A kind of polyaryletherketone coating and preparation method thereof
By designing the branched structure PAEK resin and using hydrophilic structure capping agent, the problems of high shrinkage rate of polyaryletherketone coatings and poor dispersion of resin particles are solved, and the molding shrinkage rate, improved adhesion and dispersion are achieved. Sexual effect.
Patent Information
- Application Number
- CN202411349340.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-26
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2044-09-26
AI Technical Summary
The existing polyaryletherketone coatings have problems such as high molding shrinkage and poor dispersion of resin particles, which affect the durability and reliability of the coating.
By designing the branched structure PAEK resin and using hydrophilic structure (sulfonic acid) blocking agent, the compatibility of resin particles and coating system is improved, the molding shrinkage rate is reduced, and the PAEK micropowder particles are improved in the aqueous coating system. Dispersibility.
It achieves the reduction of the molding shrinkage rate of PAEK resin, improves the adhesion and uniformity of the coating, reduces the amount of dispersant, and improves the performance of the coating.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention belongs to the field of polyaryletherketone materials, in particular to a water-soluble polyaryletherketone coating and a preparation method thereof. Background Art
[0002] Polyaryletherketoneketone (PAEK) is a type of high-performance thermoplastic resin with excellent mechanical properties, processing properties, chemical resistance, impact resistance, radiation resistance, self-lubrication, etc. Common polyaryletherketones are linear structures, including polyetheretherketone (PEEK), polyetherketone (PEK), polyetheretherketoneketone (PEEKK), etc., which are widely used in high-end equipment and daily necessities.
[0003] Polyaryletherketone coatings are composed of base resin, additives, and solvents. The construction process is relatively simple, usually air spraying, and the curing temperature is 380°C, which makes them very practical in industrial applications. Due to the high temperature resistance of these coatings, they have broad application prospects in aerospace, national defense, chemical industry, petroleum, and machinery. At present, polyarylether coatings have been applied in the fields of petroleum (such as pipelines, valve covers, etc.), machinery (valve plates, impellers, etc.), medical treatment (sampling needles, etc.), kitchen and bathroom (non-stick cookware, etc.). However, with the increase in application scenarios, new requirements for the performance of coatings are constantly emerging.
[0004] Taking the most widely used PEEK as an example, its molding shrinkage is about 1%. High molding shrinkage will cause higher internal stress inside the coating during the curing process, which may affect the durability and reliability of the coating. Therefore, reducing the molding shrinkage of the base resin helps to improve the adhesion of the coating to the substrate, and also helps to maintain the uniformity of the coating, especially in the scenario of large-area spraying. This effect is more obvious.
[0005] In addition, existing PAEK coatings have problems such as poor dispersion of resin particles, which need to be solved urgently. Summary of the invention
[0006] In order to solve the above problems and obtain a PAEK material with a smaller molding shrinkage and a coating with a better coating effect, the present invention provides a polyaryletherketone coating. The technical solution of the present invention is as follows:
[0007] A method for preparing a water-soluble PAEK coating comprises the following steps:
[0008] (1) Synthesis of PAEK
[0009] Bisphenol structure monomer and difluorobenzene structure ketone monomer are used as raw materials, diphenyl sulfone is used as solvent, alkali metal carbonate is used as catalyst, 1,3,5-tris(4-(4-fluorobenzoyl)phenoxy)benzene (CAS No.: 473816-20-5) is used as cross-linking agent, sulfonated 4,4'-difluorobenzophenone is used as end-capping agent, and nucleophilic polycondensation reaction is carried out. The specific preparation process includes the following steps:
[0010] 1) Putting raw materials including bisphenol structure monomer, difluorobenzene structure ketone monomer and alkali metal carbonate into a reaction container, wherein the molar number of bisphenol structure monomer is higher than the molar number of difluorobenzene structure ketone monomer, adding molten diphenyl sulfone solvent under the condition of keeping argon gas flowing at 50-100 ml / min;
[0011] 2) Continue heating and stirring until the raw materials in the reaction container are fully mixed, raise the temperature of the reaction container to 200-220°C, and stir at a constant temperature for 60 minutes; then raise the temperature to 260-290°C, and stir at a constant temperature for 60 minutes; then raise the temperature to 310-330°C, and stir at a constant temperature for 60-120 minutes. During this process, keep argon gas flowing into the reaction container at 50-100 ml / min;
[0012] 3) Dissolve the cross-linking agent 1,3,5-tris(4-(4-fluorobenzoyl)phenoxy)benzene in diphenyl sulfone at a concentration of 10%, add it dropwise into the reaction system within 5-10 minutes, stir at a constant temperature of 310-330°C for 30-60 minutes, and keep argon gas flowing into the reaction vessel at 50-100 ml / min during the process;
[0013] 4) Add the end-capping agent sulfonated 4,4'-difluorobenzophenone into the reaction system, stir at a constant temperature of 310-330°C for 30-60 minutes, and keep argon gas flowing into the reaction vessel at a rate of 50-100 ml / min during the process;
[0014] 5) Finally, the reaction product is poured into cold water to cool and solidify, then crushed, refluxed with ethanol and boiled in water to remove impurities, and dried to obtain the PAEK product.
[0015] Preferably, the molar number of the bisphenol structure monomer is 1.01 to 1.20 times the molar number of the bisfluorobenzene structure ketone monomer.
[0016] Preferably, the dosage of the cross-linking agent 1,3,5-tris(4-(4-fluorobenzoyl)phenoxy)benzene is calculated by the following formula:
[0017] The molar amount (1,3,5-tris(4-(4-fluorobenzoyl)phenoxy)benzene) is ≤ 1 / 3*[molar amount (bisphenol structure monomer) - molar amount (bisfluorobenzene structure ketone monomer)]; the molar amount of the end-capping agent sulfonated 4,4'-difluorobenzophenone is 3-4 times that of the cross-linking agent.
[0018] Preferably, the bisphenol structural monomer is one or more of hydroquinone, biphenol, and 4,4'-dihydroxybenzophenone.
[0019] Preferably, the ketone monomer of the difluorobenzene structure is one or more of 4,4'-difluorobenzophenone, 4,4'-difluorotriphenyldione, and 4,4'-difluorobiphenyldione.
[0020] Preferably, in the method for preparing the meta-phenyl polyaryletherketone, the alkali metal carbonate is preferably one or both of sodium carbonate and potassium carbonate.
[0021] (2) Preparation of PAEK dispersion:
[0022] The particles treated in step (1) are crushed to 90-100 microns by a high-speed crusher, and the above-mentioned micro-powder particles are dispersed in chloroform and methanol, and the mixed liquid is fully stirred at a high speed for mixing and dispersion.
[0023] The material ratio of the above reaction is as follows:
[0024] In parts by weight, PAEK powder: 10-15 parts, chloroform: 60-80 parts, methanol: 10-15 parts.
[0025] (3) Preparation of aqueous solution:
[0026] Sodium dodecylbenzene sulfonate, polyacrylamide, N-methylpyrrolidone and pure water are mixed in proportion; the PAEK dispersion prepared in step (2) is fully mixed with the mixture; chloroform and methanol are removed by distillation at 70-75° C. under stirring conditions to obtain a coating product.
[0027] The material ratio of the above reaction is as follows:
[0028] In parts by weight, the PAEK dispersion prepared in step (2) is 45-55 parts; sodium dodecylbenzene sulfonate is 0.5-1 parts; polyacrylamide is 1-2 parts; N-methylpyrrolidone is 3-5 parts; and pure water is 45-55 parts.
[0029] Preferably, in parts by weight, the amount of sodium dodecylbenzene sulfonate added in step (3) is 0.8 parts.
[0030] (4) Painting and curing
[0031] The substrate device is cleaned, degreased, and sandblasted before spraying. After spraying, the device is left at room temperature for 5-10 minutes, then placed in a 120℃ oven for 10-20 minutes, then the oven is heated to 400℃, kept at 400℃ for 5-10 minutes, and finally the device is taken out and naturally cooled to room temperature.
[0032] Preferably, in step (4), "raising the temperature of the oven to 400° C." is changed to "placing the device in an oven maintained at a constant temperature of 400° C."
[0033] Compared with the prior art, the present invention has the following beneficial effects:
[0034] The use of a capping agent with a hydrophilic structure (sulfonic acid group) improves the compatibility of PAEK resin particles with the coating system.
[0035] The branched PAEK resin was designed and synthesized, which not only reduced the regularity and crystallinity of PAEK from the molecular chain structure, thereby reducing the molding shrinkage; but also introduced more hydrophilic structures (sulfonic acid groups) at the ends of the molecular chains through the branched structure, further improving the effect of the end-capping agent.
[0036] The amount and addition method of the cross-linking agent can ensure the full formation of the branched structure and avoid the network structure as much as possible, thus ensuring that the product has good film-forming properties.
[0037] Since the PAEK prepared in this application has better affinity for water-based systems, compared with traditional PEEK water-based coatings, less dispersant can be added during the coating preparation process to achieve a good dispersion effect. As is known to all, commonly used dispersants are small molecule surfactants, and the presence of these additives in the paint film will reduce the performance of the paint film to a certain extent.
[0038] Compared with traditional PEEK water-based paint films, PAEK resin with low molding shrinkage has less stress on the bonding surface with the substrate during the cooling process after sintering, and the bond is stronger. DETAILED DESCRIPTION
[0039] The present invention is further described in detail through specific embodiments. Example 1
[0040] (1) Synthesis of PAEK:
[0041] 1) 1.02 mol of hydroquinone, 1 mol of 4,4'-difluorobenzophenone and 1.2 mol of sodium carbonate were placed in a 1.5 L reaction vessel, and 661 g of molten diphenyl sulfone solvent was added while argon was introduced at a rate of 10 ml / min;
[0042] 2) Continue heating and stirring until the raw materials in the reaction container are fully mixed, raise the temperature of the reaction container to 200°C, and stir at this constant temperature for 60 minutes; then raise the temperature to 285°C, and stir at this constant temperature for 60 minutes; then raise the temperature to 310°C, and stir at this constant temperature for 90 minutes. During this process, keep argon gas flowing into the reaction container at 10 ml / min;
[0043] 3) 0.005 mol of the cross-linking agent 1,3,5-tris(4-(4-fluorobenzoyl)phenoxy)benzene was dissolved in diphenyl sulfone at a concentration of 10%, and added dropwise into the reaction system within 10 minutes. The mixture was stirred at a constant temperature of 310°C for 60 minutes. During the process, argon was kept flowing into the reaction vessel at a rate of 10 ml / min.
[0044] 4) Add 0.015 mol of sulfonated 4,4'-difluorobenzophenone as a capping agent into the reaction system and stir at 310°C for 60 min. During the process, argon gas is passed into the reaction vessel at a rate of 10 ml / min.
[0045] 5) Finally, the reaction product is poured into cold water, cooled and solidified, and then crushed, and impurities are removed by ethanol reflux and water boiling, and dried to obtain the PAEK product. The PAEK product is subjected to DSC analysis, and its glass transition temperature and melting point are shown in Table 1.
[0046] (2) Preparation of PAEK dispersion:
[0047] The particles treated in step (1) are crushed to 300 meshes by a high-speed crusher. 13 parts of the above-mentioned micro-powder particles are dispersed in 75 parts of chloroform and 12 parts of methanol, and the mixed solution is fully stirred at a high speed to mix and disperse.
[0048] (3) Preparation of aqueous solution:
[0049] 0.6 parts of sodium dodecylbenzene sulfonate, 1.2 parts of polyacrylamide, 4 parts of N-methylpyrrolidone and 48.2 parts of pure water were mixed; 46 parts of the PAEK dispersion prepared in step (2) were fully mixed therewith, and chloroform and methanol were distilled off at 75° C. under stirring to obtain a coating product.
[0050] (4) Painting and curing:
[0051] After cleaning, degreasing, and sandblasting, the substrate device was sprayed. After spraying, the device was left at room temperature for 10 minutes, then placed in a 120°C oven for 20 minutes, and then placed in a 400°C oven for 10 minutes. Finally, the device was taken out and naturally cooled to room temperature. The state of the cured paint film was observed and recorded, and its thickness and adhesion were measured (GB / T 9286-2021). The data is shown in Table 1. Example 2
[0052] (1) Synthesis of PAEK:
[0053] 1) 1.17 mol of 4,4'-dihydroxybenzophenone, 1 mol of 4,4'-difluorobenzophenone, 1.2 mol of sodium carbonate and 0.1 mol of potassium carbonate were placed in a 1.5 L reaction vessel, and 937.6 g of molten diphenyl sulfone solvent was added while argon was introduced at a rate of 10 ml / min;
[0054] 2) Continue heating and stirring until the raw materials in the reaction container are fully mixed, raise the temperature of the reaction container to 220°C, and stir at this constant temperature for 60 minutes; then raise the temperature to 260°C, and stir at this constant temperature for 60 minutes; then raise the temperature to 330°C, and stir at this constant temperature for 90 minutes. During this process, keep argon gas flowing into the reaction container at 10 ml / min;
[0055] 3) 0.04 mol of the cross-linking agent 1,3,5-tris(4-(4-fluorobenzoyl)phenoxy)benzene was dissolved in diphenyl sulfone at a concentration of 10%, and added dropwise into the reaction system within 10 min. The mixture was stirred at a constant temperature of 310°C for 60 min. During the process, argon was kept flowing into the reaction vessel at a rate of 10 ml / min.
[0056] 4) Add 0.16 mol of sulfonated 4,4'-difluorobenzophenone as a capping agent into the reaction system and stir at 310°C for 60 min. During the process, argon gas is passed into the reaction vessel at a rate of 10 ml / min.
[0057] 5) Finally, the reaction product is poured into cold water, cooled and solidified, and then crushed, and impurities are removed by ethanol reflux and water boiling, and dried to obtain the PAEK product. The PAEK product is subjected to DSC analysis, and its glass transition temperature and melting point are shown in Table 1.
[0058] (2) Preparation of PAEK dispersion:
[0059] The particles treated in step (1) are crushed to 300 meshes by a high-speed crusher. 13 parts of the above-mentioned micro-powder particles are dispersed in 75 parts of chloroform and 12 parts of methanol, and the mixed solution is fully stirred at a high speed to mix and disperse.
[0060] (3) Preparation of aqueous solution:
[0061] 0.8 parts of sodium dodecylbenzene sulfonate, 1.2 parts of polyacrylamide, 4 parts of N-methylpyrrolidone and 48 parts of pure water were mixed; 46 parts of the PAEK dispersion prepared in step (2) were fully mixed therewith, and chloroform and methanol were distilled off at 75° C. under stirring to obtain a coating product.
[0062] (4) Painting and curing:
[0063] After cleaning, degreasing, and sandblasting, the substrate device was sprayed. After spraying, the device was left at room temperature for 10 minutes, then placed in a 120°C oven for 20 minutes, and then placed in a 400°C oven for 10 minutes. Finally, the device was taken out and naturally cooled to room temperature. The state of the cured paint film was observed and recorded, and its thickness and adhesion were measured (GB / T 9286-2021). The data is shown in Table 1. Example 3
[0064] (1) Synthesis of PAEK:
[0065] 1) 0.8 mol of hydroquinone, 0.4 mol of biphenol, 1 mol of 4,4'-difluorobenzophenone and 1.4 mol of sodium carbonate were placed in a 1.5 L reaction vessel, and 761.5 g of molten diphenyl sulfone solvent was added while argon was introduced at a rate of 10 ml / min;
[0066] 2) Continue heating and stirring until the raw materials in the reaction container are fully mixed, raise the temperature of the reaction container to 200°C, and stir at this constant temperature for 60 minutes; then raise the temperature to 285°C, and stir at this constant temperature for 60 minutes; then raise the temperature to 310°C, and stir at this constant temperature for 90 minutes. During this process, keep argon gas flowing into the reaction container at 10 ml / min;
[0067] 3) 0.06 mol of the cross-linking agent 1,3,5-tris(4-(4-fluorobenzoyl)phenoxy)benzene was dissolved in diphenyl sulfone at a concentration of 10%, and added dropwise into the reaction system within 10 min. The mixture was stirred at a constant temperature of 310°C for 60 min. During the process, argon was kept flowing into the reaction vessel at a rate of 10 ml / min.
[0068] 4) Add 0.24 mol of sulfonated 4,4'-difluorobenzophenone as a capping agent into the reaction system and stir at 310°C for 60 min. During the process, argon gas is passed into the reaction vessel at a rate of 10 ml / min.
[0069] 5) Finally, the reaction product is poured into cold water, cooled and solidified, and then crushed, and impurities are removed by ethanol reflux and water boiling, and dried to obtain the PAEK product. The PAEK product is subjected to DSC analysis, and its glass transition temperature and melting point are shown in Table 1.
[0070] (2) Preparation of PAEK dispersion:
[0071] The particles treated in step (1) are crushed to 300 meshes by a high-speed crusher. 13 parts of the above-mentioned micro-powder particles are dispersed in 75 parts of chloroform and 12 parts of methanol, and the mixed solution is fully stirred at a high speed to mix and disperse.
[0072] (3) Preparation of aqueous solution:
[0073] 0.7 parts of sodium dodecylbenzene sulfonate, 1.2 parts of polyacrylamide, 4 parts of N-methylpyrrolidone and 46.1 parts of pure water were mixed; 48 parts of the PAEK dispersion prepared in step (2) were fully mixed therewith, and chloroform and methanol were distilled off at 75° C. under stirring to obtain a coating product.
[0074] (4) Painting and curing:
[0075] After cleaning, degreasing, and sandblasting, the substrate device was sprayed. After spraying, the device was left at room temperature for 10 minutes, then placed in a 120°C oven for 20 minutes, and then placed in a 400°C oven for 10 minutes. Finally, the device was taken out and naturally cooled to room temperature. The state of the cured paint film was observed and recorded, and its thickness and adhesion were measured (GB / T 9286-2021). The data is shown in Table 1. Example 4
[0076] (1) Synthesis of PAEK:
[0077] 1) 1.02 mol of hydroquinone, 0.95 mol of 4,4'-difluorobenzophenone, 0.05 mol of 4,4'-difluorotriphenyldione, and 1.2 mol of sodium carbonate were placed in a 1.5 L reaction vessel, and 671.4 g of molten diphenyl sulfone solvent was added while maintaining the flow of argon at 10 ml / min;
[0078] 2) Continue heating and stirring until the raw materials in the reaction container are fully mixed, raise the temperature of the reaction container to 200°C, and stir at this constant temperature for 60 minutes; then raise the temperature to 285°C, and stir at this constant temperature for 60 minutes; then raise the temperature to 310°C, and stir at this constant temperature for 90 minutes. During this process, keep argon gas flowing into the reaction container at 10 ml / min;
[0079] 3) 0.005 mol of the cross-linking agent 1,3,5-tris(4-(4-fluorobenzoyl)phenoxy)benzene was dissolved in diphenyl sulfone at a concentration of 10%, and added dropwise into the reaction system within 10 minutes. The mixture was stirred at a constant temperature of 310°C for 60 minutes. During the process, argon was kept flowing into the reaction vessel at a rate of 10 ml / min.
[0080] 4) Add 0.02 mol of sulfonated 4,4'-difluorobenzophenone as a capping agent into the reaction system and stir at 310°C for 60 min. During the process, argon gas is passed into the reaction vessel at a rate of 10 ml / min.
[0081] 5) Finally, the reaction product is poured into cold water, cooled and solidified, and then crushed, and impurities are removed by ethanol reflux and water boiling, and dried to obtain the PAEK product. The PAEK product is subjected to DSC analysis, and its glass transition temperature and melting point are shown in Table 1.
[0082] (2) Preparation of PAEK dispersion:
[0083] The particles treated in step (1) are crushed to 300 meshes by a high-speed crusher. 13 parts of the above-mentioned micro-powder particles are dispersed in 75 parts of chloroform and 12 parts of methanol, and the mixed solution is fully stirred at a high speed to mix and disperse.
[0084] (3) Preparation of aqueous solution:
[0085] 0.8 parts of sodium dodecylbenzene sulfonate, 1.4 parts of polyacrylamide, 4 parts of N-methylpyrrolidone and 48 parts of pure water were mixed; 45.8 parts of the PAEK dispersion prepared in step (2) were fully mixed therewith, and chloroform and methanol were distilled off at 75° C. under stirring to obtain a coating product.
[0086] (4) Painting and curing:
[0087] After cleaning, degreasing, and sandblasting, the substrate device was sprayed. After spraying, the device was left at room temperature for 10 minutes, then placed in a 120°C oven for 20 minutes, and then placed in a 400°C oven for 10 minutes. Finally, the device was taken out and naturally cooled to room temperature. The state of the cured paint film was observed and recorded, and its thickness and adhesion were measured (GB / T 9286-2021). The data is shown in Table 1. Example 5
[0088] (1) Synthesis of PAEK:
[0089] 1) 1.02 mol of hydroquinone, 0.95 mol of 4,4'-difluorobenzophenone, 0.05 mol of 4,4'-difluorobiphenyldione, and 1.2 mol of sodium carbonate were placed in a 1.5 L reaction vessel, and 679 g of molten diphenyl sulfone solvent was added while maintaining the flow of argon at 10 ml / min;
[0090] 2) Continue heating and stirring until the raw materials in the reaction container are fully mixed, raise the temperature of the reaction container to 200°C, and stir at this constant temperature for 60 minutes; then raise the temperature to 285°C, and stir at this constant temperature for 60 minutes; then raise the temperature to 310°C, and stir at this constant temperature for 90 minutes. During this process, keep argon gas flowing into the reaction container at 10 ml / min;
[0091] 3) 0.005 mol of the cross-linking agent 1,3,5-tris(4-(4-fluorobenzoyl)phenoxy)benzene was dissolved in diphenyl sulfone at a concentration of 10%, and added dropwise into the reaction system within 10 minutes. The mixture was stirred at a constant temperature of 310°C for 60 minutes. During the process, argon was kept flowing into the reaction vessel at a rate of 10 ml / min.
[0092] 4) Add 0.02 mol of sulfonated 4,4'-difluorobenzophenone as a capping agent into the reaction system and stir at 310°C for 60 min. During the process, argon gas is passed into the reaction vessel at a rate of 10 ml / min.
[0093] 5) Finally, the reaction product is poured into cold water, cooled and solidified, and then crushed, and impurities are removed by ethanol reflux and water boiling, and dried to obtain the PAEK product. The PAEK product is subjected to DSC analysis, and its glass transition temperature and melting point are shown in Table 1.
[0094] (2) Preparation of PAEK dispersion:
[0095] The particles treated in step (1) are crushed to 300 meshes by a high-speed crusher. 13 parts of the above-mentioned micro-powder particles are dispersed in 75 parts of chloroform and 12 parts of methanol, and the mixed solution is fully stirred at a high speed to mix and disperse.
[0096] (3) Preparation of aqueous solution:
[0097] 0.9 parts of sodium dodecylbenzene sulfonate, 1.2 parts of polyacrylamide, 4 parts of N-methylpyrrolidone and 48 parts of pure water were mixed; 45.9 parts of the PAEK dispersion prepared in step (2) were fully mixed therewith, and chloroform and methanol were distilled off at 75° C. under stirring to obtain a coating product.
[0098] (4) Painting and curing:
[0099] After cleaning, degreasing, and sandblasting, the substrate device was sprayed. After spraying, the device was left at room temperature for 10 minutes, then placed in a 120°C oven for 20 minutes, and then placed in a 400°C oven for 10 minutes. Finally, the device was taken out and naturally cooled to room temperature. The state of the cured paint film was observed and recorded, and its thickness and adhesion were measured (GB / T 9286-2021). The data is shown in Table 1. Comparative Example 1
[0100] (1) Synthesis of PAEK:
[0101] 1) 1.02 mol of hydroquinone, 1 mol of 4,4'-difluorobenzophenone and 1.2 mol of sodium carbonate were placed in a 1.5 L reaction vessel, and 661 g of molten diphenyl sulfone solvent was added while argon was introduced at a rate of 10 ml / min;
[0102] 2) Continue heating and stirring until the raw materials in the reaction container are fully mixed, raise the temperature of the reaction container to 200°C, and stir at this constant temperature for 60 minutes; then raise the temperature to 285°C, and stir at this constant temperature for 60 minutes; then raise the temperature to 310°C, and stir at this constant temperature for 90 minutes. During this process, keep argon gas flowing into the reaction container at 10 ml / min;
[0103] 3) Add 0.04 mol of sulfonated 4,4'-difluorobenzophenone as a capping agent into the reaction system and stir at 310°C for 60 min. During this process, argon gas is passed into the reaction vessel at a rate of 10 ml / min.
[0104] 4) Finally, the reaction product is poured into cold water, cooled and solidified, and then crushed, and impurities are removed by ethanol reflux and water boiling, and dried to obtain the PAEK product. The PAEK product is subjected to DSC analysis, and its glass transition temperature and melting point are shown in Table 1.
[0105] (2) Preparation of PAEK dispersion:
[0106] The particles treated in step (1) are crushed to 300 meshes by a high-speed crusher. 13 parts of the above-mentioned micro-powder particles are dispersed in 75 parts of chloroform and 12 parts of methanol, and the mixed solution is fully stirred at a high speed to mix and disperse.
[0107] (3) Preparation of aqueous solution:
[0108] 0.6 parts of sodium dodecylbenzene sulfonate, 1.2 parts of polyacrylamide, 4 parts of N-methylpyrrolidone and 48.2 parts of pure water were mixed; 46 parts of the PAEK dispersion prepared in step (2) were fully mixed therewith, and chloroform and methanol were distilled off at 75° C. under stirring to obtain a coating product.
[0109] (4) Painting and curing:
[0110] After cleaning, degreasing, and sandblasting, the substrate device was sprayed. After spraying, the device was left at room temperature for 10 minutes, then placed in a 120°C oven for 20 minutes, and then placed in a 400°C oven for 10 minutes. Finally, the device was taken out and naturally cooled to room temperature. The state of the cured paint film was observed and recorded, and its thickness and adhesion were measured (GB / T 9286-2021). The data is shown in Table 1. Comparative Example 2
[0111] (1) Synthesis of PAEK:
[0112] 1) 1.02 mol of hydroquinone, 1 mol of 4,4'-difluorobenzophenone and 1.2 mol of sodium carbonate were placed in a 1.5 L reaction vessel, and 661 g of molten diphenyl sulfone solvent was added while argon was introduced at a rate of 10 ml / min;
[0113] 2) Continue heating and stirring until the raw materials in the reaction container are fully mixed, raise the temperature of the reaction container to 200°C, and stir at this constant temperature for 60 minutes; then raise the temperature to 285°C, and stir at this constant temperature for 60 minutes; then raise the temperature to 310°C, and stir at this constant temperature for 90 minutes. During this process, keep argon gas flowing into the reaction container at 10 ml / min;
[0114] 3) 0.005 mol of the cross-linking agent 1,3,5-tris(4-(4-fluorobenzoyl)phenoxy)benzene was dissolved in diphenyl sulfone at a concentration of 10%, and added dropwise into the reaction system within 10 minutes. The mixture was stirred at a constant temperature of 310°C for 60 minutes. During the process, argon was kept flowing into the reaction vessel at a rate of 10 ml / min.
[0115] 4) Add 0.015 mol of the end-capping agent 4,4'-difluorobenzophenone into the reaction system and stir at 310°C for 60 min. During the process, argon gas is passed into the reaction vessel at a rate of 10 ml / min.
[0116] 5) Finally, the reaction product is poured into cold water, cooled and solidified, and then crushed, and impurities are removed by ethanol reflux and water boiling, and dried to obtain the PAEK product. The PAEK product is subjected to DSC analysis, and its glass transition temperature and melting point are shown in Table 1.
[0117] (2) Preparation of PAEK dispersion:
[0118] The particles treated in step (1) are crushed to 300 meshes by a high-speed crusher. 13 parts of the above-mentioned micro-powder particles are dispersed in 75 parts of chloroform and 12 parts of methanol, and the mixed solution is fully stirred at a high speed to mix and disperse.
[0119] (3) Preparation of aqueous solution:
[0120] 0.6 parts of sodium dodecylbenzene sulfonate, 1.2 parts of polyacrylamide, 4 parts of N-methylpyrrolidone and 48.2 parts of pure water were mixed; 46 parts of the PAEK dispersion prepared in step (2) were fully mixed therewith, and chloroform and methanol were distilled off at 75° C. under stirring to obtain a coating product.
[0121] (4) Painting and curing:
[0122] After cleaning, degreasing, and sandblasting, the substrate device was sprayed. After spraying, the device was left at room temperature for 10 minutes, then placed in a 120°C oven for 20 minutes, and then placed in a 400°C oven for 10 minutes. Finally, the device was taken out and naturally cooled to room temperature. The state of the cured paint film was observed and recorded, and its thickness and adhesion were measured (GB / T 9286-2021). The data is shown in Table 1.
[0123] Table 1
[0124]
[0125] By comparing the film state and film adhesion of Example 1 with that of Comparative Example 1, it can be clearly found that the PAEK coating in Example 1 has better adhesion. The glass transition temperature of the synthesized PAEK resin in Comparative Example 1 is slightly higher than that of the synthesized PAEK resin in Example 1, which is due to the lower regularity of the molecular chain of the branched structure than that of the linear structure.
[0126] Comparative Example 2 does not use a capping agent with a hydrophilic structure (sulfonic acid group), and the amount of dispersant sodium dodecylbenzene sulfonate used is the same as that of Example 1. Comparing the paint film state and paint film adhesion of Example 1 and Comparative Example 2, it can be clearly found that PAEK micropowder particles without hydrophilic groups are difficult to disperse well in the paint, which directly leads to pitting of the paint film. This uneven dispersion also directly affects the adhesion of the paint film.
[0127] In summary, this application reduces the crystallinity of PAEK resin and increases the number of molecular chain end groups by constructing a branched structure; improves the dispersibility of PAEK micropowder particles in water-based coating systems by modifying the end groups with hydrophilic groups; and by using highly hydrophilic PAEK micropowder particles, the dispersion effect of PAEK in the coating can be maintained under the condition of low dispersant dosage, thereby achieving the purpose of reducing the amount of dispersant (low molecular weight additive). The above effects are superimposed to obtain a polyaryletherketone coating with low molding shrinkage, high adhesion, and good dispersion of PAEK micropowder particles.
Claims
1. A method for preparing a polyaryletherketone coating, characterized in that: The steps include: (1) Synthesis of PAEK: Bisphenol structure monomer and difluorobenzene structure ketone monomer are used as raw materials, diphenyl sulfone is used as solvent, alkali metal carbonate is used as catalyst, 1,3,5-tris(4-(4-fluorobenzoyl)phenoxy)benzene is used as cross-linking agent, sulfonated 4,4'-difluorobenzophenone is used as end-capping agent, and nucleophilic polycondensation reaction is carried out. The specific preparation process includes the following steps: 1) Putting raw materials including bisphenol structure monomer, difluorobenzene structure ketone monomer and alkali metal carbonate into a reaction container, wherein the molar number of bisphenol structure monomer is higher than the molar number of difluorobenzene structure ketone monomer, adding molten diphenyl sulfone solvent under the condition of keeping argon gas flowing at 50-100 ml / min; 2) Continue heating and stirring until the raw materials in the reaction container are fully mixed, raise the temperature of the reaction container to 200-220°C, and stir at a constant temperature for 60 minutes; then raise the temperature to 260-290°C, and stir at a constant temperature for 60 minutes; then raise the temperature to 310-330°C, and stir at a constant temperature for 60-120 minutes. During this process, keep argon gas flowing into the reaction container at 50-100 ml / min; 3) Dissolve the cross-linking agent 1,3,5-tris(4-(4-fluorobenzoyl)phenoxy)benzene in diphenyl sulfone at a concentration of 10%, add it dropwise into the reaction system within 5-10 minutes, stir at a constant temperature of 310-330°C for 30-60 minutes, and keep argon gas flowing into the reaction vessel at 50-100 ml / min during the process; 4) Add the end-capping agent sulfonated 4,4'-difluorobenzophenone into the reaction system, stir at a constant temperature of 310-330°C for 30-60 minutes, and keep argon gas flowing into the reaction vessel at a rate of 50-100 ml / min during the process; 5) Finally, the reaction product is poured into cold water and cooled and solidified, then crushed, refluxed with ethanol and boiled in water to remove impurities, and dried to obtain the PAEK product; (2) Preparation of PAEK dispersion: The particles treated in step (1) are crushed into 90-100 microns by a high-speed crusher, and the above-mentioned micro-powder particles are dispersed in chloroform and methanol, and the mixed solution is fully stirred at a high speed for mixing and dispersion; The material ratio of the above reaction is as follows: In parts by weight, PAEK powder: 10-15 parts, chloroform: 60-80 parts, methanol: 10-15 parts; (3) Preparation of aqueous solution: Sodium dodecylbenzene sulfonate, polyacrylamide, N-methylpyrrolidone and pure water are mixed in proportion; the PAEK dispersion prepared in step (2) is fully mixed with the mixture; chloroform and methanol are removed by distillation at 70-75° C. under stirring conditions to obtain a coating product; The material ratio of the above reaction is as follows: In parts by weight, the PAEK dispersion prepared in step (2): 45-55 parts; sodium dodecylbenzene sulfonate: 0.5-1 parts; polyacrylamide: 1-2 parts; N-methylpyrrolidone: 3-5 parts; pure water: 45-55 parts; (4) Painting and curing: The substrate device is cleaned, degreased, and sandblasted before spraying. After spraying, the device is left at room temperature for 5-10 minutes, then placed in a 120℃ oven for 10-20 minutes, then the oven is heated to 400℃, kept at 400℃ for 5-10 minutes, and finally the device is taken out and naturally cooled to room temperature.
2. The method for preparing a polyaryletherketone coating according to claim 1, characterized in that: The molar number of the bisphenol structure monomer is 1.01 to 1.20 times the molar number of the ketone monomer of the difluorobenzene structure.
3. The method for preparing a polyaryletherketone coating according to claim 1, characterized in that: The dosage of the cross-linking agent 1,3,5-tris(4-(4-fluorobenzoyl)phenoxy)benzene is calculated by the following formula: The molar amount of 1,3,5-tris(4-(4-fluorobenzoyl)phenoxy)benzene is ≤1 / 3*(the molar amount of the bisphenol structure monomer-the molar amount of the ketone monomer of the difluorobenzene structure); The molar amount of the end-capping agent sulfonated 4,4'-difluorobenzophenone added is 3-4 times that of the cross-linking agent.
4. The method for preparing a polyaryletherketone coating according to claim 1, characterized in that: The bisphenol structural monomer is one or more of hydroquinone, biphenol and 4,4'-dihydroxybenzophenone.
5. The method for preparing a polyaryletherketone coating according to claim 1, characterized in that: The ketone monomer with a difluorobenzene structure is one or more of 4,4'-difluorobenzophenone, 4,4'-difluorotriphenyldione and 4,4'-difluorobiphenyldione.
6. The method for preparing a polyaryletherketone coating according to claim 1, characterized in that: The alkali metal carbonate is one or both of sodium carbonate and potassium carbonate.
7. The method for preparing a polyaryletherketone coating according to claim 1, characterized in that: In parts by weight, the amount of sodium dodecylbenzene sulfonate added in step (3) is 0.8 parts.
8. A polyaryletherketone coating, characterized in that: The polyaryletherketone coating is prepared by the preparation method of the polyaryletherketone coating according to claim 1.
Citation Information
Patent Citations
Bis(tetraphenylmethane)-substituted terminated monomer, preparation method and application in preparation of terminated-type polyether sulfone material and post-sulfonation treatment
CN105646174A
Sulfonated polyaryl ether ketone (SFPAEK) ion exchange membrane preparation method and application
CN107394240A