Atomic-level controllable high-entropy catalyst as well as preparation method and application thereof
The atomically dispersed metal catalyst supported on a catalytic substrate is prepared by the lithium melting method, which solves the problems of low selectivity and high cost of existing catalysts, achieves efficient and stable carbon dioxide reduction and electrolysis of water for hydrogen production, and is suitable for large-scale applications.
Patent Information
- Application Number
- CN202410847893.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-08-29
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-27
AI Technical Summary
Existing catalysts have low selectivity and high overpotential in the carbon dioxide reduction process, and commercial catalysts are costly and have poor stability, making it difficult to achieve large-scale application.
The atomically dispersed metal catalyst supported on the catalytic substrate is prepared by the molten lithium method. The molten alkali metal is prepared in an anhydrous and oxygen-free environment, the catalytic metal is added to form an alkali metal hydroxide mixture, and the alkali metal hydroxide is removed in a humid environment. materials to obtain high-entropy catalysts controllable at the atomic level.
It achieves carbon dioxide reduction with high selectivity and low overpotential. The catalyst has high stability and low cost, and is suitable for large-scale electrocatalytic reduction of CO2 into high-value fuels and electrolysis of water for hydrogen production.
Smart Images

Figure CN118847148A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of electrocatalysis technology, and in particular to an atomic-level controllable high-entropy catalyst and a preparation method and application thereof. Background Art
[0002] With the extensive use of fossil fuels, global energy is being consumed rapidly. Renewable resources such as solar energy, wind energy, and electric energy are used to convert carbon dioxide into fuels with high chemical value such as ethanol and formic acid, but the thermodynamic energy barrier for carbon dioxide reduction is high. Therefore, the development of catalysts with high selectivity and low overpotential is the key to its widespread application. Hydrogen energy is a clean and renewable energy source that can be applied to a variety of scenarios. It is also key in the future global energy strategy system, but the efficient production of hydrogen urgently needs to be supported by stable and economical catalysts. In addition, fuel cells are more environmentally friendly and pollution-free because there is no involvement of carbon-containing materials in the energy conversion process. However, most of the current commercial catalysts are precious metal catalysts, which are relatively expensive. In addition, they have poor stability during actual applications. Therefore, it is also necessary to develop a low-cost and highly stable electrocatalyst.
[0003] High entropy alloys, also known as multi-principal alloys, are composed of multiple metals mixed in appropriate proportions to form a solid solution structure. Multiple elements can play a synergistic role, thereby providing multiple adsorption sites for catalytic reactions. The high mechanical strength and corrosion resistance of high entropy materials are conducive to their stable application in a variety of catalytic environments. Compared with nanoparticle material catalysts, single-atom catalysts have an increased active area and improved catalytic activity. However, the preparation of high-entropy single-atom catalysts still has problems such as complex processes and unstable catalysts. Therefore, a preparation method for atomic-level controllable high-entropy catalysts will help achieve efficient catalysis and large-scale industrial applications. Summary of the invention
[0004] The present invention aims to provide a large-scale atomic-level controllable high-entropy catalyst and its preparation method and application, respectively realize the high energy density reduction of carbon dioxide to high-value fuel, low overpotential catalytic hydrogen production by electrolysis of water, and the preparation and application of efficient and stable atomic-level dispersed high-entropy catalysts in oxygen reduction fuel cells. The present invention uses a molten lithium (sodium, potassium, rubidium, cesium) method to prepare an atomically dispersed metal catalyst supported by a catalytic substrate, wherein the catalytic metal mainly exists in the form of a single atom, and these electrocatalysts are proven to have high efficiency and low overpotential, and have high selectivity and high stability for the formation of carbon dioxide reduction products ethanol and hydrocarbons. According to an embodiment, highly selective electrocatalytic carbon dioxide reduction is achieved to formic acid, methanol, ethanol, etc., which is suitable for large-scale electrocatalytic CO2 reduction.
[0005] The first aspect of the present invention provides a method for preparing an atomic-level controllable high-entropy catalyst, comprising the following steps:
[0006] (1) preparing molten alkali metal in the absence of water and oxygen;
[0007] (2) adding a catalytic metal to a molten alkali metal to obtain a molten alkali metal-catalytic metal mixture;
[0008] (3) cooling the molten alkali metal-catalytic metal mixture and placing it in a humid environment to obtain an alkali metal hydroxide-catalytic metal mixture;
[0009] (4) The alkali metal hydroxide-catalytic metal mixture is uniformly mixed with the catalyst support, and then slowly rinsed with a dropping funnel while removing the alkali metal hydroxide and then dried to obtain an atomic-level controllable high entropy catalyst.
[0010] In the technical solution of the invention, the operation of removing the alkali metal hydroxide is to add water and slowly rinse with a dropping funnel to remove the alkali metal hydroxide, and the process can be filtered or not filtered.
[0011] As a preferred embodiment,
[0012] In step (1), the alkali metal in the molten alkali metal is selected from one of lithium, sodium, potassium, rubidium and cesium.
[0013] As a preferred embodiment,
[0014] In step (2), the number of metal species corresponding to the catalytic metal is ≥ 4;
[0015] Preferably, the catalytic metal is selected from transition metals, main group metals, lanthanide metals and actinide metals;
[0016] More preferably,
[0017] The transition metal is selected from at least one of Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Pt and Cd; and / or,
[0018] The main group metal is at least one selected from Mg, Ca, Sr, Ba, B, Al, Ga, In, Tl, Ge, Sn, Pb, As, Sb, Bi, Se, Te or Po; and / or,
[0019] The lanthanide metal is at least one selected from lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium or lutetium; and / or,
[0020] The actinide metal is at least one selected from actinium, thorium, protactinium, uranium, neptunium, plutonium, americium, curium or berkelium;
[0021] More preferably, the number of metal species corresponding to the catalytic metal is ≥5.
[0022] In the technical solution of the present invention, the catalytic metal is selected from a plurality of metals, and the present invention finds that the synergistic effect of the metal atoms in the above-mentioned multi-metal catalyst forms more catalytic centers, further improving the catalytic activity of the catalyst; since different metals have different adsorption reaction sites, the selectivity of the product can be improved by regulating the d-band electronic structure.
[0023] As a preferred embodiment,
[0024] The catalytic metal is selected from four or more metals selected from Mg, Ca, Sr, Ba, Al, Ga, In, Tl, Ge, Sn, Pb, As, Sb, Bi, Se, Te, Po, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La series, Ac series, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg;
[0025] Preferably, the catalytic metal is selected from five metals of Cu, Sn, In, Bi, Pt, Ag, Ni, Ir, Pd, Ru, Rh, Fe, and Co;
[0026] Further preferably, the catalytic metal is Cu, Sn, In, Bi, Pt, and the molar ratio of the five metals is preferably 1:1:1:1:1; and / or,
[0027] The catalytic metals are Sn, In, Cu, Ag, and Ni, and preferably the molar ratio of the five metals is 1:1:1:1:1; and / or,
[0028] The catalytic metals are Ir, Pd, Ru, Rh and Pt, and preferably the molar ratio of the five metals is 1:1:1:1:1; and / or,
[0029] The catalytic metals are five metals: Pt, Fe, Sn, Cu, and Co. Preferably, the molar ratio of the five metals is 1:1:1:1:1.
[0030] As a preferred embodiment,
[0031] In the catalytic metal, the sum of the stoichiometric ratios of four or more metals selected from transition metals, main group metals, lanthanide metals and actinide metals should be 100%, wherein the mass content of transition metals, main group metals, lanthanide metals and actinide metals is independently selected from 10% to 60%;
[0032] Preferably,
[0033] Among the catalytic metals, the sum of the stoichiometric ratios of five or more metals selected from transition metals, main group metals, lanthanide metals and actinide metals should be 100%, wherein the mass content of transition metals, main group metals, lanthanide metals and actinide metals are each independently selected from 10% to 60%.
[0034] As a preferred embodiment,
[0035] The molar ratio of the total mass of the catalytic metal to the alkali metal is (0.01% to 25%):1; for example, 0.01%:1, 0.1%:1, 1%:1, 4%:1, 10%:1, 15%:1, 20%:1, 25%:1.
[0036] The time for maintaining the alkali metal in the molten state is 0.5 to 10 hours; for example, 0.5, 1, 3, 5, 7, 10 hours.
[0037] As a preferred embodiment,
[0038] Cooling time ≤ 20 minutes;
[0039] The humid environment is a humid air environment, preferably the relative humidity (RH) of the humid air is 50% to 100%;
[0040] The placement time is 24h to 72h; for example, 24, 30, 35, 40, 50, 60, 72 hours.
[0041] As a preferred embodiment,
[0042] In step (4), the catalyst carrier is selected from a carbon carrier, preferably one or more of common commercial carbon powder, carbon black, high specific surface area carbon such as graphene, and carbon nanotubes; and / or,
[0043] In the catalyst, the mass ratio of the catalytic metal to the catalyst carrier is 0.01% to 10%; preferably in the range of 0.01% to 5%; for example, 0.01%, 0.1%, 0.5%, 0.8%, 1%, 1.5%, 2%, 3%, 5%, 8%, 10%; and / or,
[0044] The method of mixing uniformly is mechanical mixing, and preferably the method of mechanical mixing is mixing uniformly by grinding; and / or,
[0045] The drying method is vacuum drying at 50-100°C.
[0046] The second aspect of the present invention provides a catalyst prepared by the method for preparing an atomic-level controllable high-entropy catalyst as described in any one of the first aspects of the present invention, the catalyst comprising a carrier and an active component; the active component is selected from four or more metals with catalytic effect; wherein the metal atoms in the active component are dispersed at the atomic level on the carrier to which they belong; preferably, the active component is selected from five or more metals with catalytic effect.
[0047] In the catalyst described in the present invention, the mass ratio of the catalytic metal to the catalyst carrier is 0.01% to 10%; the preferred range is 0.01% to 5%; further preferably 0.01% to 1%; for example, 0.01%, 0.1%, 0.5%, 0.8%, 1%, 1.5%, 2%, 3%, 5%, 8%, 10%.
[0048] The third aspect of the present invention provides a catalyst prepared by the method for preparing an atomic-level controllable high-entropy catalyst as described in the first aspect of the present invention or the use of the catalyst as described in the second aspect of the present invention in an electrocatalyst in an electroreduction reaction; preferably,
[0049] Application of the catalyst as an electrocatalyst for the reduction of CO2 to produce formic acid; and / or,
[0050] Application of the catalyst as an electrocatalyst for CO2 reduction to methanol; and / or,
[0051] Application of the catalyst as an electrocatalyst for CO2 reduction to ethanol; and / or,
[0052] Application of the catalyst as an electrocatalyst for CO2 reduction to produce acetic acid; and / or,
[0053] Application of the catalyst as an electrocatalyst for producing hydrogen by electrolysis of water; and / or,
[0054] The catalyst is used as an electrocatalyst for an oxygen reduction fuel cell.
[0055] More specifically, a technical solution for large-scale preparation of atomic-level controllable high-entropy catalysts in the present invention comprises the following steps:
[0056] Step 1: adding a plurality of catalytic metals in the form of bulk metals to a molten alkaline metal, wherein the catalytic metal source added to the molten metal should include at least five metals;
[0057] Step 2: adding catalytic metal atoms to the molten alkali metal obtained in step 1 until uniformly dispersed, and then rapidly quenching the molten body to form a solid solution and avoiding aggregation of metal components, thereby forming an alkali metal-high entropy metal solid;
[0058] Step 3: Cut the alkali metal-high entropy metal solid obtained in step 2 into small pieces, and place them in a humid environment to convert the alkali metal into an alkali metal hydroxide to form a high entropy metal-alkali metal hydroxide solid;
[0059] Step 4: mixing the high entropy metal-alkaline metal hydroxide solid described in step 3 with a catalytic base material;
[0060] Step 5: removing alkaline metal hydroxide from the mixture in step 4, leaving an atomically dispersed high entropy metal mixture on the catalytic substrate material (i.e., the catalyst carrier), i.e., filtering the mixture in step 4 while slowly washing it to remove the alkali metal hydroxide;
[0061] Step 6: Drying the catalytic substrate-loaded atomically dispersed metal mixture described in step 5, thereby preparing an electrocatalyst with a catalytic substrate-loaded high-entropy metal atomically dispersed.
[0062] The catalytic metal, according to an embodiment, is suitable for the preparation of the electrocatalyst of the present invention, including four or more metals of Mg, Ca, Sr, Ba, Al, Ga, In, Tl, Ge, Sn, Pb, As, Sb, Bi, Se, Te, Po, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La series, Ac series, Hf, Ta, W, Re, Os, Ir, Pt, Au, and Hg, and molten lithium to form a Li-multimetal melt.
[0063] Among them, metals with a melting point below 300°C that can form a solid solution with lithium can be selected first in the preparation of electrocatalysts, such as Mg, Ca, Sr, Ba, Al, Ga, In, Tl, Ge, Sn, Pb, As, Sb, Bi, Se, Te, Po, Cu, Zn, Mo, Tc, Ru, Rh, Pd, Ag, and Cd. It is particularly emphasized that metal single atoms can be directly formed in the form of ingots, wires, powders, fragments, etc., followed by steps such as drying and reduction. Under an inert atmosphere, the transition metal is dispersed in a hot lithium solution, and the temperature of the molten lithium is between 180°C and 1330°C, that is, between the melting point and boiling point of lithium. For other alkaline metals used in the melt, the temperature range is also between their respective melting points and boiling points;
[0064] The alkaline metal, including other alkaline materials such as Li, Na, K, Rb, Cs, etc., can be used as a molten medium to dissolve the above metals into a solid solution. In a preferred embodiment, lithium is added to the melt (usually referred to as a lithium melt) as a molten medium because the span between the melting point and the boiling point of lithium is the largest.
[0065] The cutting method may also use one of rolling, punching or other mechanical methods to reduce the size or break the solid solution into finer fragments to promote interaction with moisture and air, wherein the relative humidity (RH) of the humidified air should preferably be 50% to 100%;
[0066] The surface area of the catalytic substrate carrier is greater than 20 m 2 / g. Range can be 20m 2 / g to 800m 2 / g. The catalyst substrate can be a commercial carbon carrier, such as graphene, carbon nanotubes, common commercial carbon powder, carbon black, metal oxides, or a high surface area material, such as but not limited to metal-organic frameworks and chitosan-derived carbon carriers, etc., which satisfies that the metal atoms can be evenly dispersed on a carrier carbon matrix with a high specific surface area and high porosity. The use of a carbon matrix carrier can ensure that the metal atoms (single metal or multi-metal) are evenly distributed on the above support to avoid or reduce agglomeration.
[0067] The catalyst has the following advantages:
[0068] 1. The catalyst prepared by the present invention has good stability and catalytic activity. According to the preparation method of the present invention, during the flushing process of the alkaline hydroxide, oxygen-containing functional groups such as -OH and -COOH are generated to serve as anchoring points, so that the metal atoms remain in a highly dispersed state. Therefore, the catalyst of the present invention has long-term stability.
[0069] 2. The catalyst of the present invention can electrocatalyze the reduction of carbon dioxide into a single product with high selectivity, thus overcoming the shortcomings of low selectivity and low Faraday efficiency in the existing carbon dioxide reduction process.
[0070] 3. The active components of the present invention can be selected from transition metal and non-transition metal materials with relatively high existing reserves, and the cost is relatively low.
[0071] 4. The atomic dispersion in the present invention is high, and only a relatively low loading is required to achieve high catalytic activity, further reducing the cost of the catalyst.
[0072] 6. The high entropy catalyst prepared by the present invention can realize the synergistic effect of multiple metals and achieve a synergistic response through structural adaptation and electronic conversion, thereby achieving high activity and selectivity. BRIEF DESCRIPTION OF THE DRAWINGS
[0073] The foregoing and other features of the present invention will become more fully apparent from the following description and the appended claims, taken in conjunction with the accompanying drawings. Since these drawings describe only a few embodiments of the present invention and are not to be considered limiting of its scope, the present invention will be described in further detail through the use of the accompanying drawings.
[0074] Figure 1 Schematic diagram of the synthesis steps of CuSnInBiPt high entropy metal single atoms dispersed using the lithium melt method;
[0075] Figure 2 This is the nuclear magnetic resonance spectrum of formic acid produced by the carbon-supported CuSnInBiPt catalyst with a total mass fraction of catalytic metal of 0.1% at -0.6V;
[0076] Figure 3 The time-current density curve (It graph) of the carbon-supported CuSnInBiPt catalyst with a total mass fraction of catalytic metal of 0.1% tested at -0.6V;
[0077] Figure 4 The current-voltage polarization curves of SnInCuAgNi high entropy catalyst with a total carbon loading of 0.8% under different atmospheres;
[0078] Figure 5 The cyclic voltammetry curves and fitted electrochemical active areas of SnInCuAgNi high entropy catalyst with a total carbon loading of 0.8% at different scan rates;
[0079] Figure 6 This is the time-current density curve (It graph) of the SnInCuAgNi high entropy catalyst with a total carbon loading mass fraction of 0.8% tested at -0.8V. DETAILED DESCRIPTION
[0080] The technical solution of the present invention is further described below in conjunction with the accompanying drawings, but is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention should be included in the protection scope of the present invention.
[0081] Embodiments described in the present invention relate to methods for preparing carbon-supported high entropy atomic electrocatalysts using a molten lithium process. The electrocatalysts prepared by the method of the present invention can be used for electrocatalytic carbon dioxide reduction (CO2RR) to valuable chemicals such as formic acid, acetic acid, ethanol, etc. The electrocatalysts prepared by the method of the present invention can also be used in water electrolysis to produce hydrogen and oxygen reduction fuel cells. According to embodiments, the catalyst has high selectivity and stability for the reduction of carbon dioxide to hydrocarbons.
[0082] The following examples are provided for illustrative purposes and should not be construed as limiting the scope of the present invention.
[0083] Example 1
[0084] This embodiment provides a method for preparing a carbon-supported Cu, Sn, In, Bi, Pt high entropy catalyst with high selectivity and high stability for ethanol. A molten lithium method is used to prepare an electrocatalyst for CO2RR. The collective preparation process is as follows: Figure 1 The specific steps are as follows:
[0085] (1) In an argon glove box (oxygen level <0.3ppm), using a nickel crucible, 0.256mol lithium (99.9%) was heated to 220°C, and 0.019mmol copper wire (99.9%), 0.019mmol tin sheet (99.9%), 0.019mmol indium wire (99.9%), 0.019mmol bismuth block (99.9%) and 0.019mmol platinum wire (99.9%) were added.
[0086] (2) A cutting-edge ultrasonic homogenizer is used to ensure uniform dispersion of metal atoms while the lithium melt is kept at 220°C for 1 hour. During the heating process, the liquid surface always remains mirror-like and uniform. The ultrasonic action helps to disperse large pieces of metal into individual atoms, preventing them from precipitating, reaggregating or settling in the molten lithium.
[0087] (3) Quickly pour the molten liquid onto a clean stainless steel plate to form a solid solution.
[0088] (4) After the solid solution is cooled, the solid is taken out from the glove box, cut into small pieces, and lithium is slowly converted into LiOH in humidified air.
[0089] (5) The copper, indium, tin, bismuth, platinum atoms / LiOH materials were mixed with the required amount of carbon black (Vulcan XC-72R) and mixed with an agate mortar and pestle until homogeneous.
[0090] (6) LiOH was leached out with a large amount of distilled water, leaving Cu, Sn, In, Bi, and Pt atoms embedded in the amorphous carbon support. The sample was vacuum dried at 100°C for 24 hours. Samples with different mass loadings were prepared on carbon black: Product 1: Cu, Sn, In, Bi, and Pt loaded on carbon with a total mass fraction of catalytic metals of 0.1% (0.1% refers to the mass fraction of the catalyst to the mass fraction of the catalytic metal + the catalyst support, and the same expressions below have the same meaning and are not repeated here) or Product 2: Cu, Sn, In, Bi, and Pt loaded on carbon with a total mass fraction of catalytic metals of 0.4%.
[0091] (7) 15 μL of electrocatalyst ink was dropped onto the RDE electrode. The ink was prepared by adding 5 mg of catalyst powder to 50 mg of Nafion (perfluorinated resin solution) and 200 mg of methanol. The electrode was dried for 10 minutes before testing.
[0092] (8) The reaction rate and selectivity of formic acid reduction by CO2 were measured at room temperature and pressure using 0.149 mg of catalyst and 30 mL of NaHCO3 in a 250 mL reactor. Prior to the test, the electrolyte was purged with argon for 30 minutes to remove air from the environment. The electrolyte was then purged with CO2 for 30 minutes to fully saturate the electrolyte and form a NaHCO3 buffer solution with a pH of 6.8.
[0093] The stability of the catalyst was determined by time amperometry. The carbon-supported Cu, Sn, In, Bi, and Pt catalysts with a total catalytic metal mass fraction of 0.1% were stable for more than 16 hours at -0.6 V. The specific results are as follows: Figure 3 As shown, the catalyst has a Faradaic efficiency of 95% for formic acid at -0.6 V and exceeds 90% during the entire stability test period.
[0094] The NMR images of the products measured for the carbon-supported Cu, Sn, In, Bi, and Pt catalysts with a total mass fraction of 0.1% catalytic metal are shown in Figure 2 shown.
[0095] Example 2
[0096] This embodiment provides a method for preparing a carbon-supported Sn, In, Cu, Ag, Ni high entropy metal catalyst with high stability and high Faraday efficiency, and the specific steps are as follows:
[0097] (1) A carbon-supported Sn, In, Cu, Ag, Ni high entropy catalyst (the atomic ratio of Sn, In, Pd, Bi, and Ni is 1:1:1:1:1) was prepared by the same preparation method as in Example 1, and the total mass fraction of catalytic metals in the catalyst was 0.8%.
[0098] (2) The prepared sample, including 5 mg of catalyst, was mixed with 50 mg of Nafion (perfluorinated resin solution) and 200 mg of methanol. The resulting solution was sonicated for 60 min to ensure that the electrocatalyst was fully dispersed and deposited on a rotating disk electrode (RDE) glassy carbon electrode in batches of 15 μL, with 5 μL deposited each time. The surface area of the RRDE glassy carbon electrode was 0.196 cm 2 .
[0099] (3) The catalyst was tested in a carbon dioxide saturated bicarbonate solution (pH 6.8) using an RDE (rotating disk electrode) at 1600 rpm with an initial scan rate of 50 mV / s from 0 to -1.5 V (compared to a standard hydrogen electrode) to ensure full range of carbon dioxide reduction activity. Figure 4 As shown in Figure 2, the starting potential of the catalyst in a carbon dioxide atmosphere is lower than that in an argon background, indicating that the catalyst has a higher carbon dioxide catalytic activity. Figure 5 As shown in Figure 2, the scan rate was increased to 100 mV / s at 10 mV intervals to evaluate the electrochemically active area of the catalyst, which was as high as 4.99 mF cm -2 .
[0100] (4) The catalyst performance was studied by using a physical and chemical characterization method similar to that of Example 1. For a carbon-supported Sn, In, Cu, Ag, Ni high entropy catalyst with a mass fraction of 0.8%, when the electrode polarization potential was -0.8 V (compared to the standard hydrogen electrode), the results were as follows: Figure 6 As shown, the catalyst has a stability of 20 h and a selectivity (ie, Faraday efficiency) to acetic acid product close to 90%.
[0101] Example 3
[0102] This embodiment provides a method for preparing a carbon-supported Ir, Pd, Ru, Rh, Pt high entropy atomic dispersion catalyst for reducing the overpotential of water decomposition, and the specific steps are as follows:
[0103] (1) Carbon-supported Ir, Pd, Ru, Rh, and Pt high entropy single-atom catalysts were prepared by the same method as in Example 1, wherein the mass fraction of each catalytic metal in the catalyst was 0.2% (the molar ratio of the catalytic metal atoms was 1:1:1:1:1).
[0104] (2) The prepared sample, including 5 mg of catalyst, was mixed with 50 mg of Nafion (perfluorinated resin solution) and 200 mg of isopropanol. The resulting solution was ultrasonicated for 60 minutes to ensure that the electrocatalyst was fully dispersed, and 15 μL was deposited on the gold electrode in batches. Then, the electrolysis reaction of water was tested using RDE. The prepared metal hydrogen evolution overpotential was 0.502 V, while the commercial iridium oxide was 0.579 V. It can be seen that the metal hydrogen evolution overpotential of the catalyst prepared by the present invention is lower than that of the commercial material, indicating that its catalytic performance is improved.
[0105] Example 4
[0106] This embodiment provides a method for preparing a catalyst for improving the half-wave potential in an oxygen reduction fuel cell, and the specific steps are as follows:
[0107] (1) A carbon-supported PtFeSnCuCo high entropy atomic catalyst was prepared by the same method as in Example 1, and the total mass fraction of metal on the catalytic substrate was 0.2% (the ratio of catalytic metal atoms was 1:1:1:1:1).
[0108] (2) The prepared sample, including 5 mg of catalyst, was mixed with 50 mg of Nafion (perfluorinated resin solution) and 200 mg of isopropanol. The resulting solution was sonicated for 60 min to ensure that the electrocatalyst was fully dispersed, and 15 μL was deposited on the glassy carbon disk electrode and the Pt metal ring in batches, and then the oxygen reduction reaction was tested using RRDE.
[0109] (3) The catalyst of the present invention has the advantages of improving half-wave potential and active quality when used in oxygen reduction fuel cells, and the prepared noble metal single atom catalyst reduces the cost of using noble metal catalysts in fuel cells. According to the embodiment, it is shown that on the carbon-supported PtFeSnCuCo high entropy single atom catalyst, the half-wave potential is 0.92V.
[0110] Example 5
[0111] This embodiment provides a method for preparing a carbon-supported SnInPdFe high entropy metal catalyst with high stability and high Faraday efficiency, and the specific steps are as follows:
[0112] (1) According to Example 1, a carbon-supported SnInPdFe high entropy catalyst (the atomic ratio of Sn, In, Pd, and Bi is 3:3:2:2) was prepared, and the total mass fraction of metal on the catalytic substrate was 0.12%
[0113] (2) The prepared sample, including 5 mg of catalyst, was mixed with 50 mg of Nafion (perfluorinated resin solution) and 200 mg of methanol. The resulting solution was sonicated for 60 min to ensure that the electrocatalyst was fully dispersed and deposited on a rotating disk electrode (RDE) glassy carbon electrode in batches of 15 μL, with 5 μL deposited each time. The surface area of the RRDE glassy carbon electrode was 0.196 cm 2 .
[0114] (3) The catalyst performance was studied using a physical and chemical characterization method similar to that in Example 1. For a carbon-supported SnInPdFe high entropy catalyst with a mass fraction of 0.12%, the selectivity for acetic acid product was close to 90% when the electrode polarization potential was -0.6 V (compared to a standard hydrogen electrode).
[0115] Comparative Example 1
[0116] The method is basically the same as that of Example 1, with the only difference being that the same mass of Cu is loaded on the catalyst to replace CuSnInBiPt.
[0117] Comparative Example 2
[0118] The method is basically the same as that of Example 1, with the only difference being that the same mass of Sn is loaded on the catalyst to replace CuSnInBiPt.
[0119] Comparative Example 3
[0120] The method is basically the same as that of Example 1, with the only difference being that the same mass of In is loaded on the catalyst to replace CuSnInBiPt.
[0121] Comparative Example 4
[0122] The method is basically the same as that of Example 1, with the only difference being that the same mass of Bi is loaded on the catalyst to replace CuSnInBiPt.
[0123] Comparative Example 5
[0124] The method is basically the same as that of Example 1, with the only difference being that the same mass of Pt is loaded on the catalyst to replace CuSnInBiPt.
[0125] Comparative Examples 1 to 5 The catalysts were prepared and tested in the same manner as in Example 1. The Faraday efficiencies of the catalysts for formic acid at -0.6 V are shown in Table 1.
[0126] Table 1 Faraday efficiency of catalysts prepared from Comparative Examples 1 to 5 for CO2 reduction to formic acid at -0.6 V
[0127] Comparative Example Faradaic efficiency for formic acid (%) Comparative Example 1 0.2 Comparative Example 2 82.1 Comparative Example 3 90.6 Comparative Example 4 88 Comparative Example 5 0
[0128] From the comparison of the results of Example 1 and Comparative Examples 1-5, it can be seen that the high entropy catalyst prepared by the present invention can achieve the synergistic effect of multiple metals, and can achieve a synergistic response through structural adaptation and electronic conversion, thereby achieving high activity and selectivity of the catalyst.
[0129] The catalysts prepared in other embodiments of the present invention can also achieve the synergistic effect of multiple metals to improve the high activity and selectivity of the catalyst.
[0130] It should be noted that the construction and arrangement of the various exemplary embodiments are illustrative only. Although only a few embodiments are described in detail in the present disclosure, those skilled in the art who review the present disclosure will readily appreciate that many modifications are possible (e.g., changes in the size, dimensions, structure, shape and proportion of the various elements, parameter values, mounting arrangements, use of materials, colors, orientations, etc.) without substantially departing from the novel teachings and advantages of the subject matter described herein. Other substitutions, modifications, changes, and omissions may also be made to the design, operating conditions, and arrangements of the various exemplary embodiments without departing from the scope of the present invention.
[0131] While this specification contains many specific implementation details, these should not be construed as limitations on the scope or claimable content of any invention, but rather as specific descriptions of features of particular implementations of particular inventions. Certain features described in this specification in the context of separate implementations may also be implemented in combination in a single implementation. Conversely, various features described in the context of a single implementation may also be implemented in multiple implementations, either separately or in any suitable subcombination.
Claims
1. A method for preparing an atomic-level controllable high-entropy catalyst, characterized in that: The following steps are involved: (1) preparing molten alkali metal in the absence of water and oxygen; (2) adding a catalytic metal to a molten alkali metal to obtain a molten alkali metal-catalytic metal mixture; (3) cooling the molten alkali metal-catalytic metal mixture and placing it in a humid environment to obtain an alkali metal hydroxide-catalytic metal mixture; (4) The alkali metal hydroxide-catalytic metal mixture is uniformly mixed with the catalyst carrier, and then the alkali metal hydroxide is removed and then dried to obtain an atomic-level controllable high entropy catalyst.
2. The method for preparing an atomic-level controllable high-entropy catalyst according to claim 1, characterized in that: In step (1), the alkali metal in the molten alkali metal is selected from one of lithium, sodium, potassium, rubidium and cesium.
3. The method for preparing an atomic-level controllable high-entropy catalyst according to claim 1, characterized in that: In step (2), the number of metal species corresponding to the catalytic metal is ≥ 4; Preferably, the catalytic metal is selected from transition metals, main group metals, lanthanide metals and actinide metals; More preferably, The transition metal is selected from at least one of Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Pt and Cd; and / or, The main group metal is at least one selected from Mg, Ca, Sr, Ba, B, Al, Ga, In, Tl, Ge, Sn, Pb, As, Sb, Bi, Se, Te or Po; and / or, The lanthanide metal is at least one selected from lanthanum, cerium, praseodymium, neodymium, promethium, samarium, europium, gadolinium, terbium, dysprosium, holmium, erbium, thulium, ytterbium or lutetium; and / or, The actinide metal is at least one selected from actinium, thorium, protactinium, uranium, neptunium, plutonium, americium, curium or berkelium; More preferably, the number of metal species corresponding to the catalytic metal is ≥5.
4. The method for preparing an atomic-level controllable high-entropy catalyst according to claim 1, characterized in that: The catalytic metal is selected from four or more metals selected from Mg, Ca, Sr, Ba, Al, Ga, In, Tl, Ge, Sn, Pb, As, Sb, Bi, Se, Te, Po, Sc, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Zn, Y, Zr, Nb, Mo, Tc, Ru, Rh, Pd, Ag, Cd, La series, Ac series, Hf, Ta, W, Re, Os, Ir, Pt, Au, Hg; Preferably, the catalytic metal is selected from five metals of Cu, Sn, In, Bi, Pt, Ag, Ni, Ir, Pd, Ru, Rh, Fe, and Co; Further preferably, the catalytic metal is Cu, Sn, In, Bi, Pt, and the molar ratio of the five metals is preferably 1:1:1:1:1; and / or, The catalytic metals are Sn, In, Cu, Ag, and Ni, and preferably the molar ratio of the five metals is 1:1:1:1:1; and / or, The catalytic metals are Ir, Pd, Ru, Rh and Pt, and preferably the molar ratio of the five metals is 1:1:1:1:1; and / or, The catalytic metals are five metals: Pt, Fe, Sn, Cu, and Co. Preferably, the molar ratio of the five metals is 1:1:1:1:
1.
5. The method for preparing an atomic-level controllable high-entropy catalyst according to claim 3, characterized in that: In the catalytic metal, the sum of the stoichiometric ratios of four or more metals selected from transition metals, main group metals, lanthanide metals and actinide metals should be 100%, wherein the mass content of transition metals, main group metals, lanthanide metals and actinide metals is independently selected from 10% to 60%; Preferably, Among the catalytic metals, the sum of the stoichiometric ratios of five or more metals selected from transition metals, main group metals, lanthanide metals and actinide metals should be 100%, wherein the mass content of transition metals, main group metals, lanthanide metals and actinide metals are each independently selected from 10% to 60%.
6. The method for preparing an atomic-level controllable high-entropy catalyst according to claim 2, characterized in that: In step (2), The molar ratio of the total mass of the catalytic metal to the alkali metal is (0.1% to 25%): 1; The time for maintaining the alkali metal in the molten state is 0.5 to 10 hours.
7. The method for preparing an atomic-level controllable high-entropy catalyst according to claim 1, characterized in that: In step (3), Cooling time ≤ 20 minutes; The humid environment is a humid air environment, preferably the relative humidity of the humid air is 50% to 100%; The placement time is 24h to 72h.
8. The method for preparing an atomic-level controllable high-entropy catalyst according to claim 1, characterized in that: In step (4), the catalyst carrier is selected from a carbon carrier, preferably one or more of common commercial carbon powder, carbon black, graphene, and carbon nanotubes; and / or, In the catalyst, the mass ratio of the catalytic metal to the catalyst carrier is 0.01% to 10%; preferably in the range of 0.01% to 5%; and / or, The method of mixing uniformly is mechanical mixing, and preferably the method of mechanical mixing is mixing uniformly by grinding; and / or, The drying method is vacuum drying at 50-100°C.
9. A catalyst prepared by the method for preparing an atomic-level controllable high-entropy catalyst as claimed in any one of claims 1 to 8, the catalyst comprising a carrier and an active component; the active component is selected from four or more metals having catalytic effects; wherein, The metal in the active component is dispersed at the atomic level on the carrier; Preferably, the active components are selected from five or more metals having catalytic effects.
10. Use of a catalyst prepared by the method for preparing an atomic-level controllable high-entropy catalyst as claimed in any one of claims 1 to 8 or a catalyst as claimed in claim 9 as an electrocatalyst in an electroreduction reaction; preferably, Application of the catalyst as an electrocatalyst for the reduction of CO2 to produce formic acid; and / or, Application of the catalyst as an electrocatalyst for CO2 reduction to methanol; and / or, Application of the catalyst as an electrocatalyst for CO2 reduction to ethanol; and / or, Application of the catalyst as an electrocatalyst for CO2 reduction to produce acetic acid; and / or, Application of the catalyst as an electrocatalyst for producing hydrogen by electrolysis of water; and / or, The catalyst is used as an electrocatalyst for an oxygen reduction fuel cell.
Citation Information
Patent Citations
High-entropy intermetallic compound with ordered structure, preparation method of high-entropy intermetallic compound and application of high-entropy intermetallic compound as fuel cell cathode catalyst
CN114566662A
Porous alloy with hierarchical pore structure for catalytic electrode and preparation method of porous alloy
CN116397259A
Catalyst as well as preparation method and application thereof
CN117418269A
Carbon supported single atom carbon dioxide reduction electro catalysts
US20190276943A1
Method of preparing electrocatalysts for converting carbon dioxide to chemicals
US20220062864A1
Cited By
Carbon-loaded multi-metal electro-catalytic material, fused salt electrochemical preparation thereof and application of carbon-loaded multi-metal electro-catalytic material in OER / ORR
CN119530893A
Carbon-supported multimetallic electrocatalysts and their molten salt electrochemical preparation and application in OER / ORR
CN119530893B
Cascaded catalyst and preparation method and application thereof
CN120919991A
Precious metal catalyst as well as preparation method and application thereof
CN120967401A
High-entropy alloy catalyst as well as preparation method and application thereof
CN121360588A