hours to obtain a catalyst suspension.

[0088] 2. Apply the obtained catalyst suspension on the surface of carbon paper (double-sided coating), with a single-sided loading of 2 mg / cm 2 The mixture was dried at room temperature for 24 hours to obtain a hydrogen evolution electrode.

[0089] In this example, the obtained hydrogen evolution electrode was tested for its catalytic activity. Test conditions: a standard three-electrode system was used as the test system, the obtained catalyst material was used as the working electrode, saturated Ag / AgCl was used as the reference electrode, a graphite rod was used as the counter electrode, and 1 mol L -1 The KOH solution was used as the electrolyte and the test instrument was Shanghai Chenhua 660E electrochemical workstation. The linear sweep voltammetric curve was tested at room temperature of 25°C. The obtained linear sweep voltammetric curve is shown in Figure 5 shown.

[0090] Data Analysis:

[0091] The X-ray diffraction patterns of the electrocatalysts obtained in the comparative example and Example 1 are as follows: Figure 2 , XPS O1s spectrum as Figure 3 .

[0092] like Figure 2 As shown, the BaCo obtained in Example 1 and the comparative example 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 3-δ Compared with the electrocatalyst, the BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 2.95-δ F 0.1 The X-ray diffraction pattern of the electrocatalyst shifts significantly toward high angles, indicating that BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 2.95-δ F 0.1 The electrocatalyst has a smaller lattice. In addition, Figure 3 As shown, the BaCo obtained in Example 1 and the comparative example 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 3-δ Compared with the electrocatalyst, the BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 2.95-δ F 0.1The lattice oxygen signal in the O1s XPS spectrum of the electrocatalyst is lower, indicating that BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 2.95-δ F 0.1 The lattice oxygen of the electrocatalyst is activated because the F element has a higher electronegativity and is more likely to capture electrons from the oxygen site, thereby activating the lattice oxygen and promoting the BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 3-δ-0.5α F α Formation of oxygen vacancies in materials.

[0093] The linear sweep voltammetric curves of Examples 1-3 and Comparative Examples are as follows: Figure 1 , Figure 4 , Figure 5 ; Overpotentials are shown in Table 1.

[0094] As shown in Table 1, the electrocatalysts obtained in the comparative example, example 1, example 2 and example 3 have a conductivity of 10 mA / cm 2 The overpotentials at the current density are 320mV, 275mV, 249mV and 300mV respectively. 2 The overpotentials at the current density were 452 mV, 351 mV, 330 mV and 377 mV respectively. 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 3-δ-0.5α F α The electrocatalyst exhibited a lower overpotential of 10 mA / cm 2 The overpotentials at the current density decreased by 45mV, 71mV and 20mV respectively. 2 The overpotentials at the current densities decreased by 101mV, 122mV, and 75mV, respectively.

[0095] Table 1. Electrocatalysts obtained in comparative examples and examples at 10 mA / cm 2 and 100mA / cm 2 Overpotential at current density

[0096] <![CDATA[10mA / cm 2 Overpotential]]> <![CDATA[100mA / cm 2 Overpotential]]> Comparative Example 320mV 452mV Example 1 275mV 351mV Example 2 249mV 330mV Example 3 300mV 377mV

[0097] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications made without departing from the spirit and principle of the present invention shall be equivalent replacement modes and shall be included in the protection scope of the present invention.

Claims

1. A fluorine-doped transition metal oxide hydrogen evolution electrocatalyst, characterized in that: The chemical formula is BaCo 0.4 Fe 0.4 Zr 0.1 Y 0.1 O 3-δ-0.5α F α , where δ is the oxygen defect stoichiometry, δ ranges from 0<δ<2, α is the F doping amount, α ranges from 0.01≤α≤0.

5.

2. The fluorine-doped transition metal oxide hydrogen evolution electrocatalyst according to claim 1, characterized in that The value range of α is 0.1≤α≤0.

3.

3. The method for preparing the fluorine-doped transition metal oxide hydrogen evolution electrocatalyst according to any one of claims 1 to 2, characterized in that: The steps include: (1) mixing barium oxide, cobalt oxide, iron oxide, zirconium oxide, yttrium oxide, and yttrium fluoride powders according to a stoichiometric ratio, adding anhydrous ethanol to obtain a mixed solution, and then ball milling the mixed solution; (2) heating the mixed solution after ball milling until the anhydrous ethanol is completely volatilized to obtain a mixed powder; (3) grinding the mixed powder and calcining it at high temperature; (4) ball milling the calcined powder to obtain a fluorine-doped transition metal oxide hydrogen evolution electrocatalyst.

4. The method for preparing the fluorine-doped transition metal oxide hydrogen evolution electrocatalyst according to claim 3, characterized in that: The volume ratio of liquid to solid in the mixed solution described in step (1) is 2:1 to 3:1; The ball milling time in step (1) is 5-15 hours; The rotation speed of the ball mill in step (1) is 800-1500 rpm; The heating in step (2) is performed under an infrared lamp; the heating temperature is 60-80°C.

5. The method for preparing the fluorine-doped transition metal oxide hydrogen evolution electrocatalyst according to claim 3, characterized in that: The calcination temperature in step (3) is 1000-1200°C; The calcination time in step (3) is 8-12 hours.

6. The method for preparing the fluorine-doped transition metal oxide hydrogen evolution electrocatalyst according to claim 3, characterized in that: The ball milling time in step (4) is 18-30 hours; The rotation speed of the ball mill described in step (4) is 800-1500rpm.

7. A hydrogen evolution electrode, characterized in that The invention comprises the fluorine-doped transition metal oxide hydrogen evolution electrocatalyst as described in any one of claims 1 to 2.

8. A method for preparing a hydrogen evolution electrode, characterized in that: The steps include: (a) dispersing the fluorine-doped transition metal oxide hydrogen evolution electrocatalyst according to any one of claims 1 to 2 in a mixed solution of isopropanol, water and perfluorosulfonic acid resin, and subjecting the mixture to ultrasonic treatment to obtain a catalyst suspension; (b) coating the catalyst suspension obtained in step (a) on the surface of carbon paper and drying at room temperature to obtain a hydrogen evolution electrode.

9. The method for preparing a hydrogen evolution electrode according to claim 8, characterized in that: The concentration of the fluorine-doped transition metal oxide hydrogen evolution electrocatalyst in the catalyst suspension in step (a) is 5 to 20 mg / mL; The volume percentages of isopropanol, water and perfluorosulfonic acid resin calculated as 5wt% of the dispersion in the mixed solution of step (a) are 10-80%, 10-80% and 5-20%; The ultrasonic treatment time in step (a) is 1 to 5 hours; The catalyst suspension in step (b) is coated on the carbon paper surface with a single-sided loading of 1 to 5 mg / cm 2 ; The carbon paper surface in step (b) is coated on both sides; The time of room temperature drying in step (b) is 6 to 36 hours.

10. Use of the fluorine-doped transition metal oxide hydrogen evolution electrocatalyst according to any one of claims 1 to 2, the hydrogen evolution electrode according to claim 7, or the hydrogen evolution electrode prepared by the preparation method according to any one of claims 8 to 9 in a hydrogen evolution reaction.

Citation Information

Patent Citations

  • Cation co-doped perovskite catalyst for oxygen evolution reaction and preparation method thereof

    CN110860292A

  • Fluorine-doped non-noble metal electrocatalyst as well as preparation method and application thereof

    CN115522223A

  • High-entropy perovskite electrolyte, preparation method and application thereof, and battery

    CN115692806A