Hard alloy holding-up hammer material with symmetrical structure and preparation method thereof

A multi-layer symmetrical structure is formed through vacuum hot pressing and hot isostatic pressing, combined with magnetron sputtering technology, which solves the problem of insufficient toughness and high-temperature hardness of carbide top hammers in high-pressure and high-temperature environments, and significantly improves its compressive strength. and high temperature performance, extending service life.

CN118847996AInactive Publication Date: 2024-10-29SHAANXI SCI TECH UNIV
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202410916183.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-10-29
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing carbide top hammers have low toughness and high-temperature hardness in high-pressure and high-temperature environments, and are prone to fatigue problems, affecting the stable operation and service life of the equipment.

Method used

Use vacuum hot pressing and hot isostatic pressing methods to prepare multi-layer symmetric structure cemented carbide, combine with magnetron sputtering technology to deposit conductive wear-resistant coating, optimize the composition and structural design of the cemented carbide, and improve the toughness, hardness and toughness of the material. Conductive properties.

Benefits of technology

The fracture toughness, compressive strength and high-temperature hardness of the cemented carbide top hammer are significantly improved to ensure the stability and service life in high-temperature and high-pressure environments and meet the needs of efficient and stable operation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118847996A_ABST
    Figure CN118847996A_ABST
Patent Text Reader

Abstract

The invention discloses a hard alloy holding-up hammer material with a symmetrical structure and a preparation method thereof, and belongs to the technical field of hard alloy holding-up hammer preparation. The method comprises the following steps: selecting three hard alloy components, and pre-sintering by a vacuum hot pressing method to obtain a hard alloy sheet; a cube hard alloy serves as a core material, and the periphery of the core material is wrapped with hard alloy pieces through a hot isostatic pressing method to form a multilayer symmetrical structure hard alloy. A conductive wear-resistant coating is prepared on the surface of the multilayer symmetrical-structure hard alloy through a magnetron sputtering method, and the symmetrical-structure hard alloy holding-up hammer material is obtained. The method has the advantages of high component control precision, high process stability and high repeatability, and obdurability and excellent high-temperature mechanical properties of the hard alloy holding-up hammer material can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of cemented carbide anvil preparation, and in particular to a cemented carbide anvil material with a symmetrical structure and a preparation method thereof. Background Art

[0002] In the field of high-voltage equipment, carbide top hammers are the core high-voltage components, and their performance is directly related to the operating efficiency and stability of high-voltage equipment. At present, high-voltage equipment such as two-sided top hammers, six-sided top hammers and eight-sided top hammers are widely used in many fields such as material synthesis, scientific research and industrial production, among which the role of carbide top hammers is particularly critical.

[0003] However, existing commercial cemented carbide top hammers have some obvious deficiencies in performance. First of all, low toughness and high-temperature hardness are one of its main problems. Under high-pressure and high-temperature working environments, the top hammer needs to withstand huge stress and temperature changes. If its toughness is insufficient, it is easy to break or deform, causing equipment failure; at the same time, insufficient high-temperature hardness will affect the working performance of the top hammer at high temperatures and reduce its service life.

[0004] Secondly, fatigue problems are prone to occur under long-term service conditions, which is also an important challenge currently faced by cemented carbide top hammers. Since high-pressure equipment often needs to operate continuously for a long time, the top hammer works under continuous high stress and high temperature conditions, which is prone to fatigue cracks, and then causes serious problems such as fracture, which not only affects the normal operation of the equipment, but also may pose a threat to the safety of operators.

[0005] The cemented carbide top hammer is an important high-voltage component of high-voltage equipment such as two-sided top hammer, six-sided top hammer and eight-sided top hammer. It is responsible for transmitting high voltage, electricity and heat conduction. Therefore, its compressive strength and electrical and thermal conductivity are key factors in determining the production efficiency of high-voltage equipment and the stability of high-voltage process parameters. Existing commercial cemented carbide top hammers have low toughness and high-temperature hardness, and are prone to fatigue problems under long-term service conditions, which affects the stable operation of high-voltage equipment. In order to solve the above problems, it is urgent to develop a method for preparing a cemented carbide top hammer. Summary of the invention

[0006] In view of the engineering problems that the existing cemented carbide anvils have low toughness and high temperature hardness, and are prone to fatigue under long-term service conditions, the present invention provides a symmetrical structure cemented carbide anvil material and a preparation method thereof. A series of technologies using a cemented carbide blank as the core material, vacuum hot pressing and hot isostatic pressing methods to form a multi-layer symmetrical structure, and then depositing a conductive wear-resistant coating are the key means to solve the above engineering problems.

[0007] In order to achieve the above object, the present invention is implemented by adopting the following technical scheme:

[0008] In a first aspect, the present invention provides a method for preparing a symmetrically structured cemented carbide anvil material, comprising:

[0009] Three cemented carbide components were selected and pre-burned by vacuum hot pressing to obtain cemented carbide sheets;

[0010] A cube of cemented carbide is used as the core material, and cemented carbide sheets are wrapped around the core material by hot isostatic pressing to form a multi-layer symmetrical structure of cemented carbide;

[0011] A conductive wear-resistant coating was prepared on the surface of multi-layer symmetrically structured cemented carbide by magnetron sputtering to obtain a symmetrically structured cemented carbide anvil material.

[0012] As a further improvement of the present invention, the cemented carbide is YG10 cemented carbide.

[0013] As a further improvement of the present invention, the cemented carbide core material is a coarse-grained structure with an average grain size of 5 to 8 microns, a relative density of 99.3 to 99.5%, a hardness of 16.3 to 16.7 GPa, and a fracture toughness of 11.6 to 12.2 MPa·m 1 / 2 .

[0014] As a further improvement of the present invention, the mass percentages of tungsten carbide and cobalt in the three cemented carbides are respectively (91-93):(7-9), (93-95):(5-7) and (96-98):(2-4).

[0015] As a further improvement of the present invention, the vacuum hot pressing method is to pre-sinter the three components into green bodies at 740-780°C for 18-24 minutes respectively; and arrange the pre-sintered green bodies of the three components symmetrically in a manner of increasing cobalt content and then decreasing cobalt content.

[0016] As a further improvement of the present invention, the hot isostatic pressing method is to sinter the cemented carbide sheets to the six surfaces of the core material layer by layer at 1310-1380° C. for 32-41 minutes.

[0017] As a further improvement of the present invention, in the preparation of the conductive wear-resistant coating on the surface of the multi-layer symmetrical structure cemented carbide by the magnetron sputtering method, the magnetron sputtering target is pure tungsten carbide, the sputtering time is 78 to 89 minutes, and the heating temperature is 430 to 510°C.

[0018] As a further improvement of the present invention, the conductive wear-resistant coating is a deposited tungsten carbide layer with a thickness of 3.2 to 3.8 microns.

[0019] In a second aspect, the present invention provides a symmetrically structured cemented carbide top hammer material, which is prepared by the preparation method of the symmetrically structured cemented carbide top hammer material described in the claims.

[0020] As a further improvement of the present invention, the prepared cemented carbide top hammer material has a symmetrical structure, and the fracture toughness of the material is greater than or equal to 13.5 MPa·m 1 / 2 , microhardness greater than or equal to 24.2GPa, compressive strength greater than or equal to 4750MPa, high temperature (1000℃) hardness greater than or equal to 20.3GPa.

[0021] Compared with the prior art, the present invention has the following characteristics and advantages:

[0022] The present invention first uses a cemented carbide blank as a core material, selects three cemented carbide components, pre-sinters cemented carbide sheets by a vacuum hot pressing method, wraps a multi-layer symmetrical structure cemented carbide around the core material by a hot isostatic pressing method, and then uses a magnetron sputtering method to prepare a conductive wear-resistant coating on the surface of the multi-layer symmetrical structure cemented carbide; wherein coarse-grained cemented carbide is used as the core material to ensure the toughness performance of the overall material; the three components are designed and arranged on the six surfaces of the core material from large to small according to the cobalt content, which not only forms a gradient structure with different toughness and hardness, and realizes an effective combination of hardness, strength and toughness, but also ensures the symmetry of the performance due to the symmetry of the structure, and improves the uniformity and stability of high-voltage transmission; pure tungsten carbide with better conductivity and wear resistance is deposited on the surface of the symmetrical structure, which on the one hand ensures the stability of the current and improves the high-temperature and high-pressure sintering quality, and on the other hand improves the surface accuracy of the top hammer and extends its service life.

[0023] The hard alloy anvil material prepared by the present invention has a symmetrical structure, and the fracture toughness of the material is greater than or equal to 13.5 MPa·m 1 / 2 , microhardness greater than or equal to 24.2GPa, compressive strength greater than or equal to 4750MPa, high temperature (1000℃) hardness greater than or equal to 20.3GPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a schematic diagram of a method for preparing a symmetrically structured cemented carbide top hammer material according to the present invention, wherein 1, 2, and 3 are three types of cemented carbides. DETAILED DESCRIPTION

[0025] In order to make the method problems, method solutions and beneficial effects to be solved by the present application more clearly understood, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present application and are not used to limit the present application.

[0026] In this application, the term "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural. The character " / " generally indicates that the associated objects are in an "or" relationship.

[0027] In this application, "at least one" means one or more, and "plurality" means two or more. "At least one of the following" or similar expressions refers to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e. a and b), ac, bc, or abc, where a, b, c can be single or multiple.

[0028] It should be understood that in the various embodiments of the present application, the size of the serial numbers of the above-mentioned processes does not mean the order of execution, some or all of the steps can be executed in parallel or sequentially, and the execution order of each process should be determined by its function and internal logic, and should not constitute any limitation on the implementation process of the embodiments of the present application.

[0029] The terms used in the embodiments of the present application are only for the purpose of describing specific embodiments, and are not intended to limit the present application. The singular forms "a", "an" and "the" used in the embodiments of the present application and the appended claims are also intended to include plural forms, unless the context clearly indicates other meanings.

[0030] The weight of the relevant components mentioned in the embodiment description of the present application can not only refer to the specific content of each component, but also represent the proportional relationship between the weights of the components. Therefore, as long as the content of the relevant components is proportionally enlarged or reduced according to the embodiment description of the present application, it is within the scope disclosed in the embodiment description of the present application. Specifically, the mass in the embodiment description of the present application can be μg, mg, g, kg and other mass units known in the chemical industry.

[0031] The terms "first" and "second" are used only for descriptive purposes to distinguish objects such as substances from each other, and should not be understood as indicating or implying relative importance or implicitly indicating the number of method features indicated. For example, without departing from the scope of the embodiments of the present application, the first XX may also be referred to as the second XX, and similarly, the second XX may also be referred to as the first XX. Thus, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features.

[0032] The following is an explanation of the terms used for vacuum hot pressing, magnetron sputtering, and hot isostatic pressing:

[0033] Vacuum hot pressing is a molding process mainly used to prepare composite materials. The method includes the following steps: The required materials are arranged in a certain shape and layer to form a preform. After the preform is placed in the mold, it is evacuated to the required vacuum level. This is to exclude air and impurities and ensure that the material is not affected by oxidation or other gas reactions during the pressing process. The preform is heated and pressurized in a vacuum environment. The high temperature and high pressure environment helps to eliminate the pores between the preforms and the gaps between the fibers and the matrix. After reaching the required temperature and pressure, it is maintained for a period of time to ensure sufficient interdiffusion between the elements, so that the materials are tightly bonded.

[0034] Magnetron sputtering is a technology that uses magnetic fields and electric fields to sputter atoms or molecules on a target material onto a substrate to form a thin film under vacuum conditions. The specific process is as follows: Operate in a relatively stable vacuum state to reduce the impact of impurities and gases on the sputtering process. A glow discharge is generated by a high voltage between the cathode and the anode, ionizing gas molecules to generate electric charges. A magnetic field is introduced on the cathode surface of the target, and the magnetic field is used to confine charged particles, increase plasma density, and thus increase the sputtering rate. Charged particles (such as Ar ions) are accelerated to fly toward the target material under the action of the electric field, hit the target surface, and cause the target atoms or molecules to be sputtered out and deposited on the substrate to form a thin film.

[0035] Hot Isostatic Pressing (HIP) is a molding process that places the product in a closed container and sintering and densifying the product under high temperature and high pressure. The specific steps are as follows: Place the product (such as powder, preform, etc.) into a package made of metal or ceramic materials. Place the package into the hot isostatic pressing equipment, and under the action of high temperature (usually up to about 2000℃) and isostatic pressure (up to 200MPa or higher), the material undergoes plastic flow and densification. Keep it in a high temperature and high pressure environment for a period of time to ensure that the material is fully sintered and densified. After a certain holding time, slowly cool and take out the product.

[0036] like Figure 1 As shown, the present invention provides a symmetrical structure cemented carbide top hammer material and a preparation method thereof, comprising the following steps:

[0037] Three cemented carbide components were selected and pre-burned by vacuum hot pressing to obtain cemented carbide sheets;

[0038] A cube of cemented carbide is used as the core material, and cemented carbide sheets are wrapped around the core material by hot isostatic pressing to form a multi-layer symmetrical structure of cemented carbide;

[0039] A conductive wear-resistant coating was prepared on the surface of multi-layer symmetrically structured cemented carbide by magnetron sputtering to obtain a symmetrically structured cemented carbide anvil material.

[0040] The principle of the present invention is to improve the comprehensive performance of cemented carbide top hammer by carefully selecting cemented carbide components, adopting hot pressing technology, designing multi-layer symmetrical structure and applying magnetron sputtering coating, so as to meet the stability and durability requirements of high-voltage equipment under extreme working conditions. The specific analysis is as follows:

[0041] The present invention selects three different cemented carbide components. These components may differ in cobalt content, tungsten carbide particle size or other alloying elements, thereby giving each component specific physical and mechanical properties. Pre-sintering by vacuum hot pressing method can ensure that the alloy components are tightly combined under controlled oxygen content and pressure, reduce pores and impurities, and improve the density and mechanical strength of the cemented carbide sheet.

[0042] A cube of cemented carbide is selected as the core material. This core material usually has high toughness and strength and can withstand the huge pressure during the operation of high-pressure equipment. Subsequently, the pre-fired cemented carbide sheet is wrapped around the core material using hot isostatic pressing technology to form a multi-layer symmetrical structure. Hot isostatic pressing technology can uniformly press the material under high temperature and high pressure, eliminate internal pores, and enhance the bonding force between layers, thereby improving the uniformity and mechanical properties of the overall material.

[0043] The multi-layer symmetrical structure is designed to achieve comprehensive optimization of the top hammer performance. By arranging carbide sheets with different performances around the core material in a certain order, a performance gradient can be formed, which enables the top hammer to disperse stress more effectively when under pressure, reduce stress concentration, and thus improve compressive strength and durability. At the same time, the symmetrical structure ensures that the top hammer has consistent performance in all directions, which is crucial to maintaining uniform pressure distribution in high-pressure equipment.

[0044] A conductive and wear-resistant coating is deposited on the surface of the multi-layer symmetrical cemented carbide using magnetron sputtering technology. Magnetron sputtering technology can form a uniform and dense coating on the surface of the material, significantly improving the conductivity and wear resistance of the top hammer. The improvement in conductivity helps to maintain the stability of the current, ensuring that the high-voltage equipment can continuously and stably transmit current during operation. The enhancement of wear resistance can extend the service life of the top hammer and reduce the performance degradation caused by wear.

[0045] The specific steps include the following:

[0046] 1) The core material is cubic YG10 cemented carbide with an average grain size of 5 to 8 microns, with a relative density of 99.3 to 99.5%, a hardness of 16.3 to 16.7 GPa, and a fracture toughness of 11.6 to 12.2 MPa·m 1 / 2, weigh three components according to the mass percentage of tungsten carbide to cobalt of 91-93:7-9, 93-95:5-7 and 96-98:2-4 and mix them evenly, then use a vacuum hot pressing method to pre-sinter the three components into green bodies at 740-780°C for 18-24 minutes, then arrange the pre-sintered green bodies of the three components symmetrically according to the cobalt content from small to large and then from large to small, and use a hot isostatic pressing method to sinter them layer by layer to the six surfaces of the core material at 1310-1380°C for 32-41 minutes.

[0047] 2) A conductive wear-resistant coating was prepared on the surface of a multi-layer symmetrically structured cemented carbide by magnetron sputtering. The magnetron sputtering target was pure tungsten carbide. The sputtering time was 78 to 89 minutes, the heating temperature was 430 to 510°C, and the thickness of the deposited tungsten carbide layer was 3.2 to 3.8 microns. Finally, a symmetrically structured cemented carbide top hammer material was obtained.

[0048] Furthermore, in the process of preparing cemented carbide top hammer materials, the present invention aims at the engineering problems that the existing cemented carbide top hammers have low toughness and high temperature hardness, and are prone to fatigue under long-term service conditions. The present invention uses cemented carbide blanks as core materials, vacuum hot pressing and hot isostatic pressing methods to make multi-layer symmetrical structures, and then deposits a series of technologies for conductive wear-resistant coatings to study the relationship between cemented carbide core material performance, component ratio of gradient symmetrical structure, sintering process parameters, magnetron sputtering process parameters and cemented carbide top hammer strength and toughness, and high temperature mechanical properties, that is: for cemented carbide top hammer materials, the best cemented carbide core material performance, component ratio of gradient symmetrical structure, sintering process parameters and magnetron sputtering process parameters that maintain high strength and toughness and high temperature mechanical properties are studied. This method has high component control accuracy, strong process stability and repeatability, and can achieve the strength and toughness and excellent high temperature mechanical properties of cemented carbide top hammer materials.

[0049] The present invention proposes a method for preparing a symmetrically structured cemented carbide anvil material, which combines material science, vacuum hot pressing technology, hot isostatic pressing technology and magnetron sputtering technology. The core principle is to optimize the mechanical properties and conductive wear resistance of the anvil by constructing a multi-layer symmetrically structured cemented carbide.

[0050] Optionally, coarse-grained cemented carbide is selected as the core material. This material has good toughness, can withstand large impacts and deformations, and provides basic mechanical support for the top hammer. Three cemented carbide sheets with different cobalt contents are pre-sintered by vacuum hot pressing, and these alloy sheets are arranged on the six surfaces of the core material in order from high to low cobalt content. This gradient structure design aims to achieve a balance between hardness, strength and toughness, while ensuring the symmetry of performance, thereby improving the uniformity and stability of high-pressure transmission. The cemented carbide sheets are tightly wrapped around the core material by hot isostatic pressing to form a multi-layer symmetrical structure. This technology can ensure close bonding between the layers, reduce internal defects, and improve the density and mechanical properties of the overall material. A conductive wear-resistant coating is prepared on the surface of the cemented carbide with a multi-layer symmetrical structure. This step is intended to improve the conductivity and wear resistance of the top hammer, ensure the stable transmission of current under high temperature and high pressure environments, and extend the service life of the top hammer.

[0051] Further optionally, the preparation method of the present invention significantly optimizes the performance of the cemented carbide top hammer through a carefully designed gradient structure and surface coating. This symmetrical structural design not only improves the hardness, strength and toughness of the top hammer, but also ensures the symmetry of the performance, making the top hammer more uniform and stable when transmitting high pressure. The present invention combines advanced technologies such as vacuum hot pressing, hot isostatic pressing and magnetron sputtering, and the integrated application of these technologies provides an innovative way to prepare high-performance cemented carbide top hammers. Compared with traditional methods, the present invention has achieved significant improvements in material structure and performance. Cemented carbide top hammers play a key role in high-voltage equipment. The symmetrically structured cemented carbide top hammer prepared by the present invention has excellent mechanical properties and conductive wear resistance, and can meet the use requirements in harsh environments such as high temperature and high pressure. The preparation method of the symmetrically structured cemented carbide top hammer material of the present invention can significantly improve the performance and service life of the top hammer, and provide a strong guarantee for the efficient and stable operation of high-voltage equipment.

[0052] The toughness and high temperature properties of the cemented carbide butt hammer materials prepared in the following examples are shown in Table 1.

[0053] Example 1

[0054] 1) The core material is a cubic YG10 cemented carbide with an average grain size of 8 microns, with a relative density of 99.5%, a hardness of 16.3 GPa, and a fracture toughness of 11.6 MPa·m 1 / 2 , three components are weighed and mixed evenly according to the mass percentage of tungsten carbide to cobalt of 91:9, 93:7 and 96:4, and then the three components are pre-sintered into green bodies at 740°C for 18 minutes by vacuum hot pressing. The pre-sintered green bodies of the three components are arranged symmetrically according to the cobalt content from small to large and then from large to small, and are fired layer by layer to the six surfaces of the core material by hot isostatic pressing at 1380°C for 32 minutes.

[0055] 2) A conductive wear-resistant coating was prepared on the surface of a multi-layer symmetrically structured cemented carbide by magnetron sputtering. The magnetron sputtering target was pure tungsten carbide. The sputtering time was 78 minutes, the heating temperature was 510°C, and the thickness of the deposited tungsten carbide layer was 3.2 μm. Finally, a symmetrically structured cemented carbide top hammer material was obtained.

[0056] Example 2

[0057] 1) The core material is a cubic YG10 cemented carbide with an average grain size of 6 microns, with a relative density of 99.4%, a hardness of 16.4 GPa, and a fracture toughness of 11.8 MPa·m 1 / 2 , three components are weighed and mixed evenly according to the mass percentage of tungsten carbide to cobalt of 92:8, 94:6 and 97:3, and then the three components are pre-sintered into green bodies at 750°C for 20 minutes by vacuum hot pressing. The pre-sintered green bodies of the three components are arranged symmetrically according to the cobalt content from small to large and then from large to small, and are fired layer by layer to the six surfaces of the core material by hot isostatic pressing at 1330°C for 35 minutes.

[0058] 2) A conductive wear-resistant coating was prepared on the surface of a multi-layer symmetrically structured cemented carbide by magnetron sputtering. The magnetron sputtering target was pure tungsten carbide. The sputtering time was 80 minutes, the heating temperature was 450°C, and the thickness of the deposited tungsten carbide layer was 3.4 μm. Finally, a symmetrically structured cemented carbide top hammer material was obtained.

[0059] Example 3

[0060] 1) The core material is a cubic YG10 cemented carbide with an average grain size of 7 microns, with a relative density of 99.5%, a hardness of 16.6 GPa, and a fracture toughness of 12.2 MPa·m 1 / 2 The three components were weighed and mixed evenly according to the mass percentage of tungsten carbide to cobalt of 93:7, 95:5 and 98:2, and then pre-sintered into green bodies at 770°C for 23 minutes by vacuum hot pressing. The pre-sintered green bodies of the three components were symmetrically arranged in an increasing order of cobalt content and then from large to small, and then fired layer by layer to the six surfaces of the core material by hot isostatic pressing at 1360°C for 39 minutes.

[0061] 2) A conductive wear-resistant coating was prepared on the surface of a multi-layer symmetrically structured cemented carbide by magnetron sputtering. The magnetron sputtering target was pure tungsten carbide. The sputtering time was 83 minutes, the heating temperature was 510°C, and the thickness of the deposited tungsten carbide layer was 3.6 μm. Finally, a symmetrically structured cemented carbide top hammer material was obtained.

[0062] Example 4

[0063] 1) The core material is a cubic YG10 cemented carbide with an average grain size of 8 microns, with a relative density of 99.5%, a hardness of 16.7 GPa, and a fracture toughness of 12.2 MPa·m1 / 2 , three components were weighed and mixed evenly according to the mass percentage of tungsten carbide to cobalt of 91:9, 95:5 and 96:4, and then the three components were pre-sintered into green bodies at 780°C for 18 minutes by vacuum hot pressing. The pre-sintered green bodies of the three components were arranged symmetrically according to the cobalt content from small to large and then from large to small, and were fired layer by layer to the six surfaces of the core material by hot isostatic pressing at 1310°C for 32 minutes.

[0064] 2) A conductive wear-resistant coating was prepared on the surface of a multi-layer symmetrically structured cemented carbide by magnetron sputtering. The magnetron sputtering target was pure tungsten carbide. The sputtering time was 89 minutes, the heating temperature was 510°C, and the thickness of the deposited tungsten carbide layer was 3.2 μm. Finally, a symmetrically structured cemented carbide top hammer material was obtained.

[0065] The performance parameters of the cemented carbide anvil materials prepared in Examples 1 to 4 are shown in Table 1:

[0066] Table 1

[0067]

[0068] It can be concluded from the above table that the cemented carbide anvil material prepared by the present invention has a symmetrical structure, and the fracture toughness of the material is greater than or equal to 13.5 MPa·m 1 / 2 , microhardness greater than or equal to 24.2GPa, compressive strength greater than or equal to 4750MPa, high temperature (1000℃) hardness greater than or equal to 20.3GPa.

[0069] Example 5

[0070] 1) The core material is a cubic YG10 cemented carbide with an average grain size of 6 microns, with a relative density of 99.3%, a hardness of 16.4 GPa, and a fracture toughness of 11.7 MPa·m 1 / 2 The three components were weighed and mixed evenly according to the mass percentage of tungsten carbide to cobalt of 92:8, 94:6 and 97:3, and then pre-sintered into green bodies at 750°C for 19 minutes by vacuum hot pressing. The pre-sintered green bodies of the three components were arranged symmetrically according to the cobalt content from small to large and then from large to small, and then fired layer by layer to the six surfaces of the core material by hot isostatic pressing at 1320°C for 33 minutes.

[0071] 2) A conductive wear-resistant coating was prepared on the surface of a multi-layer symmetrically structured cemented carbide by magnetron sputtering. The magnetron sputtering target was pure tungsten carbide. The sputtering time was 79 minutes, the heating temperature was 440°C, and the thickness of the deposited tungsten carbide layer was 3.3 μm. Finally, a symmetrically structured cemented carbide top hammer material was obtained.

[0072] Example 6

[0073] 1) The core material is a cubic YG10 cemented carbide with an average grain size of 7 microns, with a relative density of 99.4%, a hardness of 16.7 GPa, and a fracture toughness of 12.0 MPa·m 1 / 2 , three components are weighed and mixed evenly according to the mass percentage of tungsten carbide to cobalt of 93:7, 94:6 and 98:2, and then the three components are pre-sintered into green bodies at 760°C for 19 minutes by vacuum hot pressing. The pre-sintered green bodies of the three components are symmetrically arranged in an increasing order of cobalt content and then from large to small, and are fired layer by layer to the six surfaces of the core material by hot isostatic pressing at 1330°C for 34 minutes.

[0074] 2) A conductive wear-resistant coating was prepared on the surface of a multi-layer symmetrically structured cemented carbide by magnetron sputtering. The magnetron sputtering target was pure tungsten carbide. The sputtering time was 80 minutes, the heating temperature was 450°C, and the thickness of the deposited tungsten carbide layer was 3.4 μm. Finally, a symmetrically structured cemented carbide top hammer material was obtained.

[0075] Example 7

[0076] 1) The core material is cubic YG10 cemented carbide with an average grain size of 5 to 8 microns, with a relative density of 99.4%, a hardness of 16.5 GPa, and a fracture toughness of 11.8 MPa·m 1 / 2 , three components are weighed and mixed evenly according to the mass percentage of tungsten carbide to cobalt of 92:8, 93:7 and 96:4, and then the three components are pre-sintered into green bodies at 770°C for 20 minutes by vacuum hot pressing. The pre-sintered green bodies of the three components are arranged symmetrically according to the cobalt content from small to large and then from large to small, and are fired layer by layer to the six surfaces of the core material by hot isostatic pressing at 1360°C for 38 minutes.

[0077] 2) A conductive wear-resistant coating was prepared on the surface of a multi-layer symmetrically structured cemented carbide by magnetron sputtering. The magnetron sputtering target was pure tungsten carbide. The sputtering time was 84 minutes, the heating temperature was 470°C, and the thickness of the deposited tungsten carbide layer was 3.6 μm. Finally, a symmetrically structured cemented carbide top hammer material was obtained.

[0078] Example 8

[0079] 1) The core material is a cubic YG10 cemented carbide with an average grain size of 8 microns, with a relative density of 99.3%, a hardness of 16.3 GPa, and a fracture toughness of 11.6 MPa·m 1 / 2 , three components were weighed and mixed evenly according to the mass percentage of tungsten carbide to cobalt of 91:9, 93:7 and 97:3, and then the three components were pre-sintered into green bodies at 740°C for 22 minutes by vacuum hot pressing. The pre-sintered green bodies of the three components were arranged symmetrically according to the cobalt content from small to large and then from large to small, and were fired layer by layer to the six surfaces of the core material by hot isostatic pressing at 1370°C for 38 minutes.

[0080] 2) A conductive wear-resistant coating was prepared on the surface of a multi-layer symmetrically structured cemented carbide by magnetron sputtering. The magnetron sputtering target was pure tungsten carbide. The sputtering time was 86 minutes, the heating temperature was 500°C, and the thickness of the deposited tungsten carbide layer was 3.6 microns. Finally, a symmetrically structured cemented carbide top hammer material was obtained.

[0081] The hard alloy anvil materials obtained in Examples 4 to 8 have a symmetrical structure and a fracture toughness greater than or equal to 13.5 MPa·m 1 / 2 , microhardness greater than or equal to 24.2GPa, compressive strength greater than or equal to 4750MPa, high temperature (1000℃) hardness greater than or equal to 20.3GPa. Toughness, high temperature hardness and long-term service conditions all meet the performance requirements.

[0082] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a symmetrically structured cemented carbide anvil material, characterized in that: include: Three cemented carbide components were selected and pre-burned by vacuum hot pressing to obtain cemented carbide sheets; A cube of cemented carbide is used as the core material, and cemented carbide sheets are wrapped around the core material by hot isostatic pressing to form a multi-layer symmetrical structure of cemented carbide; A conductive wear-resistant coating was prepared on the surface of multi-layer symmetrically structured cemented carbide by magnetron sputtering to obtain a symmetrically structured cemented carbide anvil material.

2. The method for preparing a symmetrically structured cemented carbide anvil material according to claim 1, characterized in that: The cemented carbide is YG10 cemented carbide.

3. The method for preparing a symmetrically structured cemented carbide anvil material according to claim 2, characterized in that: The cemented carbide core material is a coarse-grained structure with an average grain size of 5 to 8 microns, a relative density of 99.3 to 99.5%, a hardness of 16.3 to 16.7 GPa, and a fracture toughness of 11.6 to 12.2 MPa·m 1 / 2 .

4. The method for preparing a symmetrically structured cemented carbide anvil material according to claim 1, characterized in that: The mass percentages of tungsten carbide and cobalt in the three cemented carbides are (91-93):(7-9), (93-95):(5-7) and (96-98):(2-4), respectively.

5. The method for preparing a symmetrically structured cemented carbide anvil material according to claim 1, characterized in that: The vacuum hot pressing method comprises pre-sintering the three components into green bodies at 740-780° C. for 18-24 minutes respectively; and symmetrically arranging the pre-sintered green bodies of the three components in a manner of increasing cobalt content and then decreasing cobalt content.

6. The method for preparing a symmetrically structured cemented carbide anvil material according to claim 1, characterized in that: The hot isostatic pressing method is to burn the cemented carbide sheets to the six surfaces of the core material layer by layer at 1310-1380° C. for 32-41 minutes.

7. The method for preparing a symmetrically structured cemented carbide anvil material according to claim 1, characterized in that: In the preparation of the conductive wear-resistant coating on the surface of the multi-layer symmetrical structure cemented carbide by the magnetron sputtering method, the magnetron sputtering target is pure tungsten carbide, the sputtering time is 78 to 89 minutes, and the heating temperature is 430 to 510°C.

8. The method for preparing a symmetrically structured cemented carbide anvil material according to claim 1, characterized in that: The conductive wear-resistant coating is a deposited tungsten carbide layer with a thickness of 3.2 to 3.8 microns.

9. A symmetrically structured cemented carbide top hammer material, characterized in that: The material is prepared by the method for preparing a symmetrically structured cemented carbide anvil material as claimed in any one of claims 1 to 8.

10. The preparation method according to claim 9, characterized in that: The prepared cemented carbide anvil material has a symmetrical structure, and the fracture toughness of the material is greater than or equal to 13.5MPa·m 1 / 2 , microhardness greater than or equal to 24.2GPa, compressive strength greater than or equal to 4750MPa, high temperature (1000℃) hardness greater than or equal to 20.3GPa.

Citation Information

Cited By

  • Manufacturing method of stainless steel wire with multi-layer composite structure

    CN119927005A

  • A method for manufacturing multi-layer composite structure stainless steel wire

    CN119927005B