Method for comprehensively utilizing main associated elements in underground brine

By optimizing the extraction sequence and process flow of the main associated elements in brine, and using technologies such as hydrogen sulfide removal, oxidant iron removal, lithium adsorption, evaporation concentration, acid adjustment and chlorine oxidation, the element loss and process complexity in the existing technology are solved. problem, achieving efficient resource recycling and utilization.

CN118851218APending Publication Date: 2024-10-29INST OF MULTIPURPOSE UTILIZATION OF MINERAL RESOURCES CHINESE ACAD OF GEOLOGICAL SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410855572.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The existing technology's extraction sequence of valuable elements in brine results in the loss of some elements, the process is cumbersome, the cost is high, and efficient recycling cannot be achieved.

Method used

Through steps such as hydrogen sulfide removal, oxidant iron removal, lithium adsorption, evaporation concentration, acid adjustment, chlorine oxidation and solvent extraction, the extraction sequence and process flow of the main associated elements in brine are optimized to achieve efficient separation and recovery of elements.

Benefits of technology

It improves the recovery rate of lithium, sodium, potassium, boron, iodine, bromine and other elements, reduces resource waste and environmental pollution, reduces process costs, and maximizes the utilization of resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118851218A_ABST
    Figure CN118851218A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of salt chemical industry, and particularly discloses a method for comprehensively utilizing main associated elements in underground brine, which sequentially comprises the following steps: removing hydrogen sulfide, removing iron, extracting lithium, evaporating to prepare salt, separating potassium, precipitating boron, extracting iodine, extracting bromine, preparing boric acid and recovering residual liquid. A separation and extraction line of elements such as Li < + >, Na < + >, K < + >, B < 3 + >, I <-> and Br <-> is provided, all elements in the brine are naturally enriched along with evaporation and concentration of the brine, subsequent efficient separation and extraction of the elements are facilitated, and maximization of resource utilization is facilitated. The elements extracted by the method are high in recycling rate, and the prepared sodium chloride, potassium chloride and other products are high in quality.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of salt chemical industry, in particular to a method for comprehensive utilization of main and associated elements in underground brine. Background Art

[0002] Natural deep underground brine is rich in resources and of high quality. It is rich in sodium, potassium, lithium, bromine, iodine, boron and other high value-added elements. The content of many elements is higher than the national standard for mining grades of individual minerals, and its comprehensive utilization value is huge. In view of the comprehensive utilization of brine associated elements, after the extraction of potassium and lithium, the balance of sodium salts and the disposal of tailings and tailings are proposed to reduce resource waste and environmental pollution, so as to alleviate the pressure of resource scarcity, support national economic construction, and improve the sustainability of comprehensive extraction and utilization of underground brine.

[0003] In existing research, a comprehensive utilization method for extracting various elements from brine has been proposed. For example, the Chinese patent with publication number CN114348970A discloses a method for comprehensive utilization of complex underground brine. The method comprises the following steps: step 1: desulfurization of hydrogen; step 2: one-stage salt production; step 3: precipitation of boron and magnesium, and returning the separated precipitate to step 2; step 4: precipitation of calcium; step 5: blowing bromine and iodine; step 6: two-stage salt production; step 7: three-stage salt production, the separated salt slurry is added to condensed water for re-dissolution and then returned to step 6; step 8: precipitation of lithium; step 9: precipitation of rubidium and cesium. If the concentration of rubidium in the brine is not reached, return to step 7 to continue concentration and complete the cycle. The Chinese patent with publication number CN101691239B discloses a method for comprehensive utilization of brine. The method realizes the step-by-step orderly extraction of the main components of the brine by reasonably combining the processes of dehydrogen sulfide, magnesium precipitation, calcium precipitation and preparation of calcium carbonate, one-stage salt production, two-stage salt production to produce potassium-sodium mixed salt, flotation to extract potassium chloride, acidification to extract boron, iodine extraction, bromine extraction, rubidium and cesium extraction and preparation of rubidium chloride, cesium chloride, and lithium extraction.

[0004] However, although the above schemes can extract many valuable elements from brine, there are still problems such as serious loss of valuable elements, complicated process flow, high cost, etc., which make it impossible to achieve efficient recycling of valuable elements. The main reason is the extraction order of each element. The first extraction process leads to partial loss of the elements extracted later. In order to improve the recycling rate of valuable elements in underground brine, an efficient method for comprehensive utilization of main and associated elements in underground brine is urgently needed. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a method for comprehensive utilization of main and associated elements in underground brine, so as to at least achieve the effect of efficient separation and extraction of valuable elements.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] A method for comprehensive utilization of main and associated elements in underground brine, comprising the following steps:

[0008] S1: removing hydrogen sulfide from the underground brine, and then adding an oxidant to remove iron to obtain a purified liquid;

[0009] S2: adding the purified liquid to an adsorbent to adsorb lithium, adding dilute hydrochloric acid to desorb to obtain a desorbed liquid, concentrating the desorbed liquid to precipitate lithium, and then filtering and drying in sequence to obtain a lithium extraction mother liquor and lithium carbonate;

[0010] S3: evaporating and concentrating the lithium extraction mother liquor to a water loss rate of 7-55%, then filtering and cooling to obtain a sodium extraction mother liquor and sodium chloride;

[0011] S4: continuing to evaporate and concentrate the sodium precipitation mother liquor to a water loss rate of 55-65%, then filtering to obtain a potassium precipitation mother liquor and a potassium mixed salt, and cold decomposing the potassium mixed salt to obtain potassium chloride;

[0012] S5: adding acid to the potassium precipitation mother liquor to adjust the pH value, standing and filtering to obtain precipitated boric acid and boron precipitation mother liquor;

[0013] S6: introducing chlorine gas into the boron precipitation mother liquor for oxidation, and then performing air blowing to strip iodine to obtain elemental iodine and iodine stripping mother liquor.

[0014] S7: introducing chlorine gas into the iodine extraction mother liquor for oxidation, and then distilling the iodine extraction mother liquor to obtain elemental bromine and bromine extraction mother liquor;

[0015] S8: subjecting the bromine extraction mother liquor to solvent extraction to obtain boric acid and raffinate;

[0016] S9: recovering the raffinate.

[0017] Furthermore, the pH value of the underground brine is 6.5-6.8, the sodium ion concentration is 91.0-98.8 g / L, the potassium ion concentration is 5.2-24.2 g / L, the lithium ion concentration is 172-335 mg / L, the bromide ion concentration is 1540-1610 mg / L, the iodide ion concentration is 11-35 mg / L, and the boron ion concentration is 452-1490 mg / L.

[0018] Furthermore, in step S1, the method for removing hydrogen sulfide includes air blowing or mechanical stirring.

[0019] Furthermore, in step S1, the oxidant includes hydrogen peroxide or oxygen.

[0020] Furthermore, in step S2, the adsorbent includes at least one of aluminum-based, manganese-based and titanium-based adsorbents.

[0021] Furthermore, in step S3, the temperature of the evaporation and concentration is 106-109°C.

[0022] Furthermore, in step S5, the acid includes hydrochloric acid, acetic acid, sulfuric acid and nitric acid; preferably hydrochloric acid.

[0023] Furthermore, in step S5, the pH value is 1.5-4.5.

[0024] Furthermore, in step S6, the redox potential of the chlorine oxidation is 490-610 mv.

[0025] Furthermore, the air stripping of iodine includes: after the chlorine gas oxidizes the iodine ions in the brine into free iodine, a large amount of air or oxygen-enriched air is blown into the iodine-containing brine to blow the iodine out of the solution in the form of vapor, and then the iodine is stripped through condensation, absorption and other steps.

[0026] Furthermore, in step S7, the redox potential of the chlorine oxidation is 960-1000 mv.

[0027] Furthermore, in step S8, the solvent extraction is: extraction with 60-100% alcohol and back extraction with dilute hydrochloric acid.

[0028] Furthermore, in step S9, the method for recovering the raffinate is: concentrating, evaporating, crystallizing, and drying the raffinate in sequence to prepare calcium chloride and multi-element mixed fertilizer.

[0029] The beneficial effects of the present invention are:

[0030] 1. The present invention proposes Li + 、Na + , K + , B 3+ ,I - Br - The separation and extraction line of elements such as chlorine and brine, as the brine evaporates and concentrates, the elements in the brine are naturally enriched, which is conducive to the subsequent efficient separation and extraction of elements and the maximization of resource utilization.

[0031] 2. The sodium chloride and potassium chloride extracted by the present invention are of high quality and are suitable for the production of industrial salt and potash fertilizer, and can provide raw materials for the preparation of soda ash and caustic soda.

[0032] 3. Extract lithium by adsorption in the brine purification liquid, effectively reduce the loss of lithium caused by complicated process in comprehensive utilization of brine, and improve the recovery rate of lithium. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a process flow chart of the present invention. DETAILED DESCRIPTION

[0034] The technical solution of the present invention is further described in detail below in conjunction with the accompanying drawings, but the protection scope of the present invention is not limited to the following.

[0035] Example 1

[0036] S1: Take 10L of raw brine mined from the well, the pH value is 6.5, the density is 1.211g / ml, air is introduced into the brine and mechanically stirred at room temperature for 1-2h to remove hydrogen sulfide with the smell of rotten eggs; at the same time, add 100mL of hydrogen peroxide to the brine to oxidize and remove iron ions in the raw brine to obtain a purified liquid, and the pH value of the purified liquid is measured to be 6.5;

[0037] S2: 1000g of titanium-based adsorbent and dilute hydrochloric acid are used to selectively adsorb and desorb lithium ions from the purified liquid, and the flow rate is controlled to be 1ml / min. The desorbed liquid is concentrated to precipitate lithium, and the lithium mother liquor and lithium carbonate are obtained after filtering and drying;

[0038] S3: Evaporate and concentrate the lithium extraction mother liquor, crystallize sodium chloride at high temperature, and when the water loss rate of the brine is reduced to 40%, the boiling temperature is 106°C, and filter to obtain the sodium extraction mother liquor and sodium chloride;

[0039] S4: Continue to evaporate and concentrate the filtered sodium precipitation mother liquor, the potassium chloride concentration is 68.43 g / L, and when the evaporation water loss rate is 60%, the potassium mixed salt and the potassium precipitation mother liquor are filtered out, the potassium mixed salt is subjected to cold decomposition method, and the evaporated mother liquor is cooled to room temperature to obtain the corresponding potassium chloride product, the brine pH value is 4.5, and the density is 1.301 g / ml;

[0040] S5: adding 36% hydrochloric acid to the potassium precipitation mother liquor for acidification, adjusting the pH to 4, and allowing to stand for precipitation for 12 hours to obtain a boric acid paste, thereby preparing boric acid (partial boric acid is extracted preferentially to avoid the loss of boron due to the long process and the influence of boron on the quality of subsequent products);

[0041] S6: I in the boron mother liquor - ≥39 mg / L, Br - ≥7.7g / L. Oxidize chlorine to a potential of 500mv (detected by potentiometric titration), perform air stripping of iodine, then oxidize with chlorine to a potential of 960mv, perform distillation to extract bromine, and obtain iodine-extracting bromine mother liquor;

[0042] S7: adding 60% alcohol and dilute hydrochloric acid to the iodine-bromine extraction mother liquor to extract and back-extract to recover boric acid;

[0043] S8: Finally, the raffinate (Ca 2+ ≥110g / L) is concentrated, evaporated, crystallized and dried to prepare calcium chloride and multi-element mixed fertilizer.

[0044] Through titration detection, the single recovery rates of lithium, sodium, potassium, boron, iodine and bromine in this example are 65%, 80%, 73%, 60%, 93% and 92% respectively.

[0045] Example 2

[0046] S1: 10L of raw brine mined from underground wells was selected, and the pH value was measured to be 6.7 and the density was 1.215g / ml. Air was introduced into the brine and mechanically stirred at room temperature for 3 hours to remove hydrogen sulfide with a rotten egg smell. At the same time, 200mL of hydrogen peroxide was added to the brine to oxidize and remove iron ions in the raw brine to obtain a purified liquid, and the pH value of the purified liquid was measured to be 6.5;

[0047] S2: 1000g of titanium adsorbent and dilute hydrochloric acid are used to selectively adsorb and desorb lithium ions from the purified liquid, and the flow rate is controlled to be 0.5ml / min. The desorbed liquid is concentrated to precipitate lithium, and the lithium mother liquor and lithium carbonate are obtained after filtering and drying;

[0048] S3: Evaporate and concentrate the lithium extraction mother liquor, crystallize sodium chloride at high temperature, and when the water loss rate of the brine is evaporated to 55%, the boiling temperature is 107°C, and filter to obtain the sodium extraction mother liquor and sodium chloride;

[0049] S4: Continue to evaporate and concentrate the filtered sodium precipitation mother liquor, and the potassium chloride concentration is 85.68 g / L. When the evaporation rate is 65%, the potassium mixed salt and the potassium precipitation mother liquor are filtered out, and the potassium mixed salt is subjected to cold decomposition method and the evaporated mother liquor is cooled to room temperature to obtain the corresponding potassium chloride product. At this time, the pH value of the brine is 4.0 and the density is 1.375 g / ml;

[0050] S5: Add 36% hydrochloric acid to the potassium precipitation mother liquor for acidification, adjust the pH to 2, and let it stand for 24 hours to obtain boric acid paste, thereby preparing boric acid.

[0051] S6: I in the boron mother liquor - ≥51 mg / L, Br - ≥9.8g / L. Oxidize chlorine gas to a potential of 600mv, perform air blowing to strip iodine, then oxidize chlorine gas to a potential of 1000mv, perform distillation to strip bromine, and obtain iodine-stripping bromine mother liquor;

[0052] S7: adding 70% alcohol and dilute hydrochloric acid to the iodine-bromine extraction mother liquor for extraction and back extraction to recover boric acid;

[0053] S8: Finally, the raffinate (Ca 2+ ≥135g / L) concentration, evaporation, crystallization and drying to prepare calcium chloride and multi-element mixed fertilizer.

[0054] According to the titration method, the single yields of lithium, sodium, potassium, boron, iodine and bromine in this example are 73%, 87%, 70%, 64%, 90% and 91% respectively.

[0055] Comparative Example 1

[0056] A comprehensive utilization of brine, which differs from Example 1 in that the extraction order of the main and associated elements is different, and the specific method is as follows:

[0057] S1: Take 10L of raw brine mined from the well, the pH value is 6.5, the density is 1.211g / ml, air is introduced into the brine and mechanically stirred at room temperature for 1-2h to remove hydrogen sulfide with the smell of rotten eggs; at the same time, add 100mL of hydrogen peroxide to the brine to oxidize and remove iron ions in the raw brine to obtain a purified liquid, and the pH value of the purified liquid is measured to be 6.5;

[0058] S2: Evaporate and concentrate the purified liquid, crystallize sodium chloride at high temperature, and when the water loss rate of the brine is evaporated to 40%, the boiling temperature is 105°C, and filter to obtain the sodium precipitation mother liquor and sodium chloride;

[0059] S3: Continue to evaporate and concentrate the filtered sodium precipitation mother liquor, the potassium chloride concentration is 74.56g / L, and when the evaporation is to a water loss rate of 60%, potassium mixed salt and potassium precipitation mother liquor are filtered out, the potassium mixed salt is subjected to cold decomposition method, and the evaporated mother liquor is cooled to room temperature to obtain the corresponding potassium chloride product, the brine pH value is 4.5, and the density is 1.303g / ml;

[0060] S4: adding 36% hydrochloric acid to the potassium precipitation mother liquor to acidify it, adjusting the pH to 4, and allowing it to stand for precipitation for 12 hours to obtain boric acid paste, thereby preparing boric acid;

[0061] S5: I in the boron mother liquor - ≥39 mg / L, Br - ≥7.7g / L. Oxidize chlorine to a potential of 500mv (detected by potentiometric titration), perform air stripping of iodine, then oxidize with chlorine to a potential of 960mv, perform distillation to extract bromine, and obtain iodine-extracting bromine mother liquor;

[0062] S6: Using 1000g of titanium-based adsorbent and dilute hydrochloric acid to selectively adsorb and desorb lithium ions in the iodine-bromine extraction mother liquor, the flow rate is controlled to be 1ml / min, the desorbed liquid is concentrated to precipitate lithium, and after filtering and drying, the lithium extraction mother liquor and lithium carbonate are obtained;

[0063] S7: adding 60% alcohol and dilute hydrochloric acid to the iodine-bromine extraction mother liquor to extract and back-extract to recover boric acid;

[0064] S8: Finally, the raffinate (Ca 2+ ≥112g / L) is concentrated, evaporated, crystallized and dried to prepare calcium chloride and multi-element mixed fertilizer.

[0065] According to the titration method, the single recovery rates of lithium, sodium, potassium, boron, iodine and bromine in this example are 55%, 79%, 69%, 56%, 83% and 81% respectively.

[0066] Comparative Example 2

[0067] A comprehensive utilization of brine, which differs from Example 2 in that the extraction order of the main and associated elements is different, and the specific method is as follows:

[0068] S1: 10L of raw brine mined from underground wells was selected, and the pH value was measured to be 6.7 and the density was 1.215g / ml. Air was introduced into the brine and mechanically stirred at room temperature for 3 hours to remove hydrogen sulfide with a rotten egg smell. At the same time, 200mL of hydrogen peroxide was added to the brine to oxidize and remove iron ions in the raw brine to obtain a purified liquid, and the pH value of the purified liquid was measured to be 6.5;

[0069] S2: adding 36% hydrochloric acid to the purified liquid to acidify it, adjusting the pH to 4, and letting it stand for 12 hours to obtain boric acid paste, thereby preparing boric acid;

[0070] S3: I in the boron mother liquor - ≥11 mg / L, Br - ≥1.54g / L. Oxidize chlorine to a potential of 500mv (detected by potentiometric titration), perform air blowing to strip iodine, then oxidize with chlorine to a potential of 960mv, perform distillation to strip bromine, and obtain iodine-stripping bromine mother liquor;

[0071] S4: using 1000g of titanium-based adsorbent and dilute hydrochloric acid to selectively adsorb and desorb lithium ions in the iodine-bromine extraction mother liquor, the flow rate is controlled to be 1ml / min, the desorbed liquid is concentrated to precipitate lithium, and the lithium extraction mother liquor and lithium carbonate are obtained after filtering and drying;

[0072] S5: evaporating and concentrating the lithium extraction mother liquor, crystallizing sodium chloride at high temperature, and filtering to obtain the sodium extraction mother liquor and sodium chloride when the water loss rate of the brine is reduced to 55% and the boiling temperature is 107°C;

[0073] S6: Continue to evaporate and concentrate the filtered sodium precipitation mother liquor, and the potassium chloride concentration is 85.68 g / L. When the evaporation rate is 65%, the potassium mixed salt and the potassium precipitation mother liquor are filtered out, and the potassium mixed salt is subjected to cold decomposition method and the evaporated mother liquor is cooled to room temperature to obtain the corresponding potassium chloride product. At this time, the pH value of the brine is 4.0 and the density is 1.371 g / ml;

[0074] S7: adding 60% alcohol and dilute hydrochloric acid to the iodine-bromine extraction mother liquor to extract and back-extract to recover boric acid;

[0075] S8: Finally, the raffinate (Ca 2+ ≥129g / L) is concentrated, evaporated, crystallized and dried to prepare calcium chloride and multi-element mixed fertilizer.

[0076] Through titration detection, the single recovery rates of lithium, sodium, potassium, boron, iodine and bromine in this example are 49%, 86%, 66%, 58%, 64% and 67%, respectively.

[0077] The above is only a preferred embodiment of the present invention. It should be understood that the present invention is not limited to the form disclosed herein, and should not be regarded as excluding other embodiments, but can be used in various other combinations, modifications and environments, and can be modified within the scope of the concept described herein through the above teachings or the technology or knowledge of the relevant field. The changes and modifications made by those skilled in the art shall not deviate from the spirit and scope of the present invention, and shall be within the scope of protection of the claims attached to the present invention.

Claims

1. A method for comprehensive utilization of main and associated elements in underground brine, characterized in that: The following steps are involved: S1: removing hydrogen sulfide from the underground brine, and then adding an oxidant to remove iron to obtain a purified liquid; S2: adding the purified liquid to an adsorbent to adsorb lithium, adding dilute hydrochloric acid to desorb to obtain a desorbed liquid, concentrating the desorbed liquid to precipitate lithium, and then filtering and drying in sequence to obtain a lithium extraction mother liquor and lithium carbonate; S3: evaporating and concentrating the lithium extraction mother liquor to a water loss rate of 7-55%, then filtering and cooling to obtain a sodium extraction mother liquor and sodium chloride; S4: continuing to evaporate and concentrate the sodium precipitation mother liquor to a water loss rate of 55-65%, then filtering to obtain a potassium precipitation mother liquor and a potassium mixed salt, and cold decomposing the potassium mixed salt to obtain potassium chloride; S5: adding acid to the potassium precipitation mother liquor to adjust the pH value, standing and filtering to obtain precipitated boric acid and boron precipitation mother liquor; S6: introducing chlorine gas into the boron precipitation mother liquor for oxidation, and then performing air blowing to strip iodine to obtain elemental iodine and iodine stripping mother liquor; S7: introducing chlorine gas into the iodine extraction mother liquor for oxidation, and then distilling the iodine extraction mother liquor to obtain elemental bromine and bromine extraction mother liquor; S8: subjecting the bromine extraction mother liquor to solvent extraction to obtain boric acid and raffinate; S9: recovering the raffinate.

2. The method according to claim 1, characterized in that: In step S1, the method for removing hydrogen sulfide includes air blowing or mechanical stirring.

3. The method according to claim 1, characterized in that: In step S1, the oxidant includes hydrogen peroxide or oxygen.

4. The method according to claim 1, characterized in that: In step S2, the adsorbent includes at least one of aluminum-based, manganese-based and titanium-based adsorbents.

5. The method according to claim 1, characterized in that: In step S3, the temperature of the evaporation and concentration is 106-109°C.

6. The method according to claim 1, characterized in that: In step S5, the pH value is 1.5-4.

5.

7. The method according to claim 1, characterized in that: In step S6, the redox potential of the chlorine oxidation is 490-610 mv.

8. The method according to claim 1, characterized in that: In step S7, the redox potential of the chlorine oxidation is 960-1000 mv.

9. The method according to claim 1, characterized in that: In step S8, the solvent extraction is: extraction with 60-100% alcohol and back extraction with dilute hydrochloric acid.

10. The method according to claim 1, characterized in that In step S9, the method for recovering the raffinate is: concentrating, evaporating, crystallizing and drying the raffinate in sequence to prepare calcium chloride and multi-element mixed fertilizer.