Thermosensitive film based on modified cellulose and preparation method thereof
By using modified cellulose polyol and fluorosilicone elements in the thermal film, the hydrophobic properties are enhanced and a network cross-linked structure is formed, which solves the problem of poor waterproof performance and adhesion of the thermal film, and improves the color rendering effect and equipment stability.
Patent Information
- Application Number
- CN202410858619.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-28
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-06-28
AI Technical Summary
The existing thermal film has poor waterproof performance, is prone to moisture, and has high friction and adhesion, which affects the color development effect and may damage the equipment.
Modified cellulose polyol is used as the protective layer material, fluorosilicone element is introduced through esterification reaction to enhance hydrophobic properties, and a network cross-linked structure is formed through dehydration and condensation reaction to protect the thermal imaging layer and reduce the risk of adhesion.
It significantly improves the waterproof and moisture-proof performance of thermal film, reduces the impact of water vapor on dyes and friction and adhesion, and improves the stability of the printing process.
Smart Images

Figure BDA0004918708180000081 
Figure BDA0004918708180000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of thermal printing materials, in particular to a thermal film based on modified cellulose and a preparation method thereof. Background Art
[0002] Thermal film is a type of film commonly used in medical imaging. It works by using heat-sensitive dyes to develop in the film after being stimulated by heat, thereby preserving medical images.
[0003] However, existing thermal films have poor waterproof performance, are easily affected by moisture, have high friction and are easy to stick together, which often affects the color development effect during use and even damages the thermal imaging equipment. Summary of the invention
[0004] The object of the present invention is to provide a thermal film based on modified cellulose and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solution: a thermal film based on modified cellulose, having the following technical features: the thermal film comprises a protective layer, a thermal imaging layer, a polyester substrate layer and a backing layer from top to bottom;
[0006] Wherein, the protective layer is formed by uniformly mixing 21-28 parts of modified cellulose polyol, 9-14 parts of isophorone diisocyanate, and 1-3.5 parts of nano-silicon dioxide, and then coating the mixture on the thermal imaging layer and drying and curing it;
[0007] The thermal imaging layer is prepared by uniformly mixing 20-25 parts of cellulose, 30-40 parts of bisphenol A, 10-20 parts of fluorane dye and 50-60 parts of deionized water, coating the mixture on the polyester substrate layer and drying the mixture.
[0008] The back layer is prepared by uniformly mixing 7-10 parts of polyethyleneimine and 7-15 parts of deionized water, coating the mixture on the lower surface of the polyester substrate layer, and then drying the mixture.
[0009] Furthermore, the preparation method of the modified cellulose polyol is:
[0010] a. Disperse tetrafluorophthalic acid in deionized water, disperse with ultrasonic vibration for 35-60 minutes, add 4,4-dimethylaminopyridine, continue stirring and mixing for 15-30 minutes, and then add it dropwise to 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane under nitrogen atmosphere. Stir continuously during the addition process. After the addition is completed, heat the mixed solution to 150-160°C, reflux and stir for 2-18 hours, remove excess solvent by rotary evaporation, wash 2-3 times with deionized water at a temperature of 0-4°C, and vacuum dry to constant weight to obtain a terminal hydroxyl fluoride intermediate;
[0011] b. Mix the terminal hydroxyl fluorine intermediate with the polyether polyol, heat to 105-110°C, heat for 20-60 minutes, cool to room temperature, add concentrated sulfuric acid and pentaerythritol, ultrasonically mix for 15-30 minutes, protect under nitrogen atmosphere, heat to 158-162°C, stir to react for 40-80 minutes, add carboxymethyl cellulose, continue stirring to react and mix for 2-4 hours, stop heating, and obtain modified cellulose polyol.
[0012] Furthermore, in step a, the mass ratio of tetrafluorophthalic acid, 4,4-dimethylaminopyridine and 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane is 1:(0.05-0.08):(1.9-2.4).
[0013] Furthermore, in step b, the mass ratio of the terminal hydroxyl fluorine intermediate, the polyether polyol and the concentrated sulfuric acid is 1:
[0014] (2-4):(0.08-0.15).
[0015] Furthermore, in step b, the mass ratio of the terminal hydroxyl fluorine intermediate, pentaerythritol, and carboxymethyl cellulose is 1:(0.4-0.8):(0.5-1.2).
[0016] Furthermore, in step b, the carboxymethyl cellulose has a molecular weight of 80,000-100,000, a degree of substitution of 0.65-0.75, and a viscosity of 50-100 mPa.s.
[0017] Furthermore, in step b, the polyether polyol is any one or more of polytetrahydrofuran diol and polyethylene adipate diol.
[0018] Furthermore, a method for preparing a thermal film based on modified cellulose comprises the following steps:
[0019] S1. The polyethyleneimine is mixed with deionized water, stirred evenly and defoamed, and then coated on the lower surface of the polyester substrate layer, and after drying and shaping, a back layer of the thermal film is formed;
[0020] S2. After cellulose, fluorane dye and deionized water are mixed evenly, bisphenol A is added, and mixing is continued for 5-8 minutes, and the mixture is coated on the upper surface of the polyester substrate layer to obtain a thermal imaging layer of the thermal film;
[0021] S3. The modified cellulose polyol is mixed with nano-silicon dioxide, and after ultrasonic dispersion for 30-60 minutes, isophorone diisocyanate is added, and the mixing is continued for 3-5 minutes, and the mixture is coated on the upper surface of the thermal imaging layer. After drying and setting, a protective layer of the thermal film is formed, and the thermal film based on modified cellulose is obtained by winding.
[0022] Compared with the prior art, the beneficial effects achieved by the present invention are:
[0023] In order to improve the waterproof and moisture-proof performance of the thermal film, the present invention improves the thermal film protective layer;
[0024] The present invention first uses tetrafluorophthalic acid containing a large amount of fluorine elements as a raw material, and then, under the catalysis of 4,4-dimethylaminopyridine, an esterification reaction occurs between the hydroxyl groups contained in the tetrafluorophthalic acid and the hydroxyl groups in 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane, thereby generating a terminal hydroxyl fluorine intermediate containing fluorine and silicon elements;
[0025] Fluorine and silicon both have high electronegativity. Adding them to the raw materials of the protective layer can effectively improve the hydrophobicity of the protective layer to water vapor, thereby avoiding the influence of water vapor on the dye in the thermal imaging layer of the thermal film. The introduction of fluorine and silicon elements can further reduce the surface energy of the protective layer, thereby reducing the friction between the protective layer and other objects, reducing the adhesion between thermal films, and reducing printing problems during the thermal film printing process.
[0026] And on this basis, the present application mixes the terminal hydroxyl fluorine intermediate with the polyether polyol, and then mixes it with concentrated sulfuric acid and carboxymethyl cellulose. Under the catalysis of concentrated sulfuric acid, the hydroxyl groups on the carbon chain of carboxymethyl cellulose will undergo dehydration condensation with the hydroxyl groups in the terminal hydroxyl fluorine intermediate and the polyether polyol, thereby grafting the polyether polyol and the terminal hydroxyl fluorine intermediate into the cellulose carbon chain; at the same time, the present invention also strictly limits the addition amount of the terminal hydroxyl fluorine intermediate, the polyether polyol and the carboxymethyl cellulose, so as to ensure that after dehydration condensation, the terminal hydroxyl fluorine intermediate, the polyether polyol and the carboxymethyl cellulose still retain enough hydroxyl groups to cross-link with isocyanate, thereby forming a network cross-linking structure, thereby protecting the thermal imaging layer in the thermal film. DETAILED DESCRIPTION
[0027] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] The coating method used for the back layer, thermal imaging layer and protective layer in this application is curtain coating, and the coating amount is 20g / m 2 , 100g / m 2 , 25g / m 2 ;
[0029] The cellulose used in this application is hydroxypropyl methylcellulose with a viscosity of 4000-6500 mPa.s; the nano-silica used is AEROSIL R972 hydrophobic white carbon black; the polyether polyol used is polytetramethylene glycol, M w The molecular weight of the carboxymethyl cellulose used is 90000, the degree of substitution is 0.7, and the viscosity is 50-100mPa.s
[0030] Embodiment 1. A method for preparing a thermal film based on modified cellulose, comprising the following steps:
[0031] S1. By weight, 8 parts of polyethyleneimine and 12 parts of deionized water were mixed, stirred and defoamed, and then coated on the lower surface of the polyester substrate layer, and dried and formed to form a back layer of the thermal film;
[0032] S2. After 25 parts of cellulose, 15 parts of fluoran dye and 55 parts of deionized water were mixed uniformly by weight, 30 parts of bisphenol A were added, and mixing was continued for 5 minutes, and the mixture was coated on the upper surface of the polyester substrate layer to obtain a thermal imaging layer of the thermal film;
[0033] S3. By weight, 21 parts of modified cellulose polyol and 2.5 parts of nano-silicon dioxide were mixed, ultrasonically dispersed for 30 min, 12 parts of isophorone diisocyanate were added, and mixing was continued for 3 min, which was coated on the upper surface of the thermal imaging layer, and after drying and shaping, a protective layer of the thermal film was formed, and the thermal film was rolled up to obtain a thermal film based on modified cellulose;
[0034] Wherein, the preparation method of the modified cellulose polyol is:
[0035] a. Disperse 1 part of tetrafluorophthalic acid in deionized water by weight, disperse it by ultrasonic vibration for 45 minutes, add 0.08 parts of 4,4-dimethylaminopyridine, continue to stir and mix for 15 minutes, and then add it dropwise to 1.9 parts of 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane under nitrogen atmosphere. Stir continuously during the addition process. After the addition is completed, the mixed solution is heated to 155°C, refluxed and stirred for 12 hours, and then the excess solvent is removed by rotary evaporation. After washing twice with deionized water at 4°C, it is vacuum dried to constant weight to obtain a terminal hydroxyl fluoride intermediate;
[0036] b. By weight, 1 part of the terminal hydroxyl fluorine intermediate was mixed with 2 parts of the polyether polyol, the temperature was raised to 105°C, heated for 30 minutes, and then cooled to room temperature. 0.15 parts of concentrated sulfuric acid and 0.4 parts of pentaerythritol were added thereto. After ultrasonic mixing for 15 minutes, nitrogen atmosphere was protected, the temperature was raised to 160°C, stirred for reaction for 40 minutes, 0.5 parts of carboxymethyl cellulose was added, the stirring reaction was continued for 2 hours, and the heating was stopped to obtain a modified cellulose polyol.
[0037] Embodiment 2. A method for preparing a thermal film based on modified cellulose, comprising the following steps:
[0038] Compared with Example 1, this example increases the amount of modified cellulose polyol added in step S3;
[0039] S3. By weight, 28 parts of modified cellulose polyol and 2.5 parts of nano-silicon dioxide were mixed, ultrasonically dispersed for 30 min, 12 parts of isophorone diisocyanate were added, and mixing was continued for 3 min, which was coated on the upper surface of the thermal imaging layer, and after drying and shaping, a protective layer of the thermal film was formed, and the thermal film was rolled up to obtain a thermal film based on modified cellulose;
[0040] Wherein, the preparation method of the modified cellulose polyol is:
[0041] a. Disperse 1 part of tetrafluorophthalic acid in deionized water by weight, disperse it by ultrasonic vibration for 45 minutes, add 0.08 parts of 4,4-dimethylaminopyridine, continue to stir and mix for 15 minutes, and then add it dropwise to 1.9 parts of 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane under nitrogen atmosphere. Stir continuously during the addition process. After the addition is completed, the mixed solution is heated to 155°C, refluxed and stirred for 12 hours, and then the excess solvent is removed by rotary evaporation. After washing twice with deionized water at 4°C, it is vacuum dried to constant weight to obtain a terminal hydroxyl fluoride intermediate;
[0042] b. By weight, 1 part of the terminal hydroxyl fluorine intermediate was mixed with 2 parts of the polyether polyol, the temperature was raised to 105°C, heated for 30 minutes, and then cooled to room temperature. 0.15 parts of concentrated sulfuric acid and 0.4 parts of pentaerythritol were added thereto. After ultrasonic mixing for 15 minutes, nitrogen atmosphere was protected, the temperature was raised to 160°C, stirred for reaction for 40 minutes, 0.5 parts of carboxymethyl cellulose was added, the stirring reaction was continued for 2 hours, and the heating was stopped to obtain a modified cellulose polyol.
[0043] Embodiment 3. A method for preparing a thermal film based on modified cellulose, comprising the following steps:
[0044] Compared with Example 1, this example increases the amount of 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane added in step a;
[0045] S3. By weight, 28 parts of modified cellulose polyol and 2.5 parts of nano-silicon dioxide were mixed, ultrasonically dispersed for 30 min, 12 parts of isophorone diisocyanate were added, and mixing was continued for 3 min, which was coated on the upper surface of the thermal imaging layer, and after drying and shaping, a protective layer of the thermal film was formed, and the thermal film was rolled up to obtain a thermal film based on modified cellulose;
[0046] Wherein, the preparation method of the modified cellulose polyol is:
[0047] a. Disperse 1 part of tetrafluorophthalic acid in deionized water by weight, disperse it by ultrasonic vibration for 45 minutes, add 0.08 parts of 4,4-dimethylaminopyridine, continue to stir and mix for 15 minutes, and then add it dropwise to 2.4 parts of 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane under nitrogen atmosphere. Stir continuously during the addition process. After the addition is completed, the mixed solution is heated to 155°C, refluxed and stirred for 12 hours, and then the excess solvent is removed by rotary evaporation. After washing twice with deionized water at 4°C, it is vacuum dried to constant weight to obtain a terminal hydroxyl fluoride intermediate;
[0048] b. By weight, 1 part of the terminal hydroxyl fluorine intermediate was mixed with 2 parts of the polyether polyol, the temperature was raised to 105°C, heated for 30 minutes, and then cooled to room temperature. 0.15 parts of concentrated sulfuric acid and 0.4 parts of pentaerythritol were added thereto. After ultrasonic mixing for 15 minutes, nitrogen atmosphere was protected, the temperature was raised to 160°C, stirred for reaction for 40 minutes, 0.5 parts of carboxymethyl cellulose was added, the stirring reaction was continued for 2 hours, and the heating was stopped to obtain a modified cellulose polyol.
[0049] Embodiment 4. A method for preparing a thermal film based on modified cellulose, comprising the following steps:
[0050] Compared with Example 1, this example increases the amount of polyether polyol added in step b;
[0051] S3. By weight, 28 parts of modified cellulose polyol and 2.5 parts of nano-silicon dioxide were mixed, ultrasonically dispersed for 30 min, 12 parts of isophorone diisocyanate were added, and mixing was continued for 3 min, which was coated on the upper surface of the thermal imaging layer, and after drying and shaping, a protective layer of the thermal film was formed, and the thermal film was rolled up to obtain a thermal film based on modified cellulose;
[0052] Wherein, the preparation method of the modified cellulose polyol is:
[0053] a. Disperse 1 part of tetrafluorophthalic acid in deionized water by weight, disperse it by ultrasonic vibration for 45 minutes, add 0.08 parts of 4,4-dimethylaminopyridine, continue to stir and mix for 15 minutes, and then add it dropwise to 2.4 parts of 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane under nitrogen atmosphere. Stir continuously during the addition process. After the addition is completed, the mixed solution is heated to 155°C, refluxed and stirred for 12 hours, and then the excess solvent is removed by rotary evaporation. After washing twice with deionized water at 4°C, it is vacuum dried to constant weight to obtain a terminal hydroxyl fluoride intermediate;
[0054] b. By weight, 1 part of the terminal hydroxyl fluorine intermediate was mixed with 3 parts of polyether polyol, the temperature was raised to 105°C, heated for 30 minutes, and then cooled to room temperature. 0.15 parts of concentrated sulfuric acid and 0.4 parts of pentaerythritol were added thereto. After ultrasonic mixing for 15 minutes, nitrogen atmosphere was protected, the temperature was raised to 160°C, stirred for reaction for 40 minutes, 0.5 parts of carboxymethyl cellulose was added, the stirring reaction was continued for 2 hours, and the heating was stopped to obtain a modified cellulose polyol.
[0055] Embodiment 5. A method for preparing a thermal film based on modified cellulose, comprising the following steps:
[0056] Compared with Example 4, this example increases the amount of polyether polyol added in step b;
[0057] S3. By weight, 28 parts of modified cellulose polyol and 2.5 parts of nano-silicon dioxide were mixed, ultrasonically dispersed for 30 min, 12 parts of isophorone diisocyanate were added, and mixing was continued for 3 min, which was coated on the upper surface of the thermal imaging layer, and after drying and shaping, a protective layer of the thermal film was formed, and the thermal film was rolled up to obtain a thermal film based on modified cellulose;
[0058] Wherein, the preparation method of the modified cellulose polyol is:
[0059] a. Disperse 1 part of tetrafluorophthalic acid in deionized water by weight, disperse it by ultrasonic vibration for 45 minutes, add 0.08 parts of 4,4-dimethylaminopyridine, continue to stir and mix for 15 minutes, and then add it dropwise to 2.4 parts of 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane under nitrogen atmosphere. Stir continuously during the addition process. After the addition is completed, the mixed solution is heated to 155°C, refluxed and stirred for 12 hours, and then the excess solvent is removed by rotary evaporation. After washing twice with deionized water at 4°C, it is vacuum dried to constant weight to obtain a terminal hydroxyl fluoride intermediate;
[0060] b. By weight, 1 part of the terminal hydroxyl fluorine intermediate was mixed with 4 parts of polyether polyol, the temperature was raised to 105°C, heated for 30 minutes, cooled to room temperature, 0.15 parts of concentrated sulfuric acid and 0.4 parts of pentaerythritol were added thereto, ultrasonically mixed for 15 minutes, nitrogen atmosphere was protected, the temperature was raised to 160°C, stirred for reaction for 40 minutes, 0.5 parts of carboxymethyl cellulose were added, the stirring reaction was continued for 2 hours, and the heating was stopped to obtain a modified cellulose polyol.
[0061] Embodiment 6. A method for preparing a thermal film based on modified cellulose, comprising the following steps:
[0062] Compared with Example 1, the amount of carboxymethyl cellulose added in step b is increased in this example;
[0063] S3. By weight, 28 parts of modified cellulose polyol and 2.5 parts of nano-silicon dioxide were mixed, ultrasonically dispersed for 30 min, 12 parts of isophorone diisocyanate were added, and mixing was continued for 3 min, which was coated on the upper surface of the thermal imaging layer, and after drying and shaping, a protective layer of the thermal film was formed, and the thermal film was rolled up to obtain a thermal film based on modified cellulose;
[0064] Wherein, the preparation method of the modified cellulose polyol is:
[0065] a. Disperse 1 part of tetrafluorophthalic acid in deionized water by weight, disperse it by ultrasonic vibration for 45 minutes, add 0.08 parts of 4,4-dimethylaminopyridine, continue to stir and mix for 15 minutes, and then add it dropwise to 2.4 parts of 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane under nitrogen atmosphere. Stir continuously during the addition process. After the addition is completed, the mixed solution is heated to 155°C, refluxed and stirred for 12 hours, and then the excess solvent is removed by rotary evaporation. After washing twice with deionized water at 4°C, it is vacuum dried to constant weight to obtain a terminal hydroxyl fluoride intermediate;
[0066] b. By weight, 1 part of the terminal hydroxyl fluorine intermediate was mixed with 2 parts of the polyether polyol, the temperature was raised to 105°C, heated for 30 minutes, and then cooled to room temperature. 0.15 parts of concentrated sulfuric acid and 0.4 parts of pentaerythritol were added thereto. After ultrasonic mixing for 15 minutes, nitrogen atmosphere was protected, the temperature was raised to 160°C, stirred for reaction for 40 minutes, 1.2 parts of carboxymethyl cellulose were added, the stirring reaction was continued for 2 hours, and the heating was stopped to obtain a modified cellulose polyol.
[0067] Comparative Example 1. A method for preparing a thermal film based on modified cellulose, comprising the following steps:
[0068] Compared with Example 1, this comparative example did not use modified cellulose polyol, but directly used an equal amount of polyether polyol;
[0069] S1. By weight, 8 parts of polyethyleneimine and 12 parts of deionized water were mixed, stirred and defoamed, and then coated on the lower surface of the polyester substrate layer, and dried and formed to form a back layer of the thermal film;
[0070] S2. After 25 parts of cellulose, 15 parts of fluoran dye and 55 parts of deionized water were mixed uniformly by weight, 30 parts of bisphenol A were added, and mixing was continued for 5 minutes, and the mixture was coated on the upper surface of the polyester substrate layer to obtain a thermal imaging layer of the thermal film;
[0071] S3. By weight, 21 parts of polyether polyol and 2.5 parts of nano-silicon dioxide were mixed, ultrasonically dispersed for 30 min, 12 parts of isophorone diisocyanate were added, and mixing was continued for 3 min, which was coated on the upper surface of the thermal imaging layer, and after drying and shaping, a protective layer of the thermal film was formed, and the thermal film was wound to obtain a modified cellulose-based thermal film;
[0072] Comparative Example 2. A method for preparing a thermal film based on modified cellulose, comprising the following steps:
[0073] Compared with Example 1, this comparative example increases the amount of carboxymethyl cellulose added in step b;
[0074] S3. By weight, 21 parts of modified cellulose polyol and 2.5 parts of nano-silicon dioxide were mixed, ultrasonically dispersed for 30 min, 12 parts of isophorone diisocyanate were added, and mixing was continued for 3 min, which was coated on the upper surface of the thermal imaging layer, and after drying and shaping, a protective layer of the thermal film was formed, and the thermal film was rolled up to obtain a thermal film based on modified cellulose;
[0075] Wherein, the preparation method of the modified cellulose polyol is:
[0076] a. Disperse 1 part of tetrafluorophthalic acid in deionized water by weight, disperse it by ultrasonic vibration for 45 minutes, add 0.08 parts of 4,4-dimethylaminopyridine, continue to stir and mix for 15 minutes, and then add it dropwise to 1.9 parts of 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane under nitrogen atmosphere. Stir continuously during the addition process. After the addition is completed, the mixed solution is heated to 155°C, refluxed and stirred for 12 hours, and then the excess solvent is removed by rotary evaporation. After washing twice with deionized water at 4°C, it is vacuum dried to constant weight to obtain a terminal hydroxyl fluoride intermediate;
[0077] b. By weight, 1 part of the terminal hydroxyl fluorine intermediate was mixed with 2 parts of the polyether polyol, the temperature was raised to 105°C, heated for 30 minutes, and then cooled to room temperature. 0.15 parts of concentrated sulfuric acid and 0.4 parts of pentaerythritol were added thereto. After ultrasonic mixing for 15 minutes, nitrogen atmosphere was protected, the temperature was raised to 160°C, stirred for reaction for 40 minutes, and 2.5 parts of carboxymethyl cellulose were added. After stirring and mixing for 2 hours, the heating was stopped to obtain a modified cellulose polyol.
[0078] Testing: The thermal films prepared in Examples 1-6 and Comparative Examples 1-2 were placed in an environment with a humidity of 100% and an ambient temperature of 100°C for 30 days, and taken out after 30 days. After removing the water stains on the surface, color printing was performed on the films, and the color development performance was observed;
[0079] The thermal films prepared in Examples 1-6 and Comparative Examples 1-2 were placed in deionized water at an ambient temperature of 40° C. After immersion for 4 hours, the thermal films were taken out and the protective layers thereof were rubbed with a rubber to observe whether there was any material dropped;
[0080] The thermal films prepared in Examples 1-6 and Comparative Examples 1-2 were used for film printing, and after printing, the surfaces of the protective layers were tested for scratches;
[0081] The test results are shown in the table below;
[0082]
[0083]
[0084] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A thermal film based on modified cellulose, characterized in that: The thermal film comprises a protective layer, a thermal imaging layer, a polyester substrate layer and a back layer from top to bottom; Wherein, the protective layer is formed by uniformly mixing 21-28 parts of modified cellulose polyol, 9-14 parts of isophorone diisocyanate, and 1-3.5 parts of nano-silicon dioxide, and then coating the mixture on the thermal imaging layer and drying and curing it; The thermal imaging layer is prepared by uniformly mixing 20-25 parts of cellulose, 30-40 parts of bisphenol A, 10-20 parts of fluorane dye and 50-60 parts of deionized water, coating the mixture on the polyester substrate layer and drying the mixture. The back layer is prepared by uniformly mixing 7-10 parts of polyethyleneimine and 7-15 parts of deionized water, coating the mixture on the lower surface of the polyester substrate layer, and then drying the mixture.
2. A thermal film based on modified cellulose according to claim 1, characterized in that: The preparation method of the modified cellulose polyol is: a. Disperse tetrafluorophthalic acid in deionized water, disperse with ultrasonic vibration for 35-60 minutes, add 4,4-dimethylaminopyridine, continue stirring and mixing for 15-30 minutes, and then add it dropwise to 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane under nitrogen atmosphere. Stir continuously during the addition process. After the addition is completed, heat the mixed solution to 150-160°C, reflux and stir for 2-18 hours, remove excess solvent by rotary evaporation, wash 2-3 times with deionized water at a temperature of 0-4°C, and vacuum dry to constant weight to obtain a terminal hydroxyl fluoride intermediate; b. Mix the terminal hydroxyl fluorine intermediate with the polyether polyol, heat to 105-110°C, heat for 20-60 minutes, cool to room temperature, add concentrated sulfuric acid and pentaerythritol, ultrasonically mix for 15-30 minutes, protect under nitrogen atmosphere, heat to 158-162°C, stir to react for 40-80 minutes, add carboxymethyl cellulose, continue stirring to react and mix for 2-4 hours, stop heating, and obtain modified cellulose polyol.
3. A thermal film based on modified cellulose according to claim 2, characterized in that: In step a, the mass ratio of tetrafluorophthalic acid, 4,4-dimethylaminopyridine and 1,3-bis(4-hydroxybutyl)-1,1,3,3-tetramethyldisiloxane is 1:(0.05-0.08):(1.9-2.4).
4. A thermal film based on modified cellulose according to claim 2, characterized in that: In step b, the mass ratio of the terminal hydroxyl fluorine intermediate, the polyether polyol and the concentrated sulfuric acid is 1:(2-4):(0.08-0.15).
5. The modified cellulose-based thermal film according to claim 2, characterized in that: In step b, the mass ratio of the terminal hydroxyl fluorine intermediate, pentaerythritol and carboxymethyl cellulose is 1:(0.4-0.8):(0.5-1.2).
6. A thermal film based on modified cellulose according to claim 2, characterized in that: In step b, the carboxymethyl cellulose has a molecular weight of 80,000-100,000, a degree of substitution of 0.65-0.75, and a viscosity of 50-100 mPa.s.
7. The modified cellulose-based thermal film according to claim 2, characterized in that: In step b, the polyether polyol is any one or more of polytetrahydrofuran diol and polyethylene adipate diol.
8. A method for preparing a thermal film based on modified cellulose according to any one of claims 1 to 7, characterized in that: The following steps are involved: S1. The polyethyleneimine is mixed with deionized water, stirred evenly and defoamed, and then coated on the lower surface of the polyester substrate layer, and after drying and shaping, a back layer of the thermal film is formed; S2. After cellulose, fluorane dye and deionized water are mixed evenly, bisphenol A is added, and mixing is continued for 5-8 minutes, and the mixture is coated on the upper surface of the polyester substrate layer to obtain a thermal imaging layer of the thermal film; S3. The modified cellulose polyol is mixed with nano-silicon dioxide, and after ultrasonic dispersion for 30-60 minutes, isophorone diisocyanate is added, and the mixing is continued for 3-5 minutes, and the mixture is coated on the upper surface of the thermal imaging layer. After drying and setting, a protective layer of the thermal film is formed, and the thermal film based on modified cellulose is obtained by winding.
Citation Information
Patent Citations
Special waterproof coating for shell of communication equipment and preparation method thereof
CN108841319A
Degradable thermosensitive film coating based on gamma-cyclodextrin modified cellulose and preparation method thereof
CN115612396A
Degradable thermosensitive film and preparation method thereof
CN116515155A
High-transparency thermosensitive film based on microcapsule technology and processing technology thereof
CN116533667A
Polytetrafluoroethylene sealing gasket for electrolytic bath and preparation process of polytetrafluoroethylene sealing gasket
CN117343465A