High-temperature-resistant composite polytetrafluoroethylene cable and preparation method thereof
By using composite modified nano-silica and nano-tungsten trioxide and other materials in PTFE cables, combined with glass fiber and flame retardant, and using high-temperature sintering technology, the problem of high temperature resistance of PTFE cables is solved. , wear resistance and mechanical properties, significantly improving its overall performance.
Patent Information
- Application Number
- CN202411312442.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-10-25
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The overall performance of PTFE cables is poor, especially in terms of high temperature resistance, wear resistance and mechanical properties.
Composite modified nano-silica and nano-tungsten trioxide are used as filling materials, combined with glass fiber and flame retardant, and a tight insulation layer and shielding layer are formed through high-temperature sintering technology to improve the mechanical properties and high temperature resistance of the cable.
Significantly improves the hardness, wear resistance and flame retardancy of PTFE cables, improves the overall performance of the cable, and achieves tight bonding with conductors, making it suitable for applications in harsh environments.
Smart Images

Figure CN118841208A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cables, and in particular to a high temperature resistant composite polytetrafluoroethylene cable and a preparation method thereof. Background Art
[0002] With the development of society, people are using more and more electricity, and cables undoubtedly play an extremely important role. Cables are used to transmit electricity, signals or data, and are widely used in power plants, transmission systems, distribution systems and final power terminals. In actual applications, cables are more often used outdoors and are affected by various harsh environments and weather, as well as various construction environments. Therefore, people have higher and higher requirements for the comprehensive performance of cables, especially high temperature resistance and mechanical properties.
[0003] Polytetrafluoroethylene is a thermoplastic plastic whose carbon chain is wrapped by fluorine atoms to form a spiral structure. The carbon-fluorine bond has high bond energy and is not easy to break. Therefore, polytetrafluoroethylene has excellent chemical stability, corrosion resistance and temperature resistance, and is widely used in electrical appliances, chemical industry, aerospace and other fields. Polyimide is a material with excellent comprehensive performance. It is a kind of polymer material containing imide rings on the main chain. It has excellent heat resistance, low temperature resistance, solvent resistance, self-lubrication and flame retardancy. In recent years, research on polytetrafluoroethylene-polyimide composite insulated cables has become popular. However, defects may occur in the process of wrapping polyimide and polytetrafluoroethylene around the conductor, and the bonding between the conductor and the conductor may not be tight enough, which may affect the performance of the wire. In addition, polytetrafluoroethylene has poor wear resistance and mechanical properties.
[0004] Therefore, how to improve the comprehensive performance of polytetrafluoroethylene cables so that they have better high temperature resistance, wear resistance and mechanical properties is still an urgent problem to be solved. Summary of the invention
[0005] In view of this, the purpose of the present invention is to provide a high temperature resistant composite polytetrafluoroethylene cable and a preparation method thereof, so as to solve the problem that the current polytetrafluoroethylene cable has poor comprehensive performance.
[0006] Based on the above purpose, the present invention provides a high temperature resistant composite polytetrafluoroethylene cable, comprising a cable core, a protective layer wrapped outside the cable core, and a shielding layer wrapped outside the protective layer; the cable core comprises a plurality of insulating cores and a filling layer, the insulating cores are arranged parallel and longitudinally in the filling layer, and the filling layer tightly wraps the plurality of insulating cores; the insulating core comprises a cable obtained by winding a plurality of conducting wires, and an insulating layer wrapped outside the cable; The filling layer is a polytetrafluoroethylene mixed melt, which includes the following raw materials in parts by weight: 40-60 parts of polytetrafluoroethylene, 5-10 parts of tetrafluororubber, 2-6 parts of modified nano silicon dioxide, 0.8-1.5 parts of modified nano tungsten trioxide, 1-3 parts of glass fiber, 0.05-1 parts of antioxidant, and 0.5-1 parts of flame retardant; Wherein, the modified nano silicon dioxide and the modified nano tungsten trioxide are modified by a composite modifier, and the composite modifier consists of propylene glycol, acetic acid and silane coupling agent KH560.
[0007] Furthermore, the method for preparing the polytetrafluoroethylene mixed melt comprises the following steps: S1. Add nano silicon dioxide and nano tungsten trioxide to a mixture of propylene glycol and acetic acid, respectively, and then add silane coupling agent KH560 thereto, and then stir at 40-60r / min for 40-50min. After mixing evenly, dry at 70-80℃ for 6-8h to obtain modified nano silicon dioxide and modified nano tungsten trioxide. S2. After uniformly mixing polytetrafluoroethylene, tetrafluororubber, modified nano silicon dioxide, modified nano tungsten trioxide, glass fiber, antioxidant and flame retardant, smelting at 330-350° C. to obtain the polytetrafluoroethylene mixed melt.
[0008] Furthermore, the mass ratio of the polytetrafluoroethylene, the modified nano silicon dioxide and the modified nano tungsten trioxide is 20-30:1-3:0.5-1.
[0009] Furthermore, the mass ratio of the polytetrafluoroethylene, the modified nano silicon dioxide and the modified nano tungsten trioxide is 30:1:0.6.
[0010] Furthermore, the mass ratio of the mixed solution of propylene glycol and acetic acid in the composite modifier to the silane coupling agent KH560 is 1-3:3-5.
[0011] Furthermore, the mass ratio of the mixed solution of propylene glycol and acetic acid in the composite modifier to the silane coupling agent KH560 is 1:3.
[0012] Furthermore, the mass ratio of the propylene glycol to the acetic acid is 1-2:1-3; furthermore, the mass ratio of the propylene glycol to the acetic acid is 1:1.
[0013] Furthermore, the insulating layer includes a polytetrafluoroethylene sheath and a polyimide sheath; the polytetrafluoroethylene sheath is wrapped outside the polyimide sheath.
[0014] Furthermore, the thickness of the polyimide wrapping layer is 0.02-0.04 mm; the thickness of the polytetrafluoroethylene wrapping layer is 0.04-0.05 mm.
[0015] Furthermore, the thickness of the polyimide wrapping layer is 0.03 mm; the thickness of the polytetrafluoroethylene wrapping layer is 0.05 mm.
[0016] Furthermore, the protective layer is a glass fiber woven layer.
[0017] Furthermore, the shielding layer is a metal braided layer.
[0018] Furthermore, the shielding layer is a tinned copper wire braided layer.
[0019] Furthermore, the preparation method of the polytetrafluoroethylene mixed melt also includes pretreatment of glass fibers, and the glass fiber pretreatment method includes: placing the glass fibers in a silane coupling agent KH-550 solution, soaking for 1-2 hours at 25-30° C., and heat-treating and activating for 1-2 hours after drying.
[0020] The present invention also provides a method for preparing the high temperature resistant composite polytetrafluoroethylene cable, comprising the following steps: S1. Use a wrapping machine to wrap polyimide on the surface of the cable to obtain a polyimide wrapping layer, and then wrap a polytetrafluoroethylene raw tape on the outside of the polyimide wrapping layer to obtain a polytetrafluoroethylene wrapping layer; S2, sintering the polyimide sheath and the polytetrafluoroethylene sheath obtained in step S1 at a high temperature of 400-550° C. to obtain an insulated wire core wrapped by an insulating layer; S3, placing multiple insulated wire cores spaced apart from each other and parallel to each other in a screw extruder, and then extruding a tetrafluoroethylene mixed melt onto the surface of the insulated wire core through the screw extruder, so that the tetrafluoroethylene mixed melt is fully filled into the gaps between the multiple insulated wire cores, and the insulated wire cores are tightly wrapped, and a filling layer is formed after cooling to obtain a cable core wrapped by the filling layer; S4, weaving glass fiber on the surface of the cable core to form a protective layer; S5. Weave metal wires on the surface of the protective layer to form a shielding layer, and produce a high-temperature resistant composite polytetrafluoroethylene cable.
[0021] Beneficial effects of the present invention: The present invention provides a high-temperature resistant composite polytetrafluoroethylene cable and a preparation method thereof, which comprises a cable core, a protective layer and a shielding layer from the inside to the outside, wherein the cable core comprises an insulating core and a filling layer tightly wrapping the insulating core. The filling layer is a polytetrafluoroethylene mixed melt, and nano silicon dioxide and nano tungsten trioxide modified by a composite modifier are added to the melt. The addition of nano silicon dioxide and nano tungsten trioxide can synergistically improve the mechanical properties of polytetrafluoroethylene, improve its hardness, wear resistance, etc., and can reduce its water absorption; further, the present invention uses a composite modifier composed of propylene glycol, acetic acid and silane coupling agent KH560 to modify nano silicon dioxide and nano tungsten trioxide, and the mixed solution of propylene glycol and acetic acid can promote the hydrolysis of the silane coupling agent, thereby promoting the modification effect, reducing the agglomeration phenomenon, and significantly improving the dispersibility of nano silicon dioxide and nano tungsten trioxide in polytetrafluoroethylene. In addition, glass fiber is added to the filling layer to further improve the high temperature resistance and mechanical properties of the cable, and the added flame retardant can improve the flame retardancy of the cable.
[0022] In a high-temperature resistant composite polytetrafluoroethylene cable and a preparation method thereof provided by the present invention, the insulating layer wrapping the cable includes a polytetrafluoroethylene sheath and a polyimide sheath. The present invention adopts a high-temperature baking method to firmly combine the polytetrafluoroethylene sheath and the polyimide sheath into a whole, and also closely fit with the internal conductor, thereby improving the problem of loose bonding between the polyimide sheath and the conductor, and between the polyimide layer and the polytetrafluoroethylene layer in traditional polytetrafluoroethylene-polyimide cables.
[0023] The invention provides a high temperature resistant composite polytetrafluoroethylene cable and a preparation method thereof, which improves the mechanical properties and high temperature resistance of the cable, improves the comprehensive performance of the cable, and the preparation method is simple and can realize large-scale industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the drawings required to be used in the embodiments or the description of the prior art are briefly introduced below.
[0025] Figure 1 This is a schematic structural diagram of a high temperature resistant composite polytetrafluoroethylene cable prepared in Example 1 of the present invention; The markings in the figure are: 1. Cable; 2. Insulation layer; 21. Polyimide sheath; 22. Polytetrafluoroethylene sheath; 3. Filling layer; 4. Protective layer; 5. Shielding layer. DETAILED DESCRIPTION
[0026] In order to make the purpose, technical scheme and advantages of the present invention more clear, the present invention is further described in detail below in conjunction with specific embodiments. The present invention provides these embodiments to make the present invention thorough and complete, and to fully express the scope of the present invention to those skilled in the art. It should be noted that unless otherwise specifically stated, the relative arrangement of the parts and steps, the composition of the materials, the numerical expressions and the numerical values described in these embodiments should be interpreted as merely exemplary, rather than as limiting.
[0027] The embodiment of the present invention provides a high-temperature resistant composite polytetrafluoroethylene cable, comprising a cable core, a protective layer wrapped outside the cable core, and a shielding layer wrapped outside the protective layer; wherein the cable core comprises a plurality of insulating cores and a filling layer, the insulating cores are arranged parallel and longitudinally in the filling layer, and the filling layer tightly wraps the plurality of insulating cores; the insulating core comprises a cable obtained by winding a plurality of conductors, and an insulating layer wrapped outside the cable; wherein the filling layer is a polytetrafluoroethylene mixed melt, comprising the following raw materials in parts by weight: 40-60 parts of polytetrafluoroethylene , 5-10 parts of tetrafluororubber, 2-6 parts of modified nano-silicon dioxide, 0.8-1.5 parts of modified nano-tungsten trioxide, 1-3 parts of glass fiber, 0.05-1 parts of antioxidant, 0.5-1 parts of flame retardant; further, the mass ratio of polytetrafluoroethylene, modified nano-silicon dioxide and modified nano-tungsten trioxide is 20-30:1-3:0.5-1; and when the mass ratio of polytetrafluoroethylene, modified nano-silicon dioxide and modified nano-tungsten trioxide is 30:1:0.6, the mechanical properties of the cable are the best. When the amount of modified nano-silicon dioxide and modified nano-tungsten trioxide added is too small, the effect is not obvious, and when the amount added is too much, it will affect its dispersibility in polytetrafluoroethylene.
[0028] Furthermore, the modified nano-silicon dioxide and modified nano-tungsten trioxide are modified by a composite modifier, which is composed of propylene glycol, acetic acid and silane coupling agent KH560. Among them, the mixed solution of propylene glycol and acetic acid can promote the hydrolysis of the silane coupling agent, and further improve the dispersibility of nano-silicon dioxide and nano-tungsten trioxide. Among them, the mass ratio of the mixed solution of propylene glycol and acetic acid to the silane coupling agent KH560 is 1-3:3-5. When the mass ratio is 1:3, the mixed solution of propylene glycol and acetic acid has the greatest promoting effect on the silane coupling agent.
[0029] In the embodiment of the present invention, the insulating layer includes an inner polyimide sheath and an outer polytetrafluoroethylene sheath; the thickness of the polyimide sheath is 0.02-0.04 mm; the thickness of the polytetrafluoroethylene sheath is 0.04-0.05 mm. In the embodiment of the present invention, the protective layer is a glass fiber braided layer; the shielding layer is a metal braided layer, which can be a tinned copper wire braided layer.
[0030] In an embodiment of the present invention, the method for preparing a polytetrafluoroethylene mixed melt comprises the following steps: S1. Add nano silicon dioxide and nano tungsten trioxide to a mixture of propylene glycol and acetic acid, respectively, and then add silane coupling agent KH560 thereto, and then stir at 40-60r / min for 40-50min. After mixing evenly, dry at 70-80℃ for 6-8h to obtain modified nano silicon dioxide and modified nano tungsten trioxide. S2. After uniformly mixing polytetrafluoroethylene, tetrafluororubber, modified nano-silicon dioxide, modified nano-tungsten trioxide, glass fiber, antioxidant and flame retardant, smelting at 330-350° C. to obtain a polytetrafluoroethylene mixed melt.
[0031] The glass fiber can also be pre-treated glass fiber, which is first placed in a silane coupling agent KH-550 solution, soaked at 25-30°C for 1-2 hours, and then heat-treated and activated for 1-2 hours after drying. The glass fiber pre-treated with the coupling agent can be better dispersed in the melt.
[0032] Another embodiment of the present invention provides a method for preparing a high temperature resistant composite polytetrafluoroethylene cable, comprising the following steps: S1. Use a wrapping machine to wrap polyimide on the surface of the cable to obtain a polyimide wrapping layer, and then wrap a polytetrafluoroethylene raw tape on the outside of the polyimide wrapping layer to obtain a polytetrafluoroethylene wrapping layer; S2, sintering the polyimide sheath and the polytetrafluoroethylene sheath obtained in step S1 at a high temperature of 400-550° C. to obtain an insulated wire core wrapped by an insulating layer; S3, placing multiple insulated wire cores spaced apart from each other and parallel to each other in a screw extruder, and then extruding a tetrafluoroethylene mixed melt onto the surface of the insulated wire core through the screw extruder, so that the tetrafluoroethylene mixed melt is fully filled into the gaps between the multiple insulated wire cores, and the insulated wire cores are tightly wrapped, and a filling layer is formed after cooling to obtain a cable core wrapped by the filling layer; S4, weaving glass fiber on the surface of the cable core to form a protective layer; S5. Weave metal wires on the surface of the protective layer to form a shielding layer, and produce a high-temperature resistant composite polytetrafluoroethylene cable.
[0033] The present invention will be further described below in conjunction with specific embodiments, but this should not be construed as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by technicians in this field based on the above-mentioned contents of the present invention still fall within the scope of protection of the present invention.
[0034] Unless otherwise specified, the materials, reagents, etc. involved below are all commercially available products well known to those skilled in the art; unless otherwise specified, the methods described are all methods well known in the art. Unless otherwise defined, the technical terms or scientific terms used should have the common meanings understood by ordinary technicians in the field to which the present invention belongs.
[0035] Example 1
[0036] S1. Use a wrapping machine to wrap polyimide on the surface of the cable to obtain a polyimide wrapping layer, and then wrap a polytetrafluoroethylene raw tape on the outside of the polyimide wrapping layer to obtain a polytetrafluoroethylene wrapping layer; S2, sintering the polyimide sheath and the polytetrafluoroethylene sheath obtained in step S1 at a high temperature of 500° C. to obtain an insulated wire core wrapped by an insulating layer; S3, placing the glass fiber in a silane coupling agent KH-550 solution, soaking it at 28°C for 1.5 hours, and then heat-treating and activating it for 1.5 hours after drying; S4, adding nano silicon dioxide to a mixture of propylene glycol and acetic acid, then adding silane coupling agent KH560, stirring at 55r / min for 40min, mixing evenly, and drying at 75°C for 8h to obtain modified nano silicon dioxide; adding nano tungsten trioxide to a mixture of propylene glycol and acetic acid, then adding silane coupling agent KH560, stirring at 45r / min for 40min, mixing evenly, and drying at 75°C for 8h to obtain modified nano tungsten trioxide; wherein the mass ratio of propylene glycol, acetic acid and silane coupling agent is 1:1:6; S5, after uniformly mixing 60 parts of polytetrafluoroethylene, 8 parts of tetrafluororubber, 2 parts of modified nano-silicon dioxide, 1.2 parts of modified nano-tungsten trioxide, 1 part of glass fiber, 0.5 parts of antioxidant and 0.8 parts of flame retardant, smelting at 345° C. to obtain the polytetrafluoroethylene mixed melt; S6, placing multiple insulated wire cores spaced apart from each other and parallel to each other in a screw extruder, and then extruding a tetrafluoroethylene mixed melt onto the surface of the insulated wire core through the screw extruder, so that the tetrafluoroethylene mixed melt is fully filled into the gaps between the multiple insulated wire cores, and the insulated wire cores are tightly wrapped, and a filling layer is formed after cooling to obtain a cable core wrapped by the filling layer; S7. Weave glass fiber on the surface of the cable core to form a protective layer; S8. Weave metal wires on the surface of the protective layer to form a shielding layer to obtain a high-temperature resistant composite polytetrafluoroethylene cable.
[0037] Example 2
[0038] S1. Use a wrapping machine to wrap polyimide on the surface of the cable to obtain a polyimide wrapping layer, and then wrap a polytetrafluoroethylene raw tape on the outside of the polyimide wrapping layer to obtain a polytetrafluoroethylene wrapping layer; S2, sintering the polyimide sheath and the polytetrafluoroethylene sheath obtained in step S1 at a high temperature of 480° C. to obtain an insulated wire core wrapped by an insulating layer; S3, placing the glass fiber in a silane coupling agent KH-550 solution, soaking it at 28°C for 1 hour, and then heat-treating and activating it for 1.5 hours after drying; S4, adding nano silicon dioxide to a mixture of propylene glycol and acetic acid, then adding silane coupling agent KH560, stirring at 50r / min for 45min, mixing evenly, and drying at 70°C for 8h to obtain modified nano silicon dioxide; adding nano tungsten trioxide to a mixture of propylene glycol and acetic acid, then adding silane coupling agent KH560, stirring at 50r / min for 45min, mixing evenly, and drying at 70°C for 8h to obtain modified nano tungsten trioxide; wherein the mass ratio of propylene glycol, acetic acid and silane coupling agent is 1:1:5; S5, after uniformly mixing 55 parts of polytetrafluoroethylene, 6 parts of tetrafluororubber, 3 parts of modified nano-silicon dioxide, 1 part of modified nano-tungsten trioxide, 2 parts of glass fiber, 0.1 parts of antioxidant and 0.5 parts of flame retardant, smelting at 350° C. to obtain the polytetrafluoroethylene mixed melt; S6, placing multiple insulated wire cores spaced apart from each other and parallel to each other in a screw extruder, and then extruding a tetrafluoroethylene mixed melt onto the surface of the insulated wire core through the screw extruder, so that the tetrafluoroethylene mixed melt is fully filled into the gaps between the multiple insulated wire cores, and the insulated wire cores are tightly wrapped, and a filling layer is formed after cooling to obtain a cable core wrapped by the filling layer; S7. Weave glass fiber on the surface of the cable core to form a protective layer; S8. Weave metal wires on the surface of the protective layer to form a shielding layer to obtain a high-temperature resistant composite polytetrafluoroethylene cable.
[0039] Example 3
[0040] S1. Use a wrapping machine to wrap polyimide on the surface of the cable to obtain a polyimide wrapping layer, and then wrap a polytetrafluoroethylene raw tape on the outside of the polyimide wrapping layer to obtain a polytetrafluoroethylene wrapping layer; S2, sintering the polyimide sheath and the polytetrafluoroethylene sheath obtained in step S1 at a high temperature of 420° C. to obtain an insulated wire core wrapped by an insulating layer; S3, placing the glass fiber in a silane coupling agent KH-550 solution, soaking it at 30°C for 1.5 hours, and then heat-treating and activating it for 1 hour after drying; S4, adding nano silicon dioxide to a mixture of propylene glycol and acetic acid, then adding silane coupling agent KH560, stirring at 60r / min for 40min, mixing evenly, and drying at 75°C for 6h to obtain modified nano silicon dioxide; adding nano tungsten trioxide to a mixture of propylene glycol and acetic acid, then adding silane coupling agent KH560, stirring at 60r / min for 40min, mixing evenly, and drying at 75°C for 6h to obtain modified nano tungsten trioxide; wherein the mass ratio of propylene glycol, acetic acid and silane coupling agent is 1:2:6; S5, after uniformly mixing 40 parts of polytetrafluoroethylene, 6 parts of tetrafluororubber, 2 parts of modified nano-silicon dioxide, 1 part of modified nano-tungsten trioxide, 1 part of glass fiber, 0.06 parts of antioxidant and 0.5 parts of flame retardant, smelting at 350° C. to obtain the polytetrafluoroethylene mixed melt; S6, placing multiple insulated wire cores spaced apart from each other and parallel to each other in a screw extruder, and then extruding a tetrafluoroethylene mixed melt onto the surface of the insulated wire core through the screw extruder, so that the tetrafluoroethylene mixed melt is fully filled into the gaps between the multiple insulated wire cores, and the insulated wire cores are tightly wrapped, and a filling layer is formed after cooling to obtain a cable core wrapped by the filling layer; S7. Weave glass fiber on the surface of the cable core to form a protective layer; S8. Weave metal wires on the surface of the protective layer to form a shielding layer to obtain a high-temperature resistant composite polytetrafluoroethylene cable.
[0041] Example 4
[0042] S1. Use a wrapping machine to wrap polyimide on the surface of the cable to obtain a polyimide wrapping layer, and then wrap a polytetrafluoroethylene raw tape on the outside of the polyimide wrapping layer to obtain a polytetrafluoroethylene wrapping layer; S2, sintering the polyimide sheath and the polytetrafluoroethylene sheath obtained in step S1 at a high temperature of 550° C. to obtain an insulated wire core wrapped by an insulating layer; S3, adding nano silicon dioxide to a mixture of propylene glycol and acetic acid, then adding silane coupling agent KH560, stirring at 48r / min for 50min, mixing evenly, and drying at 80°C for 6.5h to obtain modified nano silicon dioxide; adding nano tungsten trioxide to a mixture of propylene glycol and acetic acid, then adding silane coupling agent KH560, stirring at 48r / min for 50min, mixing evenly, and drying at 80°C for 6.5h to obtain modified nano tungsten trioxide; wherein the mass ratio of propylene glycol, acetic acid and silane coupling agent is 1.5:1:5; S4, after uniformly mixing 58 parts of polytetrafluoroethylene, 7 parts of tetrafluororubber, 6 parts of modified nano-silicon dioxide, 1.5 parts of modified nano-tungsten trioxide, 3 parts of glass fiber, 0.9 parts of antioxidant and 0.8 parts of flame retardant, smelting at 350° C. to obtain the polytetrafluoroethylene mixed melt; S5, placing multiple insulated wire cores spaced apart from each other and parallel to each other in a screw extruder, and then extruding a tetrafluoroethylene mixed melt onto the surface of the insulated wire core through the screw extruder, so that the tetrafluoroethylene mixed melt is fully filled into the gaps between the multiple insulated wire cores, and the insulated wire cores are tightly wrapped, and a filling layer is formed after cooling to obtain a cable core wrapped by the filling layer; S6. Weave glass fiber on the surface of the cable core to form a protective layer; S7. Weave metal wires on the surface of the protective layer to form a shielding layer to obtain a high-temperature resistant composite polytetrafluoroethylene cable.
[0043] Comparative Example 1 The difference between Comparative Example 1 and Example 1 is that step S4 is omitted, the nano silicon dioxide and nano tungsten trioxide added in step S5 are not modified, and the remaining steps are the same as those in Example 1.
[0044] Comparative Example 2 The difference between Comparative Example 2 and Example 1 is that the nano silicon dioxide and nano tungsten trioxide in step S4 are only modified with a silane coupling agent, and the remaining steps are the same as those in Example 1.
[0045] Comparative Example 3 The difference between Comparative Example 3 and Example 1 is that the mass ratio of polytetrafluoroethylene, modified nano-silicon dioxide and modified nano-tungsten trioxide is 20:5:2, and the remaining steps are the same as those in Example 1.
[0046] Comparative Example 4 The difference between Comparative Example 4 and Example 1 is that step S2 is omitted, the insulating layer is a polyimide sheathing layer and a polytetrafluoroethylene sheathing layer that are not sintered, and the remaining steps are the same as those in Example 1.
[0047] Performance Testing The high temperature resistant cables prepared in Examples 1-4 and Comparative Examples 1-4 were cut into 1.2 m lengths and subjected to the following tests.
[0048] Hardness: According to GB / T 2411-2008 test, the same sample is 6 mm apart, 5 hardness values are measured and the average value is calculated; Wear performance: The test load is 15N, the reciprocating frequency is 1Hz, the time is 15 min, the grinding distance is 10 mm, and the grinding ball is a 304 stainless steel ball with a diameter of 10 mm. The friction coefficient of the composite material is recorded. Each sample is repeated 6 times and the average value is taken. The wear scar morphology of the composite material is observed using a three-dimensional profiler, the wear amount is analyzed, and the wear rate is calculated; Fire resistance: According to GB / T 19216.2-2021 Line integrity test for cables or optical cables under flame conditions Part 2: Fire with a flame temperature of not less than 830 °C and impact vibration, test method for cables with a rated voltage of 0.6 / 1kV and below and an outer diameter not exceeding 20 mm, the test cable length is 1.2m, the voltage is 380v, and the impact generating device is started after the blowtorch is ignited. After 5 minutes and every 5 minutes thereafter, knock on the test ladder. Each time the knocking rod is lifted from the test ladder within 20 seconds after knocking, turn on the power after the timer starts. The fire supply and knocking time is 90 minutes. Determine whether the power supply can be sustained based on the indication of the terminal indicator light. If it goes out within 30 minutes, the fire resistance level is judged to be V3. If it goes out within 30-60 minutes, the fire resistance level is judged to be V2. If it goes out within 60-90 minutes, the fire resistance level is judged to be V1. If it does not go out within 90 minutes, the fire resistance level is judged to be V0, where V0 indicates the best fire resistance performance, V1 is the second, and V3 is the worst. The test results are shown in Table 1.
[0049] Table 1 Performance test results Shore Hardness Wear rate μm / s Fire resistance level Example 1 72 0.05 V0 Example 2 68 0.08 V0 Example 3 71 0.07 V0 Example 4 65 0.09 V0 Comparative Example 1 49 0.11 V1 Comparative Example 2 55 0.15 V0 Comparative Example 3 51 0.09 V0 Comparative Example 4 61 0.085 V1 It is not difficult to see from the above test results that the high temperature resistant composite polytetrafluoroethylene cable prepared in Example 1 of the present invention has reached the best level in hardness, wear resistance and fire resistance. When nano silicon dioxide and nano tungsten trioxide are not modified or only modified with coupling agent, their hardness and wear resistance are reduced; according to the comparison between comparative example 4 and example 1, it can also be seen that when the insulation layer is treated by high temperature sintering during the preparation of the cable, the fire resistance of the prepared cable is reduced. In summary, the high temperature resistant composite polytetrafluoroethylene cable proposed by the present invention has excellent mechanical properties and high temperature resistance.
[0050] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.
Claims
1. A high temperature resistant composite polytetrafluoroethylene cable, characterized in that: The cable comprises a cable core, a protective layer wrapped around the cable core, and a shielding layer wrapped around the protective layer; the cable core comprises multiple insulated wire cores and a filling layer, the insulated wire cores are arranged parallel and longitudinally in the filling layer, and the filling layer tightly wraps the multiple insulated wire cores; the insulated wire core comprises a cable obtained by winding a plurality of wires, and an insulating layer wrapped around the cable; The filling layer is a polytetrafluoroethylene mixed melt, which includes the following raw materials in parts by weight: 40-60 parts of polytetrafluoroethylene, 5-10 parts of tetrafluororubber, 2-6 parts of modified nano-silicon dioxide, 0.8-1.5 parts of modified nano-tungsten trioxide, 1-3 parts of glass fiber, 0.05-1 parts of antioxidant, and 0.5-1 parts of flame retardant; The modified nano silicon dioxide and the modified nano tungsten trioxide are modified by a composite modifier, and the composite modifier consists of propylene glycol, acetic acid and silane coupling agent KH560.
2. The high temperature resistant composite polytetrafluoroethylene cable according to claim 1, characterized in that: The preparation method of the polytetrafluoroethylene mixed melt comprises the following steps: S1. Add nano-silicon dioxide and nano-tungsten trioxide to a mixture of propylene glycol and acetic acid, respectively, and then add silane coupling agent KH560 thereto, and then stir at 40-60 r / min for 40-50 min. After mixing evenly, dry at 70-80 ° C for 6-8 h to obtain modified nano-silicon dioxide and modified nano-tungsten trioxide; S2. After uniformly mixing polytetrafluoroethylene, tetrafluororubber, modified nano-silicon dioxide, modified nano-tungsten trioxide, glass fiber, antioxidant and flame retardant, smelting at 330-350° C. to obtain the polytetrafluoroethylene mixed melt.
3. The high temperature resistant composite polytetrafluoroethylene cable according to claim 1, characterized in that: The mass ratio of the polytetrafluoroethylene, the modified nano-silicon dioxide and the modified nano-tungsten trioxide is 20-30:1-3:0.5-1.
4. The high temperature resistant composite polytetrafluoroethylene cable according to claim 1, characterized in that: The mass ratio of the mixed solution of propylene glycol and acetic acid in the composite modifier to the silane coupling agent KH560 is 1-3:3-5.
5. The high temperature resistant composite polytetrafluoroethylene cable according to claim 1, characterized in that: The insulating layer comprises a polytetrafluoroethylene wrapping layer and a polyimide wrapping layer; the polytetrafluoroethylene wrapping layer is wrapped outside the polyimide wrapping layer.
6. The high temperature resistant composite polytetrafluoroethylene cable according to claim 5, characterized in that: The thickness of the polyimide wrapping layer is 0.02-0.04 mm; the thickness of the polytetrafluoroethylene wrapping layer is 0.04-0.05 mm.
7. The high temperature resistant composite polytetrafluoroethylene cable according to claim 1, characterized in that: The protective layer is a glass fiber braided layer.
8. The high temperature resistant composite polytetrafluoroethylene cable according to claim 1, characterized in that: The shielding layer is a metal braided layer.
9. The high temperature resistant composite polytetrafluoroethylene cable according to claim 1, characterized in that: The preparation method of the polytetrafluoroethylene mixed melt further includes pretreatment of glass fibers, wherein the glass fibers are placed in a silane coupling agent KH-550 solution, immersed at 25-30° C. for 1-2 hours, and then heat-treated and activated for 1-2 hours after drying.
10. The method for preparing a high temperature resistant composite polytetrafluoroethylene cable according to any one of claims 1 to 9, characterized in that: The steps include: S1. Using a wrapping machine, first wrap polyimide around the surface of the cable to obtain a polyimide wrapping layer, and then wrap polytetrafluoroethylene raw tape around the polyimide wrapping layer to obtain a polytetrafluoroethylene wrapping layer; S2, sintering the polyimide wrapping layer and the polytetrafluoroethylene wrapping layer obtained in step S1 at a high temperature of 400-550° C. to obtain an insulated wire core wrapped by an insulating layer; S3, placing multiple insulated wire cores spaced apart and parallel to each other longitudinally in a screw extruder, and then extruding a tetrafluoroethylene mixed melt onto the surface of the insulated wire cores through the screw extruder, so that the tetrafluoroethylene mixed melt fully fills the gaps between the multiple insulated wire cores, and tightly wraps the insulated wire cores, and forming a filling layer after cooling to obtain a cable core wrapped by the filling layer; S4. Weave glass fiber on the surface of the cable core to form a protective layer; S5. Weaving metal wires on the surface of the protective layer to form a shielding layer, and preparing a high-temperature resistant composite polytetrafluoroethylene cable.
Citation Information
Patent Citations
Preparation method of coupled graft polymerization modified nanometer yttrium oxide lubricating material
CN103627211A
High-temperature electric cable
CN103680715A
Nano silicon dioxide modified epoxy resin composite material and preparation method thereof
CN104448716A
Modified nano-zinc oxide varistor material and preparation method thereof
CN108264343A
Flame-resistant toughening nylon composite material for new energy automobile accessories as well as preparation method thereof
CN109233262A
Cited By
High-temperature engine cable assembly
CN120601350A