Method for producing spacing capillary tubes through assembling and wire drawing process
Through the assembly and drawing process, the problem of difficulty in controlling the inner and outer diameters of the high borosilicate spacing capillary mother tube is solved, and the flexible change of the inner hole spacing and cost reduction are achieved, which is suitable for the production of diversified products.
Patent Information
- Application Number
- CN202411111481.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-10-29
AI Technical Summary
The existing high borosilicate spacing capillary production process has material characteristics limitations, which makes it difficult to meet the requirements for the inner and outer diameter and straightness of the mother tube. The processing is difficult and costly. The inner hole spacing size is single, which cannot meet the needs of diversified products.
Using the assembly drawing process, the glass wool, central tube and outer tube are prepared, polished and pickled, assembled into a mother tube, and the outer tube and the central tube are fused through a vacuum device at high temperature to control the size of the wool. Achieve flexible changes in inner hole spacing.
The processing cost is reduced, the wool length is increased, the material stocking requirements are reduced, the inner hole spacing can be quickly changed and diversified production is achieved, and the finished product cost is reduced.
Smart Images

Figure CN118851558A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of production and processing of spaced capillaries, and in particular to a method for producing spaced capillaries through an assembly wire drawing process. Background Art
[0002] High borosilicate spacing capillaries are important basic materials for passive devices such as pigtails, collimators, WDMs, circulators, isolators, etc. because their expansion coefficient, light transmittance, and glue compatibility all meet the requirements of passive products.
[0003] At present, the manufacturing process of high borosilicate spacing capillaries is divided into the following two conventional paths: 1. A mother tube with an outer diameter of 30-35mm and an inner diameter of 3.5-4mm is manufactured by the continuous melting method, and then a semi-finished wool wire (outer diameter 1.8mm or 1.0mm) is drawn by a two-step method, and the wool wire is post-processed to make a finished product; 2. A solid mother rod with an outer diameter of 30-35mm is used, and an inner hole is made by mechanical punching, and then a semi-finished wool wire is drawn by a two-step method, and the wool wire is post-processed to make a finished product.
[0004] The above two paths for making high borosilicate spacing capillaries have the following problems: the first path is limited by domestic technology and material characteristics. The inner and outer diameters, straightness, roundness, etc. of the mother tubes currently produced cannot meet the requirements of direct tower pulling. They need to be repaired by secondary mechanical or chemical methods to meet the requirements of tower pulling. However, because the straightness and size of the inner hole are too small, the processing is very difficult. At present, there are very few machinery factories that can perform processing. Moreover, the spacing size between the two inner holes of the mother tube made by the continuous melting method is relatively simple, and each processing is made according to the amount of several tons. Changing the spacing size requires modifying the configuration of the furnace, which is very costly. At present, there are many specifications for the spacing between the two holes of the spacing capillary. If the mother tube is prepared by this method, the materials required to be stocked are quite large, and the investment cost is very high. It is not suitable for the current situation of most manufacturers. The second path requires first processing a very small inner hole on the solid mother rod, which is technically difficult, so there are very few manufacturers that can process it. Moreover, due to the characteristics of the glass material, the length that can be processed is also relatively short. The length of the mother tube produced in the end is very short, and the number of hair strands drawn at one time is relatively small, so the corresponding production cost of the finished product is very high. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a method for producing spaced capillaries through an assembly wire drawing process.
[0006] The technical solution of the present invention to solve the above technical problem is as follows: A method for producing a spacing capillary by an assembly wire drawing process, comprising the following steps:
[0007] S1. Material preparation and pretreatment: prepare glass wool, center tube and outer tube, and according to the inner hole spacing requirements of the spacing capillary products to be produced, first grind the fitting side of each center tube with a center hole and a flat elliptical cross section, then pickle the glass wool, center tube and outer tube, and dry them for use after pickling;
[0008] S2. Mother tube assembly: stack and assemble the spare glass wool and the central tube on the fixture, first stack the glass wool layer by layer, and place two central tubes after stacking to a set height, and then stack the glass wool layer by layer upwards, and after stacking, a central body approximately cylindrical is obtained, and the central body is bundled into a whole by high temperature resistant wire, and inserted into the spare outer sleeve to form an assembled mother tube;
[0009] S3. Mother tube drawing: fix the upper tail of the assembled mother tube on the vacuum device and keep the center hole of the central tube connected to the atmosphere. After raising the furnace temperature, extend the lower head of the assembled mother tube into the furnace and naturally shrink and taper the lower tail of the assembled mother tube through the furnace temperature to seal it. Then start the vacuum device to extract the air between the outer sleeve and the central tube. At the same time, due to the atmospheric pressure and furnace temperature, the outer sleeve, glass wool and central tube are squeezed and fused into a whole. Finally, the subsequent wire drawing process is carried out according to the one-piece mother tube.
[0010] On the basis of the above technical solutions, the present invention can also make the following further specific options.
[0011] Specifically, grinding the fitting side surfaces of each center tube in S1 refers to placing the center tube on a surface grinder for grinding.
[0012] Specifically, there are at least two fixtures in S2, which are clamped from the front end and the rear end of the center body respectively. The fixture includes a lower half clamp and an upper half clamp. When stacking, the glass wool is first stacked layer by layer in the semicircular groove of the lower clamp. Stacking to a set height means that when the two center tubes are placed in a fitted manner above the stacked glass wool, the fitted sides of the two center tubes pass through the center of the semicircular groove in a horizontal direction.
[0013] Specifically, the glass wool is solid wool, and at least two specifications of glass wool, one thick and one thin, are prepared to fully fill the cylindrical cavity formed by the two semicircular grooves of the fixture being buckled together.
[0014] Specifically, the glass wool has two specifications: coarse wool and fine wool. The diameter of the coarse wool is 2.0-5.2 mm, and the diameter of the fine wool is 0.5-1.9 mm.
[0015] Specifically, the high temperature resistant wire in S2 is a metal wire that can withstand 950°C.
[0016] Specifically, the vacuum pump in S3 is a device that can generate a pressure of -1 bar.
[0017] Specifically, the outer sleeve is a round tube with an outer diameter of 40-60mm and an inner diameter of 30-50mm. The center tube is an elliptical tube with a circular center hole in the center, with a major axis of 29-49mm, a minor axis of 5-15mm, and a center hole diameter of 2.2-6.2mm.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The present invention is assembled by an outer sleeve, two central tubes and a certain amount of filling glass wool. After the upper tower is cone-dropped, vacuuming begins. Under a high temperature environment, all the assembled materials are fused together. Because of the low expansion coefficient of high borosilicate, the equivalent outer diameter and inner diameter of the mother tube after assembly can be converted by the equal volume method, thereby achieving the purpose of controlling the size of the wool. The inner hole spacing of the two central tubes can be machined with different margins by a simple surface grinder, so that the spacing size of the inner holes can be quickly changed according to the specific product specification requirements, thereby achieving the purpose of producing wool with different spacings of inner holes.
[0020] Since the assembly materials used in the present invention are relatively conventional, the cost is relatively low, and the mechanical processing method is also very common, with basically no processing difficulty, so it is easy to operate. In addition, the mother tubes that are assembled equivalently are larger than the mother tubes used in traditional wire drawing, and the number of semi-finished hair fibers drawn at one time will be more than that of the traditional method, and the production cost of semi-finished hair fibers of the same length is greatly reduced compared to the production of the two paths mentioned above. The present invention has the advantages of low processing cost, sufficient materials, and the inner hole spacing of the target product can be quickly changed. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 An axonometric diagram after a center body is formed on a fixture in a mother tube assembly step in a method for producing a spaced capillary tube by an assembly wire drawing process provided by the present invention;
[0022] Figure 2 for Figure 1 A schematic diagram showing an enlarged view of one end of the centrosome;
[0023] Figure 3 The invention provides a method for producing spaced capillaries by an assembly wire drawing process, in which a schematic diagram of the end face of one end of the assembled mother tube is obtained in the mother tube assembly step.
[0024] In the accompanying drawings, the components represented by the reference numerals are listed as follows:
[0025] 10. Glass wool; 20. Center tube; 30. Outer sleeve; 40. Fixture; 101. Coarse wool; 102. Fine wool; 201. Center hole. DETAILED DESCRIPTION
[0026] The principles and features of the present invention are described below in conjunction with the accompanying drawings and specific embodiments. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.
[0027] To avoid redundant description, a unified explanation is given here. The materials used in the following embodiments of the present invention are relatively mature products on the market, and the product stability is very good. The center tube is also called a flat capillary tube, which has a center hole channel. In actual production, according to the specific specifications of the target spacing capillary tube, the center tube needs to be ground on one side in advance using a conventional surface grinder. By controlling the difference in the grinding amount, the spacing size of the inner holes of the two center tubes is changed, thereby producing hair threads with a specified spacing size.
[0028] like Figures 1 to 3 As shown, the present invention provides a method for producing a spacing capillary by an assembly wire drawing process, which comprises the following steps:
[0029] S1. Material preparation and pretreatment: prepare glass wool 10, center tube 20 and outer tube 30. According to the inner hole spacing requirements of the spacing capillary products to be produced, first grind the fitting side of each center tube 20 having a center hole 201 and a flat elliptical cross section. Figure 1 The distance between the center holes on the two center tubes can be controlled by controlling the degree of grinding on the sides of the two center tubes that fit each other. After grinding, the glass wool 10, the center tube 20 and the outer sleeve 30 are pickled and dried for later use. The specific operation of pickling and the solution used are well known to those skilled in the art and will not be described in detail here.
[0030] S2. Mother tube assembly: The spare glass wool 10 and the center tube 20 are stacked and assembled on the fixture 40. The glass wool 10 is first stacked layer by layer. After the stacking reaches a set height, two center tubes 20 are placed. Stacking to a set height means that when the two center tubes 20 are placed on top of the stacked glass wool 10, the fitted sides of the two center tubes 20 pass through the center of the semicircular groove in the horizontal direction. After the two center tubes are placed in a fitted manner, the glass wool 10 is stacked layer by layer on the upper surface of the upper center tube. After the stacking is completed, a center body approximately cylindrical is obtained. The center body is bundled into a whole by high-temperature resistant silk thread, and is inserted into the spare outer sleeve 30 to form an assembled mother tube. The glass wool 10 is solid wool, and at least two specifications of glass wool 10, one thick and one thin, are prepared to fully fill the cylindrical cavity formed after the two semicircular grooves of the fixture 40 are buckled together. In this embodiment, Figure 3 As shown, the glass wool 10 has two specifications: thick wool 101 and thin wool 102. The diameter of the thick wool 101 is about 2 mm, and the diameter of the thin wool 102 is about 0.8 mm.
[0031] S3. Mother tube drawing: fix the upper end of the assembled mother tube to the vacuum pump (vacuum pump) and keep the central hole 201 of the central tube 20 connected to the atmosphere. After raising the furnace temperature, extend the lower end of the assembled mother tube into the furnace and naturally shrink the cone by the furnace temperature to seal the lower end of the assembled mother tube. Then start the vacuum pump to remove the air between the outer sleeve 30 and the central tube 20. At the same time, due to the atmospheric pressure and furnace temperature, the outer sleeve 30, glass wool 10 and central tube 20 are squeezed and fused into a whole. Finally, the subsequent drawing process is carried out according to the integrated mother tube. The furnace temperature control and specific drawing operation details are well known to those skilled in the art and will not be expanded here.
[0032] It should be noted that the thick hair and thin hair can be formed by two-step drawing using a solid rod, or commercially available products can be directly purchased. In addition, the present invention is not limited to using only hair of two specifications of thickness and thinness, and more hairs of different thickness and thinness can also be prepared. In order to ensure that when vacuuming, only the air between the outer sleeve and the central tube is evacuated, and the air in the inner hole of the central tube is not extracted, there will be extension tubes at both ends of the central tube, and the extension tubes can ensure that the inner hole of the central tube is connected to the atmosphere, so that the inner hole of the central tube is atmospheric pressure, and the outer sleeve is atmospheric pressure. After the gas is evacuated between the central tube and the hair, the two atmospheric pressures squeeze each other to ensure the full fusion of the assembly materials.
[0033] In one embodiment of the present invention, grinding the contact side surface of each central tube 20 in S1 refers to placing the central tube 20 on a surface grinder for grinding. Since the central tube itself is flat, it can be placed on the surface grinder in a balanced manner without being deliberately clamped and fixed.
[0034] In one embodiment of the present invention, Figure 1 As shown, there are at least two jigs 40 in S2, which are clamped from the front end and the rear end of the central body respectively. The jig 40 includes a lower clamp and an upper clamp. When stacking, first stack the glass wool 10 layer by layer in the semicircular groove of the lower clamp, and first put the material in the groove of the lower clamp, and stack it up layer by layer. After stacking about half, lock the upper and lower clamps with screws, and then stuff the remaining filling material into the jig, and finally stuff the fine wool, fill as much as possible, ensure that the gap is filled as much as possible, and avoid looseness inside.
[0035] In the above embodiment, the high temperature resistant wire in S2 is preferably nickel wire, and it is preferably fixed at both ends of the central body and does not need to be removed after fixation. After wire drawing is completed, the two ends are removed and only the effective part in the middle is retained for use.
[0036] It should be noted that the central body obtained when the mother tube of the present invention is assembled basically presents a regular hexagonal shape (close to a cylinder), which is easy to operate during assembly, and at the same time ensures the consistency of the gap around the outer sleeve, so that the central body will not have a large offset between the outer sleeve during melting and shrinking, ensuring the concentricity of the inner hole of the hair and the outer circle (referring to the concentricity of the center of the outer sleeve and the midpoint of the line connecting the two inner diameters). The outer circle of the hair will theoretically present a certain hexagon during melting and shrinking, but because the outer sleeve 1 is relatively thick, the surface tension of the hair is acted upon at high temperature, and the gap is filled as much as possible by solid fine hair, the deformation is relatively small, and under multiple effects, the roundness of the hair is guaranteed to a certain extent.
[0037] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for producing a spaced capillary by an assembly wire drawing process, characterized in that: The steps include: S1. Material preparation and pretreatment: prepare glass wool, center tube and outer tube, and according to the inner hole spacing requirements of the spacing capillary products to be produced, first grind the fitting side of each center tube with a center hole and a flat elliptical cross section, then pickle the glass wool, center tube and outer tube, and dry them for use after pickling; S2. Mother tube assembly: stack and assemble the spare glass wool and the central tube on the fixture, first stack the glass wool layer by layer, and place two central tubes after stacking to a set height, and then stack the glass wool layer by layer upwards, and after stacking, a central body approximately cylindrical is obtained, and the central body is bundled into a whole by high temperature resistant wire, and inserted into the spare outer sleeve to form an assembled mother tube; S3. Mother tube drawing: fix the upper tail of the assembled mother tube on the vacuum device and keep the center hole of the central tube connected to the atmosphere. After raising the furnace temperature, extend the lower head of the assembled mother tube into the furnace and naturally shrink and taper the lower tail of the assembled mother tube through the furnace temperature to seal it. Then start the vacuum device to extract the air between the outer sleeve and the central tube. At the same time, due to the atmospheric pressure and furnace temperature, the outer sleeve, glass wool and central tube are squeezed and fused into a whole. Finally, the subsequent wire drawing process is carried out according to the one-piece mother tube.
2. A method for producing spaced capillaries by assembly wire drawing process according to claim 1, characterized in that: The grinding process for the fitting side surface of each center tube in S1 refers to placing the center tube on a surface grinder for grinding.
3. A method for producing a spaced capillary by an assembly wire drawing process according to claim 1, characterized in that There are at least two fixtures in S2, which clamp from the front end and the rear end of the center body respectively. The fixture includes a lower half clamp and an upper half clamp. When stacking, the glass wool is first stacked layer by layer in the semicircular groove of the lower clamp. Stacking to a set height means that when the two center tubes are placed in a close relationship above the stacked glass wool, the fitted sides of the two center tubes pass through the center of the semicircular groove in a horizontal direction.
4. A method for producing spaced capillaries by assembly wire drawing process according to claim 3, characterized in that: The glass wool is solid wool, and at least two specifications of glass wool, one thick and one thin, are prepared to fully fill the cylindrical cavity formed by the two semicircular grooves of the fixture being buckled together.
5. A method for producing spaced capillaries by assembly wire drawing process according to claim 4, characterized in that: The glass wool has two specifications: coarse wool and fine wool. The diameter of the coarse wool is 2.0-5.2 mm, and the diameter of the fine wool is 0.5-1.9 mm.
6. A method for producing spaced capillaries by assembly wire drawing process according to claim 1, characterized in that: The high temperature resistant wire in S2 is a metal wire that can withstand 950°C.
7. A method for producing spaced capillaries by assembly wire drawing process according to claim 1, characterized in that: The vacuum device in S3 is a device that can generate a pressure of -1 bar.
8. A method for producing spaced capillaries by assembly wire drawing process according to any one of claims 1 to 7, characterized in that: The outer sleeve is a round tube with an outer diameter of 40-60mm and an inner diameter of 30-50mm. The center tube is an elliptical tube with a circular center hole in the center, with a major axis of 29-49mm, a minor axis of 5-15mm, and a center hole diameter of 2.2-6.2mm.