Protective coating fabric based on beta-cyclodextrin and preparation method thereof

By modifying β-cyclodextrin and compounding it with two-dimensional composite materials and polyurethane resin, a protective coating is formed, which solves the problems of poor elasticity, poor smoothness and durability in the existing fabric coating technology, and achieves excellent fabric Protective properties and hydrophobic effect.

CN118835474APending Publication Date: 2024-10-25JIANGSU UNIV OF SCI & TECH
View PDF 0 Cites 3 Cited by

Patent Information

Application Number
CN202411060651.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-10-25

AI Technical Summary

Technical Problem

Existing fabric coating technology has problems such as poor elasticity, easy wrinkles, poor surface finish, difficult to adjust hand feel, short duration of coating materials, and short-lasting effects, which affect its application effect.

Method used

By modifying β-cyclodextrin, it is compounded with two-dimensional composite materials and polyurethane resin to form a protective coating. It is coated on the surface of the fabric by dropper, roller coating or spraying to form a protective coating with composite properties. coating.

Benefits of technology

It achieves excellent anti-corrosion, antibacterial, chemical resistance and other protective properties of the fabric, improves the hydrophobic performance and durability of the coating, and improves the appearance and feel of the fabric.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118835474A_ABST
    Figure CN118835474A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of functional fabric manufacturing, in particular to a protective coating fabric based on beta-cyclodextrin and a preparation method thereof.According to the protective coating fabric based on beta-cyclodextrin and the preparation method thereof, cyclodextrin is modified through the subject-object effect, so that cyclodextrin is better attached to or interacts with the surface, and therefore the property of cyclodextrin is changed; the cyclodextrin-two-dimensional composite material is further compounded with polyurethane resin and a curing agent and coats the surface of the fabric to form a protective fabric coating, so that the prepared coated fabric has the comprehensive properties of the composite two-dimensional material, modified cyclodextrin and polyurethane resin, and the fabric has excellent protective properties such as corrosion resistance, antibacterial property and chemical resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of functional fabric manufacturing, and in particular to a protective coating fabric based on beta-cyclodextrin and a preparation method thereof. Background Art

[0002] As one of the traditional industries in my country, the textile dyeing and finishing industry is also facing the problem of transformation and development in the current era. How to discover new technologies in traditional industries and combine them to meet people's requirements for new fabrics is the key to the development of the textile dyeing and finishing industry. In terms of dyeing and finishing technology, fabric finishing is the last and most important process before the fabric leaves the factory. How to perform new and effective finishing on fabrics is at an important juncture where breakthrough technology is urgently needed. In recent years, with the continuous research and advancement of textile finishing technology, a variety of new finishing methods such as low-temperature plasma treatment, bioengineering, ultrasonic technology, electron beam radiation treatment, or the popular microcapsule technology, inkjet technology, nanomaterials, etc., and the most widely used, most traditional and simplest technology is fabric coating technology.

[0003] Fabric coating technology is a branch of traditional coating technology in textile application. The so-called fabric coating technology is actually not separated from the core technologies of "coating" and "surface". On the surface, it simply refers to uniformly coating one or more layers of polymer substances or multifunctional coatings on the surface of the fabric, or certain chemical substances with corresponding functions such as rosin esters, polyurethanes, etc., so as to change the appearance, style, and function of the fabric, and make it produce different functions such as hydrophobic, flame retardant, antibacterial, deodorizing, etc., to meet people's growing demand for new fabrics. It is a traditional but dynamic surface processing technology.

[0004] Among protective coatings, the most common are water-repellent and fire-retardant coatings. Most of them are composite chemicals coated on the surface of fabrics to promote them to react with the fiber structure on the surface of fabrics, thereby forming a dense film (or coating) with specific functions to hinder or even prevent the invasion of corresponding substances. The fire-retardant coating blocks combustibles and fire sources, thereby preventing combustion; in terms of functional coatings, there are also the above-mentioned anti-allergic coatings based on the principle of absorbing and reflecting ultraviolet and infrared, and adsorption coatings that can effectively absorb harmful gases and large particle molecules. Coating finishing is developing rapidly and effectively. However, the rapid development and great potential of coating finishing are bound to be accompanied by many problems. Some coating materials, especially organic materials, will bring problems of poor elasticity and easy wrinkling; and some materials will also affect the appearance of fabrics, making their surface finish poor; the feel is difficult to adjust moderately, etc. At the same time, coating materials also have problems such as short duration and not long-lasting effect that seriously affect their application effect, and they urgently need to be further optimized.

[0005] Therefore, providing a new fabric surface coating technology to solve the existing technical defects is of great significance to the development of the current fabric surface coating technology. Summary of the invention

[0006] In order to overcome the shortcomings of the prior art, the purpose of the present invention is to provide a protective coating fabric based on β-cyclodextrin and a preparation method thereof. The present invention modifies cyclodextrin through host-guest interaction so that cyclodextrin can better adhere to or interact with the surface, thereby changing its properties; the cyclodextrin-two-dimensional composite material is further compounded with a polyurethane resin and a curing agent and coated on the surface of the fabric to form a protective fabric coating, so that the prepared coated fabric has the comprehensive properties of the composite two-dimensional material, modified cyclodextrin and polyurethane resin, so that the fabric has excellent protective properties such as corrosion resistance, antibacterial resistance, and chemical resistance.

[0007] To achieve the above object, the present invention provides the following technical solutions:

[0008] A method for preparing a protective coating fabric based on β-cyclodextrin comprises the following steps:

[0009] S1. Synthesis of β-cyclodextrin modified polyurethane

[0010] S101. Weigh 1-8 parts of ethephon, 10-50 parts of β-cyclodextrin and 0.1-0.5 parts of sodium hydroxide by mass and add them to 20-80 parts of deionized water, dissolve them evenly, heat to 40-80 ° C for 2-8h, evaporate the water and dry them to obtain ethephon-modified cyclodextrin;

[0011] S102. Weigh 12-16 parts of polycaprolactone diol by mass, add 4-5 parts of isophorone diisocyanate, add a catalyst, add a solvent to completely immerse the reactants, place the mixture solution in a three-necked flask equipped with a condenser reflux device and a mechanical stirrer, and heat the mixture in an oil bath at 65-80°C for 2-3h to obtain a waterborne polyurethane;

[0012] S103. After the prepolymerization is completed, 0.5-1 parts of dimethylolbutyric acid are added to the obtained aqueous polyurethane by mass, and after reacting at 65-80° C. for 1-2 hours, 6-8 parts of hydroxy fluorosilicone oil are added, and the temperature is raised to 70-80° C. to modify the polyurethane, and the reaction is carried out for 2-3 hours to make the mixture hydrophobic;

[0013] S104. After the reaction is completed, 2-5 parts of ethephon-modified β-cyclodextrin are added to the mixture obtained in step S103, and the mixture is reacted at 70-80°C for 1-2h; finally, 0.1-1 parts of triethylamine are added, and the reaction is maintained at the original temperature for 1-2h, and the reaction is terminated to obtain β-cyclodextrin-modified polyurethane;

[0014] S2. Preparation of protective coated fabrics

[0015] S201. The β-cyclodextrin-modified polyurethane obtained by the reaction is sucked out with a dropper, and evenly coated on the surface of the glass sheet, and then placed in an oven at 70-80°C for 30-45 minutes for drying, and then taken out, and then allowed to stand at room temperature for 30-45 minutes. If there is no stickiness when touched, it proves that the film is successfully formed;

[0016] S202. The film-forming β-cyclodextrin-modified polyurethane is applied to the surface of the fabric by roller coating, dipping or spraying, and then taken out and dried in an oven at 70-80°C. After cooling at room temperature, the β-cyclodextrin-based protective coating fabric is obtained.

[0017] Preferably, in step S102, the catalyst is dibutyltin dilaurate.

[0018] Preferably, the amount of the catalyst used is 0.5%-1% of the total volume of the mixture solution.

[0019] Preferably, in step S102, the solvent is selected from one or more of acetone and DMF.

[0020] Preferably, the structure and preparation route of the ethephon-modified cyclodextrin are as follows:

[0021]

[0022] Preferably, the structure and preparation route of the β-cyclodextrin modified polyurethane are as follows:

[0023]

[0024] Preferably, in step S202, a film-forming β-cyclodextrin-modified polyurethane is mixed with hydrophobic fumed silica and treated on the surface of the fabric by roller coating, dip coating or spraying, and then taken out and dried in an oven at 70-80°C and cooled at room temperature to obtain a super hydrophobic protective coating fabric based on β-cyclodextrin.

[0025] Preferably, the mass ratio of the film-forming β-cyclodextrin-modified polyurethane to the hydrophobic fumed silica is 40-50:4.5-5.

[0026] A protective coating fabric based on beta-cyclodextrin is prepared according to the preparation method.

[0027] Compared with the prior art, the present invention has the following beneficial effects:

[0028] The present invention modifies cyclodextrin through host-guest interaction, so that cyclodextrin can better adhere to or interact with the surface, thereby changing its properties; the cyclodextrin-two-dimensional composite material is further compounded with a polyurethane resin and a curing agent and coated on the surface of the fabric to form a protective fabric coating, so that the prepared coated fabric has the comprehensive properties of the composite two-dimensional material, modified cyclodextrin and polyurethane resin, and the fabric has excellent protective properties such as corrosion resistance, antibacterial resistance and chemical resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The present invention is a flow chart of the preparation process of the protective coating fabric based on β-cyclodextrin;

[0030] Figure 2 The present invention is a flow chart of the preparation process of the β-cyclodextrin modified polyurethane;

[0031] Figure 3 is the H NMR spectrum curve of the β-cyclodextrin modified polyurethane prepared in Example 2 of the present invention;

[0032] Figure 4 The infrared spectrum curves of the β-cyclodextrin modified polyurethanes prepared in Examples 1 and 2 of the present invention;

[0033] Figure 5 The infrared spectrum curves of the β-cyclodextrin modified polyurethanes prepared in Comparative Example 1 and Comparative Example 2;

[0034] Figure 6 The DSC curves of the β-cyclodextrin modified polyurethanes prepared in Example 1, Example 2 and Example 3;

[0035] Figure 7 The TGA curves of the β-cyclodextrin modified polyurethanes prepared in Example 1, Example 2 and Example 3;

[0036] Figure 8 A line graph showing changes in ammonia concentration of the β-cyclodextrin modified polyurethane prepared by the present invention;

[0037] Fig. 9 A line graph showing the change in absorbance of limonene of the β-cyclodextrin modified polyurethane prepared by the present invention;

[0038] Fig.10 This is an image showing the change of the peak (706 nm) in the citric acid adsorption test of the β-cyclodextrin modified polyurethane prepared by the present invention;

[0039] Fig.11The contact angle measurement diagram of the β-cyclodextrin modified polyurethane prepared by the present invention, wherein: a is the contact angle of the original cloth; b is the contact angle of formula 1; c is the contact angle of formula 2; d is the contact angle of formula 3; e is the contact angle of formula 4; f is the parallel test of formula 4; g is the contact angle of the new formula 4; h is the contact angle of the superhydrophobic formula of the preliminary test;

[0040] Fig.12 A line graph showing the change in contact angle of the β-cyclodextrin-modified polyurethane prepared by the present invention;

[0041] Fig.13 It is a line graph showing the change in contact angle of the β-cyclodextrin modified polyurethane prepared by the present invention at different pH values;

[0042] Fig.14 This is a rendering of the appearance of the protective coating fabric based on β-cyclodextrin prepared in Example 4 of the present invention before and after friction;

[0043] Fig.15 This is a graph showing the change in contact angle of the protective coating fabric based on β-cyclodextrin prepared in Example 4 of the present invention before and after friction;

[0044] Fig.16 This is a contact angle change diagram of the hydrophobic protective coating fabric based on β-cyclodextrin prepared in Comparative Example 3 of the present invention before and after friction. DETAILED DESCRIPTION

[0045] The present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0046] See also Figure 1-16 , the present invention provides a technical solution:

[0047] Example 1 (Formula 3)

[0048] A method for preparing a protective coating fabric based on β-cyclodextrin:

[0049] S1. Synthesis of β-cyclodextrin modified polyurethane

[0050] S101. Weigh 4.3 g of ethephon, 25 g of β-cyclodextrin and 0.3 g of sodium hydroxide by mass and add them to 50 g of deionized water. After dissolving evenly, heat to 60 ° C for 5 h, evaporate the water and dry to obtain ethephon-modified cyclodextrin.

[0051] S102. Weigh 14 g of polycaprolactone diol, add 4.45 g of isophorone diisocyanate, weigh and add 0.5% of dibutyltin dilaurate based on the total volume of the mixture solution, add 50 mL of acetone to completely immerse the reactants, place the mixture solution in a three-necked flask equipped with a condensing reflux device and a mechanical stirrer, and heat in an oil bath at 65° C. for 2 h to obtain a waterborne polyurethane;

[0052] S103. After the prepolymerization, 0.59 g of dimethylolbutyric acid was added to the obtained aqueous polyurethane, and the mixture was reacted at 65 ° C for 1 h, and then 6 g of hydroxy fluorosilicone oil was added, and the temperature was raised to 70 ° C to modify the polyurethane, and the reaction was carried out for 2 h to make the mixture hydrophobic;

[0053] S104. After the reaction is completed, 3.4 g of ethephon-modified β-cyclodextrin is added to the mixture obtained in step S103, and the mixture is reacted at 70° C. for 1 h; finally, 0.404 g of triethylamine is added, and the reaction is maintained at the original temperature for 1 h, and the reaction is terminated to obtain β-cyclodextrin-modified polyurethane;

[0054] S2. Preparation of protective coated fabrics

[0055] S201. The β-cyclodextrin-modified polyurethane obtained by the reaction is sucked out with a dropper, and evenly coated on the surface of the glass sheet, and then placed in a 70°C oven for drying for 30 min, and then taken out, and then allowed to stand at room temperature for 30 min. If there is no stickiness when touched, it proves that the film is successfully formed;

[0056] S202. Cut the pure cotton fabric into small pieces of 5*5 cm, and treat the film-forming β-cyclodextrin-modified polyurethane onto the surface of the fabric by impregnation for 30 minutes. After taking out, dry it in an oven at 70°C, and cool it at room temperature to obtain the β-cyclodextrin-based protective coating fabric.

[0057] Embodiment 2 (formula 4)

[0058] A method for preparing a protective coating fabric based on β-cyclodextrin:

[0059] S1. Synthesis of β-cyclodextrin modified polyurethane

[0060] S101. Weigh 1 g of ethephon, 10 g of β-cyclodextrin and 0.1 g of sodium hydroxide by mass and add them to 20 g of deionized water. After dissolving evenly, heat to 40 ° C for 2 h, evaporate the water and dry to obtain ethephon-modified cyclodextrin.

[0061] S102. Weigh 14 g of polycaprolactone diol, add 4.45 g of isophorone diisocyanate, weigh and add 0.5% of dibutyltin dilaurate based on the total volume of the mixture solution, add 40 mL of acetone to completely immerse the reactants, place the mixture solution in a three-necked flask equipped with a condensing reflux device and a mechanical stirrer, and heat in an oil bath at 65° C. for 2 h to obtain a waterborne polyurethane;

[0062] S103. After the prepolymerization, 0.74 g of dimethylolbutyric acid was added to the obtained aqueous polyurethane, and the mixture was reacted at 65 ° C for 1 h, and then 6 g of hydroxy fluorosilicone oil was added, and the temperature was raised to 70 ° C to modify the polyurethane, and the reaction was carried out for 2 h to make the mixture hydrophobic;

[0063] S104. After the reaction is completed, 2.26 g of ethephon-modified β-cyclodextrin is added to the mixture obtained in step S103, and the mixture is reacted at 70° C. for 1 h; finally, 0.404 g of triethylamine is added, and the reaction is maintained at the original temperature for 1 h, and the reaction is terminated to obtain β-cyclodextrin-modified polyurethane;

[0064] S2. Preparation of protective coated fabrics

[0065] S201. The β-cyclodextrin-modified polyurethane obtained by the reaction is sucked out with a dropper, and evenly coated on the surface of the glass sheet, and then placed in a 70°C oven for drying for 30 min, and then taken out, and then allowed to stand at room temperature for 30 min. If there is no stickiness when touched, it proves that the film is successfully formed;

[0066] S202. Cut the pure cotton fabric into small pieces of 5*5 cm, and treat the film-forming β-cyclodextrin-modified polyurethane onto the surface of the fabric by impregnation for 30 minutes. After taking out, dry it in an oven at 70°C, and cool it at room temperature to obtain the β-cyclodextrin-based protective coating fabric.

[0067] Embodiment 3 (new formula 4)

[0068] A method for preparing a protective coating fabric based on β-cyclodextrin:

[0069] S1. Synthesis of β-cyclodextrin modified polyurethane

[0070] S101. 8 g of ethephon, 50 g of β-cyclodextrin and 0.5 g of sodium hydroxide were weighed by mass and added to 80 parts of deionized water. After being uniformly dissolved, the mixture was heated to 80 ° C for reaction for 8 h. The water was evaporated and dried to obtain ethephon-modified cyclodextrin.

[0071] S102. Weigh 14 g of polycaprolactone diol, add 4.45 g of isophorone diisocyanate, weigh and add 0.5% of dibutyltin dilaurate based on the total volume of the mixture solution, add 80 mL of DMF to completely immerse the reactants, place the mixture solution in a three-necked flask equipped with a condensing reflux device and a mechanical stirrer, and heat in an oil bath at 65° C. for 2 h to obtain a waterborne polyurethane;

[0072] S103. After the prepolymerization, 0.74 g of dimethylolbutyric acid was added to the obtained aqueous polyurethane, and the mixture was reacted at 65 ° C for 1 h, and then 6 g of hydroxy fluorosilicone oil was added, and the temperature was raised to 70 ° C to modify the polyurethane, and the reaction was carried out for 2 h to make the mixture hydrophobic;

[0073] S104. After the reaction is completed, 2.26 g of ethephon-modified β-cyclodextrin is added to the mixture obtained in step S103, and the mixture is reacted at 70° C. for 1 h; finally, 0.404 g of triethylamine is added, and the reaction is maintained at the original temperature for 1 h, and the reaction is terminated to obtain β-cyclodextrin-modified polyurethane;

[0074] S2. Preparation of protective coated fabrics

[0075] S201. The β-cyclodextrin-modified polyurethane obtained by the reaction is sucked out with a dropper, and evenly coated on the surface of the glass sheet, and then placed in a 70°C oven for drying for 30 min, and then taken out, and then allowed to stand at room temperature for 30 min. If there is no stickiness when touched, it proves that the film is successfully formed;

[0076] S202. Cut the pure cotton fabric into small pieces of 5*5 cm, and treat the film-forming β-cyclodextrin-modified polyurethane onto the surface of the fabric by impregnation for 30 minutes. After taking out, dry it in an oven at 70°C, and cool it at room temperature to obtain the β-cyclodextrin-based protective coating fabric.

[0077] Embodiment 4 (super hydrophobic formula)

[0078] A method for preparing a protective coating fabric based on β-cyclodextrin:

[0079] S1. Synthesis of β-cyclodextrin modified polyurethane

[0080] S101. 8 g of ethephon, 50 g of β-cyclodextrin and 0.5 g of sodium hydroxide were weighed by mass and added to 80 parts of deionized water. After being uniformly dissolved, the mixture was heated to 80 ° C for reaction for 8 h. The water was evaporated and dried to obtain ethephon-modified cyclodextrin.

[0081] S102. Weigh 14 g of polycaprolactone diol, add 4.45 g of isophorone diisocyanate, weigh and add 0.5% of dibutyltin dilaurate based on the total volume of the mixture solution, add 80 mL of DMF to completely immerse the reactants, place the mixture solution in a three-necked flask equipped with a condensing reflux device and a mechanical stirrer, and heat in an oil bath at 65° C. for 2 h to obtain a waterborne polyurethane;

[0082] S103. After the prepolymerization, 0.74 g of dimethylolbutyric acid was added to the obtained aqueous polyurethane, and the mixture was reacted at 65 ° C for 1 h, and then 6 g of hydroxy fluorosilicone oil was added, and the temperature was raised to 70 ° C to modify the polyurethane, and the reaction was carried out for 2 h to make the mixture hydrophobic;

[0083] S104. After the reaction is completed, 2.26 g of ethephon-modified β-cyclodextrin is added to the mixture obtained in step S103, and the mixture is reacted at 70° C. for 1 h; finally, 0.404 g of triethylamine is added, and the reaction is maintained at the original temperature for 1 h, and the reaction is terminated to obtain β-cyclodextrin-modified polyurethane;

[0084] S2. Preparation of superhydrophobic protective coating fabric

[0085] S201. The β-cyclodextrin-modified polyurethane obtained by the reaction is sucked out with a dropper, and evenly coated on the surface of the glass sheet, and then placed in a 70°C oven for drying for 30 min, and then taken out, and then allowed to stand at room temperature for 30 min. If there is no stickiness when touched, it proves that the film is successfully formed;

[0086] S202. After mixing 40g of β-cyclodextrin modified polyurethane (solid content: 22%) and 4.5g of hydrophobic fumed silica, apply them evenly to the surface of the fabric by roller coating, and then dry them in an oven at 70°C to obtain the β-cyclodextrin-based super hydrophobic protective coating fabric.

[0087] Comparative Example

[0088] Comparative Example 1 (Formula 1)

[0089] S1. Synthesis of modified polyurethane

[0090] S101. Weigh 7.22 g of polycaprolactone diol, add 2.20 g of isophorone diisocyanate, weigh and add 0.5% of dibutyltin dilaurate based on the total volume of the mixture solution, add 30 mL of acetone to completely immerse the reactants, place the mixture solution in a three-necked flask equipped with a condensing reflux device and a mechanical stirrer, and heat in an oil bath at 65° C. for 2 h to obtain a waterborne polyurethane;

[0091] S103. After the prepolymerization, 0.427 g of dimethylolbutyric acid was added to the obtained aqueous polyurethane, and the mixture was reacted at 65 ° C for 1 h, and then 4.332 g of hydroxy fluorosilicone oil was added, and the temperature was raised to 70 ° C to modify the polyurethane, and the reaction was carried out for 2 h to make the mixture hydrophobic;

[0092] S104. After the reaction is completed, 0.292 g of triethylamine is added to the mixture obtained in step S103, and the reaction is maintained at the original temperature for 1 h, and the reaction is terminated to obtain a modified polyurethane;

[0093] S2. Preparation of protective coated fabrics

[0094] S201. The modified polyurethane obtained by the reaction is sucked out with a dropper, and evenly coated on the surface of the glass sheet, placed in an oven at 70°C for 30 min, and then taken out, and then allowed to stand at room temperature for 30 min. If there is no stickiness when touched, it proves that the film is successfully formed;

[0095] S202. Cut the pure cotton fabric into small pieces of 5*5 cm, and treat the film-forming modified polyurethane onto the fabric surface by dipping for 30 minutes. After taking out, dry it in an oven at 70°C, and cool it at room temperature to obtain a protective coating fabric.

[0096] Comparative Example 2

[0097] S1. Synthesis of modified polyurethane

[0098] S101. Weigh 14 g of polycaprolactone diol, add 4.45 g of isophorone diisocyanate, weigh and add 0.5% of dibutyltin dilaurate based on the total volume of the mixture solution, add 60 mL of acetone to completely immerse the reactants, place the mixture solution in a three-necked flask equipped with a condensing reflux device and a mechanical stirrer, and heat in an oil bath at 65° C. for 2 h to obtain a waterborne polyurethane;

[0099] S103. After the prepolymerization, 1.034 g of dimethylolbutyric acid was added to the obtained aqueous polyurethane, and the mixture was reacted at 65 ° C for 1 h, and then 6 g of hydroxy fluorosilicone oil was added, and the temperature was raised to 70 ° C to modify the polyurethane, and the reaction was carried out for 2 h to make the mixture hydrophobic;

[0100] S104. After the reaction is completed, 0.404 g of triethylamine is added to the mixture obtained in step S103, and the reaction is maintained at the original temperature for 1 h, and the reaction is terminated to obtain a modified polyurethane;

[0101] S2. Preparation of protective coated fabrics

[0102] S201. The modified polyurethane obtained by the reaction is sucked out with a dropper, and evenly coated on the surface of the glass sheet, placed in an oven at 70°C for 30 min, and then taken out, and then allowed to stand at room temperature for 30 min. If there is no stickiness when touched, it proves that the film is successfully formed;

[0103] S202. Cut the pure cotton fabric into small pieces of 5*5 cm, and treat the film-forming modified polyurethane onto the fabric surface by dipping for 30 minutes. After taking out, dry it in an oven at 70°C, and cool it at room temperature to obtain a protective coating fabric.

[0104] Comparative Example 3

[0105] S1. Synthesis of β-cyclodextrin modified polyurethane

[0106] S101. Weigh 12 g of polycaprolactone diol, add 5.55 g of isophorone diisocyanate, weigh and add 0.5% of dibutyltin dilaurate based on the total volume of the mixture solution, add 60 mL of acetone to completely immerse the reactants, place the mixture solution in a three-necked flask equipped with a condensing reflux device and a mechanical stirrer, and heat in an oil bath at 65° C. for 2 h to obtain a waterborne polyurethane;

[0107] S102. After the prepolymerization, 0.74 g of dimethylolbutyric acid was added to the obtained aqueous polyurethane, and the mixture was reacted at 65 ° C for 1 h, and then 5 g of hydroxy fluorosilicone oil was added, and the temperature was raised to 70 ° C to modify the polyurethane, and the reaction was carried out for 2 h to make the mixture hydrophobic;

[0108] S103. After the reaction is completed, 3 g of β-cyclodextrin is added to the mixture obtained in step S103, and the mixture is reacted at 70° C. for 1 h; finally, 0.404 g of triethylamine is added, and the reaction is maintained at the original temperature for 1 h, and the reaction is terminated to obtain β-cyclodextrin modified polyurethane (without ethephon);

[0109] S2. Preparation of protective coated fabrics

[0110] S201. The β-cyclodextrin-modified polyurethane obtained by the reaction is sucked out with a dropper, and evenly coated on the surface of the glass sheet, and then placed in a 70°C oven for drying for 30 min, and then taken out, and then allowed to stand at room temperature for 30 min. If there is no stickiness when touched, it proves that the film is successfully formed;

[0111] S202. After mixing 40 g of β-cyclodextrin modified polyurethane (solid content: 22%) and 4.5 g of hydrophobic fumed silica, apply them evenly to the surface of the fabric by roller coating, and then dry them in an oven at 70°C to obtain the β-cyclodextrin-based hydrophobic protective coating fabric.

[0112] Characterization and performance testing:

[0113] 1. Adsorption performance test

[0114] Two 200mL wide-mouth bottles were numbered respectively: 50mL of ammonia solution with an initial concentration of 1mol / L (simulating harmful gas) was placed in bottle No. 1, and 50mL of limonene ethanol solution with an initial concentration of 2mol / L (simulating harmful absorbent) was placed in bottle No. 2. The wide-mouth bottles were then sealed with perforated rubber stoppers, and a line was inserted to hang the impregnated fabrics, which were suspended in the air to adsorb the volatile gas and test its adsorption performance. Measurements were performed every 2 hours.

[0115] After every 2 hours, use 1 mol / L acetic acid for titration, extract 10 mL from the original ammonia solution for titration, record the amount of acetic acid solution used, and calculate the concentration of the remaining solution. Calculate the weight change of the fabric by weighing method and the mass of the adsorbed substance. After the end, replenish the ammonia solution appropriately according to the concentration of the new solution to keep its volume unchanged and reduce the error.

[0116] After every 2 hours, the limonene solution was further tested using ultraviolet absorption spectrophotometry to observe changes in its peak value, thereby characterizing its concentration changes. The weight change of the fabric was calculated by weighing, and the mass of the adsorbed substance was calculated to analyze its adsorption performance. After the end, the limonene solution was appropriately supplemented according to the concentration of the new solution to keep its volume unchanged and reduce errors, which was conducive to further analysis and refinement of the experimental results.

[0117] 2. Contact angle test

[0118] The prepared fabric sample is immersed in the sample solution by the above method, taken out and dried, and the contact angle and rolling angle of the fabric are measured by a contact angle meter. A 5-6uL water droplet is used to test the contact angle, and four to five positions are randomly selected on the same fabric for testing, and the average value is taken as the final contact angle value of the fabric. When the contact angle is greater than 90°, it can be roughly considered to have a hydrophobic effect. The best effect is that it can roll on the fabric.

[0119] 3. MRI test

[0120] The transparent film-like surface formed by the cyclodextrin composite coating material on the glass sheet was observed using a SU-1510 scanning electron microscope from Hitachi, Japan, and scanned using an accelerating voltage of 5kV. The sample was placed in the main unit after the air was inflated and deflated, and vacuum pressurized. The sample was observed, and the appropriate magnification was found and selected to facilitate the observation of the sample and its molecular chemical structure. The internal molecular structure information was obtained through chemical shift, and its microscopic characteristics were studied.

[0121] 4. Infrared spectrum test

[0122] The untreated cotton fabric and the prepared β-cyclodextrin composite coatings with different proportions were tested using the NICOLET.is10 Fourier transform infrared spectrometer from Thermo Fisher Scientific. A small amount of prepared polyurethane was placed on a glass slide, and the residual acetone solvent was evaporated in the air. Then, the Fourier transform infrared spectrometer was used to measure the infrared spectrum of the synthetic product using the total reflection method at room temperature. The test range was 4000cm -1 ~500cm -1 , by testing the molecular structure of the substance and identifying the specific composition of the compound, it is convenient to observe whether β-cyclodextrin is successfully covered on the surface of cotton fabric and verify the role of each substance.

[0123] 5.DSC (Differential Scanning Calorimetry) Test

[0124] A certain amount of product sample was absorbed onto a glass slide, and the solvent was dried in an oven at 40°C. About 5 mg of solvent-free water-based polyurethane was weighed to prepare a test sample. Then, a differential scanning calorimeter was used to measure the thermal properties of the prepared water-based polyurethane. The temperature range was set to -80 to 250°C, and the heating rate was set to 10°C / min. After the test, the data was sorted, the results were statistically analyzed, and the transition temperature was analyzed to explore the influence of different percentages of substances on their temperature limits.

[0125] 6.TGA (thermogravimetric analysis) test

[0126] When conducting thermal stability analysis on the prepared waterborne polyurethane-β-cyclodextrin composite, first absorb a certain amount of product sample onto a glass slide, dry the solvent in a 60°C oven, and then put about 5 mg of the weighed sample into a Q500 thermogravimetric analyzer. The N2 flow rate was set to 20 mL / min, the measurement temperature range was 30-600°C, and the heating rate was 20°C / min. Before the experiment, the mass of the initial sample was recorded; after the experiment, the mass of the final sample was recorded to explore its heat resistance and some other physical properties.

[0127] Characterization and test results analysis:

[0128] 1. Analysis of NMR Results

[0129] Figure 3 The H NMR spectrum of the sample (Example 3) is shown in Figure 1. The solvent is N,N-dimethylformamide. According to the literature, the absorption peak with a chemical shift (δ) between 2.5 and 3.5 is the solvent peak. After removing it and another free hydroxyl peak, we analyzed these 9 absorption peaks.

[0130] The polyurethane body we initially synthesized is a symmetrical linear / chain structure, so the H peak in its structure is completely symmetrical. We can find that it has four absorption peaks, which can be judged to be exactly the same as 1, 2, 5 and 3; at the same time, fluorosilicone oil has three hydrogen absorption peaks, and the areas of two of the absorption peaks are exactly the same, so it can be judged that peaks 7, 8, and 9 are the hydrogen absorption peaks of hydroxyfluorosilicone oil; finally, due to the particularity of the β-cyclodextrin structure, the number of its hydroxyl hydrogens is huge, so it can be judged that 4 is its hydrogen absorption peak.

[0131] The structural formulas of the isophorone diisocyanate, polyurethane and hydroxy fluorosilicone oil are as follows:

[0132] Isophorone diisocyanate:

[0133] Polyurethane:

[0134] Hydroxyfluorosilicone oil:

[0135] 2. Analysis of infrared spectroscopy results

[0136] The chemical raw materials, prepolymers and samples of the prepared polyurethane were placed in sample bottles, and infrared spectroscopy (FT-IR) tests were performed on them. The charts were exported and analyzed in an integrated manner. The data were processed as follows: Figure 4 , 5 shown.

[0137] Through analysis, it can be seen that all samples (including polyurethane prepolymer) have similar infrared characteristic curves, and their absorption peaks have similar characteristics to those of polyurethane bulk: polyurethane prepolymer has a peak at 1060-1150cm -1 The absorption peak of COC aliphatic chain may be caused by its irregular vibration; 1225-1235cm -1 The absorption peaks at 1450-1470cm -1 The strong absorption peaks in the range of 1715-1750cm are produced by the deformation vibration of CH2 and the asymmetric deformation vibration of CH3. -1 The stronger absorption peak in the range is generated by the ester group C=O; at 2300-2400cm -1 The absorption peaks between 2878 and 2900 cm -1 The absorption peaks generated in the interval also represent the stretching vibration of CH (CH2 or CH3); and the leftmost 3538cm -1 In each sample, we can find that 500~1300cm-1 The saturated CH deformation vibration absorption peak was reduced, proving that β-cyclodextrin was modified by polyurethane.

[0138] 3.DSC test results analysis

[0139] Glass transition temperature (Tg) is an important physical property of amorphous polymers, which represents the transition between the highly elastic state and the glassy state. Therefore, the size of Tg is the main indicator for measuring the low temperature resistance of polyurethane elastomers. For polyurethane, its influencing factors are not only conventional conditions such as molecular weight, but also the hydrogen bonds formed by the reaction connection between its segments will greatly affect its glass transition temperature. When the ester content in the soft segment increases, the probability of forming hydrogen bonds between the two will also be greater, and the glass transition temperature will also be higher.

[0140] Figure 6 The DSC curves of the coatings of Example 1 (Formula 3), Example 2 (Formula 4) and (Example 3) (Formula 4 (DMF solvent)) are shown. We can clearly find that the glass transition temperatures of the three samples are all around -50°C, which is consistent with the theoretical basis. We can find that the DSC curve of the sample is abnormal due to the excessive amount of β-cyclodextrin used in Formula 3, and the thermal effect of the DSC test is greatly affected by the sample heating rate, particle size, filling method, etc. After consulting relevant literature, we found that its overall curve is similar to the DSC curve of waterborne polyurethane, proving that β-cyclodextrin and hydroxyfluorosilicone oil successfully react with polyurethane and modify it, improving its performance to a certain extent and making it more heat-resistant.

[0141] 4. TGA test results analysis

[0142] Depend on Figure 7 It can be seen that the thermal decomposition process of the β-cyclodextrin composite coating material is divided into three stages: first, below 250°C, the thermal decomposition of polyurethane is relatively slow, which is preliminarily speculated to be the removal of solvent (acetone / DMF) and water. Formula 4 has a slightly higher weight loss than other samples due to insufficient dissolution and more solvent; then, between 250°C and 400°C, the polyurethane composite material decomposes extremely rapidly, and a large number of bonds are destroyed, resulting in serious mass loss. Formula 3 has excessive cyclodextrin and insufficient reaction, so its quality decreases rapidly and reaches the thermogravimetric analysis endpoint earlier; finally, after exceeding 400°C, the reaction tends to be complete. It can be seen that the change of solvent does not significantly improve the final heat resistance of Formula 4, but it can effectively prevent its quality from decreasing in the early stage of heating, so DMF solvent is still valuable.

[0143] 5. Analysis of adsorption performance test results

[0144] The pure cotton fabric was cut into small squares of 5x5 cm. After being impregnated according to the above method, it was hung by cotton thread and placed in reagent bottles containing ammonia water and limonene. After being sealed, it was weighed and the concentration change test was performed every 2 hours to verify its adsorption performance. The adsorption test results are as follows:

[0145] (1) Ammonia adsorption (ammonia 10 mL):

[0146] Weigh 0.86g of pure ammonia water and dissolve it in 50mL of deionized water to prepare a 1mol / L ammonia solution. We test the weight of the hanging cloth sample every 2 hours. We find that its mass has changed significantly. Considering the sealing problem, it is possible that due to its water absorption and adsorption characteristics, it has the weight of water vapor and ammonia gas. For scientific reasons, we also intend to measure the residual ammonia concentration for auxiliary evidence.

[0147] Table 1. Changes in fabric mass of blank control (polyurethane only coated on the fabric surface) adsorbed with ammonia water

[0148]

[0149] Table 2. Changes in fabric mass in ammonia adsorption test

[0150]

[0151] The ammonia solution was titrated with 1 mol / L acetic acid solution to calculate its residual concentration. From the table, we can see that the mass of the fabric has increased significantly. Compared with the blank control, it can be determined that the β-cyclodextrin coating can effectively increase the fabric's absorption of harmful substances. At the same time, since the change in ammonia concentration is inconsistent with its adsorption mass, it also proves that there is water vapor in the adsorbed substance. Through further calculation and concentration line graph ( Figure 8 ). We can know the specific mass adsorbed by the β-cyclodextrin coating, and can infer that it has excellent adsorption capacity and relatively excellent absorption capacity and performance.

[0152] (2) Limonene adsorption:

[0153] Weigh 6.81g of limonene and dissolve it in 25mL of deionized water to prepare a 2mol / L limonene solution. We also tested the weight of the hanging cloth samples every 2h. We also found that its mass changed, but with the change of time, its mass change tended to be stable. Considering the water absorption performance of the original cloth, we used UV spectrophotometry to test the adsorption peak for further research.

[0154] Table 3. Changes in fabric mass of blank control (polyurethane only coated on the fabric surface) adsorbed by limonene

[0155]

[0156] Table 4. Changes in mass of fabric samples for limonene adsorption test

[0157]

[0158] Through the experiment, we found that, like the ammonia adsorption test results, the quality of the fabric samples in the limonene adsorption test also changed significantly. However, since untreated pure cotton has the same adsorption effect on water vapor in the air, we must further explore whether it has an adsorption effect on limonene. Since limonene is difficult to test for concentration using general methods, we are preparing to perform an absorbance spectrophotometric test on it with theoretical support, and judge its concentration increase or decrease by the change in its spectral peak. The results are as follows: Fig. 9 , 10 As shown:

[0159] First, we prepared 1mol / L, 2mol / L, and 3mol / L limonene solutions, and measured their UV absorbances as standard lines for observation. Afterwards, we tested the absorbance of 0h (2mol / L), 2h, 4h, 6h, and 8h limonene solutions to verify their concentration changes. After removing some abnormal data, we found that the peak value obviously decreased significantly with the increase of time, which further proved that the concentration did change due to the absorption of volatile gases by the coated fabric.

[0160] 6. Analysis of hydrophobic performance test results

[0161] (1) Exploring the best hydrophobic formula

[0162] The impregnated fabric was placed in a hydrophobic instrument, and the contact angle of the fabric (grey fabric) impregnated with solutions of different concentrations was tested to verify its hydrophobic performance and explore the optimal formula ratio. The specific results are as follows Fig.11 , 12 shown.

[0163] Through the measurement of contact angle, we can easily find that the hydrophilicity of the original cloth is good and it can basically absorb water completely. The hydrophobic effect of formula 1 without adding fluorine is basically similar to that of the original cloth, and its contact angle is about 30°. In formula 2, we added fluorine but the effect is still not obvious. It may be due to the excessive amount of dimethylolbutyric acid and triethylamine, which leads to a significant improvement in the hydrophilicity of the original material, so that the uncoated material still has a certain degree of hydrophilicity.

[0164] After that, we tried formula 3. Although it did not perform well in terms of solubility, the appropriate ratio gave it a certain degree of hydrophobicity, and its contact angle could reach about 75°. However, there was still room for improvement. The initial inference was that due to the excessive molecular weight of cyclodextrin and the high mass we added, the sample was not only viscous and difficult to move, but also the coating lost its effect. After repeated verification, we found that formula 4 had the best hydrophobic effect, with a contact angle of nearly 130°, and the hydrophobic performance could last for more than one hour outdoors, and its durability was also guaranteed to a certain extent. At the same time, considering the problem of cyclodextrin insolubility in the previous experiment, we also conducted the same hydrophobic angle test again according to the new formula 4 using DMF instead of acetone as the solvent, and found that the difference in the results was not obvious, still about 127°. It can be seen that the influence of the solvent on the hydrophobic performance is not great. At present, it is inferred that the solvent may affect the solubility of β-cyclodextrin, which may have a certain relationship with the adsorption performance.

[0165] (2) Chemical resistance

[0166] Aqueous solutions with different pH values ​​were prepared, and their pH values ​​were adjusted to 4 (acid) and 9 (base) and multiple pH values ​​therein. The contact angles were observed and statistically plotted after the colored droplets were contacted with the fabric samples to analyze the effect of different pH values ​​on the contact angles. The results are shown in the figure. Fig.13 shown.

[0167] Experiments have shown that the coating has a certain ability to resist acid and alkali corrosion, and can maintain a good contact angle and rolling angle for a period of time. We can see from the above figure that the resistance of the β-cyclodextrin composite coating to alkaline substances is slightly stronger than that to acidic substances, but it may also be due to other reasons. After consulting the literature and encyclopedia, we learned that β-cyclodextrin is used as a leveling agent for acid dyes in dyeing and finishing, so it has a certain acid resistance. At the same time, its special ring structure protects its fragile internal structure, giving it a very good resistance to alkali corrosion. However, under the action of strong acid, β-cyclodextrin, which is essentially a polysaccharide, will still hydrolyze.

[0168] (3) Friction resistance

[0169] The friction test was carried out on the sample fabric using a friction resistance instrument, and the contact angle was measured after 10 frictions to verify the durability and some mechanical properties of the coating. At the same time, the durability of the coating was analyzed. After the same steps, the results were as follows: Fig.14 , 15 , as shown in 16:

[0170] Obviously, the coating (Example 4) is damaged under strong friction, and its various indicators including hydrophobicity, appearance, and feel are all reduced, but overall it still maintains good hydrophobicity and durability. However, its hydrophobicity will still weaken or even fail under strong friction, and other additives need to be added to maintain its performance, so that it is not easy to damage. At the same time, the multifunctional coating may still give the fabric sample a certain washability, which needs to be further explored;

[0171] Although the coated fabric (Comparative Example 3) was hydrophobic at first, after 10 frictions, the surface became hydrophilic (82°), indicating that the resin had a relatively low adhesion because it did not contain ethephon, and the phosphate groups in ethephon could enhance the adhesion between the resin and the fabric.

[0172] in conclusion:

[0173] After using isophorone diisocyanate (IPDI) and polycaprolactone diol PCL2000 and adding the catalyst dibutyltin dilaurate, the prepared waterborne polyurethane prepolymer still had no special properties. Then we used hydroxyl fluorosilicone oil to hydrophobically modify the waterborne polyurethane adhesive and used infrared spectroscopy to analyze its structure to determine that the modified polyurethane was synthesized; then we used nuclear magnetic resonance hydrogen spectrum and thermogravimetric analyzer to analyze the solid state of polyurethane to confirm its molecular characteristics and its structural properties. After conducting a hydrophobic test on it, we also proved that it has excellent hydrophobic properties; and in the thinking and exploration of the process, we quickly analyzed and characterized the optimal formula. After the completion of various tests, we concluded that the composite coating material polymerized by β-cyclodextrin and waterborne polyurethane has good viscosity and film-forming properties. After coating on the fabric, it can effectively enhance its waterproof performance and can effectively adsorb gas substances and macromolecular substances such as ammonia and limonene. The conclusions are as follows:

[0174] (1) When we use hydroxy fluorosilicone oil to further modify waterborne polyurethane, the hydrophobic property will be significantly enhanced when the amount of hydroxy fluorosilicone oil is increased. However, when the amount is increased from 6g to 10g, serious stratification will occur after standing. This may be due to the solubility problem of fluorosilicone oil. The optimal amount is controlled between 4 and 6g. If necessary, a small amount of silica can be added for enhancement.

[0175] (2) When using β-cyclodextrin to graft-modify hydrophobic raw materials, if the amount of cyclodextrin added is too large, it will lead to the same situation as in Formula 3, resulting in serious stratification, with the upper layer being a clear liquid solvent and the lower layer being deposited cyclodextrin substances, which will cause major problems in adsorption testing and coating. However, appropriately increasing the amount of cyclodextrin can enhance certain performance and feel.

[0176] (3) In the contact angle test of hydrophobicity, we found that with the appropriate reduction of cyclodextrin and the increase of fluorosilicone oil, the hydrophobicity of the fabric gradually increased, and the contact angle also increased from 70° to about 130°. Practice shows that if strong hydrophobic substances such as silica are added, the contact angle of the sample can even reach 130°, meeting the super-hydrophobic condition. However, further improvements need to be explored and tested.

[0177] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a protective coating fabric based on β-cyclodextrin, characterized in that: The following steps are involved: S1. Synthesis of β-cyclodextrin modified polyurethane: S101. Weigh 1-8 parts of ethephon, 10-50 parts of β-cyclodextrin and 0.1-0.5 parts of sodium hydroxide by mass and add them to 20-80 parts of deionized water, dissolve them evenly, heat to 40-80 ° C for 2-8h, evaporate the water and dry them to obtain ethephon-modified cyclodextrin; S102. Weigh 12-16 parts of polycaprolactone diol by mass, add 4-5 parts of isophorone diisocyanate, add a catalyst, add a solvent to completely immerse the reactants, place the mixture solution in a three-necked flask equipped with a condenser reflux device and a mechanical stirrer, and heat the mixture in an oil bath at 65-80°C for 2-3h to obtain a waterborne polyurethane; S103. After the prepolymerization is completed, 0.5-1 parts of dimethylolbutyric acid are added to the obtained aqueous polyurethane by mass, and after reacting at 65-80° C. for 1-2 hours, 6-8 parts of hydroxy fluorosilicone oil are added, and the temperature is raised to 70-80° C. to modify the polyurethane, and the reaction is carried out for 2-3 hours to make the mixture hydrophobic; S104. After the reaction is completed, 2-5 parts of ethephon-modified β-cyclodextrin are added to the mixture obtained in step S103, and the mixture is reacted at 70-80°C for 1-2h; finally, 0.1-1 parts of triethylamine are added, and the reaction is maintained at the original temperature for 1-2h, and the reaction is terminated to obtain β-cyclodextrin-modified polyurethane; S2. Preparation of protective coated fabrics: S201. The β-cyclodextrin-modified polyurethane obtained by the reaction is sucked out with a dropper, and evenly coated on the surface of the glass sheet, and then placed in an oven at 70-80°C for 30-45 minutes for drying, and then taken out, and then allowed to stand at room temperature for 30-45 minutes. If there is no stickiness when touched, it proves that the film is successfully formed; S202. The film-forming β-cyclodextrin-modified polyurethane is applied to the surface of the fabric by roller coating, dipping or spraying, and then taken out and dried in an oven at 70-80°C. After cooling at room temperature, the β-cyclodextrin-based protective coating fabric is obtained.

2. The method for preparing a protective coating fabric based on β-cyclodextrin according to claim 1, characterized in that: In step S102, the catalyst is dibutyltin dilaurate.

3. The method for preparing a protective coating fabric based on β-cyclodextrin according to claim 2, characterized in that: The amount of the catalyst used is 0.5%-1% of the total volume of the mixture solution.

4. The method for preparing a protective coating fabric based on β-cyclodextrin according to claim 1, characterized in that: In step S102, the solvent is selected from one or more of acetone and DMF.

5. The method for preparing a protective coating fabric based on β-cyclodextrin according to claim 1, characterized in that: The structure and preparation route of the ethephon-modified cyclodextrin are as follows:

6. The method for preparing a protective coating fabric based on β-cyclodextrin according to claim 5, characterized in that: The structure and preparation route of the β-cyclodextrin modified polyurethane are as follows:

7. The method for preparing a protective coating fabric based on β-cyclodextrin according to claim 1, characterized in that: In step S202, a film-forming β-cyclodextrin-modified polyurethane is mixed with hydrophobic fumed silica and treated on the surface of the fabric by roller coating, dip coating or spraying. After being taken out, it is dried in an oven at 70-80°C and cooled at room temperature to obtain a super hydrophobic protective coating fabric based on β-cyclodextrin.

8. The method for preparing a protective coating fabric based on β-cyclodextrin according to claim 7, characterized in that: The mass ratio of the film-forming β-cyclodextrin-modified polyurethane to the hydrophobic fumed silica is 40-50:4.5-5.

9. A protective coating fabric based on β-cyclodextrin, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 8.

Citation Information

Cited By

  • Cyclodextrin-based water-resistant modified polyurethane film-forming agent and preparation method thereof

    CN119143968A

  • Preparation method and application of beta-cyclodextrin-polyurethane double-shell microcapsule

    CN119897039A

  • Profile sample preparation method of beta-cyclodextrin microsphere modified resin embedded powder material

    CN120628753A