Core-shell structure PBO aerogel fiber and preparation method thereof
By imitating the core-shell structure of reindeer hair and using wet spinning technology to prepare PBO airgel fibers, it solves the problems of insufficient mechanical properties and thermal insulation properties of existing airgel fibers and achieves the effects of high-temperature insulation and low-temperature insulation. , and significantly improved the mechanical properties of composite materials with PDMS.
Patent Information
- Application Number
- CN202411083623.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-10-25
AI Technical Summary
Existing airgel fibers have deficiencies in mechanical properties and thermal insulation properties, and bulk airgel lacks flexibility and scalability, resulting in limited practical applications.
Drawing on the core-shell structure and function of reindeer hair, using poly-paraphenylene benzobisoxazole (PBO) as the basic unit, PBO aerogel fibers with core-shell structure were prepared through wet spinning technology, and were imitated using specific processing techniques. The morphological structure of reindeer hair forms excellent mechanical properties and thermal insulation properties.
Successfully prepared PBO airgel fibers with excellent mechanical properties and high-temperature insulation effects, which can provide effective insulation in extremely low-temperature environments. After compounding with PDMS, the strength is increased by 25 times, and the elongation reaches 195%. It has huge aerospace applications. and automotive application potential.
Smart Images

Figure CN118835337A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of aerogel preparation, and in particular to a core-shell structured PBO aerogel fiber and a preparation method thereof. Background Art
[0002] Due to its excellent high strength and chemical inertness, PBO has long been limited in its application in composite materials and other fields. At present, PBO is mainly used in the field of composite materials for thermal conductivity, thermal insulation, flame retardancy, radio frequency and other applications. In the thermal conductivity and flame retardancy application scenarios, researchers prepared a composite nanofilm with high thermal conductivity and electrical insulation properties by adding a low mass fraction of functionalized boron nitride nanosheets (BNNSs) to PBO. This nanofilm has a robust interconnected network structure, giving it a pearl-like structure, giving it a high thermal conductivity (21.34 Wm -1 K -1 ) and high strength (206MPa). On the other hand, the researchers also coupled well-oriented graphite nanosheets with PBO three-dimensional nanofiber networks to form modified graphite films. This modified graphite film not only has excellent mechanical properties, such as significant improvements in tensile strength, fracture strain, toughness and folding endurance, but also has excellent thermal conductivity (104.5-179.8Wm -1 K -1 ) and thermal stability (652℃). Compared with the unmodified pure graphite film, the performance of the modified graphite film is significantly improved, showing higher mechanical properties and thermal conductivity, even exceeding that of 7075 aluminum alloy. In the field of radio frequency applications, researchers made PBO into nanofiber paper and combined it with polytetrafluoroethylene (PTFE) to create a nanocomposite paper with excellent performance. This nanocomposite paper exhibited high tensile strength (271.6MPa), folding durability, superhydrophobicity and self-cleaning properties. In addition, the low dielectric constant (ε) and dielectric loss (δ) characteristics of PBO materials are used to make nanofiber paper with a low dielectric constant (2.1) and dielectric loss tangent (0.0133). When transmitting electromagnetic waves, the transmittances on both sides of the paper were 97.6% and 96.0%, respectively, showing that nanocomposite paper has great potential in wave-transmitting applications.
[0003] PBO has also gradually emerged in the field of aerogel insulation. However, due to the shortcomings of block aerogels such as lack of flexibility, scalability, low sol-gel conversion process and fragile network structure, its practical application is widely restricted. Summary of the invention
[0004] In view of the shortcomings of existing aerogel fibers in terms of mechanical properties and thermal insulation properties, the present invention draws on the structure and function of animal hair in nature, especially the excellent thermal insulation performance provided by reindeer hair in extreme environments. Based on this, the morphological structure of the aerogel fiber is designed to imitate the core-shell structure and function of reindeer hair. By selecting poly(p-phenylene benzobisoxazole) (PBO) with excellent performance as the primitive, an aerogel fiber tissue structure with excellent mechanical properties and thermal insulation properties is constructed, and through a specific processing technology, the bionic preparation of reindeer hair is achieved.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] The first aspect of the present invention provides a method for preparing a core-shell structured PBO aerogel fiber, comprising the following steps:
[0007] (1) PBO, MSA (methanesulfonic acid), and TFA (trifluoroacetic acid) are mixed and stirred to obtain a precursor solution;
[0008] (2) extruding the precursor solution into water through a dispensing needle to obtain a wet gel;
[0009] (3) placing the wet gel in ethanol, replacing the ethanol at regular intervals to remove MSA and TFA in the fiber; and then drying the fiber to obtain the core-shell structured PBO aerogel fiber.
[0010] During the wet spinning process, when the PBO solution comes into contact with the non-solvent (water), phase separation occurs rapidly at the interface, forming a dense fiber surface. Subsequently, the solvent continues to diffuse, the outer shell gradually thickens, and a cross-linked network structure is formed inside the fiber.
[0011] Preferably, in step (1), the concentration of PBO in the precursor solution is 0.5-1.5 wt %.
[0012] Preferably, in step (1), the mass ratio of MSA to TFA is (0.25-4):1; in some preferred embodiments of the present invention, the mass ratio of MSA to TFA is 4:1. When the MSA / TFA ratio is 4:1, the fiber exhibits the best comprehensive mechanical properties, including the highest breaking strength (12.1 MPa), the maximum elongation (105.1%) and the best toughness (3.5 MJ / m 3 ).
[0013] Preferably, in step (2), the temperature of the water is 0-60°C; the temperature of the non-solvent (water) has a significant effect on the micromorphology, multi-level pore structure and mechanical properties of the fiber. Higher temperatures (60°C) will accelerate the movement of molecular chains and the diffusion of solvents, causing the fibers to shrink and deform, forming large-scale irregular wrinkles, and promoting the formation of a developed mesoporous structure, thereby increasing the specific surface area and adsorption capacity. However, excessively high temperatures will also cause the fiber shell to become thinner, reducing tensile strength and elongation at break. In contrast, lower temperatures (0°C) are conducive to the formation of a thicker fiber shell, thereby significantly improving tensile strength (12.2MPa) and elongation at break (144.6%), while also helping to increase modulus (29.5MPa) and toughness (9.0MJ / m 3 ). This shows that by regulating the non-solvent temperature, the structure and mechanical properties of the fiber can be finely controlled.
[0014] Preferably, in step (2), the precursor solution is extruded into water through a 25G dispensing needle at a speed of 400 to 600 μl / min.
[0015] Preferably, in step (3), the wet gel is placed in ethanol, and the ethanol is replaced every 6 to 10 hours, for a total of 3 to 5 times.
[0016] Preferably, in step (3), the drying method is freeze drying or supercritical carbon dioxide drying.
[0017] Further preferably, in step (3), the drying method is carbon dioxide supercritical drying; the drying conditions are 30-55° C., 7.4-16 MPa, and drying for 3-5 hours.
[0018] The second aspect of the present invention provides a core-shell structured PBO aerogel fiber, which is prepared by the preparation method of the core-shell structured PBO aerogel fiber.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] PBO aerogel fibers were successfully prepared by wet spinning, and a unique core-shell structure was obtained. After forming a composite fabric, PBO aerogel fibers can not only provide excellent high-temperature thermal insulation, but also provide effective thermal insulation in extreme low-temperature environments. The composite material obtained by compounding PBO fibers with PDMS is 25 times stronger than pure PDMS, with an elongation of up to 195%, and has great application potential in aerospace, automotive and other fields. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a morphology characterization diagram of aerogel fibers supercritically dried and freeze-dried with carbon dioxide in Example 1;
[0022] Figure 2 The internal pore size distribution diagram of the aerogel fibers freeze-dried and carbon dioxide supercritically dried in Example 1;
[0023] Figure 3 is a stress-strain curve diagram of aerogel fibers obtained by supercritical drying in Example 1;
[0024] Figure 4 This is a morphology characterization diagram of the aerogel fiber of Example 2;
[0025] Figure 5 is the internal pore size distribution diagram of Example 2;
[0026] Figure 6 is a stress-strain curve diagram of the aerogel fiber of Example 2;
[0027] Figure 7 The morphology of aerogel fibers prepared at different ratios of MSA / TFA in Example 3;
[0028] Figure 8 This is a diagram of the mechanical properties of the aerogel fiber prepared in Example 3;
[0029] Fig. 9 is a scanning electron microscope image of aerogel fibers at different non-solvent temperatures in Example 3;
[0030] Fig.10 are the BET adsorption isotherms and corresponding pore size distribution curves of the aerogel fibers at different non-solvent temperatures in Example 3;
[0031] Fig.11 The mechanical properties of aerogel fibers at different non-solvent temperatures in Example 3;
[0032] Fig.12 This is a performance comparison chart of the aerogel fiber prepared in Example 3 and other materials;
[0033] Fig.13 This is a flame retardant performance test diagram of aerogel fiber under a butane flame gun;
[0034] Fig.14 is the temperature-time curve of aerogel fiber on the hot stage;
[0035] Fig.15 This is a test diagram of thermal insulation and heat preservation of composite fabrics made by combining aerogel fibers with traditional sweater materials;
[0036] Fig.16 This is the stress-strain curve of pure PDMS and PBO composite. DETAILED DESCRIPTION
[0037] The specific embodiments of the present invention are further described below. It should be noted that the description of these embodiments is used to help understand the present invention, but does not constitute a limitation of the present invention. In addition, the technical features involved in each embodiment of the present invention described below can be combined with each other as long as they do not conflict with each other.
[0038] The experimental methods in the following examples are conventional methods unless otherwise specified, and the experimental materials used in the following examples are commercially available unless otherwise specified.
[0039] Example 1
[0040] The specific steps of preparing aerogel fibers using sulfuric acid as solvent are as follows:
[0041] (1) Precursor preparation: 150 mg of PBO was mixed with 19.85 g of H2SO4 and stirred in an oil bath at 150°C for 3 hours to obtain a PBO / H2SO4 precursor solution with a mass fraction of 0.75 wt%.
[0042] (2) Wet spinning: The precursor solution obtained in the above process is extracted into a syringe and extruded from a 15G dispensing needle into a non-solvent (0°C) at a rate of 2 ml / min using a syringe pump. After the solvent is completely exchanged, a wet gel is obtained. In order to maintain the fiber surface morphology, ethylene glycol is selected as a non-solvent to slow down the exchange rate of the fiber solvent and maintain the internal skeleton structure of the fiber.
[0043] (3) Preparation before drying: The wet gel was placed in ethanol and deionized water, respectively, and replaced every 8 hours for a total of 4 times to remove ethylene glycol and sulfuric acid from the fiber.
[0044] (4) Drying: 1) Supercritical drying: The fiber obtained by ethanol exchange is placed in a supercritical dryer and dried at 50°C and 15.0MPa for 4 hours. During the drying process, a magnetic stirrer is used to continuously stir the liquid carbon dioxide in the sealed chamber at a speed of 500rpm, and the exhaust is carried out at a rate of 200ml / min. Water is used for absorption and filtration at the exhaust end. 2) Freeze drying: The fiber obtained by deionized water exchange is frozen at -20°C for 10 hours, and then the fiber is placed in a freeze dryer and freeze-dried at -50°C and 0.05mbar for 24 hours.
[0045] Characterization of aerogel fibers using two different drying techniques: supercritical carbon dioxide drying and freeze drying. Figure 1As shown, ad is the image obtained by supercritical drying of carbon dioxide, and eh is the image obtained by freeze drying. During the supercritical drying process, the optical image of the aerogel fiber (a) shows that the curl is high and tightly distributed, and the smoothness of its surface is confirmed in the SEM image (bd). There are fewer surface defects and a uniform three-dimensional PBO nanofiber network inside. This uniform structure is extremely critical to strengthening the overall mechanical properties of the fiber, which means that the internal stress is more evenly distributed, thereby improving the material's resistance to fracture and deformation. In addition, the uniform pore size is also conducive to achieving stable and efficient thermal and sound insulation performance. The structure can effectively scatter and absorb energy.
[0046] In contrast, the freeze-dried samples show a significant difference between the fiber and block structures in the optical image (e), which is not only uneven in morphology, but also chaotic in arrangement. The SEM images (fh) further reveal a more complex microscopic scene, in which the surface roughness increases significantly, and the distribution of holes is not only uneven, but also varies in size, reflecting the internal structure rupture and deformation caused by ice crystal growth and sublimation during the freeze-drying process. These irregular holes may cause inconsistencies in mechanical properties, making the material prone to local damage when subjected to external forces. Although freeze-drying may be simpler and more cost-effective in operation, from the perspective of material properties, supercritical drying provides an effective way to prepare aerogel fibers with highly uniform microstructures and superior physical properties.
[0047] Figure 2 The internal pore size distribution of aerogel fibers obtained by freeze drying and supercritical carbon dioxide drying technology was compared and analyzed. Figure 2 (a) shows the internal diameter distribution of freeze-dried aerogel fibers, showing a wide distribution range (50-210nm), which reflects a loose and irregular pore structure. This is consistent with the previous optical and SEM image analysis, indicating that the uneven freezing that may occur during the freeze-drying process and the changes in the internal structure caused by the growth and sublimation of ice crystals. In contrast, Figure 2 The internal diameter statistics of the carbon dioxide supercritical dried aerogel fibers shown in (b) present a peak distribution, indicating a relatively uniform pore size. Such uniformity indicates that the supercritical drying process can better maintain the consistency of the pore structure and the integrity of the fiber. This is because the rapid removal of the solvent under supercritical conditions reduces the capillary force inside the material, thereby avoiding large-scale deformation and damage to the structure. Aerogel fibers with more uniform and predictable physical properties may exhibit superior mechanical stability and thermal and acoustic insulation properties. These characteristics make aerogel fibers obtained by supercritical drying have potential advantages in industrial applications.
[0048] The stress-strain curve of aerogel fibers obtained by supercritical drying is shown in Figure 3 As shown, by analyzing the initial linear region from 0 to 2%, the elastic modulus of the fibers is calculated to be between 0.35 and 0.56 MPa, which indicates that the material has a relatively weak resistance to initial elastic deformation. Due to the lack of a clear yield point on the curve, the 0.2% offset method was used to estimate the yield strength. The calculated results show a low yield strength, indicating that these fibers quickly transition from elastic deformation to plastic deformation with almost no obvious yield process, which is a typical feature of high fracture strain fibers. The ultimate tensile strength (UTS) of the fibers ranges from 0.4 to 0.58 MPa, and the relatively low UTS values suggest that the fibers have limited load-bearing capacity under high loads. Nevertheless, the samples can reach a maximum fracture strain of 20%, showing significant ductility and significant elongation before fracture.
[0049] By calculating the area under the stress-strain curve, the toughness of PBO aerogel fibers is between 2.18 and 3.18 MJ / m 3 This indicates that the fiber has the ability to absorb a large amount of energy before breaking. The mechanical response between samples is consistent, and the slight differences between curves may be due to inherent differences in the materials or slight changes in experimental conditions. This consistency and repeatability confirms the reliability of the obtained mechanical properties data.
[0050] Example 2
[0051] The experimental steps for preparing aerogel fibers using sulfuric acid as the solvent system are as follows:
[0052] (1) Precursor preparation: 150 mg of PBO was mixed with 19.85 g of sulfuric acid, placed in a 150° C. oil bath and stirred for 3 hours to form a 0.75 wt % PBO / H 2 SO 4 solution.
[0053] (2) Wet spinning: The precursor solution was extruded through a 15G dispensing needle at a rate of 2 ml / min using a syringe pump and entered into ethylene glycol at 30 °C. After the solvent was completely exchanged, a wet gel was obtained.
[0054] (3) Preparation before drying: Soak the wet gel in ethanol, changing the ethanol every 8 hours for 32 hours to remove the ethylene glycol and sulfuric acid in the fiber.
[0055] (4) Supercritical drying: The fiber was placed in a supercritical dryer and dried at 50°C and 15 MPa for 4 hours. During the drying process, a magnetic stirrer was used to continuously stir the liquid carbon dioxide in the sealed chamber at a speed of 500 rpm, and exhaust was performed at a speed of 200 ml / min.
[0056] The experimental steps for preparing aerogel fibers using MSA / TFA as the solvent system are as follows:
[0057] (1) Precursor preparation: A mixture of 225 mg PBO and 29.7 g MSA / TFA was stirred at room temperature for 5 hours to form a 0.75 wt% precursor solution. The mass ratio of MSA to TFA was adjusted to 1:1.
[0058] (2) Wet spinning: The spinning solution was extruded into 30°C water at a speed of 500 μl / min through a 25G dispensing needle using a syringe pump. After the solvent was completely exchanged, a wet gel was obtained.
[0059] (3) Preparation before drying: Place the wet gel in ethanol and change it every 8 hours for a total of 4 times to remove MSA / TFA from the fibers.
[0060] (4) Supercritical drying: The fiber was placed in a supercritical dryer and dried at 50°C and 15.0 MPa for 4 hours. During the drying process, a magnetic stirrer was used to continuously stir the liquid carbon dioxide in the sealed chamber at a speed of 500 rpm, and exhaust was performed at a speed of 200 ml / min.
[0061] The morphology of aerogel fibers with a solvent ratio of MSA / TFA of 1:1 is shown in Figure 4 As shown in ad, the morphology of aerogel fibers using sulfuric acid as solvent is characterized as follows Figure 4 eh. The aerogel fibers prepared in the MSA / TFA system appear as uniform and continuous yellow transparent fiber bundles in the optical image (Figure a). In addition, the cross-section (Figure c) and magnified image (Figure d) of the fiber reveal a uniformly distributed microporous structure with basically regular pore shapes and relatively uniform pore size distribution. This indicates that the gelation process under the MSA / TFA system is more stable and the formation of gel pores is well controlled.
[0062] In contrast, the aerogel fibers prepared in the sulfuric acid system (Figure eh) also appear as yellow fiber bundles in the optical image (Figure e), but their surface structure (Figure f) is obviously rough and shows more bumps. This may be due to the stronger solvent effect in the sulfuric acid system, which causes the polymer chains to be more disturbed during the gelation process, thus forming a rough surface structure. The pore structure in the fiber cross section (Figure g) and the enlarged cross section (Figure h) is more complex, the pore size distribution is extremely uneven, and the connectivity between the pores is more complex. This structure may promote more physical entanglement, thereby enhancing the structural strength of the fiber to a certain extent, but it also affects other properties of the fiber, such as elasticity and air permeability.
[0063] The statistics of nanofiber diameter inside aerogel fibers with MSA / TFA solvent ratio of 1:1 are as follows Figure 5 a, Statistics of nanofiber diameter inside aerogel fibers obtained using sulfuric acid system Figure 5 b. Figure 5 In a, the statistics of the diameter of nanofibers inside the aerogel fibers prepared under the MSA / TFA system show that the diameter distribution presents a narrow peak, which indicates that the nanofibers have a relatively uniform diameter (19.5±9.3nm). The concentrated distribution of diameters may be due to the relatively uniform solution environment and gelation process under the MSA / TFA solvent system, which allows the polymer chains to aggregate and condense uniformly to form nanofibers with uniform diameters. In contrast, in Figure 5 In Figure b, the diameter distribution of nanofibers inside aerogel fibers prepared using a sulfuric acid system shows a wider distribution curve (27.0-72.0nm), and the diameter is mainly concentrated at 49.5±15.1nm. This wide diameter distribution may be due to the strong acidic environment and solvent effect in the sulfuric acid system, which causes the inhomogeneity in the condensation process of the polymer chain, thereby forming nanofibers of different diameters. The uneven distribution of nanofiber diameters may lead to the inhomogeneity of the mechanical properties inside the aerogel fibers, thereby affecting their overall mechanical and physical properties.
[0064] The analysis of the fiber surface morphology and the internal nanofiber diameter predicted that the aerogel fibers prepared using the sulfuric acid system had poor mechanical properties. Figure 6 The mechanical property curves of aerogel fibers prepared using different solvent systems are shown in ab. The aerogel fibers prepared in the sulfuric acid solvent system exhibit typical stress-strain behavior, that is, they show a clear linear region in the initial loading stage, reflecting the elastic properties of the material at this stage. In contrast, the fibers prepared using the MSA / TFA solvent system rise faster in the initial stage of the stress-strain curve, indicating that the fibers of this system exhibit a higher stress response at a smaller strain. The calculated elastic modulus shows that the MSA / TFA system fibers (39.7MPa) are significantly higher than the sulfuric acid system fibers (2.9MPa). This result indicates that the MSA / TFA system fibers have higher rigidity in the initial loading stage and can withstand greater stress under smaller deformations. This property provides strong material support for applications that require high-rigidity materials. Further analysis shows that the breaking strength of the MSA / TFA system fibers (12.1MPa) is significantly higher than that of the sulfuric acid system fibers (0.4MPa), indicating that the MSA / TFA system fibers have the ability to withstand greater forces before breaking. This high breaking strength property indicates that the MSA / TFA system fiber has potential advantages in high-load applications, such as as a reinforcement phase in composite materials to improve overall performance. From the perspective of toughness, the MSA / TFA system fiber (9.0MJ / m 3) is also significantly better than the sulfate system fiber, which means that the MSA / TFA fiber can absorb more energy before breaking. This high toughness is extremely important for applications that require materials to have excellent impact resistance and sudden stress resistance.
[0065] By using different solvent systems, the mechanical properties of aerogel fibers can be significantly adjusted. The MSA / TFA solvent system gives the fibers superior elastic modulus, breaking strength and toughness during the preparation process, which have broad application prospects in the field of high-performance fiber materials.
[0066] Example 3
[0067] The experimental steps for preparing aerogel fibers using MSA / TFA as the solvent system are as follows:
[0068] (1) Precursor preparation: A mixture of 225 mg PBO and 29.7 g MSA / TFA was stirred at room temperature for 5 hours to form a 0.75 wt% precursor solution. The mass ratio of MSA to TFA was adjusted to 4:1, 2:1, 1:1, 1:2, and 1:4.
[0069] (2) Wet spinning: The spinning solution was extruded into water at different temperatures of 0, 15, 30, 45, and 60 °C using a syringe pump at a speed of 500 μl / min through a 25G dispensing needle. After the solvent was completely exchanged, a wet gel was obtained.
[0070] (3) Preparation before drying: Place the wet gel in ethanol and change it every 8 hours for a total of 4 times to remove MSA / TFA from the fibers.
[0071] (4) Supercritical drying: The fiber was placed in a supercritical dryer and dried at 50°C and 15.0 MPa for 4 hours. During the drying process, a magnetic stirrer was used to continuously stir the liquid carbon dioxide in the sealed chamber at a speed of 500 rpm, and exhaust was performed at a speed of 200 ml / min.
[0072] The parameters for sample preparation are shown in Table 1 below.
[0073] Table 1
[0074]
[0075] The morphology of aerogel fibers prepared at different ratios of MSA / TFA in group 2 is shown in Figure 2. Figure 7As shown in the figure, the fiber diameters are 205.0μm, 150.0μm and 218.6μm, respectively. As the MSA ratio decreases, the fiber surface texture evolves from dense wrinkles to a smoother appearance, while the radial wrinkles on the fiber become more obvious. The reason for this may be that the difference in the protonation degree of the PBO molecular chain caused by different solvent ratios leads to different shear forces on the fiber after solution extrusion, causing different Kelvin–Helmholtz instability wave evolution processes. The cross-sectional magnified image further reveals the role of the solvent ratio in regulating the shell thickness and internal pore structure of the aerogel fiber. When the MSA / TFA ratio is 4:1, the fiber cross section presents a relatively uniform nanoporous structure. When the TFA content increases to be equal to that of MSA (1:1), the pore size distribution of the fiber cross section gradually widens. In addition, the magnified cross-sectional image shows that as the MSA ratio decreases, the shell wall thickness of the aerogel fiber gradually decreases from about 9.5μm to 0.5μm, highlighting the significant effect of the solvent ratio on the shell thickness.
[0076] Based on the characterization and analysis of PBO aerogel fibers prepared from different solvent systems, the following conclusions can be drawn: With the increase of TFA content during the gelation process, the degree of phase separation during the PBO sol-gel transformation process intensifies, resulting in an increase in the pore size of the resulting aerogel fiber, a widening of the pore size distribution, a thinning of the pore wall, and an increase in the heterogeneity of the overall porous structure. These structural changes will significantly affect the mechanical properties, specific surface area, thermal conductivity and other properties of the aerogel fiber. For example, the loose porous structure formed at a high TFA content has a lower density and thermal conductivity, but reduces the mechanical strength.
[0077] By analyzing the stress-strain curves of aerogel fibers prepared with different solvent ratios, the effect of MSA / TFA ratio on the properties of PBO aerogel fibers can be further elucidated. Figure 8 In a), it is observed that with the increase of MSA / TFA ratio, the strain of the fiber increases from 56.6% to 105.1%, showing a clear upward trend. This trend is consistently confirmed at different non-solvent temperatures, and the strain range of the fiber is wider at 0°C, ranging from 76.3% to 144.6%.
[0078] also, Figure 8The data in b show that as the MSA / TFA ratio increases, the tensile strength gradually increases from 6.9 MPa to 12.1 MPa. This indicates that under specific preparation conditions, a higher proportion of MSA is beneficial to improving fiber strength. However, when the MSA / TFA ratio reaches 1:4, although the Young's modulus reaches a maximum value of 24.89 MPa, the strain and tensile strength also decrease, falling to 56.6% and 9.5 MPa, respectively. This result shows that although the addition of TFA increases the rigidity of the material, it also increases its brittleness. (c), (d) are the changing trends of the breaking strength, maximum elongation, toughness and Young's modulus of aerogel fibers prepared at different MSA / TFA solvent ratios in non-solvent (water) at 30°C.
[0079] Through comprehensive analysis Figure 8 (a) and (d), it was found that at a solvent ratio of 4:1, the material exhibited the best toughness (3.46 MJ / m 3 ), which is consistent with the fact that it has the highest tensile strength and elongation at break under the same conditions. Toughness, a measure of the energy a material can absorb before breaking, shows that the fiber's energy absorption capacity increases with increasing MSA content. In contrast, when the TFA content is high, despite the increase in Young's modulus, the decrease in toughness and tensile strength indicates that the material becomes more fragile.
[0080] In summary, the adjustment of the MSA / TFA ratio is a key factor affecting the mechanical properties of PBO aerogel fibers. An appropriate MSA ratio can enhance the toughness and elongation of the fiber, while a higher TFA ratio is beneficial to improve the rigidity, but may sacrifice the toughness and strength of the fiber.
[0081] When the MSA / TFA ratio is fixed at 4:1, the scanning electron microscope (SEM) images of PBO aerogel fibers prepared at non-solvent temperatures of 0°C, 30°C, and 60°C are shown in Figure 2. Fig. 9 As shown, and the corresponding magnified SEM images are (d), (e) and (f). At the same time, the corresponding fiber surface wrinkle widths were also counted, as shown in (g), (h) and (i). Under 0℃ conditions, the fiber surface presents a fine and uniform small wrinkle structure, and the wrinkle width is mainly concentrated in the range of 150-750nm, with a peak value of about 250nm ( Fig. 9 (g)). When the temperature rises to 30°C, the fiber surface gradually changes from small wrinkles to large wrinkles, the wrinkle width range expands to 150-950nm, and the peak shifts to 350nm. When the temperature is further raised to 60°C, obvious large-scale irregular wrinkles appear on the fiber surface, the width distribution range further expands, and the peak migrates to a wider wrinkle area ( Fig. 9(i)). This temperature-induced morphological change is mainly due to the fact that temperature affects the mobility of PBO molecular chains and the diffusion behavior of solvents. At higher temperatures, the molecular chain movement is enhanced and the solvent is more likely to seep out, causing the fiber to shrink and deform and form large-scale wrinkles. Statistical data further verified that the fiber density decreased significantly with increasing temperature (174.1 mg / cm at 0 °C). 3 , 60℃ is 74.5mg / cm 3 ).
[0082] When the MSA / TFA ratio is 4:1, the BET adsorption isotherms and corresponding pore size distribution curves of PBO aerogel fibers prepared under non-solvent temperatures of 0°C, 30°C, and 60°C are shown in Figure 2. Fig.10 According to the experimental data, when the temperature rises from 0℃ to 60℃, the specific surface area gradually increases from 458.8m 2 / g increased to 517.1m 2 / g. Fig.10 (a) shows the BET adsorption isotherms of PBO aerogel fibers prepared at different non-solvent temperatures. According to the shape characteristics of the three adsorption isotherms in the figure, they belong to type IV adsorption isotherms. Type IV isotherm is an IUPAC classification of the adsorption behavior of porous solid adsorbent materials, with the following typical characteristics: (1) In the low relative pressure region, the curve shows a monotonic rise similar to type I, indicating the presence of micropore filling; (2) In the medium relative pressure region, the curve approximates a horizontal line parallel to the relative pressure axis, corresponding to capillary condensation; (3) In the high relative pressure region, the curve shows a steep rise again, indicating that multilayer adsorption occurs; (4) Hysteresis loops appear at high relative pressures, which is caused by the irreversibility of the adsorption and desorption processes. As Fig.10 As shown in (a), the adsorption isotherms of all samples show a typical IV type curve, indicating the presence of a mesoporous structure, which is consistent with the hierarchical porous characteristics. It is worth noting that as the temperature rises from 0°C to 60°C, the adsorption amount of the isotherm in the medium and high pressure region gradually increases, indicating that higher temperatures are conducive to increasing the specific surface area and improving the adsorption capacity.
[0083] Pore size distribution curve ( Fig.10 (b)) further reveals the difference between micropore and mesoporous structures. Under the three temperature conditions, the fibers are rich in 1-2nm micropores and 3-50nm mesopores, forming a multi-level pore distribution. However, at 60℃, the relative content of 3-50nm mesopores is significantly higher than that at 0℃ and 30℃, indicating that higher temperatures are more conducive to the formation of a developed mesoporous structure. This may be due to the fact that high temperature promotes molecular chain movement and pore growth. In contrast, the changes in microporous structure at different temperatures are not significant.
[0084] In summary, non-solvent temperature is a key factor affecting the multi-level pore structure of PBO aerogel fibers. Temperature increase accelerates molecular chain rearrangement and solvent diffusion, triggers fiber shrinkage and large-scale wrinkle formation, and promotes the development of mesopores, thereby increasing the specific surface area and adsorption capacity, but the effect on the microporous structure is relatively limited. This temperature effect is crucial for fine-tuning the pore structure, density, and surface morphology of the fiber.
[0085] Fig.11 The significant effect of non-solvent temperature on the mechanical properties of PBO aerogel fibers is demonstrated in detail. Fig.11 (a) shows the stress-strain curves of the fibers prepared at the MSA / TFA ratio of 4:1 and non-solvent temperatures of 0°C, 15°C, 30°C, 45°C, and 60°C. The curve has a typical trilinear segment, with the initial segment corresponding to the initial tensile linear deformation stage of the fiber, followed by a nonlinear yield zone, and finally a strain hardening zone until the fiber breaks. Fig.11 (b) shows the situation of 50.0g load suspended in the air, which intuitively demonstrates the excellent specific strength and toughness of aerogel fibers. Fig.11 (cd) The effects of different non-solvent temperatures (0-60℃) on the mechanical properties of PBO aerogel fibers, such as tensile strength, elongation at break, toughness and modulus, are summarized. It is worth noting that when the non-solvent temperature decreases from 60℃ to 0℃, the tensile strength and elongation at break of the fiber show a significant upward trend, especially the elongation at break increases significantly from 90.2% to 144.6%, while the tensile strength also increases from 7.6 to 12.2MPa. This significant improvement in mechanical properties is mainly due to the regulation of the non-solvent temperature on the core-shell structure of the fiber. Through a comprehensive analysis of the stress-strain curves and SEM characterization results, the thickness of the fiber shell gradually increases when the non-solvent temperature decreases from 60℃ to 0℃. The thicker shell can more effectively support and constrain the deformation of the fiber core, thereby giving the fiber higher tensile strength and elongation at break. The optimization and regulation of this core-shell structure is crucial to improving the comprehensive mechanical properties of the fiber.
[0086] It is worth noting that the effect of non-solvent temperature on fiber modulus and toughness is somewhat different. In the range of 15-60℃, the modulus and toughness of the fiber are relatively stable, maintaining at 7.2-11.3MPa and 2.6-4.1MJ / m 3 Although the value is low, it still has certain advantages over other aerogel fibers. However, when the temperature drops to 0°C, the modulus and toughness of the fiber increase significantly, reaching 29.5MPa and 9.0MJ / m 3The reason for this phenomenon may be that low temperature (0°C) has a positive effect on inhibiting the movement of PBO molecular segments, making them easier to orient and form an ordered crystalline phase, thereby significantly improving the rigidity (modulus) and energy dissipation capacity (toughness) of the fiber. However, too high a temperature (15-60°C) will over-activate the movement of the molecular chains, weaken the ordered structure, and lead to reduced modulus and toughness. Therefore, 0°C conditions are conducive to obtaining PBO aerogel fibers with high modulus and high toughness, which can be used in application scenarios with higher requirements for mechanical properties.
[0087] The mechanical properties of PBO aerogel fibers (experimental conditions: MSA / TFA ratio 4:1, 0℃ non-solvent) and aerogel fibers prepared from several other common materials were compared. Fig.12 As shown in Figure 2, the PBO aerogel fiber prepared by the present invention exhibits excellent mechanical properties, with maximum stress and strain reaching 12.2MPa and 144.6%, respectively, which is significantly better than graphene, cellulose, Kevlar, silica, and silk protein ( Fig.12 (a)). In addition, PBO aerogel fiber also has excellent toughness, reaching 9.0MJ / m 3 , which is 1-3 orders of magnitude higher than other materials, indicating that it has excellent energy absorption and fracture resistance ( Fig.12 (b)).
[0088] Flame retardant and thermal insulation performance test:
[0089] The aerogel fibers prepared with MSA / TFA ratio of 4:1 and non-solvent temperature of 0 °C were made into cylindrical blocks with a diameter of 33 mm and a thickness of 11 mm for flame retardant and thermal insulation tests. Fig.13 As shown in the figure, (a) shows the flame retardant performance test of aerogel fibers in block form (11 mm thick) under a butane flame gun, and (b) shows the temperature curve behind the block aerogel during the loss process. Fig.13 As shown in (a), the bulk aerogel fiber is placed in front of the insulation board, and the thermocouple is placed on the back of the bulk aerogel. A butane flame spray gun is used to continuously spray flames at a fixed position (the distance between the spray gun mouth and the aerogel is 3 cm) to the aerogel block. During the experiment, the bulk aerogel gradually decomposes under the continuous action of the butane flame spray gun, but no open flame is observed during the whole process, which strongly proves the excellent flame retardant properties of PBO aerogel fiber. The time-temperature curve of the back temperature ( Fig.13 (b)), the temperature on the back of the aerogel block gradually rises from the initial 30°C to 250°C, demonstrating its good thermal insulation performance under continuous high temperature. The uniformity of its internal structure provides a guarantee for its stability at high temperatures.
[0090] The aerogel fiber prepared at a MSA / TFA ratio of 4:1 and a non-solvent temperature of 0°C was made into a 6 mm thick sample and placed on a heating table. Thermocouples were inserted into the upper and lower surfaces to measure the temperature change, thereby obtaining a time-temperature curve. Fig.14 As shown in (a), when the temperature of the hot stage rises to 250°C, the temperature of the material surface only remains at around 100°C. This result highlights the excellent thermal insulation performance of PBO aerogel fibers.
[0091] Furthermore, by comparison with commercial silica aerogels ( Fig.14 (b)), it can be seen that when the heat source reaches the maximum value, the surface temperature peak of the PBO aerogel block (126.2℃) is lower than that of the commercial silica aerogel (137.4℃), which proves the advantage of PBO aerogel in thermal stability. It is worth noting that the surface temperature of the commercial silica aerogel shows a spike as the temperature of the hot stage changes, while the PBO aerogel shows stability after the temperature peak and will not rise significantly with the further increase of the hot stage temperature, which reflects the high stability and reliability of PBO aerogel in thermal response.
[0092] The thermal insulation and heat preservation capabilities of composite fabrics formed by combining PBO aerogel fibers with traditional sweater materials were further explored. Fig.15 As shown in (ab), the tests conducted on the hot and cold stages reveal the performance of the composite fabric under extreme temperature conditions. Fig.15 In (a), the composite fabric is placed on a hot stage for testing, and the thermocouples are in contact with the yellow PBO aerogel fiber with a thickness of 0.5 mm and the green sweater material with a thickness of 2 mm. Fig.15 (c) shows that when the temperature of the hot plate is stabilized at about 100°C, the surface temperature of the PBO aerogel fiber only rises to 47°C, while the surface temperature of the sweater rises to 62°C. This result highlights the significant advantage of PBO composite fabrics in thermal insulation performance compared to traditional sweaters. Fig.15 From the temperature change curve of (d), it can be seen that even when the cold table is maintained at about -55°C, the surface temperature of the fabric can still be maintained at -3°C, while the surface temperature of the sweater drops to -22°C, which once again verifies the excellent thermal insulation performance of PBO aerogel fiber. These experimental results show that after forming a composite fabric, PBO aerogel fiber can not only provide excellent high-temperature thermal insulation effect, but also provide effective thermal insulation in extreme low temperature environments. Therefore, PBO aerogel composite fabrics have great application potential and value in various practical applications that require high thermal insulation or thermal insulation performance, such as winter clothing, high-latitude expedition equipment, aerospace thermal insulation materials, and low-temperature storage and transportation containers.
[0093] Example 4
[0094] In order to explore the potential of PBO aerogel fibers in composite materials, they were combined with polydimethylsiloxane (PDMS) to prepare PDMS-PBO composite materials. The preparation method is as follows: a dumbbell-shaped mold is prepared using an acrylic plate. First, the oriented PBO fibers are placed in the lower mold, and then the defoamed PDMS is used to fill the gaps in the PBO fibers. After the bubbles between the fibers are emptied, the upper mold is covered with the lower mold, and finally, it is left to stand in a 70°C oven for 12 hours before being taken out for testing. By embedding the PBO fibers into the PDMS matrix, the tensile strength and elongation of the composite material are improved.
[0095] The stress-strain curve of pure PDMS and PBO composite is shown in Fig.16 As shown, Fig.16 The stress-strain curves shown reveal that the mechanical properties of the polydimethylsiloxane-poly(p-phenylene benzobisoxazole) (PDMS-PBO) composite material are significantly improved compared to the pure PDMS matrix. The tensile strength of the composite material reaches 5.1MPa, which is 25 times higher than that of pure PDMS (0.2MPa), and its elongation at break also reaches a high level of 195%. By numerically integrating the stress-strain curves, the toughness of the composite material is 4.1MJ / cm 3 , purer PDMS (0.17MJ / cm 3 ) increased by 24 times. The above results show that the introduction of PBO fibers can significantly improve the mechanical properties of the PDMS matrix. On the one hand, this is attributed to the excellent mechanical properties of the PBO fibers themselves, such as high strength and high modulus; on the other hand, the unique multi-level structure on the surface of the PBO fibers is conducive to the formation of a strong interface bond between it and the PDMS matrix, thereby achieving effective stress transfer during the load-bearing process of the composite material. The synergistic reinforcement effect between the fiber / matrix is the key factor in the overall superior mechanical properties of the composite material over those of each component. Therefore, it is crucial to rationally design the surface and interface structure of the PBO fiber and optimize its interfacial compatibility with the matrix to give full play to the reinforcement effect of the PBO aerogel fiber and obtain high-performance PDMS-based composites.
[0096] The embodiments of the present invention are described in detail above, but the present invention is not limited to the described embodiments. For those skilled in the art, various changes, modifications, substitutions and variations of these embodiments are made without departing from the principles and spirit of the present invention, and still fall within the protection scope of the present invention.
Claims
1. A method for preparing a core-shell structured PBO aerogel fiber, characterized in that: The following steps are involved: (1) PBO, MSA and TFA are mixed and stirred to obtain a precursor solution; (2) extruding the precursor solution into water through a dispensing needle to obtain a wet gel; (3) placing the wet gel in ethanol, replacing the ethanol at regular intervals to remove MSA and TFA in the fiber; and then drying the fiber to obtain the core-shell structured PBO aerogel fiber.
2. The method for preparing the core-shell structured PBO aerogel fiber according to claim 1, characterized in that: In step (1), the concentration of PBO in the precursor solution is 0.5-1.5 wt %.
3. The method for preparing the core-shell structured PBO aerogel fiber according to claim 1, characterized in that: In step (1), the mass ratio of MSA to TFA is (0.25-4):
1.
4. The method for preparing the core-shell structured PBO aerogel fiber according to claim 1, characterized in that: In step (2), the temperature of the water is 0 to 60°C.
5. The method for preparing the core-shell structured PBO aerogel fiber according to claim 1, characterized in that: In step (2), the precursor solution is extruded into water through a 25G dispensing needle at a speed of 400 to 600 μl / min.
6. The method for preparing core-shell PBO aerogel fiber according to claim 1, characterized in that: In step (3), the wet gel is placed in ethanol, and the ethanol is replaced every 6 to 10 hours, for a total of 3 to 5 times.
7. The method for preparing core-shell PBO aerogel fiber according to claim 1, characterized in that: In step (3), the drying method is freeze drying or supercritical carbon dioxide drying.
8. The method for preparing core-shell structured PBO aerogel fiber according to claim 7, characterized in that: In step (3), the drying method is supercritical carbon dioxide drying; the drying conditions are 30-55° C., 7.4-16 MPa, and drying for 3-5 hours.
9. A core-shell structured PBO aerogel fiber, characterized in that: The fiber is prepared by the method for preparing the core-shell structured PBO aerogel fiber according to any one of claims 1 to 8.