Bio-based polymer melt blending functional fiber and preparation method thereof

By combining polylactic acid and liquid crystal elastomer through blending melt spinning technology, liquid crystal-polylactic acid fibers with excellent mechanical properties and temperature response characteristics are prepared, which solves the problem of insufficient mechanical properties of polylactic acid fibers and achieves efficient production of fibers. and widely used.

CN118835348AActive Publication Date: 2024-10-25ZHEJIANG SCI-TECH UNIV

Patent Information

Application Number
CN202411063314.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-25
Estimated Expiration
2044-08-05

AI Technical Summary

Technical Problem

Polylactic acid fiber has poor mechanical properties and toughness and is prone to fracture when subjected to force, which limits its wide application.

Method used

Using blending melt spinning technology, polylactic acid and liquid crystal elastomer are mixed, and liquid crystal-polylactic acid fibers are prepared through melt extrusion, spinning, stretching and winding processes. The added amount of liquid crystal elastomer is the quality of dry polylactic acid slices. 2% to 50%, the melting temperature is 180°C, the stretching process adopts double-roller drafting, the winding speed is 50mm/min, and the take-up speed is 300rpm.

Benefits of technology

The mechanical properties and temperature response characteristics of liquid crystal-polylactic acid fiber are significantly improved. The average strength of the fiber can reach 2.54cN/dtex, the elongation is 110.24%, and it has excellent color and heat shrinkage properties, making it suitable as an environmentally friendly and sustainable fiber. Material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118835348A_ABST
    Figure CN118835348A_ABST
Patent Text Reader

Abstract

The invention discloses a bio-based polymer melt blending functional fiber and a preparation method thereof, which are characterized in that a liquid crystal elastomer is added in the melt spinning process of bio-based polymer polylactic acid fiber to carry out blending melt spinning so as to improve the physical and mechanical properties of the fiber and form the functional fiber. Specifically, polylactic acid slices are mixed with a liquid crystal elastomer, and then the liquid crystal-polylactic acid blend fiber is prepared according to a melt spinning process. According to the liquid crystal-polylactic acid blended fiber and the preparation method thereof, the liquid crystal-polylactic acid fiber can be successfully prepared through spinning by regulating and controlling specific process parameters, the prepared liquid crystal-polylactic acid blended fiber has excellent physical and mechanical properties, the average strength of the fiber can reach 2.54 cN / dtex, and the average elongation reaches 110.24%; meanwhile, the special performance of the liquid crystal elastomer is achieved. The dope-dyed fiber with excellent performance can be directly prepared by adopting the method, the average elongation of the fiber reaches 196.02%, and the dope-dyed fiber has obvious temperature response characteristics. The method disclosed by the invention is simple, can be used for large-scale production, is a degradable environment-friendly fiber, and has an extremely high application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of chemical fiber preparation, and specifically relates to a bio-based polymer melt-blended functional fiber and a preparation method thereof. Background Art

[0002] In the field of fiber preparation technology, blended melt spinning technology has attracted much attention due to its unique advantages, especially in the production of synthetic fibers. This technology involves mixing two or more different types of polymers and heating them to a molten state. When the mixture reaches a predetermined uniformity and fluidity, it is spun into filaments through special equipment such as a nozzle or a rotary spinneret.

[0003] The significant advantages of blended melt spinning technology are its high flexibility and cost control capabilities. By selecting polymers with different characteristics for mixing, the performance of the final product, such as strength, softness, etc., can be effectively adjusted to meet diverse market demands. In addition, this technology can also significantly reduce production costs while maintaining certain performance by mixing cheap polymers with high-performance polymers, achieving a balance between performance and cost.

[0004] In practical applications, blended melt spinning technology has shown its great potential in the field of fiber preparation. Taking polylactic acid (PLA) fiber as an example, as an environmentally friendly biodegradable material, its market demand is growing. However, the softness of pure PLA fiber is limited, which restricts its application in some fields.

[0005] In order to solve this problem, the present invention proposes a method for preparing melt-blended fibers by combining blended melt spinning technology with liquid crystal polymers. This method can effectively improve the softness of PLA fibers and improve their mechanical properties, providing new possibilities for the wide application of PLA fibers. The present invention develops a more efficient and economical method for preparing PLA toughened blends, and further optimizes its spinning process to achieve large-scale production and wide application of PLA blended fibers, which has important research significance and application value. Summary of the invention

[0006] The purpose of the present invention is to solve the shortcomings of the current polylactic acid fiber in mechanical properties, such as poor toughness and easy breakage under stress, and to provide a bio-based polymer melt-blended functional fiber and a preparation method thereof. The liquid crystal-polylactic acid fiber prepared by the method has excellent mechanical properties and has great application prospects as an environmentally friendly and sustainable material.

[0007] The present invention adopts the following technical solutions:

[0008] A bio-based polymer melt-blended functional fiber and a preparation method thereof, comprising:

[0009] The method is prepared by melt spinning using polylactic acid chips and liquid crystal elastomer (prepared from 2-methyl-1,4-phenylenebis(4-(3-(acryloyloxy)propoxy)benzoate) as raw materials. Specifically, in the spinning process, the polylactic acid chips are dried and mixed with a certain proportion of liquid crystal elastomer before adding the spinning raw materials. Subsequently, liquid crystal-polylactic acid fibers are prepared according to a series of spinning processes including melt extrusion, spinning, stretching, and winding.

[0010] The liquid crystal elastomer is prepared from diacrylate reaction intermediate (RM82), 2,2'-(ethylenedioxy)dialkylthiol (EDDT), toluene, dipropylamine (DPA), dibutyltin dilaurate (DBTDL), butylated hydroxytoluene (BHT), and poly(cyclohexane diisocyanate) (Tris-Iso) as raw materials.

[0011] In the above technical solution, further, the amount of the liquid crystal elastomer added is 2% to 50% of the mass of the dry polylactic acid slices.

[0012] Furthermore, the melting temperature is 180° C. and the extrusion speed is 10 mm / min.

[0013] Furthermore, the stretching process is: double-roller stretching, the rotation speed of roller 1 is 150 rpm, the rotation speed of roller 2 is 225 rpm, and the spun fiber is first stretched by roller 1 and then by roller 2.

[0014] Furthermore, the winding process is as follows: reciprocating speed: 50 mm / min, winding speed: 300 rpm.

[0015] The liquid crystal-polylactic acid fiber prepared by the method has excellent mechanical properties and properties unique to liquid crystal materials. The obtained fiber linear density is 25-40 dtex, the average fiber strength can reach 2.54 cN / dtex, and the average fiber elongation is 110.24%.

[0016] In addition, by adding coloring masterbatch to the raw materials, the above method can be used to conveniently obtain liquid-colored fibers. Usually, the added mass of liquid crystal elastomer in the raw materials is 5.0% of the mass of dry polylactic acid chips, and the added amount of coloring masterbatch is 0.1% to 0.5% of the mass of dry polylactic acid chips; the obtained fiber line density is 22 to 37 dtex, the average strength of the fiber is 1.44 cN / dtex, and the average elongation of the fiber can reach 196.02%.

[0017] The beneficial effects of the present invention are:

[0018] In view of the shortcomings of current polylactic acid fibers in mechanical properties, such as poor toughness and easy breakage under stress, the present invention provides a bio-based polymer melt-blended functional fiber and a preparation method thereof. The liquid crystal-polylactic acid fiber prepared by the method has excellent mechanical properties and color, and has obvious temperature response characteristics, and has great application prospects as an environmentally friendly and sustainable material.

[0019] The present invention adopts a blended melt spinning method to spin polylactic acid and a liquid crystal elastomer to prepare liquid crystal-polylactic acid fibers with excellent mechanical properties, which provides a new idea for the performance optimization of polylactic acid materials and a new reference for the application and promotion of polylactic acid materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 Liquid crystal-polylactic acid fibers are obtained by spinning liquid crystal elastomers with different proportions;

[0021] Figure 2 Liquid crystal-polylactic acid fibers are obtained by spinning liquid crystal elastomers with the same proportion and masterbatches with different proportions.

[0022] Figure 3 It is a liquid crystal elastomer particle;

[0023] Figure 4 is the stress-strain diagram of liquid crystal-polylactic acid fiber with different proportions of liquid crystal content;

[0024] Figure 5 This is the stress-strain diagram of liquid crystal-polylactic acid fiber with the same proportion of liquid crystal content and different proportions of masterbatch content;

[0025] Figure 6 It is the spinning effect of liquid crystal elastomer and non-bio-based polymer polypropylene (PP) after compounding (no stable, uniform, continuous fibers, and no obvious temperature response characteristics)

[0026] Figure 7 It is a bar graph of the shrinkage state of the liquid crystal-fiber colored by the original solution at 70°C (the upper right corner is the heating time);

[0027] Figure 8 It is a bar graph of the shrinkage state of the liquid crystal-fiber colored by the original solution at 90°C (the upper right corner is the heating time);

[0028] Fig. 9 This is an optical microscope image of the liquid crystal-fiber colored with the original solution, magnified 100 times. DETAILED DESCRIPTION

[0029] The present invention is further described in detail below with reference to the accompanying drawings and specific examples.

[0030] Process route: PLA slice drying and raw material preparation → melt extrusion → spinning → stretching → winding spinning operation:

[0031] (1) Pour the material into the hopper (when the equipment is working, pay attention to add granular material in time);

[0032] (2) Set the temperature and install a suitable extruder head;

[0033] (3) Wait for 5-10 minutes for the temperature to reach the set temperature, allowing the machine temperature to balance;

[0034] (4) Adjust the appropriate extrusion speed, press the start button, and start the motor to extrude the fiber;

[0035] (5) After the material is extruded, start the drafting machine and the winding machine, and use tweezers to send the fiber to the drafting roller and the winding roller;

[0036] (6) The temperature and extrusion speed can be fine-tuned during the spinning process, and the corresponding drawing machine speed and winding speed also need to be fine-tuned accordingly.

[0037] Polylactic acid slice drying:

[0038] The polylactic acid slices were spread flat on a tray, placed in a vacuum oven, and dried at 80°C for 24 hours.

[0039] (1) Remove moisture

[0040] Polylactic acid is polymerized from lactic acid. There are ester bonds in the polylactic acid molecule, and the ester bonds are easily hydrolyzed. Ester bond hydrolysis is the main way of polylactic acid degradation. Moreover, the hydrolysis reaction can be automatically catalyzed by the groups (—COOH) produced by hydrolysis. The ester bond hydrolysis is slow at first, but then it will accelerate. The hydrolysis reaction occurs not only on the surface of polylactic acid, but also penetrates into the entire polymer. For semi-crystalline polylactic acid, hydrolysis is divided into two stages: in the first stage, water molecules diffuse rapidly into the amorphous region, followed by hydrolysis; the second stage is the hydrolysis of the crystalline region, which is relatively slow. For polylactic acid with an amorphous structure, hydrolysis only has the first stage.

[0041] In addition, water in the melt will form bubbles during spinning, and the bubbles will be mixed in the melt stream, which is very likely to cause spinning drifting, hairy, broken, etc., and even leave hidden dangers in the monofilament, causing hairy or broken ends during post-stretching. Therefore, the slices must be dried before the high-temperature spinning process.

[0042] (2) Improve the softening point

[0043] The raw material polylactic acid chips are amorphous structures with a very low softening point. When spinning with such chips, the chips will quickly soften and become sticky after entering the screw extruder, causing "ring knots" to block and interrupt production. However, the dried chips will form partial crystals, which greatly increases the softening point. The higher the crystallinity, the higher the softening point and the harder the chips. After such chips enter the screw extruder, the "ring knot" phenomenon will be avoided.

[0044] The dried polylactic acid chips are fully mixed with a compatibilizer and masterbatch in an appropriate proportion, and then the mixture is fed into a screw extruder for melting and extrusion. In order to ensure uniform and smooth filament output and not affect the subsequent spinning process, the raw materials should be kept uniform and stable at the feeding port. Balanced and stable feeding is a key factor affecting the quality of product fibers. In addition, since the extrusion speed of polylactic acid during the spinning process is not fast, the polylactic acid raw material stays in the screw for a relatively long time, and the probability of polylactic acid degradation increases. In order to reduce the degradation of polylactic acid raw materials and thus affect the quality of spinning, high-speed discharge should be performed at regular intervals to obtain a polylactic acid melt with a relatively low degradation rate.

[0045] The melt extrusion of polylactic acid chips in the extruder is an extrusion process from solid state to high-temperature viscous flow state. The extruder must simultaneously perform the dual functions of extrusion and transportation and heating and melting. The chips move along the screw groove toward the die head, and the physical state undergoes the transformation from glassy state, high elastic state, to viscous flow state.

[0046] This experiment uses Huizhi electrospinning desktop melt spinning equipment.

[0047] Spinning:

[0048] After the melt is ejected from the spinneret into a thin stream, it gradually cools and forms along the path of the filament. The temperature, diameter, movement speed, force, viscosity and internal structure of each point on the filament are changing. External conditions have a great influence on the uniformity of the fineness, unevenness of strength and elongation and post-stretching properties of the filament.

[0049] Along the spinning direction, the cooling process of the filament can be divided into three regions: flow deformation zone, solidification deformation zone and solid state movement zone.

[0050] 1. Flow deformation zone

[0051] After the melt leaves the control of the spinneret micropores, it will expand within a distance of about 5 to 10 mm from the spinneret surface. This is due to the release of elastic deformation energy and static pressure energy generated by the sudden change in melt flow rate, which causes the diameter to expand. The expansion phenomenon is not good for spinning. It not only causes uneven filaments, but also causes adhesion to the spinneret, broken ends, and hairy filaments. If measures such as appropriately reducing the viscosity of the melt, increasing the spinning temperature, and selecting spinnerets with a larger aspect ratio are taken, the degree of expansion can be reduced.

[0052] Although the temperature has dropped in the flow deformation zone, the flow properties are very good, so it is easy to become thinner after being pulled. The resulting macromolecules have a low degree of axial arrangement and a small degree of orientation.

[0053] 2. Solidification deformation zone

[0054] The solidification deformation zone is the most important area for cooling and solidification. Under the traction of the winding mechanism and certain cooling conditions, the melt flow changes the most in this area, and changes occur in temperature, viscosity, diameter and macromolecular structure, and gradually solidifies into filaments.

[0055] (1) Diameter change. Because the winding mechanism pulling speed V (called spinning speed or winding speed) greatly exceeds the spinning speed V0 (that is, the speed at which the melt is ejected in the micropores), the filaments are stretched and thinned until the solidification point, and the diameter remains basically unchanged.

[0056] (2) Changes in melt temperature and viscosity. The melt stream is cooled by the surrounding air, and its temperature drops rapidly, while its viscosity rises quickly. When the viscosity reaches a certain value, it loses fluidity and becomes solid.

[0057] (3) Changes in the internal structure of the filaments. The internal structure of the filaments mainly includes orientation and crystallinity. Since the crystallization temperature needs to be below the melting point and above the glass transition temperature, and it takes a certain amount of time to proceed, the glass transition temperature of polylactic acid fiber is relatively high, and the temperature drops very quickly, so it has fallen below the glass transition temperature before crystallization, resulting in the internal structure of the filaments being in an amorphous (non-crystalline) state.

[0058] The degree to which the macromolecular chains are regularly arranged along the axial direction of the filament under the action of external force is called the degree of orientation, and the size of the birefringence "Δn" is used to measure the degree of orientation (a large Δn means a large degree of orientation).

[0059] 3. Solid state mobile area

[0060] From the solidification point, the filaments move at the same pulling speed, and the forming is completed. In order to reduce the temperature of the filaments when they enter the filament reel or winding mechanism, a certain cooling distance is generally required, so there is a tunnel for a distance under the filament chamber. However, when the spinning speed increases, the role of the tunnel becomes smaller.

[0061] draft:

[0062] Drafting is a process of stretching and heat setting the spun fibers, the purpose of which is to improve the quality of the fibers by changing the microstructural characteristics inside the fibers. The polylactic acid fibers are transferred from the spinneret to the drafting mechanism and the drafting process is completed by two drafting rollers.

[0063] Drawing machine: Drawing roller: double roller, circumference 20 cm, speed: 0.1-300rpm, accuracy 0.1rpm, steering: one-button adjustment of roller steering.

[0064] Winding:

[0065] The winding process is the last step in the entire production process, which is used to wind the produced fibers or yarns into rolls for storage, transportation and subsequent processing. This step is the last link in the entire production chain and is very important for ensuring product quality and facilitating subsequent processing.

[0066] Fiber winder: Collecting roller: circumference 10cm, length 10cm, rotation speed: 0.1-300rpm, precision 0.1rpm reciprocating distance: 0-15cm adjustable, reciprocating speed: 1-1000mm / min, precision 1mm / min.

[0067] The liquid crystal elastomer used in the embodiment of the present invention is prepared using a diacrylate reaction intermediate (RM82), 2,2'-(ethylenedioxy)dialkylthiol (EDDT), toluene, dipropylamine (DPA), dibutyltin dilaurate (DBTDL), butylated hydroxytoluene (BHT), and poly(cyclohexane diisocyanate) (Tris-Iso) as raw materials.

[0068] Example 1

[0069] The above method was used to set the liquid crystal elastomer addition amount to 2%, 5%, 10%, 20%, 30%, and 50% of the mass of the dry polylactic acid slices, a total of six groups. Spinning temperature: 180°C, screw extrusion speed: 10mm / min, roller 1: 150rpm, roller 2: 225rpm, reciprocating speed: 50rpm, take-up speed: 300rpm, winding time: 12min, and experiments were carried out; liquid crystal-polylactic acid fibers were successfully obtained, and the obtained samples were as follows Figure 1 As shown in the figure, from left to right are 2%, 5%, 10%, 20%, 30%, and 50% liquid crystal-polylactic acid fiber samples.

[0070] Example 2

[0071] Using the above method, the amount of liquid crystal elastomer added was set to 5% of the mass of dry polylactic acid chips, and the amount of masterbatch added was set to 0.1%, 0.3%, and 0.5% of the mass of dry polylactic acid chips, a total of three groups. Spinning temperature: 180°C, screw extrusion speed: 10mm / min, roller 1: 150rpm, roller 2: 225rpm, reciprocating speed: 50mm / min, take-up speed: 300rpm, winding time: 12min, and the experiment was carried out;

[0072] In the process of melt spinning of polylactic acid, a certain proportion of liquid crystal elastomer is added. Figure 4 This method significantly improved the strength, elongation and modulus of polylactic acid fibers, providing a new way to prepare high-performance bio-based fibers.

[0073] In the preparation process of liquid crystal-polylactic acid fiber, the addition of masterbatch has a certain influence on the mechanical properties of the fiber. Figure 5 As the proportion of masterbatch increases, the mechanical properties of the fiber decrease to a certain extent. Therefore, it is necessary to optimize the combination ratio of masterbatch and liquid crystal elastomer during the preparation process to obtain the best fiber performance.

[0074] The experiment further found that the liquid crystal-polylactic acid fiber has thermal shrinkage characteristics within a specific temperature range. Figures 7 and 8 When the temperature is 50℃, the fiber does not shrink. As shown in Table 1, it is the shrinkage deformation data of liquid crystal PLA fiber with different masterbatch addition ratios at 50℃. It can be seen that when the fiber is at 50℃, there is no dimensional change. When the temperature is at a certain value between 50℃ and 70℃, the fiber begins to shrink thermally and reaches the maximum shrinkage rate at 90℃. Figure 7 , Figure 8 In addition, the experiment also found that within the selected temperature range, the less the liquid crystal content, the greater the shrinkage of the fiber. This discovery is of great significance for understanding the thermal shrinkage mechanism of liquid crystal-polylactic acid fibers and optimizing their performance.

[0075] Table 1

[0076]

[0077] The present invention also tests and analyzes the color performance of the liquid crystal-polylactic acid colored yarn with added color masterbatch. Fig. 9 The liquid solution coloring of liquid crystal-polylactic acid colored fibers also has good results, providing a new idea for the preparation of colored bio-based fibers.

[0078] It can be seen that the present invention successfully spun uniform continuous fibers by selecting bio-based fiber polylactic acid and liquid crystal elastomer, combined with regulating melt spinning parameters, and obtained functional fibers with excellent physical and mechanical properties while retaining the special properties of liquid crystal elastomer. It is worth noting that it is difficult to compound liquid crystal elastomer with polymer to maintain its spinnability. After a large number of experimental studies, liquid crystal elastomer and most common polymers cannot be successfully spun. When the composite liquid crystal elastomer is mixed with non-bio-based polymer polypropylene (PP) and melt spinning is used, uneven fibers can be spun, such as Figure 6 What is shown is the spinning effect. There are no stable, uniform, continuous fibers. More importantly, it has no obvious temperature response characteristics and cannot have the properties of liquid crystal elastomers.

[0079] The embodiments described above provide a detailed description of the preparation scheme of the present invention. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the present invention. Any modifications, supplements or similar substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing bio-based polymer melt-blended functional fibers, characterized in that: include: The polylactic acid slices and liquid crystal elastomer are used as raw materials and prepared by melt spinning. Specifically, the polylactic acid slices are dried and mixed with a certain proportion of liquid crystal elastomer, and the liquid crystal-polylactic acid blended fibers are prepared according to the spinning process of melt extrusion, spinning, stretching and winding.

2. The method for preparing bio-based polymer melt-blended functional fibers according to claim 1, characterized in that: The added amount of the liquid crystal elastomer is 2% to 50% of the mass of the dry polylactic acid slices.

3. The method for preparing bio-based polymer melt-blended functional fibers according to claim 1, characterized in that: The polylactic acid slices are dried at 80° C. for 24 hours.

4. The method for preparing bio-based polymer melt-blended functional fibers according to claim 1, characterized in that: The melt extrusion temperature is 180° C. and the extrusion speed is 10 mm / min.

5. The method for preparing bio-based polymer melt-blended functional fibers according to claim 1, characterized in that: The stretching process is: double-roller stretching, the rotation speed of roller 1 is 150 rpm, and the rotation speed of roller 2 is 225 rpm.

6. The method for preparing bio-based polymer melt-blended functional fibers according to claim 1, characterized in that: The winding process is as follows: reciprocating speed: 50 mm / min, winding speed: 300 rpm.

7. A bio-based polymer melt-blended functional fiber, characterized in that: The fiber is prepared by the method according to any one of claims 1 to 6, wherein the fiber linear density is 25 to 40 dtex, the average fiber strength is 2.54 cN / dtex, and the average fiber elongation is 110.24%.

8. A bio-based polymer melt-blended functional fiber, characterized in that: The method is adopted as claimed in any one of claims 1 to 6, and the raw materials also contain coloring masterbatch.

9. The bio-based polymer melt-blended functional fiber according to claim 8, characterized in that: The added amount of the liquid crystal elastomer in the raw materials is 5.0% of the dry polylactic acid slice mass, and the added amount of the coloring masterbatch is 0.1% to 0.5% of the dry polylactic acid slice mass.

10. The bio-based polymer melt-blended functional fiber according to claim 8, characterized in that: The fiber linear density is 22-37 dtex, the average fiber strength is 1.44 cN / dtex, and the average fiber elongation is 196.02%.

Citation Information

Patent Citations

  • Preparation method of elastic polylactic acid fiber

    CN103255503A

  • Method for large-scale preparation of continuous and uniform liquid crystal elastomer melt spinning fibers

    CN117587542A

  • Polylactic acid fiber

    JP2002030523A

Cited By

  • Preparation method of bio-based polymer melt-spun fiber with high mechanical property

    CN119824555A

  • Efficient preparation method of bio-based polymer melt-spun monofilament fiber

    CN119877121A