CdS nanorod compactly coated carbon cloth piezoelectric photocatalytic material and preparation method thereof

By forming a densely coated piezoelectric photocatalytic material with CdS nanorods on carbon cloth, the problem of low degradation and recycling efficiency of photocatalytic materials is solved, achieving efficient degradation of organic pollutants in water and simplifying the recycling process.

CN118847152AInactive Publication Date: 2024-10-29XIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410937128.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-12
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing photocatalytic materials have low degradation and recycling efficiency in sewage treatment. Nano-CdS powder is easy to agglomerate and recycling is complicated, which affects engineering applications.

Method used

The preparation method of CdS nanorod densely coated carbon cloth piezoelectric photocatalytic material is used to form CdS nanorods through activation treatment of carbon cloth, CdO gel layer coating, deep ultraviolet radiation degradation, heat treatment and hydrothermal deposition. Carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods.

Benefits of technology

It increases the contact area between the photocatalyst and pollutants, enhances the adsorption performance and recycling degradation performance, achieves efficient degradation of organic pollutants in water, and simplifies the material recycling process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118847152A_ABST
    Figure CN118847152A_ABST
Patent Text Reader

Abstract

The invention discloses a CdS nanorod compactly coated carbon cloth piezoelectric photocatalytic material and a preparation method thereof. The preparation method comprises the following specific steps: step 1, activating the surface of carbon cloth; step 2, carrying out dipping treatment on the carbon cloth treated in the step 1 in CdO sol, and then centrifuging and drying to obtain carbon cloth coated with a CdO gel layer; 3, treating the carbon cloth coated with the CdO gel layer obtained in the step 2 by adopting a deep ultraviolet irradiation degradation combined heat treatment process to obtain carbon cloth coated with a CdO ceramic layer; and 4, depositing a CdS nanorod on the carbon cloth coated with the CdO ceramic layer obtained in the step 3 by adopting a hydrothermal method to obtain the CdS nanorod densely coated carbon piezoelectric photocatalytic material. The photocatalytic material disclosed by the invention has excellent photocatalytic degradation performance, piezoelectric photocatalytic degradation performance, adsorption and desorption capability and recycling performance, and is convenient to recycle.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photocatalytic materials, and in particular relates to a preparation method of a piezoelectric photocatalytic material of CdS nanorods densely coated with carbon cloth, and also relates to a piezoelectric photocatalytic material of CdS nanorods densely coated with carbon cloth. Background Art

[0002] With the progress and development of society, the large-scale discharge of domestic sewage and industrial wastewater has caused serious environmental pressure and threatened people's health. The sources of water pollution in my country mainly include printing and dyeing wastewater, pesticide wastewater, medical wastewater, etc. Among them, the treatment of printing and dyeing wastewater is particularly difficult, and traditional treatment methods are difficult to decolorize and degrade dyes. At present, photocatalytic technology has attracted widespread attention for its ability to effectively degrade organic pollutants using solar energy, a clean energy source. However, low charge carrier mobility and rapid recombination of electron-hole pairs limit the efficiency of photocatalysis. In recent years, a large number of studies have found that the introduction of polarized electric fields into photocatalysis and the polarized electric fields generated by piezoelectric materials induced by mechanical action can effectively separate the photogenerated electron-hole pairs generated during the photocatalytic process, and it is expected to achieve the efficient degradation of organic pollutants in water by using piezoelectric effect in conjunction with visible light catalysis.

[0003] Among the numerous semiconductor photocatalysts, CdS is a promising narrow-bandgap photocatalyst with a bandgap width of 2.42 eV. It has been widely studied and applied due to its good visible light response ability and excellent carrier transport ability. At the same time, the hexagonal phase of CdS has a non-centrosymmetric crystal structure, which makes it have excellent piezoelectric properties, and can achieve the piezoelectric effect and visible light catalytic degradation of pollutants. However, the nano-CdS photocatalysts developed in recent years are mostly powders, which are prone to agglomeration and difficult to recycle during sewage treatment. At the same time, the recycling operation process of powder materials is complicated, which is bound to increase the difficulty of engineering technology and the overall cost. To solve the above problems, a simple and effective way is to load the photocatalyst on the surface of a specific substrate material to increase the contact area between the catalyst and the pollutant, improve the adsorption performance of the photocatalyst, and thus improve the photocatalytic degradation performance of the composite material. Carbon cloth has strong corrosion resistance, large specific surface area, excellent conductivity and transmittance, good stability, easy separation and high porosity that is conducive to the in-situ growth of semiconductors, making it a good substrate material for loading adsorbents and photocatalysts. Most existing technologies use a hydrothermal method to directly deposit and grow CdS nanoparticles on carbon cloth. However, this method has a low solid loading capacity, resulting in low efficiency in degradation and recycling of organic pollutants, and is therefore difficult to meet the needs of actual engineering applications. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a piezoelectric photocatalytic material of CdS nanorods densely coated with carbon cloth, so as to solve the problem of low efficiency of degradation and recycling of organic pollutants by photocatalytic materials prepared by existing methods.

[0005] Another object of the present invention is to provide a piezoelectric photocatalytic material of CdS nanorods densely coated with carbon cloth.

[0006] The technical solution adopted by the present invention is a method for preparing a piezoelectric photocatalytic material of CdS nanorods densely coated with carbon cloth, which is specifically implemented according to the following steps:

[0007] Step 1, activating the surface of the carbon cloth;

[0008] Step 2, immersing the carbon cloth treated in step 1 in CdO sol, and then centrifuging and drying to obtain a carbon cloth coated with a CdO gel layer;

[0009] Step 3, treating the carbon cloth coated with the CdO gel layer obtained in step 2 by deep ultraviolet light irradiation degradation combined with a heat treatment process to obtain a carbon cloth coated with a CdO ceramic layer;

[0010] Step 4: Depositing CdS nanorods on the carbon cloth coated with the CdO ceramic layer obtained in step 3 by a hydrothermal method to obtain a carbon piezoelectric photocatalytic material densely coated with CdS nanorods.

[0011] The present invention is also characterized in that:

[0012] The specific process of step 1 is: ultrasonically clean the carbon cloth with acetone, ethanol and deionized water in turn, then soak the cleaned carbon cloth in concentrated nitric acid solution for activation treatment for 12h to 48h, and then clean the activated carbon cloth with deionized water until it is neutral, and dry it for use.

[0013] In step 2, the preparation method of CdO sol is specifically as follows: cadmium acetate dihydrate is added to ethylene glycol monomethyl ether and stirred in a water bath, and then ethanolamine is added and stirred in a water bath, and then allowed to stand for aging to obtain CdO sol.

[0014] The concentration of CdO sol is 0.1 mol / L to 1.0 mol / L; the molar ratio of ethanolamine to cadmium acetate dihydrate is 1:1; and the temperatures of the two water baths are both 30°C to 60°C.

[0015] In step 2, the immersion time is 5 min to 20 min, the centrifugal speed is 500 r / min to 2000 r / min, the centrifugal time is 4 min to 10 min, the drying temperature is 60° C. to 80° C., and the drying time is 10 min to 40 min.

[0016] In step 3, the deep ultraviolet light irradiation degradation combined with heat treatment process is specifically as follows: the carbon cloth coated with the CdO gel layer obtained in step 2 is placed on a heating table at 100°C to 250°C, and the surface of the carbon cloth coated with the CdO gel layer is irradiated with ultraviolet light with a wavelength less than 257.3nm. The ultraviolet irradiation time is 60min to 150min, and then annealed at 100°C to 200°C for 1h to 4h.

[0017] The specific process of step 4 is:

[0018] Step 4.1, adding cadmium nitrate tetrahydrate and thiourea to deionized water, stirring, adding polyvinyl pyrrolidone, and continuing to stir to obtain a CdS hydrothermal reaction solution;

[0019] Step 4.2, transferring the CdS hydrothermal reaction solution prepared in step 4.1 to a polytetrafluoroethylene reactor, immersing the carbon cloth coated with the CdO ceramic layer obtained in step 3 into the CdS hydrothermal reaction solution for hydrothermal reaction, and after the reaction is completed, cooling the reaction solution to room temperature with the furnace and taking out the sample;

[0020] Step 4.3, rinse the sample taken out in step 4.2 with deionized water, and dry it to obtain the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods.

[0021] In step 4.1, the concentration of the CdS hydrothermal reaction solution is 0.05 mol / L to 0.15 mol / L;

[0022] In step 4.2, the temperature of the hydrothermal reaction is 160° C. to 220° C., and the reaction time is 3 h to 9 h.

[0023] Another technical solution adopted by the present invention is that the CdS nanorods densely coat the carbon cloth piezoelectric photocatalytic material, which is obtained by the above-mentioned preparation method.

[0024] The beneficial effects of the present invention are:

[0025] (1) The carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods prepared by the present invention uses carbon cloth as a substrate, which solves the problem that nano CdS powder materials are easy to agglomerate and precipitate; at the same time, the flexible carbon cloth has the characteristics of being light and buoyant, and can quickly capture mechanical energy in water, thereby stimulating the excellent piezoelectric effect of the CdS photocatalyst and obtaining better photocatalytic properties;

[0026] (2) The CdO ceramic layer prepared in the present invention serves as a mediating layer between the carbon cloth and the CdS nanophotocatalyst, thereby realizing the dense loading of the CdS nanophotocatalyst on the carbon cloth (CC), and exhibiting excellent recycling degradation performance; in addition, the CdO ceramic layer and the CdS nanorods can construct a direct Z-type heterojunction, which is beneficial to the separation of photogenerated electron-hole pairs and prevents the photocorrosion reaction of CdS; finally, under the synergistic effect of the CdO / CdS direct Z-type heterojunction and the piezoelectric effect of the CdS nanorods, the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods exhibits the performance of highly efficient degradation of organic pollutants in water. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 The XRD spectrum of the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods prepared in Example 1 of the present invention;

[0028] Figure 2 This is a SEM image of the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods prepared in Example 1 of the present invention at a magnification of 3k;

[0029] Figure 3 This is a SEM image of the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods prepared in Example 1 of the present invention at a magnification of 50k;

[0030] Figure 4 It is a line graph of the degradation efficiency of methylene blue by the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods prepared by the method of the present invention;

[0031] Figure 5 This is a graph showing the photocatalytic degradation efficiency of methylene blue (MB) by the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods prepared in Example 1 of the present invention;

[0032] Figure 6 This is a graph showing the piezoelectric photocatalytic degradation efficiency of methylene blue (MB) by the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods prepared in Example 1 of the present invention;

[0033] Figure 7 This is a stability test chart of the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0034] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0035] The preparation method of the piezoelectric photocatalytic material of CdS nanorods densely coated with carbon cloth of the present invention is specifically implemented according to the following steps:

[0036] Step 1, activating the surface of the carbon cloth;

[0037] The specific process is:

[0038] The carbon cloth was ultrasonically cleaned with acetone, ethanol and deionized water for 2 hours in sequence, and then the cleaned carbon cloth was immersed in a concentrated nitric acid solution with a mass fraction of 65% for activation treatment for 12 to 48 hours to enhance the hydrophilicity and activity of the fiber surface. After the activation treatment, the carbon cloth was washed with deionized water until it was neutral and dried at 80°C for use;

[0039] Step 2, immersing the carbon cloth treated in step 1 in CdO sol for 5 min to 20 min, centrifuging at a speed of 500 r / min to 2000 r / min for 4 min to 10 min, and drying at 60° C. to 80° C. for 10 min to 40 min to obtain a carbon cloth coated with a CdO gel layer;

[0040] The preparation method of CdO sol is as follows: 1.0661 g to 10.661 g of cadmium acetate dihydrate is added to 40 ml of ethylene glycol monomethyl ether, and stirred in a water bath at 30° C. to 60° C. for 1 hour, and then 0.244 g to 2.44 g of ethanolamine is added, and the mixture is stirred in a water bath at 30° C. to 60° C. for 6 hours to 12 hours, wherein the molar ratio of ethanolamine to cadmium acetate dihydrate is 1:1, and after the mixture is left to stand for at least 12 hours, a CdO sol with a concentration of 0.1 mol / L to 1.0 mol / L is obtained;

[0041] Step 3, treating the carbon cloth coated with the CdO gel layer obtained in step 2 by deep ultraviolet light irradiation degradation combined with a heat treatment process to obtain a carbon cloth coated with a CdO ceramic layer;

[0042] The deep ultraviolet light irradiation degradation combined with heat treatment process is specifically as follows: placing the carbon cloth coated with the CdO gel layer obtained in step 2 on a heating table at 100°C to 250°C, irradiating the surface of the carbon cloth coated with the CdO gel layer with ultraviolet light having a wavelength less than 257.3nm for 60min to 150min, and then annealing at 100°C to 200°C for 1h to 4h to convert the CdO gel layer into a CdO ceramic layer;

[0043] Step 4, using CdO as a mediating layer, using a hydrothermal method to deposit CdS nanorods on the carbon cloth coated with the CdO ceramic layer obtained in step 3, to obtain a carbon piezoelectric photocatalytic material densely coated with CdS nanorods;

[0044] The specific process is:

[0045] Step 4.1, adding 1.5424 g to 4.6262 g of cadmium nitrate tetrahydrate and 1.1418 g to 3.4254 g of thiourea to 100 ml of deionized water, stirring for 1 hour, then adding 0.2 g to 0.5 g of polyvinyl pyrrolidone, and continuing to stir for 1 hour to obtain a CdS hydrothermal reaction solution with a concentration of 0.05 mol / L to 0.15 mol / L;

[0046] Step 4.2, transferring the CdS hydrothermal reaction solution prepared in step 4.1 to a polytetrafluoroethylene reactor, immersing the carbon cloth coated with the CdO ceramic layer obtained in step 3 into the CdS hydrothermal reaction solution for hydrothermal reaction, wherein the temperature of the hydrothermal reaction is 160° C. to 220° C., and the reaction time is 3 h to 9 h. After the reaction is completed, the sample is taken out after cooling to room temperature with the furnace;

[0047] Step 4.3, rinse the sample taken out in step 4.2 with deionized water, and dry it at 80°C to obtain a carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods.

[0048] Example 1

[0049] Step 1, activating the surface of the carbon cloth;

[0050] The specific process is:

[0051] The carbon cloth was ultrasonically cleaned with acetone, ethanol and deionized water for 2 hours in sequence, and then the cleaned carbon cloth was immersed in a concentrated nitric acid solution with a mass fraction of 65% for activation treatment for 24 hours. After the activation treatment, the carbon cloth was washed with deionized water until it was neutral, and dried at 80°C for use;

[0052] Step 2, immersing the carbon cloth treated in step 1 in CdO sol for 20 minutes, centrifuging at a speed of 500 r / min for 10 minutes, and drying at 80° C. for 10 minutes to obtain a carbon cloth coated with a CdO gel layer;

[0053] The preparation method of CdO sol is as follows: 1.0661 g of cadmium acetate dihydrate is added to 40 ml of ethylene glycol monomethyl ether and stirred in a water bath at 60° C. for 1 hour, and then 0.244 g of ethanolamine is added and stirred in a water bath at 60° C. for 6 hours, wherein the molar ratio of ethanolamine to cadmium acetate dihydrate is 1:1, and then the mixture is allowed to stand and age for at least 12 hours to obtain a CdO sol with a concentration of 0.1 mol / L;

[0054] Step 3, treating the carbon cloth coated with the CdO gel layer obtained in step 2 by deep ultraviolet light irradiation degradation combined with a heat treatment process to obtain a carbon cloth coated with a CdO ceramic layer;

[0055] The deep ultraviolet light irradiation degradation combined with heat treatment process is specifically as follows: placing the carbon cloth coated with the CdO gel layer obtained in step 2 on a heating table at 200°C, irradiating the surface of the carbon cloth coated with the CdO gel layer with ultraviolet light having a wavelength less than 257.3nm for 120 minutes, and then annealing at 200°C for 1 hour to transform the CdO gel layer into a CdO ceramic layer;

[0056] Step 4, using CdO as a mediating layer, using a hydrothermal method to deposit CdS nanorods on the carbon cloth coated with the CdO ceramic layer obtained in step 3, to obtain a carbon piezoelectric photocatalytic material densely coated with CdS nanorods;

[0057] The specific process is:

[0058] Step 4.1, adding 3.0848 g of cadmium nitrate tetrahydrate and 2.2856 g of thiourea to 100 ml of deionized water, stirring for 1 hour, then adding 0.4 g of polyvinyl pyrrolidone, and continuing to stir for 1 hour to obtain a CdS hydrothermal reaction solution with a concentration of 0.1 mol / L;

[0059] Step 4.2, transferring the CdS hydrothermal reaction solution prepared in step 4.1 to a polytetrafluoroethylene reactor, immersing the carbon cloth coated with the CdO ceramic layer obtained in step 3 into the CdS hydrothermal reaction solution for hydrothermal reaction, the temperature of the hydrothermal reaction is 200°C, the reaction time is 5h, after the end, cool to room temperature with the furnace and take out the sample;

[0060] Step 4.3, rinse the sample taken out in step 4.2 with deionized water, and dry it at 80°C to obtain a carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods.

[0061] After irradiation with a xenon lamp for 240 minutes, the degradation rate of methylene blue by the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods prepared in this example was 95.2%.

[0062] Example 2

[0063] Step 1, activating the surface of the carbon cloth;

[0064] The specific process is:

[0065] The carbon cloth was ultrasonically cleaned with acetone, ethanol and deionized water for 2 hours in sequence, and then the cleaned carbon cloth was immersed in a concentrated nitric acid solution with a mass fraction of 65% for activation treatment for 12 hours. After the activation treatment, the activated carbon cloth was washed with deionized water until it was neutral, and dried at 80°C for use;

[0066] Step 2, immersing the carbon cloth treated in step 1 in CdO sol for 15 minutes, centrifuging at a speed of 1000 r / min for 8 minutes, and drying at 75° C. for 20 minutes to obtain a carbon cloth coated with a CdO gel layer;

[0067] The preparation method of CdO sol is as follows: 4.2644 g of cadmium acetate dihydrate is added to 40 ml of ethylene glycol monomethyl ether and stirred in a water bath at 50° C. for 1 hour, and then 0.976 g of ethanolamine is added and stirred in a water bath at 50° C. for 8 hours, wherein the molar ratio of ethanolamine to cadmium acetate dihydrate is 1:1, and then the mixture is allowed to stand and age for 18 hours to obtain a CdO sol with a concentration of 0.4 mol / L;

[0068] Step 3, treating the carbon cloth coated with the CdO gel layer obtained in step 2 by deep ultraviolet light irradiation degradation combined with a heat treatment process to obtain a carbon cloth coated with a CdO ceramic layer;

[0069] The deep ultraviolet light irradiation degradation combined with heat treatment process is specifically as follows: placing the carbon cloth coated with the CdO gel layer obtained in step 2 on a heating table at 250°C, irradiating the surface of the carbon cloth coated with the CdO gel layer with ultraviolet light having a wavelength less than 257.3nm for 60 minutes, and then annealing at 160°C for 2 hours to transform the CdO gel layer into a CdO ceramic layer;

[0070] Step 4, using CdO as a mediating layer, using a hydrothermal method to deposit CdS nanorods on the carbon cloth coated with the CdO ceramic layer obtained in step 3, to obtain a carbon piezoelectric photocatalytic material densely coated with CdS nanorods;

[0071] The specific process is:

[0072] Step 4.1, add 1.5424 g of cadmium nitrate tetrahydrate and 1.1418 g of thiourea to 100 ml of deionized water, stir for 1 hour, then add 0.2 g of polyvinyl pyrrolidone, continue stirring for 1 hour, and obtain a CdS hydrothermal reaction solution with a concentration of 0.05 mol / L;

[0073] Step 4.2, transferring the CdS hydrothermal reaction solution prepared in step 4.1 to a polytetrafluoroethylene reactor, immersing the carbon cloth coated with the CdO ceramic layer obtained in step 3 into the CdS hydrothermal reaction solution for hydrothermal reaction, the temperature of the hydrothermal reaction is 220°C, the reaction time is 3h, after the end, cool to room temperature with the furnace and take out the sample;

[0074] Step 4.3, rinse the sample taken out in step 4.2 with deionized water, and dry it at 80°C to obtain a carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods.

[0075] After irradiation with a xenon lamp for 240 minutes, the degradation rate of methylene blue by the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods prepared in this example was 93.3%.

[0076] Example 3

[0077] Step 1, activating the surface of the carbon cloth;

[0078] The specific process is:

[0079] The carbon cloth was ultrasonically cleaned with acetone, ethanol and deionized water for 2 hours in sequence, and then the cleaned carbon cloth was immersed in a concentrated nitric acid solution with a mass fraction of 65% for activation treatment for 36 hours. After the activation treatment, the activated carbon cloth was washed with deionized water until it was neutral, and dried at 80°C for use;

[0080] Step 2, immersing the carbon cloth treated in step 1 in CdO sol for 10 minutes, centrifuging at a speed of 1500 r / min for 6 minutes, and drying at 70° C. for 30 minutes to obtain a carbon cloth coated with a CdO gel layer;

[0081] The preparation method of CdO sol is as follows: 7.4627g of cadmium acetate dihydrate is added to 40ml of ethylene glycol monomethyl ether and stirred in a water bath at 40°C for 1h, and then 1.708g of ethanolamine is added and stirred in a water bath at 40°C for 10h, wherein the molar ratio of ethanolamine to cadmium acetate dihydrate is 1:1, and then the mixture is allowed to stand and age for 24h to obtain a CdO sol with a concentration of 0.7mol / L;

[0082] Step 3, treating the carbon cloth coated with the CdO gel layer obtained in step 2 by deep ultraviolet light irradiation degradation combined with a heat treatment process to obtain a carbon cloth coated with a CdO ceramic layer;

[0083] The deep ultraviolet light irradiation degradation combined with heat treatment process is specifically as follows: placing the carbon cloth coated with the CdO gel layer obtained in step 2 on a heating table at 150°C, irradiating the surface of the carbon cloth coated with the CdO gel layer with ultraviolet light having a wavelength less than 257.3nm for 90 minutes, and then annealing at 140°C for 3 hours to transform the CdO gel layer into a CdO ceramic layer;

[0084] Step 4, using CdO as a mediating layer, using a hydrothermal method to deposit CdS nanorods on the carbon cloth coated with the CdO ceramic layer obtained in step 3, to obtain a carbon piezoelectric photocatalytic material densely coated with CdS nanorods;

[0085] The specific process is:

[0086] Step 4.1, adding 2.3136 g of cadmium nitrate tetrahydrate and 1.7127 g of thiourea to 100 ml of deionized water, stirring for 1 hour, then adding 0.3 g of polyvinyl pyrrolidone, and continuing to stir for 1 hour to obtain a CdS hydrothermal reaction solution with a concentration of 0.075 mol / L;

[0087] Step 4.2, transferring the CdS hydrothermal reaction solution prepared in step 4.1 to a polytetrafluoroethylene reactor, immersing the carbon cloth coated with the CdO ceramic layer obtained in step 3 into the CdS hydrothermal reaction solution for hydrothermal reaction, the temperature of the hydrothermal reaction is 180°C, the reaction time is 7h, after the end, cool to room temperature with the furnace and take out the sample;

[0088] Step 4.3, rinse the sample taken out in step 4.2 with deionized water, and dry it at 80°C to obtain a carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods.

[0089] After irradiation with a xenon lamp for 240 minutes, the degradation rate of methylene blue by the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods prepared in this example was 87.3%.

[0090] Example 4

[0091] Step 1, activating the surface of the carbon cloth;

[0092] The specific process is:

[0093] The carbon cloth was ultrasonically cleaned with acetone, ethanol and deionized water for 2 hours in sequence, and then the cleaned carbon cloth was immersed in a concentrated nitric acid solution with a mass fraction of 65% for activation treatment for 48 hours. After the activation treatment, the activated carbon cloth was washed with deionized water until it was neutral, and dried at 80°C for use;

[0094] Step 2, immersing the carbon cloth treated in step 1 in CdO sol for 5 minutes, centrifuging at a speed of 2000 r / min for 4 minutes, and drying at 60° C. for 40 minutes to obtain a carbon cloth coated with a CdO gel layer;

[0095] The preparation method of CdO sol is as follows: 10.661 g of cadmium acetate dihydrate is added to 40 ml of ethylene glycol monomethyl ether and stirred in a water bath at 30° C. for 1 hour, and then 2.44 g of ethanolamine is added and stirred in a water bath at 30° C. for 12 hours, wherein the molar ratio of ethanolamine to cadmium acetate dihydrate is 1:1, and then the mixture is allowed to stand and age for 24 hours to obtain a CdO sol with a concentration of 1.0 mol / L;

[0096] Step 3, treating the carbon cloth coated with the CdO gel layer obtained in step 2 by deep ultraviolet light irradiation degradation combined with a heat treatment process to obtain a carbon cloth coated with a CdO ceramic layer;

[0097] The deep ultraviolet light irradiation degradation combined with heat treatment process is specifically as follows: placing the carbon cloth coated with the CdO gel layer obtained in step 2 on a heating table at 100°C, irradiating the surface of the carbon cloth coated with the CdO gel layer with ultraviolet light having a wavelength less than 257.3nm for 150 minutes, and then annealing at 100°C for 4 hours to transform the CdO gel layer into a CdO ceramic layer;

[0098] Step 4, using CdO as a mediating layer, using a hydrothermal method to deposit CdS nanorods on the carbon cloth coated with the CdO ceramic layer obtained in step 3, to obtain a carbon piezoelectric photocatalytic material densely coated with CdS nanorods;

[0099] The specific process is:

[0100] Step 4.1, adding 4.6262 g of cadmium nitrate tetrahydrate and 3.4254 g of thiourea to 100 ml of deionized water, stirring for 1 hour, then adding 0.5 g of polyvinyl pyrrolidone, and continuing to stir for 1 hour to obtain a CdS hydrothermal reaction solution with a concentration of 0.15 mol / L;

[0101] Step 4.2, transferring the CdS hydrothermal reaction solution prepared in step 4.1 to a polytetrafluoroethylene reactor, immersing the carbon cloth coated with the CdO ceramic layer obtained in step 3 into the CdS hydrothermal reaction solution for hydrothermal reaction, the temperature of the hydrothermal reaction is 160°C, the reaction time is 9 hours, and after the end, cooling to room temperature with the furnace and taking out the sample;

[0102] Step 4.3, rinse the sample taken out in step 4.2 with deionized water, and dry it at 80°C to obtain a carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods.

[0103] After irradiation with a xenon lamp for 240 minutes, the degradation rate of methylene blue by the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods prepared in this example was 84.4%.

[0104] from Figure 1 It can be seen that the XRD diffraction peaks of CdO@CC (carbon cloth coated with CdO ceramic layer) and CdS / CdO@CC (carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods) correspond to the diffraction peaks of standard cards PDF#05-0640 and PDF#41-1049, respectively. This shows that nano-CdS has been successfully loaded on carbon cloth coated with CdO ceramic layer, and the present invention has successfully prepared carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods.

[0105] from Figure 2 , Figure 3 and Figure 4 It can be seen that the nanorod-shaped CdS photocatalyst is uniformly and densely loaded on the surface of the carbon cloth coated with the CdO ceramic layer.

[0106] A certain amount of carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods in Examples 1 to 4 was added to a certain concentration of methylene blue (MB) to simulate the process of degrading organic pollutants in sewage. The specific operation is: add the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods loaded with 100mg CdS to 200ml of 0.1mol / L methylene blue, soak it in a dark environment for 60min to allow the surface to reach an adsorption / equilibrium state, and then collect 3ml of methylene blue solution every 30min under the conditions of xenon lamp irradiation to simulate photocatalysis and ultrasonic vibration synergistic xenon lamp irradiation to simulate piezoelectric photocatalysis, and put it into a UV-visible photometer to test the absorbance. The test results are as follows:

[0107] from Figure 4 , Figure 5 , Figure 6 It can be seen that the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods prepared by the present invention has excellent adsorption capacity and photocatalytic degradation ability. The degradation performance of the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods prepared in Examples 1 to 4 is all above 80%, among which the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods prepared in Example 1 has the best performance. After 240 minutes of xenon lamp irradiation, the degradation rate of methylene blue is 95.2%; after 120 minutes of ultrasonic vibration and xenon lamp irradiation, the piezoelectric photocatalytic degradation rate of methylene blue by the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods is 96.5%. Figure 7 It can be seen that after 5 photocatalytic cycle tests, the degradation efficiency of the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods of the present invention for methylene blue is still maintained at 87.15%, which has excellent recycling performance.

[0108] In summary, the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods prepared by the method of the present invention exhibits a more efficient performance of degrading dyes under the condition of the assistance of ultrasonic vibration, which is due to the ultrasonic vibration exciting the piezoelectric effect of CdS nanomaterials, constructing a polarized electric field inside the CdS nanorods, and accelerating the separation of photogenerated electron-hole pairs. In addition, the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods has excellent photocatalytic degradation performance, piezoelectric photocatalytic degradation performance, adsorption and desorption capacity and recycling performance, and is easy to recycle, solving the technical problem that cadmium sulfide powder is difficult to separate and recycle.

Claims

1. A method for preparing a piezoelectric photocatalytic material of CdS nanorods densely coated with carbon cloth, characterized in that: Follow the steps below to implement it: Step 1, activating the surface of the carbon cloth; Step 2, immersing the carbon cloth treated in step 1 in CdO sol, and then centrifuging and drying to obtain a carbon cloth coated with a CdO gel layer; Step 3, treating the carbon cloth coated with the CdO gel layer obtained in step 2 by deep ultraviolet light irradiation degradation combined with a heat treatment process to obtain a carbon cloth coated with a CdO ceramic layer; Step 4: Depositing CdS nanorods on the carbon cloth coated with the CdO ceramic layer obtained in step 3 by a hydrothermal method to obtain a carbon piezoelectric photocatalytic material densely coated with CdS nanorods.

2. The method for preparing the CdS nanorods densely coated carbon cloth piezoelectric photocatalytic material according to claim 1, characterized in that: The specific process of step 1 is: ultrasonically clean the carbon cloth with acetone, ethanol and deionized water in turn, then soak the cleaned carbon cloth in concentrated nitric acid solution for activation treatment for 12h to 48h, and then clean the activated carbon cloth with deionized water until it is neutral, and dry it for use.

3. The method for preparing the CdS nanorods densely coated carbon cloth piezoelectric photocatalytic material according to claim 1, characterized in that: In step 2, the preparation method of CdO sol is specifically as follows: cadmium acetate dihydrate is added to ethylene glycol monomethyl ether and stirred in a water bath, and then ethanolamine is added and stirred in a water bath, and then allowed to stand for aging to obtain CdO sol.

4. The method for preparing the CdS nanorods densely coated carbon cloth piezoelectric photocatalytic material according to claim 3, characterized in that: The concentration of CdO sol is 0.1 mol / L to 1.0 mol / L; the molar ratio of ethanolamine to cadmium acetate dihydrate is 1:1; and the temperatures of the two water baths are both 30°C to 60°C.

5. The method for preparing the CdS nanorods densely coated carbon cloth piezoelectric photocatalytic material according to claim 1, characterized in that: In step 2, the immersion time is 5 min to 20 min, the centrifugal speed is 500 r / min to 2000 r / min, the centrifugal time is 4 min to 10 min, the drying temperature is 60° C. to 80° C., and the drying time is 10 min to 40 min.

6. The method for preparing the CdS nanorods densely coated carbon cloth piezoelectric photocatalytic material according to claim 1, characterized in that: In step 3, the deep ultraviolet light irradiation degradation combined with heat treatment process is specifically as follows: the carbon cloth coated with the CdO gel layer obtained in step 2 is placed on a heating table at 100°C to 250°C, and the surface of the carbon cloth coated with the CdO gel layer is irradiated with ultraviolet light with a wavelength less than 257.3nm. The ultraviolet irradiation time is 60min to 150min, and then annealed at 100°C to 200°C for 1h to 4h.

7. The method for preparing the CdS nanorods densely coated carbon cloth piezoelectric photocatalytic material according to claim 1, characterized in that: The specific process of step 4 is: Step 4.1, adding cadmium nitrate tetrahydrate and thiourea to deionized water, stirring, adding polyvinyl pyrrolidone, and continuing to stir to obtain a CdS hydrothermal reaction solution; Step 4.2, transferring the CdS hydrothermal reaction solution prepared in step 4.1 to a polytetrafluoroethylene reactor, immersing the carbon cloth coated with the CdO ceramic layer obtained in step 3 into the CdS hydrothermal reaction solution for hydrothermal reaction, and after the reaction is completed, cooling the reaction solution to room temperature with the furnace and taking out the sample; Step 4.3, rinse the sample taken out in step 4.2 with deionized water, and dry it to obtain the carbon cloth piezoelectric photocatalytic material densely coated with CdS nanorods.

8. The method for preparing the CdS nanorods densely coated carbon cloth piezoelectric photocatalytic material according to claim 7, characterized in that: In step 4.1, the concentration of the CdS hydrothermal reaction solution is 0.05 mol / L to 0.15 mol / L; In step 4.2, the temperature of the hydrothermal reaction is 160° C. to 220° C., and the reaction time is 3 h to 9 h.