High-purity and high-performance Fe16N2 magnetic powder and preparation method thereof
By using small nanometer units to form micron-sized particles in the preparation of Fe16N2 magnetic powder, using spray pyrolysis or hydrothermal methods to prepare Fe2O3 particles with porous or flaky structures, and performing low-temperature nitriding, the problem of low nitridation purity of micron particles has been solved. and nanoparticle sintering problems, achieving the preparation of high-purity and high-performance Fe16N2 magnetic powder.
Patent Information
- Application Number
- CN202410836002.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-26
- Publication Date
- 2024-10-25
AI Technical Summary
In the existing Fe16N2 magnetic powder preparation method, the nitridation purity of micron particles is low, and the nanoparticles are easily sintered into large particles, resulting in a decrease in magnetic properties, and the process is difficult, especially high-purity preparation.
Small nano-units are used to form micron-sized particles. Fe2O3 particles with porous or flaky structures are prepared by spray pyrolysis or hydrothermal methods, and Fe16N2 magnetic powder is formed on the surface of each nano-unit through low-temperature nitridation reaction to avoid sintering and improve purity. and performance.
It achieves the preparation of high-purity (>80%) and high-performance Fe16N2 magnetic powder, simplifies the process, reduces equipment requirements and costs, avoids impurities affecting magnetic properties, and improves nitriding efficiency.
Smart Images

Figure CN118841229A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of rare earth-free permanent magnetic materials, and in particular relates to a high-purity, high-performance Fe 16 N2 magnetic powder and preparation method thereof. Background Art
[0002] Permanent magnetic materials are key materials in the industrial field and are widely used in large and small to medium-sized equipment such as generators and motors by converting electrical energy into kinetic energy. In recent years, the production and demand for new energy vehicles are rapidly increasing due to the increasing importance of replacing petroleum energy and low-carbon green growth. Since such automobile engines require high efficiency, light weight and miniaturization of electric motors, the demand and research on rare earth-based permanent magnetic materials such as neodymium iron boron, samarium cobalt, samarium iron nitrogen, etc. are increasing explosively. As the degree of dependence on energy increases, the demand for energy-saving, low-maintenance and low-cost magnetic materials is also increasing. After rare earths were positioned as strategic materials by various countries and their supply was restricted, rare earth materials had problems with unstable supply and export restrictions, resulting in rising prices. Therefore, researchers have turned their focus to rare earth-free alternatives to rare earth magnets. Among the many rare earth permanent magnet substitutes, Fe 16 N2 because the environment is rich in Fe and N elements, and Fe 16 N2 is considered the most promising alternative due to its huge saturation magnetization and relatively high magnetocrystalline anisotropy.
[0003] Fe 16 Since its discovery, N2 materials have attracted great attention from researchers. 16 Continuous work has been done on the preparation process and basic theory of N2 materials. Through continuous practice, people have developed methods such as sputtering, nitrogen ion implantation, ball milling impact and low-temperature nitriding. These methods have their own characteristics. Among them, sputtering and nitrogen ion implantation have high requirements for equipment. The purity and performance of ball milling impact in the reported literature are not very ideal. For industrial production, the equipment cost is low and it can be mass-produced. Among various methods, low-temperature nitriding is a good choice.
[0004] Metastable Fe 16 The preparation of N2 phase is difficult, especially the preparation of high purity is very difficult. In the reported studies, Fe 16N2 has a critical thickness value. If the critical thickness is exceeded, nitrides Fe4N or Fe3N with high nitrogen content will be produced. In addition, the size of the particles will greatly affect the final nitriding result. The purity of nitriding using micron particles is not high, generally around 60%. And the nitriding effect of pure iron particles is far lower than that of iron particles obtained by iron oxide reduction. In addition to being more expensive, the use of small-sized nano-iron oxide particles is also prone to sintering into large particles during the reduction process. High-pressure reduction is required to reduce the reduction temperature or surface coating with SiO2, Al2O3, etc. is required to reduce agglomeration and sintering. For example, patent CN1670870A discloses a Fe 16 The preparation method of N2 magnetic powder uses goethite with an average particle size less than or equal to 20nm and containing 0.1-30at% of solid dissolved Al, and adheres anti-sintering agents such as Al, Si, and rare earth elements (which may include Y) on the surface of the particles to reduce sintering. However, the adhesion of non-magnetic substances such as Si will inevitably lead to a decrease in overall magnetism. In order to obtain a better nitriding effect, the use of rare earth elements as anti-sintering agents has its disadvantages from the perspective of cost and resource protection.
[0005] In order to better solve the above problems, the present invention proposes a high-purity, high-performance Fe 16 N2 magnetic powder and preparation method thereof. Summary of the invention
[0006] The present invention proposes a high-purity, high-performance Fe 16 N2 magnetic powder and its preparation method. The main method is to prepare nano-units to form micron-sized particles, but still maintain a high surface area through porous or lamellar overlapping structures, so that nitridation actually still starts from the surface of each nano-unit (equivalent to non-sintered nanoparticles) to prepare high-purity Fe 16 N2.
[0007] The present invention adopts the following technical solution:
[0008] In the first aspect, the present invention provides a high-purity, high-performance Fe 16 The preparation method of N2 magnetic powder, the specific steps are as follows:
[0009] Prepare Fe2O3 particles of micrometer size composed of nano-units and retaining the independent integrity of the surface structure of the nano-units;
[0010] The prepared Fe2O3 particles are reduced to obtain micron-sized pure Fe particles consisting of nano-sized units with pores.
[0011] The prepared pure Fe particles are subjected to low-temperature nitridation reaction, which reacts on the surface of each nanounit to prepare the required Fe 16 N2 magnetic powder.
[0012] Preferably, the preparation of Fe2O3 particles is specifically as follows:
[0013] The spherical particles of Fe2O3 and pore-forming agent embedded in each other are prepared by spray thermal decomposition method, and then the pore-forming agent is removed by ultrasonic dissolution with deionized water to obtain micron-scale porous spherical Fe2O3 particles composed of overlapping nano-columnar small units;
[0014] Alternatively, a precursor composed of overlapping nanosheets is prepared by a hydrothermal method, and then a micron-sized spherical Fe2O3 particle composed of overlapping nanosheets is obtained by high-temperature heat treatment, that is, micron-sized porous spherical Fe2O3 particles.
[0015] Preferably, the spray pyrolysis method is to prepare porous spherical micron Fe2O3 particles by using a pore-forming agent to assist nano-columnar small units, specifically:
[0016] The water-soluble iron salt and the pore-forming agent are mixed and dissolved in deionized water, and a uniform precursor solution is formed by diffusion through ultrasonic vibration to obtain a spray precursor solution;
[0017] Using the principle of ultrasonic spray, the precursor solution is atomized into mist-like small droplets, which are driven by carrier gas to undergo dehydration reaction and pyrolysis oxidation reaction in a three-stage tube furnace to obtain Fe2O3 and pore-forming agent interlocking particles, which are collected in the tail collector.
[0018] The interlocking particles are ultrasonically stirred in deionized water to fully dissolve the pore-forming agent, and then centrifugally dried to obtain porous spherical micron Fe2O3 particles consisting of nano-columnar small units.
[0019] Preferably, the pore-forming agent in the precursor is a soluble metal salt such as KCl, KNO3, or NaCl, and the molar ratio of the pore-forming agent to the water-soluble iron salt is 0.5 to 10:1;
[0020] Preferably, the carrier gas in the tubular furnace is air with a flow rate of 5-10 L / min, the temperature of the first stage evaporation and dehydration is 300-500°C, and the temperature of the second and third stages decomposition and oxidation is 800°C.
[0021] Preferably, the micron-sized spherical Fe2O3 particles composed of overlapping nanosheets are obtained by hydrothermal method and high-temperature heat treatment, specifically:
[0022] The water-soluble iron salt and urea are stirred and uniformly dissolved in deionized water or an organic solvent to form a hydrothermal reaction body solution;
[0023] The hydrothermal reaction precursor solution is placed in a polytetrafluoroethylene liner, and is placed in a reaction kettle and transferred to a constant temperature oven for hydrothermal reaction.
[0024] The precursor obtained by the hydrothermal reaction is washed in deionized water and anhydrous ethanol, centrifugally dried and placed in a tubular furnace, first subjected to high-temperature treatment in an inert gas, and then subjected to high-temperature oxidation in an air atmosphere to obtain rice-like small units that overlap each other to form high specific surface area micron Fe2O3 particles.
[0025] Preferably, the water-soluble iron salt is a water-soluble ferric salt or a water-soluble ferrous salt, more preferably FeCl3·6H2O, the organic solvent is preferably ethylene glycol, and the molar ratio of urea to iron salt is 2 to 3:1.
[0026] Preferably, the hydrothermal reaction temperature is 140-180° C., and the reaction time is 10-20 h.
[0027] Preferably, the temperature of the inert gas high temperature treatment and the air atmosphere high temperature oxidation reaction is between 300°C and 400°C.
[0028] Preferably, the high temperature thermal reaction is first carried out in an inert gas for 0.5 to 2 hours to evaporate and remove organic matter or aqueous solution, and then in air for 0.5 to 2 hours to fully oxidize and form Fe2O3.
[0029] Preferably, the reducing atmosphere used in the reduction of Fe2O3 particles is hydrogen, or a mixture of hydrogen and an inert gas, with a hydrogen flow rate of 100 to 400 sccm. Since the particles are micron-sized, they are not easy to sinter and agglomerate, and increasing the reduction temperature is conducive to accelerating the hydrogen reduction rate and reducing the reduction time. Therefore, the reduction temperature is preferably 410 to 500°C, and the reduction time is 1 to 3 hours. Preferably, the inert gas used when the pure Fe particles are cooled to the nitriding temperature is helium or argon.
[0030] Preferably, the gas atmosphere used for low-temperature nitridation of pure Fe particles is ammonia, the ammonia flow rate is 100-200 sccm, the temperature is 170-190° C., and the nitridation time is 6-40 hours.
[0031] In a second aspect, the present invention provides a porous spherical micron-sized Fe 16 N2 magnetic powder.
[0032] The Fe 16 N2 magnetic powder is composed of several Fe 16 N2 nanometer-thick small units, with high specific surface area and micron-sized structure, each small unit is required to be 100nm thick, Fe 16 N2 purity is greater than 80%, and specific surface area is greater than 8.0m 2 / g, magnetic powder size is 1-10 microns.
[0033] Compared with the prior art, the beneficial effects of the present invention are at least:
[0034] The present invention mainly prepares nanometer columnar small units to form porous spherical micrometer structures by adding pore-forming agents in the precursor by spray pyrolysis method and prepares nanometer sheet-like small units to overlap each other to form a high specific surface micrometer structure by hydrothermal method, or avoids the problems of low purity of micrometer solid particles and sintering of nanometer small particles by constructing a micrometer-sized structure composed of nanometer small units with basically intact surfaces, and prepares high-purity and high-performance Fe 16 N2 magnetic powder.
[0035] The present invention manufactures high-surface-area micron-sized spherical Fe2O3 composed of nano-units. On a macro level, the micron size itself avoids or reduces sintering, and there is no need to reduce the reduction temperature by high-pressure reduction to avoid sintering or add anti-sintering agents. The process is simpler and more energy-efficient, and other impurities will not be introduced to affect the magnetic properties. In addition, the microscopic nitridation of the particles occurs in nanostructures (nano-units or nano-sheets), which have a high specific surface area. The contact area between the alloy and the reaction gas is increased during the nitridation process, and the depth required for nitridation is also reduced, which reduces the generation of high-nitrogen Fe4N or Fe3N, and can obtain Fe with higher purity and performance. 16 N2 magnetic powder; the equipment requirements are not high, and the process is simple and can meet the needs of industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 Preparation of nano-columnar units by spray pyrolysis to form porous spherical micron-Fe 16 N2 magnetic powder process route.
[0037] Figure 2 Nano-columnar small units form porous spherical micro-Fe 16 SEM image of N2 magnetic powder.
[0038] Figure 3 The hydrothermal method is used to prepare nanosheet-like small units that overlap each other to form a high specific surface area micron Fe 16 N2 magnetic powder process route.
[0039] Figure 4 Nano-sheet units are connected to form micron Fe 16 SEM image of N2 magnetic powder. DETAILED DESCRIPTION
[0040] As mentioned above, the inventor of this case proposed the technical solution of the present invention after long-term research and extensive practice, and its main basis includes at least:
[0041] (1) Pure Fe is obtained by reducing the high-surface-area micron-sized spherical Fe2O3 composed of nano-units. During the nitridation process, interstitial nitrogen atoms enter the lattice gap to form Fe 16 N2 is easier, and during the reduction process, as oxygen atoms leave the lattice, a transmission path is provided for the migration of nitrogen atoms, and pores appear to increase the surface, all of which are beneficial to Fe 16 The present invention manufactures high-surface-area micron-sized spherical Fe2O3 composed of nano-units and then reduces the obtained pure Fe with pores for nitridation, which is further beneficial to Fe 16 Formation of N2.
[0042] (2) Low-temperature nitriding As the degree of nitridation increases, high-nitrogen Fe4N or Fe3N is easily formed on the surface. The particle size of nitrided Fe has an influence on the Fe 16 The maximum yield of N2 is an important factor, Fe 16 N2 is formed from the particle surface. The larger the particle, the more Fe 16 The yield of N2 is lower. Therefore, the nitridation purity of micron-sized particles is not high, and nanoparticles are prone to sintering to form large particles during the high-temperature reduction process. Nanoparticles need to undergo special treatment. High-pressure reduction can be used to lower the reduction temperature, but the equipment and energy requirements are higher. Anti-sintering agents can also be added or the surface is coated with non-sintering materials to reduce sintering, but other elements are easily introduced to reduce magnetic properties, and the process may be more complicated and costly. The present invention adopts nano-units prepared by spraying or hydrothermal method to form micron-sized porous particles. The particles are micron-sized as a whole, but the actual nitridation occurs on the surface of each nano-sized unit, which ensures that nitridation occurs in a small size while avoiding sintering, thereby meeting the requirements for preparing high-purity Fe 16 Precursor conditions of N2.
[0043] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the accompanying drawings and Examples. In the present invention, unless otherwise specified, the raw materials used are conventional commercial products in the art. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.
[0044] The present invention provides a method for preparing high-purity and high-performance Fe16N2 magnetic powder by low-temperature nitridation of micron-sized particles composed of nano-units. It mainly includes two aspects. On the one hand, porous spherical micron Fe is prepared by spraying nano-columnar units. 16 On the other hand, the hydrothermal method is used to prepare nanosheet-like small units that overlap each other to form a high specific surface area micron Fe 16 N2 magnetic powder.
[0045] The embodiment of the present invention provides a method for preparing a porous spherical micron Fe by a spray method. 16 N2 magnetic powder, such as Figure 1 The specific steps are as follows:
[0046] Step 1: Mix and dissolve a water-soluble iron salt and a pore-forming agent in deionized water to form an atomized precursor solution;
[0047] The water-soluble iron salt is a water-soluble ferric salt or a water-soluble ferrous salt, preferably one or more combinations of ferric nitrate, ferrous nitrate, ferric chloride, ferrous chloride, ferrous sulfate, and ferrous sulfate. The pore-forming agent is a metal salt such as KCl, KNO3, and NaCl, and the molar ratio of the pore-forming agent to the iron salt is 0.5 to 10:1.
[0048] Step 2: Place the precursor solution in a container and place it in a water tank, place a 1.7MHz frequency vibrator in the tank, adjust the distance between the vibrator and the container to ensure that the precursor solution in the container can be atomized. The precursor solution is turned into an atomized state through the principle of ultrasonic spray, and the air compressed by the air compressor is used as a carrier gas to drive the atomized droplets through a tubular furnace with three temperature zones for evaporation, dehydration, decomposition and oxidation (first evaporation and dehydration in the first temperature zone, and then decomposition in the second and third temperature zones to form spherical particles of oxides and pore-forming agents interlocking with each other), forming iron oxide and pore-forming agents interlocking particles, and collected in the collection device at the end of the tubular furnace.
[0049] The flow rate of the compressed air carrier gas is 5-10L / min, which ensures that the atomized droplets undergo sufficient thermal reaction before passing through the tube furnace. The three-temperature zone tube furnace has an evaporation and dehydration temperature of 300-500°C in the first section and a decomposition and oxidation temperature of 800°C.
[0050] Step 3: The collected iron oxide and pore-forming agent particles are embedded in deionized water and fully ultrasonically stirred to dissolve and remove the pore-forming agent, and then centrifuged and dried in an oven to obtain nano-unit overlapping porous spherical micron Fe2O3 with a particle size of 0.5 to 3 μm.
[0051] Step 4: Place the obtained small-unit overlapping porous spherical micron Fe2O3 in a tubular furnace and carry out reduction reaction in a hydrogen or hydrogen and inert gas mixed gas (helium, argon) atmosphere at 410-500°C and a flow rate of 100-400sccm. By removing oxygen atoms, pure Fe particles with nano-small units overlapping and further obvious porous structure are obtained.
[0052] Step 5: After the reduction reaction is completed, the temperature is lowered under the protection of an inert gas (helium or argon), and then a nitridation reaction is performed at 170 to 190°C. The gas atmosphere is ammonia, the flow rate is 100 to 200 sccm, and the nitridation time is 6 to 40 hours to obtain a porous spherical micron Fe with a 50-100 nm nano-columnar small unit. 16 N2 magnetic powder, such as Figure 2 .
[0053] In step 4 and step 5, nitrogen was not used as the inert gas, mainly to avoid slight nitridation reaction between nitrogen and the reduced pure Fe particles. 16 N2 preparation process parameters have variable effects.
[0054] The embodiment of the present invention also provides a method for preparing a Fe nanosheet-like unit by hydrothermal method by overlapping each other to form a micron-sized Fe 16 N2 magnetic powder, such as Figure 3 The specific steps are as follows:
[0055] Step 1: Mix and dissolve water-soluble iron salt and urea in deionized water or an organic solvent, and stir thoroughly to form a uniform hydrothermal reaction precursor solution;
[0056] The water-soluble iron salt is a water-soluble ferric salt or a water-soluble ferrous salt, preferably one or more combinations of ferric nitrate, ferrous nitrate, ferric chloride, ferrous chloride, ferrous sulfate, and ferrous sulfate. The organic solvent is preferably ethylene glycol, and the molar ratio of urea to iron salt is 2 to 3:1.
[0057] Step 2: Place the hydrothermal reaction precursor solution in a polytetrafluoroethylene liner and in a reaction kettle, transfer it to an oven at 140-180° C., and react at a constant temperature for 10-20 hours.
[0058] Step 3: The precursor obtained after the reaction is washed in deionized water and anhydrous ethanol, centrifugally dried and collected, and then transferred to a tubular furnace for high-temperature treatment at 300-400°C in an inert gas atmosphere, and then subjected to high-temperature oxidation reaction in an air atmosphere to obtain nano-sheet-like small units overlapping each other to form micron-sized Fe2O3 particles with a particle size of 2-4μm.
[0059] Step 4: Place the obtained nanosheet-like small unit overlapping micron Fe2O3 particles in a tubular furnace and carry out reduction reaction in a hydrogen or hydrogen and inert gas mixed gas (helium, argon) atmosphere at a flow rate of 100 to 400 sccm at 410 to 500°C to obtain pure Fe particles with small unit overlaps with a more obvious porous structure by removing oxygen atoms.
[0060] Step 5: After the reduction reaction is completed, the temperature is lowered under the protection of an inert gas (helium or argon), and then a nitridation reaction is performed at 170 to 190°C. The gas atmosphere is ammonia, the flow rate is 100 to 200 sccm, and the nitridation time is 6 to 40 hours to obtain 50-80 nm nano-sheet small units overlapping each other. Micron Fe 16 N2 magnetic powder, such as Figure 4 .
[0061] In step 4 and step 5, nitrogen was not used as the inert gas, mainly to avoid slight nitridation reaction between nitrogen and the reduced pure Fe particles. 16 N2 preparation process parameters have variable effects.
[0062] The present invention is further described below in conjunction with specific embodiments, but the methods and technical parameters involved in the scheme should not be understood as limiting the present invention.
[0063] Example 1: Take 161.6g of Fe(NO3)3·9H2O and 74.55g of KCl and dissolve them in 2000ml of deionized water. Perform sufficient ultrasonic stirring for 30min to obtain a precursor solution with a solubility of 0.2mol / L for Fe(No3)3·9H2O, 0.5mol / L for KCl, and a molar ratio of KCl pore former to iron salt of 2.5:1. The prepared precursor solution is added to the ultrasonic atomization device through an automatic liquid replenishment device. The ultrasonic atomization device transmits vibrations to the precursor solution in the container through pure water through 6 1.7MHz frequency vibrators, and obtains atomized precursor droplets through ultrasonic spraying. The air compressor compresses air at a flow rate of 10L / min as a carrier gas to drive the atomized droplets through a three-stage tubular furnace. The first stage dehydration temperature of the tubular furnace is 300℃, and the second and third stages of pyrolysis oxidation temperature are 800℃. The atomized precursor droplets undergo dehydration reaction in the tubular furnace to obtain KCl and Fe2O3 interlocking particles, which are collected in the collection device at the end of the tubular furnace. The interlocking particle powder is placed in deionized water, and after sufficient ultrasonic stirring to wash away KCl, the wet powder is centrifuged and placed in an 80℃ oven for drying for 4h. Small unit overlapping porous spherical micron Fe2O3 with a particle size of 0.5 to 3μm is obtained through SEM observation. The obtained Fe2O3 powder is placed in a tubular furnace and reduced for 3h at 450℃ and 200sccm flow rate of hydrogen atmosphere. After the reduction reaction is completed, the hydrogen atmosphere is turned off, and the temperature is lowered in an argon atmosphere to 190℃. The nitridation reaction is carried out at 190℃ and 200sccm ammonia atmosphere for 10h. Combined with XRD test and Rietveld analysis of Fe 16 The purity of N2 reached 88.9%. SEM observation showed that the nano-columnar small units constituted porous spherical micron Fe 16N2 magnetic powder, nanometer unit is 50~100nm thick. VSM test analysis shows the coercivity reaches 1.2KOe.
[0064] Example 2: Take 80.8g of Fe(No3)3·9H2O and 149.1g of KCl and dissolve them in 2000ml of deionized water, and stir them ultrasonically for 30min to obtain a precursor solution with a solubility of 0.1mol / L Fe(No3)3·9H2O, 1mol / L KCl, and a molar ratio of KCl pore former to iron salt of 10:1. The prepared precursor solution was spray pyrolyzed according to the steps and parameters of Example 1, and KCl was washed away, and then a reduction reaction was carried out. After the reduction reaction was completed, the hydrogen atmosphere was turned off, and the temperature was lowered to 180°C under an argon atmosphere. The nitridation reaction was carried out at 180°C and 100sccm ammonia atmosphere for 40h. Combined with XRD testing and Rietveld analysis of Fe 16 The purity of N2 reached 85.5%. SEM observation showed that the nano-columnar small units constituted porous spherical micron Fe 16 N2 magnetic powder. VSM test analysis shows the coercivity reaches 1.31KOe.
[0065] Example 3: Take 0.27g of FeCl3·6H2O and 0.15g of urea and dissolve them in 50ml of ethylene glycol, and stir them ultrasonically for 10min to obtain a hydrothermal reaction precursor solution with a molar ratio of urea to iron salt of 2.5:1. Transfer it to a 100ml polytetrafluoroethylene liner, place the liner in a reactor and install the reactor. Transfer the reactor to a 160℃ oven for constant temperature hydrothermal reaction for 18h. After the hydrothermal reaction is completed, pour the precursor into deionized water, stir and clean it thoroughly, centrifuge it, and then put it into anhydrous ethanol for stirring and cleaning. After centrifugation, place it in an 80℃ oven to dry to obtain a nano-sheet overlap precursor. Then transfer it to a tubular furnace, heat treat it at 400℃ in an argon atmosphere for 1h, then change the gas atmosphere to air, and oxidize it at 400℃ for 1h to obtain a micron Fe2O3 powder with a particle size of 2 to 4μm with small units overlapping each other. The obtained flaky small unit overlapped Fe2O3 powder was placed in a tube furnace and reduced for 2 hours at 450°C and 200sccm hydrogen atmosphere. After the reduction reaction, the hydrogen atmosphere was turned off and the temperature was lowered to 190°C in an argon atmosphere. The nitridation reaction was carried out for 8 hours at 190°C and 100sccm ammonia atmosphere. Combined with XRD test and Rietveld analysis of Fe 16 The purity of N2 reached 84.4%. SEM observation showed that Fe 16 N2 magnetic powder, nanometer unit is about 50-80nm thick. VSM test analysis shows that the coercivity reaches 1.06KOe.
[0066] Table 1: Comparison of powder composition and performance of final products of Examples 1-3
[0067]
Claims
1. A high-purity, high-performance Fe 16 The preparation method of N2 magnetic powder is characterized in that The method comprises the following steps: Prepare Fe2O3 particles of micrometer size composed of nano-units and retaining the independent integrity of the surface structure of the nano-units; The prepared Fe2O3 particles are reduced to obtain micron-sized pure Fe particles consisting of nano-sized units with pores; The prepared pure Fe particles are subjected to low-temperature nitridation reaction, which reacts on the surface of each nanounit to prepare the required Fe 16 N2 magnetic powder.
2. The method according to claim 1, characterized in that: The preparation of Fe2O3 particles is specifically as follows: The spherical particles in which Fe2O3 and pore-forming agent are mutually embedded are prepared by spray thermal decomposition method, and then the pore-forming agent is removed by ultrasonic dissolution with deionized water to obtain micrometer-scale porous spherical Fe2O3 particles composed of overlapping nano-columnar small units.
3. The method according to claim 2, characterized in that: The spray pyrolysis method is to prepare nano-columnar small units to form porous spherical micron Fe2O3 particles with the aid of pore-forming agents, specifically: The water-soluble iron salt and the pore-forming agent are mixed and dissolved in deionized water, and a uniform precursor solution is formed by diffusion through ultrasonic vibration to obtain a spray precursor solution; Using the principle of ultrasonic spray, the precursor solution is atomized into mist-like small droplets, which are driven by carrier gas to undergo dehydration reaction and pyrolysis oxidation reaction in a three-stage tube furnace to obtain Fe2O3 and pore-forming agent interlocking particles, which are collected in the tail collector. The interlocking particles are ultrasonically stirred in deionized water to fully dissolve the pore-forming agent, and then centrifugally dried to obtain porous spherical micron Fe2O3 particles consisting of nano-columnar small units.
4. The method according to claim 3, characterized in that: The pore-forming agent in the precursor is a soluble metal salt, and the molar ratio of the pore-forming agent to the water-soluble iron salt is 0.5-10:1; the carrier gas in the tubular furnace is air with a flow rate of 5-10L / min, the first stage evaporation and dehydration temperature is 300-500°C, and the second and third stage decomposition and oxidation temperatures are 800°C.
5. The method according to claim 1, characterized in that: The preparation of Fe2O3 particles is specifically as follows: A precursor consisting of overlapping nanosheets is prepared by a hydrothermal method, and then micron-sized spherical Fe2O3 particles consisting of overlapping nanosheets, namely micron-sized porous spherical Fe2O3 particles, are obtained by high-temperature heat treatment.
6. The method according to claim 5, characterized in that: The hydrothermal method is specifically: The water-soluble iron salt and urea are stirred and uniformly dissolved in deionized water or an organic solvent to form a hydrothermal reaction body solution; The hydrothermal reaction precursor solution is placed in a polytetrafluoroethylene liner, and the reaction kettle is transferred to a constant temperature oven for hydrothermal reaction; The precursor obtained by the hydrothermal reaction is washed in deionized water and anhydrous ethanol, centrifugally dried and placed in a tubular furnace, first subjected to high-temperature treatment in an inert gas, and then subjected to high-temperature oxidation in an air atmosphere to obtain rice-like small units that overlap each other to form high specific surface area micron Fe2O3 particles.
7. The method according to claim 6, characterized in that: The water-soluble iron salt is a water-soluble trivalent iron salt or a water-soluble divalent iron salt, and the molar ratio of urea to the water-soluble iron salt is 2 to 3:
1.
8. The method according to claim 6, characterized in that: The hydrothermal reaction temperature is 140-180°C, and the reaction time is 10-20h; the inert gas high temperature treatment and air atmosphere high temperature oxidation reaction temperature is 300-400°C.
9. The method according to claim 1, characterized in that: The gas atmosphere used for low-temperature nitriding of pure Fe particles is ammonia, the ammonia flow rate is 100-200 sccm, the temperature is 170-190°C, and the nitriding time is 6-40h.
10. A kind of Fe 16 N2 magnetic powder is prepared by the method described in any one of claims 1 to 9.