Method for recovering fluorine by utilizing flash evaporation cooling coupled rotational flow in wet-process phosphoric acid process

Through the flash cooling coupled cyclone method, the problem of fluorine resource waste in the wet phosphoric acid process is solved, the efficient recovery of fluorosilicate is achieved, and the purity of the phosphoric acid product and the utilization rate of fluorine resources are improved.

CN118851181AActive Publication Date: 2024-10-29INSTITUTE OF PROCESS ENGINEERING CHINESE ACADEMY OF SCIENCES
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411118938.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-10-29
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

In the wet phosphoric acid process, impurities such as sodium, potassium, silicon and fluorine released during the acidolysis of medium and low-grade phosphate ores form fluorosilicates, resulting in a waste of fluorine resources and a reduction in the purity of phosphoric acid products. Existing defluoridation methods are ineffective. .

Method used

The flash cooling coupled cyclone method is used to rapidly vaporize the acid hydrolysis slurry liquid of phosphate rock and absorb heat through flash evaporation, thereby increasing the supersaturation and rapidly crystallizing fluorosilicate, and using cyclone separation to recover large particles of fluorosilicate. salt to achieve efficient recovery of fluorine resources.

Benefits of technology

It achieves efficient recovery of fluorine resources, reduces the fluorine content of phosphogypsum and phosphoric acid products, and achieves a recovery rate of more than 32.4%, simplifying the process without using chemical reagents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention provides a method for recovering fluorine by utilizing flash evaporation cooling coupled rotational flow in a wet-process phosphoric acid process, which comprises the following steps: carrying out flash evaporation cooling crystallization on slurry obtained by phosphorite acidolysis to obtain slurry after flash evaporation; and carrying out cyclone separation on the obtained slurry after flash evaporation, and recovering fluosilicate particles. According to the method provided by the invention, fluorine subjected to phosphorite acidolysis forms large-particle fluosilicate through flash evaporation cooling coupled cyclone separation for separation and recovery, the process is simple and easy to operate, no chemical reagent needs to be added, the fluorine recovery effect is good, the recovery rate reaches 32.4% or above, and the method is suitable for industrial production. The fluorine content of subsequent phosphogypsum and phosphoric acid in the wet-process phosphoric acid process can be effectively reduced, and subsequent resource utilization of fluorine resources is facilitated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of wet-process phosphoric acid and relates to a method for recovering fluorine in a wet-process phosphoric acid process, and in particular to a method for recovering fluorine in a wet-process phosphoric acid process by utilizing flash cooling coupled with cyclone flow. Background Art

[0002] The wet phosphoric acid process is a process that uses inorganic acid to decompose phosphate rock to produce phosphoric acid. The main processes of the wet phosphoric acid production process include: the phosphate rock and acid (including sulfuric acid, nitric acid, hydrochloric acid, etc.) undergo an acid hydrolysis process, the reaction slurry after acid hydrolysis is filtered to obtain a gypsum filter cake and phosphoric acid with a lower concentration, and the phosphoric acid with a lower concentration is concentrated to obtain a phosphoric acid product. Phosphate rock contains fluorine impurities. During the acid hydrolysis of phosphate rock, fluorine reacts with acid to generate hydrofluoric acid, and hydrofluoric acid reacts with silicon oxide or silicate contained in the phosphate rock to form fluorosilicic acid, allowing fluorine to enter the wet phosphoric acid process, thereby affecting the purity of the phosphoric acid product. Therefore, defluorination and purification of the wet phosphoric acid process is of great significance.

[0003] With the development of phosphate resources, the resource utilization of medium and low-grade phosphate ores has become an urgent need of the phosphorus chemical industry. Medium and low-grade phosphate ores have high impurity content. During the acid hydrolysis process, a large amount of impurities such as sodium, potassium, and silicon will be released, which will combine with fluorine to form sodium fluorosilicate and potassium fluorosilicate. As impurities continue to accumulate, they are prone to reach an oversaturated state; during the vacuum filtration process, the supersaturated sodium fluorosilicate and potassium fluorosilicate are easily precipitated and mixed in the phosphogypsum when cooled, resulting in a high fluorine content in the phosphogypsum, wasting a lot of fluorine resources; during the aging and refining process of phosphoric acid, sodium fluorosilicate and potassium fluorosilicate are easily converted into low-value fluorine-containing slag, making resource utilization difficult.

[0004] At present, the defluorination methods of wet phosphoric acid process mainly include chemical precipitation method, vacuum concentration method and steam stripping method. The chemical precipitation method is to add alkali metal salt as a defluorinating agent to generate fluorosilicate precipitate for filtration. The vacuum concentration method is to add active SiO2 to convert fluorine into fluorosilicic acid, and convert fluorine into gas by heating and concentration. The steam stripping method is to heat the acid in the concentrated phosphoric acid by high-pressure supersaturated steam to vaporize and escape fluorine. For example, CN117699760A, CN114314539A, CN110467167A, etc. disclose methods for defluorination of wet phosphoric acid, and the above-mentioned defluorination methods are all for defluorination and purification of the produced phosphoric acid and concentration to obtain phosphoric acid products. It is difficult to remove and purify fluorine impurities in the wet phosphoric acid process, and the defluorination effect in the wet phosphoric acid process cannot be guaranteed, thereby affecting the purity of the phosphogypsum product and wasting fluorine resources.

[0005] Therefore, it is necessary to provide a method for enhancing fluorine resource recovery in the phosphate ore acid hydrolysis process during the wet phosphoric acid process. Summary of the invention

[0006] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a method for recovering fluorine in a wet phosphoric acid process by utilizing flash cooling coupled with cyclone flow, and to achieve recovery of fluorine-containing impurities and waste of fluorine resources caused by the acidolysis process releasing a large amount of sodium, potassium, silicon, fluorine and other impurities to form fluorosilicates in the wet phosphoric acid process of medium and low-grade phosphate ore.

[0007] To achieve this object, the present invention adopts the following technical solutions:

[0008] The present invention provides a method for recovering fluorine by using flash cooling coupled with cyclone flow in a wet phosphoric acid process, the method comprising the following steps:

[0009] (1) subjecting the phosphate rock acid-hydrolyzed slurry to flash evaporation, cooling and crystallization to obtain a flash evaporation slurry;

[0010] (2) subjecting the flash slurry obtained in step (1) to cyclone separation to recover the fluorosilicate particles.

[0011] During the acid hydrolysis process, medium and low-grade phosphate ore releases a large amount of impurities such as sodium, potassium, silicon and fluorine, forming sodium fluorosilicate and potassium fluorosilicate. Sodium fluorosilicate and potassium fluorosilicate continue to accumulate to reach supersaturation and enter the subsequent phosphogypsum product.

[0012] The method provided by the present invention is aimed at the sources of sodium fluorosilicate and potassium fluorosilicate. After the acid hydrolysis process of phosphate rock, the characteristics of sodium fluorosilicate and potassium fluorosilicate being higher in solubility under high temperature conditions and lower in solubility under low temperature conditions are utilized. The liquid in the slurry is rapidly vaporized and a large amount of heat is absorbed by a flash evaporation method, the supersaturation of fluorosilicate in the slurry is increased, and the slurry temperature is reduced at the same time, so that the supersaturated fluorosilicate is rapidly crystallized and grows into large particles of millimeter to centimeter scale, and then the fluorosilicate particles continue to grow in the slurry system, and then the large fluorosilicate particles in the slurry are rapidly and low-costly recovered by cyclone separation, so as to realize the fluorine precipitation recovery in the wet phosphoric acid process, which is beneficial to the subsequent resource utilization of fluorine resources and reduces the entry of fluorine impurities into subsequent processes.

[0013] The process of acid hydrolysis of phosphate rock includes reacting phosphate rock with sulfuric acid.

[0014] Preferably, the composition of the phosphate rock includes: a P2O5 content of 20-30wt%, a F content of 2-4wt%, a SiO2 content of 6-12wt%, a Al2O3 content of 2-6wt%, a K2O content of 0.5-2wt%, and a Na2O content of 0.1-1wt%.

[0015] The F content is 2-4wt%, for example, 2wt%, 2.5wt%, 3wt%, 3.5wt% or 4wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0016] The SiO2 content is 6-12wt%, for example, it can be 6wt%, 7wt%, 8wt%, 9wt%, 10wt%, 11wt% or 12wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0017] The content of K2O is 0.5-2wt%, for example, 0.5wt%, 1wt%, 1.5wt% or 2wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0018] The Na2O content is 0.1-1wt%, for example, it can be 0.1wt%, 0.3wt%, 0.5wt%, 0.8wt% or 1wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0019] Preferably, the composition of the slurry of the phosphate rock acid hydrolysis includes: 30-35wt% phosphogypsum, 25-35wt% P2O5, 1-5wt% sulfuric acid, and 0.1-2wt% hydrofluoric acid.

[0020] Among them, the content of phosphogypsum is 30-35wt%, for example, it can be 30wt%, 31wt%, 32wt%, 33wt%, 34wt% or 35wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0021] The content of P2O5 is 25-35wt%, for example, it can be 25wt%, 28wt%, 30wt%, 32wt% or 35wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0022] The content of sulfuric acid is 1-5wt%, for example, 1wt%, 2wt%, 3wt%, 4wt% or 5wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0023] The content of hydrofluoric acid is 0.1-2wt%, for example, 0.1wt%, 0.5wt%, 1wt%, 1.5wt% or 2wt%, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0024] Preferably, the solid content of the slurry of the phosphate rock acid hydrolysis is 25-38%, for example, it can be 25%, 26%, 28%, 30%, 32%, 34%, 35%, 36% or 38%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0025] Preferably, the D50 particle size distribution of the solid phase in the slurry of the acid hydrolysis of the phosphate rock is 70-100 μm, for example, it can be 70 μm, 75 μm, 80 μm, 85 μm, 90 μm, 95 μm or 100 μm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, in the slurry of the acid hydrolysis of the phosphate rock, the total content of sodium and potassium in the liquid phase is 0.4-0.8%, for example, it can be 0.4%, 0.5%, 0.6%, 0.7% or 0.8%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0027] Preferably, in the slurry of the acid hydrolysis of the phosphate rock, the P2O5 content of the liquid phase is 25-35%, for example, it can be 25%, 26%, 28%, 30%, 32%, 34% or 35%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] Preferably, in the slurry of the acid hydrolysis of the phosphate rock, the F content of the liquid phase is 0.5-2.0%, for example, it can be 0.5%, 0.6%, 0.8%, 1.0%, 1.2%, 1.4%, 1.5%, 1.6%, 1.8% or 2.0%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] Preferably, the temperature of the phosphate rock acid hydrolysis slurry is 70-80°C, for example, it can be 70°C, 71°C, 72°C, 73°C, 74°C, 75°C, 76°C, 77°C, 78°C, 79°C or 80°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] Preferably, the vacuum degree of the flash cooling crystallization is 65-85 kPa, for example, it can be 65 kPa, 68 kPa, 70 kPa, 72 kPa, 75 kPa, 78 kPa, 80 kPa, 82 kPa or 85 kPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0031] Preferably, the temperature difference between the feed and the discharge of the flash cooling crystallization is 4-8°C, for example, 4°C, 5°C, 6°C, 7°C or 8°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0032] In the present invention, the flash evaporation and cooling crystallization is achieved by a conventional flash evaporation device in the art, and the present invention does not limit its structure.

[0033] Preferably, the temperature of the slurry after flash evaporation is controlled to be 70-80°C, for example, 70°C, 72°C, 75°C, 78°C or 80°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0034] Preferably, the temperature of the slurry after flash evaporation is controlled to be kept warm for 2-3 hours, for example, 2 hours, 2.2 hours, 2.4 hours, 2.5 hours, 2.6 hours, 2.8 hours or 3 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0035] In the present invention, the slurry temperature after flash evaporation is regulated and the insulation time is increased. Since impurities such as fluorine and silicon / potassium / sodium are still dissolved in large quantities during the insulation process, the system is still in an oversaturated state, and the crystallized fluorosilicate particles will further grow, thereby achieving recovery through subsequent cyclone separation.

[0036] Preferably, the feed pressure for the cyclone separation is 0.08-0.16 MPa, for example, it can be 0.08 MPa, 0.09 MPa, 0.10 MPa, 0.11 MPa, 0.12 MPa, 0.13 MPa, 0.14 MPa, 0.15 MPa or 0.16 MPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0037] Preferably, the feed flow rate of the cyclone separation is 3.0-6.0 m / s, for example, 3.0 m / s, 4.0 m / s, 5.0 m / s or 6.0 m / s, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] Preferably, the cyclone separation is performed using a cyclone separation device.

[0039] In the present invention, the cyclone separation device can be a conventional cyclone separation device in the art, and the present invention does not limit its specific structure.

[0040] Preferably, the inner diameter of the cyclone tube of the cyclone separation device is 250-300 mm, for example, it can be 250 mm, 260 mm, 270 mm, 280 mm, 290 mm or 300 mm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] Preferably, the inner diameter of the sand settling port of the cyclone separation device is 50-70 mm, for example, it can be 50 mm, 55 mm, 60 mm, 65 mm or 70 mm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0042] Preferably, the cyclone separation device comprises 3-5 cyclone tubes arranged in parallel, for example, 3, 4 or 5 cyclone tubes.

[0043] Preferably, the D50 particle size distribution of the fluorosilicate particles is 1-8 mm, for example, 1 mm, 2 mm, 3 mm, 4 mm, 5 mm, 6 mm, 7 mm or 8 mm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] As a preferred technical solution of the method for recovering fluorine by flash cooling coupled with cyclone in the wet phosphoric acid process provided by the present invention, the method comprises the following steps:

[0045] (1) subjecting the phosphate ore acid hydrolysis slurry at a temperature of 70-80° C. to flash cooling crystallization, wherein the solid content of the phosphate ore acid hydrolysis slurry is 25-38%, the D50 particle size distribution of the solid phase in the phosphate ore acid hydrolysis slurry is 70-100 μm, the P2O5 content of the liquid phase in the phosphate ore acid hydrolysis slurry is 25-35%, the total content of sodium and potassium in the liquid phase is 0.4-0.8%, and the F content of the liquid phase is 0.5-2.0%; the vacuum degree of the flash cooling crystallization is 65-85 kPa, the temperature difference between the feed and the discharge of the flash cooling crystallization is 4-8° C., and after the flash cooling crystallization is completed, the temperature of the flashed slurry is controlled to be 70-80° C. and kept warm for 2-3 hours;

[0046] (2) The slurry after flash evaporation is subjected to cyclone separation, the feed pressure of the cyclone separation is 0.08-0.16 MPa, the feed flow rate of the cyclone separation is 3.0-6.0 m / s, and the fluorosilicate particles are recovered after cyclone separation, and the D50 particle size distribution of the fluorosilicate particles is 3-8 mm.

[0047] Compared with the prior art, the present invention has the following beneficial effects:

[0048] The method provided by the present invention forms large-particle fluorosilicate from fluorine in the acid hydrolysis of phosphate rock through flash cooling coupled with cyclone separation for separation and recovery. The process is simple and easy to operate, and no chemical reagents need to be added. The fluorine recovery effect is good, and the recovery rate reaches more than 32.4%. The fluorine content of subsequent phosphogypsum and phosphoric acid in the wet phosphoric acid process can be effectively reduced, and the subsequent resource utilization of fluorine resources is beneficial. DETAILED DESCRIPTION

[0049] The technical solution of the present invention is further illustrated below through specific implementation methods.

[0050] Example 1

[0051] This embodiment provides a method for recovering fluorine by using flash cooling coupled with cyclone flow in a wet phosphoric acid process.

[0052] The composition of the slurry of phosphate ore acid hydrolysis used includes: 33wt% phosphogypsum, 25wt% P2O5, 2.5wt% sulfuric acid, 1.1wt% hydrofluoric acid, wherein the solid content is 33%, the D50 particle size distribution of the solid phase is 88μm, the total content of sodium and potassium in the liquid phase is 0.6%, the P2O5 content of the liquid phase is 25%, and the F content of the liquid phase is 1.1%.

[0053] The method comprises the following steps:

[0054] (1) The 80°C phosphate ore acid-dissolved slurry is passed through a flash evaporator for cooling and crystallization. The vacuum degree of the flash evaporator is 65 kPa, the temperature difference between the inlet and outlet materials is 7°C, and the slurry at 73°C is output. The slurry temperature is adjusted to 75°C and kept warm for 2.5 hours;

[0055] (2) The slurry is subjected to cyclone separation. The feed pressure of the cyclone separation is 0.13 MPa, the feed flow rate is 4.5 m / s, the inner diameter of the cyclone tube of the cyclone separation device used is 350 mm, the inner diameter of the sand settling port is 60 mm, and the number of cyclone tubes is 4 and arranged in parallel to recover large fluorosilicate particles in the slurry.

[0056] Example 2

[0057] This embodiment provides a method for recovering fluorine by using flash cooling coupled with cyclone flow in a wet phosphoric acid process.

[0058] The composition of the slurry of phosphate ore acid hydrolysis used includes: 30wt% phosphogypsum, 35wt% P2O5, 1wt% sulfuric acid, and 2wt% hydrofluoric acid, wherein the solid content is 38%, the D50 particle size distribution of the solid phase is 70μm, the total content of sodium and potassium in the liquid phase is 0.4%, the P2O5 content of the liquid phase is 35%, and the F content of the liquid phase is 2.0%.

[0059] The method comprises the following steps:

[0060] (1) The slurry of phosphate rock acid hydrolysis at 70°C is passed through a flash evaporator for cooling and crystallization. The vacuum degree of the flash evaporator is 85 kPa, the temperature difference between the inlet and outlet materials is 4°C, and the slurry at 66°C is output. The slurry temperature is adjusted to 70°C and kept warm for 3 hours;

[0061] (2) The slurry is subjected to cyclone separation. The feed pressure of the cyclone separation is 0.08 MPa, the feed flow rate is 6.0 m / s, the inner diameter of the cyclone tube of the cyclone separation device used is 250 mm, the inner diameter of the sand settling port is 50 mm, and the number of cyclone tubes is 5 and arranged in parallel to recover large fluorosilicate particles in the slurry.

[0062] Example 3

[0063] This embodiment provides a method for recovering fluorine by using flash cooling coupled with cyclone flow in a wet phosphoric acid process.

[0064] The composition of the slurry of phosphate ore acid hydrolysis includes: 35wt% phosphogypsum, 30wt% P2O5, 5wt% sulfuric acid, and 0.1wt% hydrofluoric acid, wherein the solid content is 25%, the D50 particle size distribution of the solid phase is 100μm, the total content of sodium and potassium in the liquid phase is 0.8%, the P2O5 content of the liquid phase is 30%, and the F content of the liquid phase is 0.5%.

[0065] The method comprises the following steps:

[0066] (1) The slurry of phosphate rock acid hydrolysis at 78°C is passed through a flash evaporator for cooling and crystallization. The vacuum degree of the flash evaporator is 70 kPa, the temperature difference between the inlet and outlet materials is 8°C, and the slurry at 70°C is output. The slurry temperature is adjusted to 73°C and 80°C in turn, and the temperature is kept for 1 hour respectively, for a total of 2 hours;

[0067] (2) The slurry is subjected to cyclone separation. The feed pressure of the cyclone separation is 0.16 MPa, the feed flow rate is 3.0 m / s, the inner diameter of the cyclone tube of the cyclone separation device used is 300 mm, the inner diameter of the sand settling port is 70 mm, and the number of cyclone tubes is 3 and arranged in parallel to recover large fluorosilicate particles in the slurry.

[0068] Example 4

[0069] This embodiment provides a method for recovering fluorine by flash cooling coupled with cyclone in a wet phosphoric acid process. Compared with Embodiment 1, the temperature difference between the feed and the discharge of the flash cooling crystallization in step (1) is controlled to be 2°C, and the rest is the same as Embodiment 1.

[0070] Example 5

[0071] This embodiment provides a method for recovering fluorine by flash cooling coupled with cyclone in a wet phosphoric acid process. Compared with Embodiment 1, the temperature difference between the feed and the discharge of the flash cooling crystallization in step (1) is controlled to be 10°C, and the rest is the same as Embodiment 1.

[0072] Example 6

[0073] This embodiment provides a method for recovering fluorine by flash cooling coupled with cyclone in a wet phosphoric acid process. Compared with Embodiment 1, the vacuum degree of flash cooling crystallization in step (1) is controlled to be 50 kPa, and the rest is the same as Embodiment 1.

[0074] Example 7

[0075] This embodiment provides a method for recovering fluorine by flash cooling coupled with cyclone in a wet phosphoric acid process. Compared with Embodiment 1, the vacuum degree of the flash cooling crystallization in step (1) is controlled to be 95 kPa, and the rest is the same as Embodiment 1.

[0076] Example 8

[0077] This embodiment provides a method for recovering fluorine by flash cooling coupled with cyclone flow in a wet phosphoric acid process. Compared with Embodiment 1, after the flash cooling crystallization in step (1) is completed, the temperature is not adjusted and the heat is not kept warm. The rest is the same as Embodiment 1.

[0078] Comparative Example 1

[0079] This comparative example provides a method for recovering fluorine in a wet phosphoric acid process. Compared with Example 1, step (2) cyclone separation is not performed, and the rest is the same as Example 1.

[0080] Comparative Example 2

[0081] This comparative example provides a method for recovering fluorine in a wet phosphoric acid process. Compared with Example 1, step (1) of flash evaporation and cooling crystallization is not performed, and the rest is the same as Example 1.

[0082] Performance Characterization

[0083] The slurry after cyclone separation in the embodiment and the comparative example was filtered to obtain filter cake phosphogypsum and filtrate wet-process phosphoric acid, and the fluorine content therein was determined and the fluorine recovery rate was calculated. The results are listed in Table 1.

[0084] The fluorine content in the acid solution was measured using the method of "GB / T 21057-2007 General method for determination of fluorine content in inorganic chemical products - ion selective electrode method".

[0085] The fluorine content in phosphate rock and phosphogypsum was detected by X-ray fluorescence spectrometer.

[0086] The D50 particle size distribution of the fluorosilicate particles was tested using a fully automatic BET specific surface (area) analysis tester.

[0087] The calculation formula of fluorine recovery rate is as follows:

[0088] Fluorine recovery rate = (mass of phosphate rock * fluorine content of phosphate rock - mass of phosphogypsum * fluorine content in phosphogypsum - mass of phosphoric acid * fluorine content in phosphoric acid) / (mass of phosphate rock * fluorine content of phosphate rock) × 100%.

[0089] Table 1

[0090]

[0091]

[0092] As can be seen from Table 1, the fluorine recovery method provided by the present invention converts the fluorine in the slurry into large-particle fluorosilicate by flash cooling crystallization, and then recovers it by cyclone separation. In Examples 1-3, large particles with a D50 particle size of more than 5.9 mm can be recovered, fluorine impurities can be effectively separated and recovered, and the fluorine content in the phosphogypsum can be reduced to below 0.18%.

[0093] Compared with Example 1, in Example 4, when the inlet and outlet temperature difference of the flash cooling crystallization is too small, the amount of water removed by vacuum flash evaporation is small, the supersaturation of fluorosilicate in the slurry is low, the particle size of the generated fluorosilicate is small, and it is difficult to carry out cyclone separation and recovery, resulting in low fluorine recovery rate and high fluorine content in phosphogypsum; in Example 5, when the inlet and outlet temperature difference of the flash cooling crystallization is too large, the amount of water removed by vacuum flash evaporation is large, the slurry temperature is reduced too much, the crystallization temperature is low, the fluorosilicate crystal growth rate in the slurry is slow, the fluorosilicate particle size generated is small, and it is difficult to carry out cyclone separation and recovery, resulting in low fluorine recovery rate and high fluorine content in phosphogypsum; in Example 6, the vacuum degree of the flash cooling crystallization is too low, the vacuum flash dehydration rate is slow, the amount of water removed by vacuum flash evaporation is also small, the supersaturation of fluorosilicate in the slurry is low, and the fluorosilicate crystals are difficult to separate and recover. The fluorosilicate particles are small due to rapid growth, which makes it difficult to carry out cyclone separation and recovery, resulting in a low fluorine recovery rate and a high fluorine content in the phosphogypsum; in Example 7, the vacuum degree of flash cooling crystallization is too high, the vacuum flash dehydration rate is too fast, a large number of small crystal nuclei are formed in the fluorosilicate in the slurry, and the fluorosilicate crystals cannot grow larger, resulting in a small fluorosilicate particle size, which makes it difficult to carry out cyclone separation and recovery, resulting in a low fluorine recovery rate and a high fluorine content in the phosphogypsum; in Example 8, the slurry temperature is not adjusted or kept warm, the fluorosilicate particles obtained after flash evaporation are small, and there is a lack of a process for the particles to continue to grow, resulting in a small size of the fluorosilicate particles, and a large amount of fluorosilicate is still present in the slurry, thereby affecting the subsequent cyclone separation, resulting in a low fluorine recovery rate, and a large amount of fluorosilicate still remains in the phosphogypsum, resulting in a high fluorine content in the phosphogypsum.

[0094] In Comparative Example 1, no cyclone separation is performed, and the large-particle fluorosilicate generated enters the phosphogypsum and cannot be separated, resulting in a fluorine recovery rate of 0 and an extremely high fluorine content in the phosphogypsum; in Comparative Example 2, no flash cooling and crystallization is performed, and the fluorosilicate in the slurry cannot grow quickly to generate large-particle fluorosilicate, and can only generate a small amount of fine-particle fluorosilicate. Only a small amount of fine-particle fluorosilicate can be separated by cyclone, resulting in a low fluorine recovery rate, and a large amount of fluorosilicate still remains in the phosphogypsum, resulting in a high fluorine content in the phosphogypsum.

[0095] In summary, the method provided by the present invention separates and recovers the fluorine from the acid hydrolysis of phosphate rock into large-particle fluorosilicates through flash cooling coupled with cyclone separation. The process is simple and easy to operate, and no chemical reagents need to be added. The fluorine recovery effect is good, and the recovery rate is more than 32.4%. It can effectively reduce the fluorine content of subsequent phosphogypsum and phosphoric acid in the wet phosphoric acid process, and is conducive to the subsequent resource utilization of fluorine resources.

[0096] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for recovering fluorine by using flash cooling coupled with cyclone flow in a wet phosphoric acid process, characterized in that: The method comprises the following steps: (1) subjecting the phosphate rock acid-hydrolyzed slurry to flash evaporation, cooling and crystallization to obtain a flash evaporation slurry; (2) subjecting the flash slurry obtained in step (1) to cyclone separation to recover the fluorosilicate particles.

2. The method according to claim 1, characterized in that The solid content of the phosphate rock acid-hydrolyzed slurry is 25-38%; The D50 particle size distribution of the solid phase in the slurry of the acid-hydrolyzed phosphate rock is 70-100 μm.

3. The method according to claim 1, characterized in that In the slurry of the acid hydrolysis of the phosphate rock, the P2O5 content of the liquid phase is 25-35%; The total content of sodium and potassium in the liquid phase is 0.4-0.8%; The F content of the liquid phase is 0.5-2.0%.

4. The method according to claim 1, characterized in that: The temperature of the phosphate rock acid-decomposed slurry is 70-80°C.

5. The method according to claim 1, characterized in that The vacuum degree of the flash cooling crystallization is 65-85 kPa.

6. The method according to claim 1, characterized in that The temperature difference between the feed and the discharge of the flash cooling crystallization is 4-8°C.

7. The method according to claim 1, characterized in that After the flash evaporation cooling and crystallization, the temperature of the slurry after the flash evaporation is adjusted to 70-80° C. and kept warm for 2-3 hours.

8. The method according to claim 1, characterized in that The feed pressure of the cyclone separation is 0.08-0.16MPa; The feed flow rate of the cyclone separation is 3.0-6.0 m / s.

9. The method according to claim 1, characterized in that: The D50 particle size distribution of the fluorosilicate particles is 1-8 mm.

10. The method according to claim 1, characterized in that The method comprises the following steps: (1) subjecting the phosphate ore acid hydrolysis slurry at a temperature of 70-80° C. to flash cooling crystallization, wherein the solid content of the phosphate ore acid hydrolysis slurry is 25-38%, the D50 particle size distribution of the solid phase in the phosphate ore acid hydrolysis slurry is 70-100 μm, the P2O5 content of the liquid phase in the phosphate ore acid hydrolysis slurry is 25-35%, the total content of sodium and potassium in the liquid phase is 0.4-0.8%, and the F content of the liquid phase is 0.5-2.0%; the vacuum degree of the flash cooling crystallization is 65-85 kPa, the temperature difference between the feed and the discharge of the flash cooling crystallization is 4-8° C., and after the flash cooling crystallization is completed, the temperature of the flashed slurry is adjusted to 70-80° C. and kept warm for 2-3 hours; (2) The slurry after flash evaporation is subjected to cyclone separation, wherein the feed pressure of the cyclone separation is 0.08-0.16 MPa, the feed flow rate of the cyclone separation is 3.0-6.0 m / s, and the fluorosilicate particles are recovered after the cyclone separation, and the D50 particle size distribution of the fluorosilicate particles is 3-8 mm.

Citation Information

Patent Citations

  • Method for recycling fluorine resources in phosphate fertilizer production

    CN105776221A

  • Method of recycling phosphorus in concentrated acid residue from wet process phosphoric acid and co-producing dihydrate gypsum and sodium fluosilicate

    CN107827114A

  • Method for utilizing fluorine and potassium associated with phosphate rock

    CN110627094A

  • Fluorine extraction and scale inhibition method for dilute phosphoric acid precipitation acidolysis

    CN117699760A

  • Method for producing sodium silicofluoride from wet process phosphoric acid

    US3506394A