Fluorine-containing hydroxyapatite nanorod as well as preparation method and application thereof

A simple method is used to prepare size-controllable fluorinated hydroxyapatite nanorods and combine them with a resin matrix, which solves the problem of insufficient performance of fluorinated hydroxyapatite nanorods and lack of medical adhesives in the existing technology. problem, achieving highly efficient remineralization and bonding effects in dentistry.

CN118851136APending Publication Date: 2024-10-29SHANGHAI NINTH PEOPLES HOSPITAL SHANGHAI JIAO TONG UNIV SCHOOL OF MEDICINE
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202410846337.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The existing technology lacks a simple method for preparing fluorohydroxyapatite nanorods with controllable size and excellent performance, as well as a process for using them as raw materials to prepare medical adhesives.

Method used

By mixing stearylamine, oleic acid and ethanol at room temperature, adding calcium nitrate tetrahydrate, sodium fluoride and sodium phosphate dodecahydrate, performing hydrothermal reaction precipitation, filtering and freeze-drying, fluorine-containing hydroxyapatite nanometers are obtained Rod, and combined with the resin matrix to prepare medical adhesive.

Benefits of technology

The size control and performance optimization of fluorohydroxyapatite nanorods are achieved, providing a highly efficient medical adhesive for dental remineralization and orthodontic bracket bonding, which can stably release calcium in a simulated oral fluid environment. ions and fluoride ions to promote the remineralization of tooth enamel.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851136A_ABST
    Figure CN118851136A_ABST
Patent Text Reader

Abstract

The invention provides a fluorine-containing hydroxyapatite nanorod and a preparation method and application thereof.The preparation method of the fluorine-containing hydroxyapatite nanorod comprises the following steps that S1, octadecylamine, oleic acid and ethyl alcohol are mixed and stirred at the room temperature till complete hydrolysis is achieved; s2, sequentially adding calcium nitrate tetrahydrate, sodium fluoride and sodium phosphate dodecahydrate, and fully stirring; s3, carrying out hydrothermal reaction on the solution obtained in the step S2, and precipitating the fluorine-containing hydroxyapatite at the bottom; s4, filtering, washing and freeze-drying the bottom precipitate obtained in the step S3, and sieving with a 400-500-mesh sieve to obtain a fluorine-containing hydroxyapatite nanorod; wherein the mass ratio of the calcium nitrate tetrahydrate to the sodium fluoride to the sodium phosphate dodecahydrate is 1: (0.01-0.0.06): 1; the invention provides a novel method for preparing the hydroxyapatite nanorod, the hydroxyapatite nanorod is used as a raw material to prepare the medical adhesive, and the medical adhesive is applied to adhesion of the demineralized tooth surface and an orthodontic bracket and the like and has a wide application prospect.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a fluorine-containing hydroxyapatite nanorod and a preparation method and application thereof, belonging to the technical field of new medical materials. Background Art

[0002] Hydroxyapatite (Ca 10 (PO4)6(OH)2, HA) is the main inorganic component of bones and teeth, has good biological activity, and is mostly used for the repair and replacement of human hard tissues (bone, teeth). Compared with pure hydroxyapatite, fluorine-substituted hydroxyapatite has superior physical and mineralization properties. However, the performance of fluorine-substituted hydroxyapatite nanorods is affected by their micromorphology and size. At present, the synthesis of hydroxyapatite nanorods of different sizes has been achieved through hydrothermal synthesis and chemical precipitation methods, such as by adjusting the temperature and adding organic modifiers, but these methods require complex equipment conditions and high costs, and the product size controllable range is small and the particles are highly agglomerated.

[0003] Fixed orthodontics, as the main orthodontic treatment method, is based on the effective bonding of brackets to the tooth surface. Whether the brackets can be firmly bonded to the tooth surface determines whether the orthodontic force can act on the teeth and jaws. The traditional method of treating the enamel surface before bonding orthodontic brackets and accessories is phosphoric acid etching, which produces a rough porous interface, greatly enhances the bonding force, and avoids the early shedding of the bracket. However, its disadvantage is that it will cause demineralization of the enamel surface, reduce the acid resistance and hardness of the enamel surface, and increase the caries rate. In order to avoid the adverse effects of demineralization, scholars have made many efforts to find alternatives to traditional bonding methods, such as laser etching and the use of resin-modified glass ionomer adhesives.

[0004] Therefore, the prior art still lacks a simple method for preparing fluorohydroxyapatite nanorods with controllable size and excellent performance, and the prior art also lacks a process for preparing medical adhesives using fluorohydroxyapatite nanorods as raw materials. Summary of the invention

[0005] The invention provides a new method for preparing hydroxyapatite nanorods, and uses the hydroxyapatite nanorods as raw materials to prepare medical adhesives.

[0006] To achieve this object, the present invention provides the following technical solutions:

[0007] The first aspect of the present invention provides a method for preparing fluorinated hydroxyapatite nanorods, comprising the following steps:

[0008] S1. Stirring octadecylamine, oleic acid and ethanol at room temperature until they are completely hydrolyzed;

[0009] S2, add calcium nitrate tetrahydrate, sodium fluoride and sodium phosphate dodecahydrate in sequence and stir thoroughly;

[0010] S3, subjecting the solution obtained in step S2 to a hydrothermal reaction, and fluorinated hydroxyapatite is precipitated at the bottom;

[0011] S4, filtering, washing, freeze-drying, and passing through a 400-500 mesh sieve to obtain fluorinated hydroxyapatite nanorods;

[0012] Among them, the mass ratio of calcium nitrate tetrahydrate, sodium fluoride and sodium phosphate dodecahydrate is 1:(0.01-0.0.06):1.

[0013] Preferably, in step S3, the hydrothermal reaction temperature is 200-250° C. and the reaction time is 10-12 hours.

[0014] Preferably, in step S4, after the precipitate is filtered, it is washed three times with anhydrous ethanol, then freeze-dried with ethanol as a solvent in a freeze dryer for 24-36 hours, and passed through a 400-mesh sieve.

[0015] According to a second aspect of the present invention, fluorine-containing hydroxyapatite nanorods are provided, wherein the length of the fluorine-containing hydroxyapatite nanorods is 80-500 nm.

[0016] Preferably, the method for preparing fluorinated hydroxyapatite nanorods comprises the following steps:

[0017] S1. Stirring octadecylamine, oleic acid and ethanol at room temperature until they are completely hydrolyzed;

[0018] S2, add calcium nitrate tetrahydrate, sodium fluoride and sodium phosphate dodecahydrate in sequence and stir thoroughly;

[0019] S3, subjecting the solution obtained in step S2 to a hydrothermal reaction, and fluorinated hydroxyapatite is precipitated at the bottom;

[0020] S4, filtering, washing, freeze-drying, and passing through a 400-500 mesh sieve to obtain fluorinated hydroxyapatite nanorods;

[0021] Among them, the mass ratio of calcium nitrate tetrahydrate, sodium fluoride and sodium phosphate dodecahydrate is 1:(0.01-0.0.06):1.

[0022] Preferably, in step S3, the hydrothermal reaction temperature is 200-250° C. and the reaction time is 10-12 hours.

[0023] Preferably, in step S4, after the precipitate is filtered, it is washed three times with anhydrous ethanol, then freeze-dried with ethanol as a solvent in a freeze dryer for 24-36 hours, and passed through a 400-mesh sieve.

[0024] The third aspect of the present invention provides a medical adhesive, comprising fluorinated hydroxyapatite nanorods prepared by the method described in the present invention and a resin matrix, wherein the resin matrix comprises the following components: methyl propionic acid modified epoxy resin, methyl methacrylate monomer, phosphate ester, and camphorquinone.

[0025] In the present invention, the medical adhesive is a bonding composite resin.

[0026] In the present invention, the role of the methyl methacrylate modified epoxy resin is: improving the bonding strength: the methyl methacrylate modified epoxy resin can increase the bonding strength of the adhesive, so that the bonded materials can be more firmly bonded together. Improving heat resistance: the methyl methacrylate modified epoxy resin can improve the high temperature resistance of the adhesive, so that the bonded materials can still maintain stable bonding performance in a high temperature environment. Improving chemical resistance: the methyl methacrylate modified epoxy resin can increase the resistance of the adhesive to chemical substances, so that the bonded materials can maintain stable bonding performance in various chemical media. Improving fluidity: the methyl methacrylate modified epoxy resin can improve the fluidity of the adhesive, making it easier to coat it on the surface of the bonded material, thereby improving the bonding effect.

[0027] In the present invention, the role of methacrylate monomers: As a diluent: methacrylate monomers can be used as diluents to adjust the viscosity and fluidity of the adhesive resin, making it easier to coat on the surface of the bonded material. Promote curing: methacrylate monomers can participate in the curing reaction of the adhesive resin as a reactant, form a cross-linked network structure through polymerization reaction, and enhance the strength and durability of the adhesive. Improve bonding performance: methacrylate monomers can improve the bonding performance of the adhesive and increase its adhesion to the bonded material, thereby improving the strength and reliability of the bond. Adjust physical properties: The introduction of methacrylate monomers can adjust the physical properties of the adhesive resin, such as hardness, elastic modulus, etc., to meet different application requirements.

[0028] In the present invention, the roles of phosphate ester in the adhesive resin include: as a cross-linking agent: phosphate ester can participate in the cross-linking reaction of the adhesive resin as a reactant, and react with other functional groups to form a cross-linked structure, thereby enhancing the strength and durability of the adhesive. Improved bonding performance: phosphate ester can improve the bonding performance of the adhesive and increase its adhesion to the bonded material, thereby improving the strength and reliability of the bond. Improved heat resistance: The introduction of phosphate ester can improve the heat resistance of the adhesive, allowing it to maintain stable performance in a high temperature environment. Increased flexibility: phosphate ester can increase the flexibility of the adhesive, allowing it to adapt to the thermal expansion and contraction and deformation of different materials, and improve the reliability of the bond.

[0029] In the present invention, camphorquinone is a commonly used photoinitiator, which is often used in adhesive resins as a starter for photocuring systems. The role of camphorquinone is mainly reflected in: Photoinitiator: camphorquinone can absorb light energy of a specific wavelength, generate active free radicals through photoexcitation, and thus start the photocuring reaction of the adhesive resin. Under light conditions, camphorquinone can effectively promote the curing speed and degree of the adhesive. Adjust the curing speed: The introduction of camphorquinone can adjust the curing speed of the adhesive resin. By adjusting the concentration of camphorquinone and the intensity of light, the curing time of the adhesive can be controlled to make it more suitable for specific application requirements. Improve the curing effect: The presence of camphorquinone can increase the curing effect of the adhesive. It can prompt the photoinitiator in the adhesive to more fully generate active free radicals, thereby improving the efficiency and quality of curing.

[0030] Preferably, the weight percentage of each component of the resin matrix is:

[0031]

[0032] Preferably, the medical adhesive is used for bonding orthodontic brackets to the surface of tooth enamel.

[0033] Preferably, the medical adhesive is used to promote remineralization, and specifically, is used in inducing calcium-phosphorus deposition to promote remineralization, and is used in dental remineralization adhesives.

[0034] Preferably, the medical adhesive is a viscous liquid.

[0035] Preferably, the method for preparing the resin matrix comprises the following steps:

[0036] Step 1, weighing methyl propionic acid modified epoxy resin, methacrylate monomer, phosphate, and camphorquinone; wherein the mass percentages of methyl propionic acid modified epoxy resin, methacrylate monomer, and phosphate are 20% to 30%: 60% to 40%: 20% to 30%, and the mass fraction of camphorquinone accounts for 0.1% to 1% of the total mass of the methyl propionic acid modified epoxy resin, methacrylate monomer, and phosphate;

[0037] Step 2: Mix and stir the above ingredients at 30°C for 30-35 minutes, then heat to 60°C and stir for another 30-35 minutes; preferably, the two stirring times are 30 minutes and 30 minutes respectively;

[0038] Step 3: Cool the mixture obtained in step 2 for later use to obtain a resin matrix.

[0039] The fourth aspect of the present invention provides use of the medical adhesive of the present invention in preparing a compound for bonding orthodontic brackets to tooth enamel surfaces.

[0040] The fifth aspect of the present invention provides use of the medical adhesive of the present invention in preparing a compound for inducing calcium and phosphate deposition and promoting remineralization.

[0041] The sixth aspect of the present invention provides use of the medical adhesive of the present invention in the preparation of a dental remineralization adhesive.

[0042] The remineralization mechanism of the medical adhesive of the present invention is as follows: calcium ions and phosphates are deposited at the demineralization gap to form an amorphous Ca-P compound, which then nucleates, crystallizes and grows into hydroxyapatite nanorods. When there are fluoride ions in the microenvironment, the calcium ion concentration of the hydroxyapatite nanorods is in an oversaturated state relative to the fluoroapatite, and the two substances exchange ions to reach equilibrium, so that the concentration of the fluoroapatite increases, and the fluoroapatite is supersaturated with calcium ions for the surrounding solution, so that the hydroxyapatite continuously generates fluoroapatite by a chain effect. And because the binding force between fluoride ions and calcium ions is greater than the binding force between oxygen and calcium, the stability of fluoroapatite is much greater than that of hydroxyapatite, and it is more difficult to demineralize and cause caries.

[0043] Compared with the prior art, the beneficial effects and significant improvements of the technical solution of the present invention are:

[0044] 1. The present invention provides a new fluorine-containing hydroxyapatite nanorod, which realizes the controllable preparation of the size of the hydroxyapatite nanorod by adjusting the fluorine concentration, and realizes the stable and continuous release of fluoride ions and calcium ions;

[0045] 2. The fluorinated hydroxyapatite nanorods obtained by the present invention are blended with resin-based materials for use in medical adhesives, which can release calcium ions and fluoride ions in a simulated oral fluid environment; experiments have observed calcium and phosphorus deposition on the surface of the medical adhesive; experiments have observed that the medical adhesive remineralizes demineralized tooth enamel. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] In order to more clearly illustrate the technical solution of the present invention, the drawings used in the embodiments of the present invention are briefly introduced below.

[0047] Figure 1 are transmission electron microscope images of fluorinated hydroxyapatite nanorods of different sizes of the present invention;

[0048] Figure 2 is the X-ray diffraction analysis diagram of the fluorine-containing hydroxyapatite nanorods of different sizes of the present invention ( Figure 2 A) Fourier infrared analysis diagram ( Figure 2 B);

[0049] Figure 3 is a scanning electron microscope image of the distribution of fluorinated hydroxyapatite nanorods in the cross section of the composite resin after photocuring of different groups of materials;

[0050] Figure 4 It is a line graph of calcium ion release of medical adhesive in Tris-HCl at pH 7.4;

[0051] Figure 5 It is a line graph of fluoride ion release of medical adhesive in Tris-HCl at pH 7.4;

[0052] Figure 6 It is the dispersion stability of fluorinated hydroxyapatite nanorods in the resin matrix in medical adhesives;

[0053] Figure 7 This is a result diagram of the light curing of medical adhesives;

[0054] Figure 8 is a schematic diagram of the bonding strength of medical adhesives;

[0055] Fig. 9 It is the result graph of remineralization performance of medical adhesive without filler and with 10% of AH1-AH3;

[0056] Fig.10 This is a graph showing the evaluation results of the remineralization effect on the demineralized enamel surface. DETAILED DESCRIPTION

[0057] To make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the present invention is further described below in conjunction with specific examples. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples that do not specify specific conditions are usually based on conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, percentages and parts are weight percentages and weight parts. The experimental materials and reagents used in the following examples can be obtained from commercial channels unless otherwise specified.

[0058] Unless otherwise specified, the technical and scientific terms used herein have the same meaning as commonly understood by ordinary technicians in the technical field to which the application belongs. It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments of the present application.

[0059] Example 1 Preparation and detection of fluorinated hydroxyapatite nanorods

[0060] Experimental methods

[0061] 1.1. First, dissolve 0.5g of octadecylamine in 4ml of oleic acid at room temperature, and then add 16ml of ethanol;

[0062] 1.2. While stirring, add 5 ml of 0.5 g of calcium nitrate tetrahydrate solution, 5 ml of sodium fluoride solution containing 0.005 g (H1), 0.015 g (H2), 0.025 g (H3), 0.035 g (H4), and 5 ml of 0.5 g of sodium phosphate dodecahydrate solution to the solution in sequence, and continue stirring for 30 minutes;

[0063] 1.3. The obtained mixed solution was transferred to a reactor and heated at 200°C for 10 hours, cooled to room temperature, and hydroxyapatite was precipitated at the bottom;

[0064] 1.4. Filter the precipitate, wash it with anhydrous ethanol for 3 times, freeze-dry it in a freeze dryer with ethanol as solvent for 24-36 hours, and pass it through a 400-mesh sieve;

[0065] 1.5. The product obtained in step 1.4 was subjected to scanning electron microscopy, X-ray diffraction analysis and Fourier transform infrared analysis.

[0066] Experimental Results

[0067] The results of scanning electron microscopy of groups H1-H4 are shown in Figure 1 As shown, the product H1 ( Figure 1 A, B); add 5ml of sodium fluoride solution containing 0.015g to obtain the product named H2( Figure 1 AC, D); add 5ml of sodium fluoride solution containing 0.025g to obtain the product named H3( Figure 1 E, F), add 5 ml of sodium fluoride solution containing 0.035 g to obtain the product named H4 ( Figure 1 G, H). As the amount of fluorine doping increases, the length of the hydroxyapatite nanorods decreases and the aspect ratio decreases. The length of the H1 nanorod is about 500nm; the length of the H2 nanorod is about 250nm; the length of the H3 nanorod is about 80nm. The H4 group shows irregular nanoparticles with uneven sizes and obvious agglomeration, indicating that the hydroxyapatite nanorods were not successfully synthesized. It can be seen that when the amount of fluorine doping is too much, the synthesis of uniform hydroxyapatite nanorods will fail. Because the H4 group failed to synthesize, only the fluorinated hydroxyapatite nanorods of the H1-H3 groups were studied in the future.

[0068] The X-ray diffraction analysis results of group H1-H3 are as follows Figure 2 As shown in A, it shows the same composition as nano-hydroxyapatite, and as the fluorine incorporation amount increases, the peak value of each peak increases, indicating the successful incorporation of fluorine in groups H1-H3.

[0069] The results of Fourier infrared analysis of groups H1-H3 are as follows Figure 2As shown in B, it shows that it has the corresponding groups, and with the increase of fluorine doping, the OH peak decreases, and the peaks of other groups remain basically unchanged, indicating that F successfully replaces OH. The above results show the successful preparation of fluorinated hydroxyapatite nanorods of different sizes in groups H1-H3.

[0070] Example 2 Preparation and Testing of Medical Adhesive

[0071] Experimental methods

[0072] 2.1. Preparation of resin matrix

[0073] The analytically pure raw materials of methylpropionic acid modified epoxy resin, methacrylate monomer, phosphate and camphorquinone were directly purchased from Shanghai Guoyao; the above-mentioned methylpropionic acid modified epoxy resin, methacrylate monomer and phosphate were mixed in a mass ratio of 30%:45%:25% with 0.5% camphorquinone based on the total mass of the above-mentioned methylpropionic acid modified epoxy resin, methacrylate monomer and phosphate at 30° C. and stirred for 30 minutes, then heated to 60° C. and stirred for another 30 minutes; the obtained mixture was cooled for standby use to obtain a resin matrix.

[0074] 2.2. Weigh 10% by mass of the fluorinated hydroxyapatite nanorods H1-H3 prepared in Example 1 of the present invention on a precision balance and add them to the resin matrix, stir at room temperature, and ultrasonicate for 30 minutes to make the fluorinated hydroxyapatite nanorods H1-H3 evenly distributed in the liquid, thus obtaining the medical adhesive (composite resin) AH1-AH3, which is stored at room temperature away from light. The control group is not added with fluorinated hydroxyapatite nanorods, and is named group A0.

[0075] 2.3. Scanning of medical adhesives AH1-AH3 under an electron microscope.

[0076] Experimental Results

[0077] Figure 3 : is a scanning electron microscope image of the distribution of fluorinated hydroxyapatite nanorods in the cross section of the composite resin after photocuring of different groups of materials of the present invention. Among them, the scanning electron microscope image of the cross section of the composite resin after photocuring of group A0 ( Figure 3 A, B), Scanning electron microscopy images of the distribution of fluorinated hydroxyapatite nanorods in the cross section of the composite resin after photocuring in the AHI group ( Figure 3 C, D), scanning electron microscopy images of the distribution of fluorinated hydroxyapatite nanorods in the cross section of the composite resin after photocuring in group AH2 ( Figure 3 E, F), scanning electron microscopy images of the distribution of fluorinated hydroxyapatite nanorods in the cross section of the composite resin after photocuring in group AH3 ( Figure 3G, H). This example proves that the fluorine-containing hydroxyapatite nanorods of different sizes prepared in Example 1 are evenly distributed in the resin matrix of the present invention, thus ensuring the functional stability of the composite resin (medical adhesive).

[0078] Example 3 Performance Testing of Medical Adhesives

[0079] 3.1. Calcium ion release of medical adhesive in Tris-HCl at pH 7.4

[0080] Cumulative calcium ion release after immersing 10% by mass of AH1-AH3 medical adhesive in Tris-HCl at pH 7.4 for 1, 5, 10, and 15 days, respectively, wherein the ratio of medical adhesive to immersion solution is 1:1 (mg / ml).

[0081] The results are as follows Figure 4 As shown, there was no significant difference in the calcium release of AH1-AH3 medical adhesives, and the cumulative calcium ion release was around 7 ppm after 15 days.

[0082] 3.2 Fluoride ion release of medical adhesive in Tris-HCl at pH 7.4

[0083] Cumulative release of fluoride ions after immersion of 10% AH1-AH3 medical adhesive in Tris-HCl at pH 7.4 for 1, 5, 10, and 15 days, respectively. The ratio of medical adhesive to immersion solution is 1:1 (mg / ml).

[0084] The results are as follows Figure 5 As shown, the fluoride ion release of AH1-AH3 medical adhesives increases with the increase of fluoride incorporation.

[0085] 3.3 Dispersion stability of fluorinated hydroxyapatite nanorods in resin matrix in medical adhesives

[0086] The results are as follows Figure 6 As shown in the figure, the dispersion stability result of fluorinated hydroxyapatite nanorods in the resin matrix in the medical adhesive doped with 10% AH1 of the present invention ( Figure 6 A) The dispersion stability results of fluorinated hydroxyapatite nanorods in the resin matrix of the medical adhesive doped with 10% AH2 according to the present invention ( Figure 6 B) The dispersion stability results of fluorinated hydroxyapatite nanorods in the resin matrix in the medical adhesive doped with 10% AH3 according to the present invention ( Figure 6 C). The results show that the three types of fluorinated hydroxyapatite nanorods can maintain good stability in the resin matrix within 2 hours.

[0087] 3.4. Photocuring properties of medical adhesives

[0088] 3 ml of the AH1-AH3 medical adhesive prepared by the above synthesis method containing 10% by mass was injected into a glass bottle with a bottom area of ​​about 2 cm 2 After standing for 30 minutes, the wavelength of 420-480nm and 1200-2000mw / cm 2 The curing lamp with high intensity light source illuminates the bottom of the bottle from 2 cm away for 0 seconds, 5 seconds, 10 seconds, and 20 seconds to observe the curing of AH1-AH3 medical adhesive. The glass bottle is inverted for 5 minutes. If the AH1-AH3 medical adhesive in the bottle does not flow, it is completely cured, and digital photos are taken.

[0089] The results are as follows Figure 7 As shown in the figure, the curing conditions of the AH1-AH3 medical adhesives containing 10% mass fraction were irradiated for 0 seconds, 5 seconds, 10 seconds and 20 seconds respectively. It can be seen that at 5 seconds, the bottom of the non-filler group was basically cured, the filler group was mostly cured, and only a few upper layers were not cured; at 10 seconds, only a few upper layers of the non-filler group were not cured, and the filler group was basically cured; at 20 seconds, all medical adhesives were completely cured.

[0090] 3.5. Changes in bonding strength of medical adhesives

[0091] Through the universal mechanical testing machine, the base plate area is selected to be 9.24mm 2 Orthodontic brackets. The ex vivo bovine incisors were fixed with the fixture of a universal mechanical testing machine. The surface was etched with 37% phosphoric acid (Guan Ya, Wuhan) for 45 seconds, and then a layer of adhesive was applied and the orthodontic brackets were placed and light-cured for 20 seconds. The shear strength between the orthodontic brackets and the ex vivo teeth of each group was tested.

[0092] The results are as follows Figure 8 As shown, the bonding strength of orthodontic brackets containing 10% by mass fraction of AH1-AH3 medical adhesives. After the powder is added, the bonding strength between the medical adhesive and the orthodontic bracket and the enamel is reduced, but it still maintains sufficient bonding strength to meet clinical needs. The minimum value for practical clinical application is 6-8MPa.

[0093] Example 4 Remineralization performance of medical adhesive surface

[0094] Test method: The photocured medical adhesive was immersed in simulated oral fluid (SOF) and incubated in a constant temperature shaker at 37°C. The SOF was replaced every day. The composite resins of each group were collected after immersion for 3 and 7 days, ultrasonically cleaned for 5 minutes, and fully dried. The surface mineralization was detected by electron scanning microscopy, and the mineralized areas were semi-quantitatively analyzed by EDS energy spectrum elements.

[0095] like Fig. 9The following are scanning electron microscope images of the present invention without filler and 10% AH1-AH3 medical adhesives immersed in SOF for 3 days and 7 days. No obvious mineralization was observed on the surface of the composite resin without filler. With the increase of fluorine doping amount and the extension of mineralization time in the AF1-AH3 filler group, the density of spherical mineralization gradually increased, and the AH3 group showed the best remineralization performance.

[0096] Table 1 shows the semi-quantitative data of various elements obtained by EDS spectrum analysis of the remineralized parts of the present invention without filler and with 10% AH1-AH3 medical adhesives immersed in SOF for 3 days and 7 days. The data show that with the increase of fluorine addition and the extension of mineralization time, the relative amount of calcium and Ca / P gradually increase, indicating the increase of mineralization amount and the maturity of mineralization. At 7 days, the Ca / P of the AH3 group is close to the calcium-phosphorus ratio of mature hydroxyapatite, 1.67.

[0097] Table 1

[0098]

[0099] Example 5 Evaluation of the remineralization effect of demineralized enamel surface

[0100] The experimental steps for preparing demineralized enamel are as follows:

[0101] Healthy bovine incisors without obvious damage and cracks were selected as samples. The labial enamel was polished with 180, 800, and 1500 grit sandpaper in sequence under running water, ultrasonically cleaned for 5 minutes, and then etched with 37% phosphoric acid (Guan Ya, Wuhan) at room temperature for 45 seconds and thoroughly rinsed with distilled water for 2 minutes to obtain demineralized enamel.

[0102] The medical adhesives without fillers and those with 10% mass fraction of AH1-AH3 were evenly coated on the surface of demineralized enamel, respectively, and fixed in the oral environment of SD rats after 20 seconds of light curing light. The excised teeth of each group were collected after 7 days of treatment, ultrasonically cleaned for 30 minutes, and fully dried, and the surface mineralization was detected by electron scanning microscopy.

[0103] Fig.10 Healthy tooth enamel ( Fig.10 A) Demineralized enamel ( Fig.10 B) Demineralized enamel treated with composite bonding resin without fillers was fixed in the oral environment of SD rats for 7 days ( Fig.10 C) Scanning electron microscopy images of demineralized enamel treated with 10% AH1-AH3 medical adhesives after being fixed in the oral cavity of SD rats for 7 days ( Fig.10DF). It can be seen that no obvious remineralization was observed in the unfilled group. As the amount of fluorine added to the filler group increased, the mineralized material gradually filled the demineralized gap. The demineralized gap in the AH3 group was basically completely filled, and obvious mineralized particle deposition was observed.

[0104] Table 2 shows the semi-quantitative data of each element obtained by EDS spectrum analysis of healthy enamel surface, demineralized enamel surface, surface remineralization site of demineralized enamel treated with composite adhesive resin without filler and fixed in the oral environment of SD rats for 7 days, and surface remineralization site of demineralized enamel treated with 10% mass fraction of AH1-AH3 medical adhesive and fixed in the oral environment of SD rats for 7 days. It can be seen that with the increase of fluoride addition, the relative amount of calcium in the remineralization site gradually increases, and the AH3 group shows the best remineralization performance.

[0105] Table 2

[0106]

[0107] The applicant declares that, in the description of the above specification:

[0108] The descriptions of the terms "this embodiment", "an embodiment of the present invention", "as shown in...", "further", "a further improved technical sub-scheme", etc., mean that the specific features, structures, materials or characteristics described in the embodiment or example are included in at least one embodiment or example of the present invention; in this specification, the schematic expressions of the above terms are not necessarily for the same embodiment or example, and the specific features, structures, materials or characteristics described may be combined or combined in a suitable manner in any one or more embodiments or examples; in addition, a person of ordinary skill in the art may combine or combine the different embodiments or examples and the features of the different embodiments or examples described in this specification without causing any contradiction.

[0109] Finally, it should be noted that:

[0110] The above embodiments are only used to illustrate the technical solutions of the present invention, but not to limit them.

[0111] Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some or all of the technical features therein, and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present invention. The non-essential improvements, adjustments or replacements made by those skilled in the art based on the contents of this specification are all within the scope of protection required by the present invention.

Claims

1. A method for preparing fluorinated hydroxyapatite nanorods, It is characterized in that The following steps are involved: S1. Stirring octadecylamine, oleic acid and ethanol at room temperature until they are completely hydrolyzed; S2, add calcium nitrate tetrahydrate, sodium fluoride and sodium phosphate dodecahydrate in sequence and stir thoroughly; S3, subjecting the solution obtained in step S2 to a hydrothermal reaction, and fluorinated hydroxyapatite is precipitated at the bottom; S4, filtering, washing, freeze-drying, and passing through a 400-500 mesh sieve to obtain fluorinated hydroxyapatite nanorods; Among them, the mass ratio of calcium nitrate tetrahydrate, sodium fluoride and sodium phosphate dodecahydrate is 1:(0.01-0.0.06):

1.

2. A method for preparing fluorinated hydroxyapatite nanorods according to claim 1, It is characterized in that In step S3, the hydrothermal reaction temperature is 200-250° C. and the reaction time is 10-12 hours.

3. A method for preparing fluorinated hydroxyapatite nanorods as claimed in claim 1, It is characterized in that In step S4, after the precipitate is filtered, it is washed with anhydrous ethanol for three times, and then freeze-dried with ethanol as a solvent in a freeze dryer for 24-36 hours and passed through a 400-mesh sieve.

4. Fluorinated hydroxyapatite nanorods prepared by the method according to any one of claims 1 to 3, It is characterized in that The length of the fluorine-containing hydroxyapatite nanorods is 80-500nm.

5. A medical adhesive, It is characterized in that The invention comprises fluorine-containing hydroxyapatite nanorods prepared by the method described in any one of claims 1 to 3 and a resin matrix, wherein the resin matrix comprises the following components: methyl propionic acid-modified epoxy resin, methyl methacrylate monomer, phosphate ester and camphorquinone.

6. The medical adhesive according to claim 5, It is characterized in that The mass parts of each component of the resin matrix are: 20-30 parts of methyl propionic acid modified epoxy resin; 40-60 parts of methacrylate monomer; Phosphate 20-30 parts; Camphorquinone 0.1-1 part.

7. The medical adhesive according to claim 5, It is characterized in that The medical adhesive is a viscous liquid.

8. Use of the medical adhesive according to any one of claims 5 to 7 in preparing a compound for bonding orthodontic brackets to tooth enamel surfaces.

9. Use of the medical adhesive according to any one of claims 5 to 7 in the preparation of a compound for inducing calcium and phosphate deposition and promoting remineralization.

10. Use of the medical adhesive according to any one of claims 5 to 7 in the preparation of a dental remineralization adhesive.

Citation Information

Patent Citations

  • Hydroxyapatite nanorod with surface grafted with EGCG (epigallocatechin gallate) as well as preparation method and application of hydroxyapatite nanorod

    CN113398326A

  • Dental adhesive composition as well as preparation method and application thereof

    CN114732740A

  • Methods for Production and Use of Synthetic Hydroxyapatite and Fluorapatite Nanorods, and Superstructures Assembled from the Same