Adhesive glue and preparation method thereof

By preparing an adhesive with a modulus controlled at 30-50Mpa, the problem of mismatched modulus of the existing adhesive is solved, the accuracy and performance of the optical fiber loop and the gyroscope are improved, and the requirements of the optical fiber loop production process are met. Require.

CN118852995APending Publication Date: 2024-10-29CHONGQING MITT TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410838677.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-26
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

The modulus of existing adhesives is too low or too high, making it difficult to match the production performance of optical fiber loops, resulting in changes in the accuracy of fiber optic gyroscopes and affecting optical performance.

Method used

An adhesive formula is used, including polyurethane modified acrylic adhesive, epoxy acrylate, hydroxyethyl methacrylate, photoinitiator and di-o-chlorodiphenylamine methane, and is prepared through steps such as distillation and vacuum stirring. Control the Young's modulus within the range of 30-50Mpa to meet the technological requirements of the optical fiber loop.

Benefits of technology

It achieves a moderate Young's modulus range of 30-50Mpa, avoids deformation caused by low modulus and applied stress caused by high modulus, meets the accuracy and performance requirements of fiber optic rings and gyroscopes, and improves production efficiency and yield. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_3
    Figure SMS_3
Patent Text Reader

Abstract

The present invention discloses an adhesive glue and a preparation method thereof, and the adhesive glue is characterized by comprising the following components by weight: 20-30 parts of a polyurethane modified acrylic acid adhesive; 70 to 80 parts of epoxy acrylate; 0.3 to 0.9 part of hydroxyethyl methylacrylate; 0.1 to 0.3 part of bis (o-chlorodiphenylamine) methane; 0.1 to 0.3 part of a photoinitiator; and 0.1 to 0.3 part of polyethoxy siloxane. The adhesive provided by the invention has the advantages of moderate modulus and capability of being matched with the production performance requirement of the fiber loop.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to an adhesive and a preparation method thereof. Background Art

[0002] At present, the adhesive for optical fiber rings is the key material for filling the medium between turns in the production process of optical fiber rings. It plays a role in fixing the winding state of the optical fiber and reducing the impact of vibration and temperature changes on the performance of the optical fiber ring, thereby improving the stability of the optical fiber ring, and further playing a favorable role in improving the performance accuracy of the optical fiber gyroscope. While the adhesive plays the role of fixing the optical fiber ring, it also has an important influence on the winding process and gluing process of the optical fiber ring. Its performance determines the winding efficiency and filling quality in the production process, and even the yield rate of the entire product.

[0003] Currently, commonly used adhesives include UV-cured polyacrylic resins, heat-cured epoxy resins, and modified silicone types. Most of these types are designed with low modulus (generally less than 5Mpa) to optimize the stress distribution of the optical fiber ring and minimize the adverse effects on optical properties.

[0004] However, as the market demands higher stability for fiber optic loops, low modulus adhesives are prone to deformation in skeleton-free fiber optic loops due to their low hardness, thus changing the stress distribution of the fiber optic loops and causing changes in the accuracy of the fiber optic gyroscope. In addition, since adhesives will shrink to varying degrees during the curing process or when the temperature rises or falls, these shrinkages will produce stress on the fiber optic loops. Therefore, adhesives with too high a modulus (such as >100Mpa) will produce excessive external stress on the fiber optic loops and affect their optical properties. Therefore, it is necessary to develop an adhesive with a moderate modulus (controlled within the range of 30-50Mpa) that can match the production process and performance of the fiber optic loops, which is of great significance to improving the accuracy of the fiber optic loops and gyroscopes. Summary of the invention

[0005] The invention provides an adhesive which solves the problem that the modulus of the existing adhesive is too low or too high and does not match the production performance of the optical fiber ring.

[0006] In order to achieve the above object, the scheme of the present invention is: an adhesive, characterized in that it comprises the following components in parts by weight:

[0007]

[0008] Preferably, the photoinitiator is of TPO type.

[0009] The present invention also discloses a preparation method, which comprises the following steps:

[0010] S10, heating dichlorodiphenylamine to boiling point, distilling, cooling and testing the water content, and setting aside after passing; heating polyethoxysiloxane to boiling point, distilling, cooling and testing the water content, and setting aside after passing;

[0011] S20, first weigh the polyurethane modified acrylic adhesive and epoxy acrylate in proportion, put them into a mixer and stir them under vacuum; then add hydroxyethyl methacrylate and di-o-chlorodiphenylamine obtained in step S10 in sequence and stir; then add a photoinitiator and the polyethoxysiloxane obtained in step S10 and stir;

[0012] S30, turning on the vacuum, gradually increasing the vacuum degree, and performing a defoaming process until there are no bubbles;

[0013] S40, putting the mixture into a container.

[0014] Furthermore, in the above step S10, the o-chlorodiphenylamine methane is distilled for 8-12 hours.

[0015] Furthermore, in the above step S10, the polyethoxysiloxane treatment is performed for 1-3 hours.

[0016] Furthermore, in the above step S20, the stirring technical requirements for the polyurethane modified acrylic adhesive and epoxy acrylate are: temperature 70° C., vacuum, stirring speed 10-50 rpm, and stirring time 2-4 hours.

[0017] Furthermore, in the above step S20, a photoinitiator and the polyethoxysiloxane obtained in step S10 are added and stirred for 20-40 minutes.

[0018] Furthermore, in the above step S20, hydroxyethyl methacrylate and di-o-chlorodiphenylamine obtained in step S10 are added in sequence and then stirred for 8-15 minutes.

[0019] Furthermore, the container is a black container.

[0020] Furthermore, the defoaming treatment time in the above step S30 is 8-12 minutes.

[0021] Beneficial effects of the present invention:

[0022] First, the adhesive of the present invention can control its Young's modulus between 30-50Mpa when used for bonding optical fiber loops, and has moderate performance, which can avoid the deformation of low-modulus adhesives due to low hardness, thereby changing the stress distribution of the optical fiber loop and changing the accuracy of the optical fiber gyroscope; at the same time, the excessively high modulus will not generate a large external stress on the optical fiber loop and affect its performance;

[0023] Second, the viscosity, refractive index, and curing conditions of the adhesive of the present invention all meet the process requirements of the optical fiber ring, and can exactly match the production performance requirements of the optical fiber ring;

[0024] Third, the adhesive of the present invention is very suitable for the preparation of optical fiber rings and optical fiber gyroscopes, can meet the technical requirements of the optical fiber ring production process, and can improve the performance of optical fiber rings and optical fiber gyroscopes. DETAILED DESCRIPTION

[0025] The experimental methods in the following examples are conventional methods unless otherwise specified. The raw materials involved in the following examples are common commercial products and can be purchased from the market unless otherwise specified.

[0026] The present invention will be further described below in conjunction with embodiments:

[0027] Embodiment 1: An adhesive comprising the following components in parts by weight:

[0028]

[0029] As in this embodiment, the polyurethane modified acrylic adhesive (a known material) can be model WU-A-60, purchased from Guangzhou Huina New Material Technology Co., Ltd.

[0030] As in this embodiment, the photoinitiator can be a TPO type purchased from I GM (IGM) of the Netherlands or IGM (Anqing) Technology Development Co., Ltd.

[0031] As in this embodiment, the epoxy acrylate can be 6233-1, which is purchased from Changxing Chemical Industry (China) Co., Ltd.

[0032] The adhesive preparation method of this embodiment includes the following steps:

[0033] S10, heating dichlorodiphenylamine to boiling point, distilling, cooling and testing the water content, and setting aside after passing; heating polyethoxysiloxane to boiling point, distilling, cooling and testing the water content, and setting aside after passing;

[0034] S20, first weigh the polyurethane modified acrylic adhesive and epoxy acrylate in proportion, put them into a mixer and stir them under vacuum; then add hydroxyethyl methacrylate and di-o-chlorodiphenylamine obtained in step S10 in sequence and stir; then add a photoinitiator and the polyethoxysiloxane obtained in step S10 and stir;

[0035] S30, turning on the vacuum, gradually increasing the vacuum degree, and performing a defoaming process until there are no bubbles;

[0036] S40, putting the mixture into a container for use in producing optical fiber rings.

[0037] In the above step S10, the o-chlorodiphenylamine methane is distilled for 10 hours.

[0038] In the above step S10, the polyethoxysiloxane treatment is performed for 2 hours.

[0039] In the above step S20, the stirring technical requirements of the polyurethane modified acrylic adhesive and epoxy acrylate are: temperature 70° C., vacuum, stirring speed 40 rpm, and stirring time 3 hours.

[0040] In the above step S20, a photoinitiator and the polyethoxysiloxane obtained in step S10 are added and stirred for 30 minutes.

[0041] In the above step S20, hydroxyethyl methacrylate and di-o-chlorodiphenylamine obtained in step S10 are added in sequence and then stirred for 10 minutes.

[0042] Wherein, the container is a black container.

[0043] The defoaming treatment time in the above step S30 is 10 minutes.

[0044] The main performance parameters of the adhesive obtained in this embodiment 1 according to the above preparation method are as follows (Table 1):

[0045]

[0046] Embodiment 2: This embodiment differs from Embodiment 1 in that:

[0047]

[0048] Specifically, the preparation method is exactly the same as that of Example 1.

[0049] The main performance parameters of the adhesive product obtained in Example 2 are as follows (Table 2):

[0050]

[0051] Embodiment 3: This embodiment differs from Embodiment 1 in that:

[0052]

[0053] Specifically, the preparation method is exactly the same as that of Example 1.

[0054] The main performance parameters of the adhesive product obtained in Example 3 are as follows (Table 3):

[0055]

[0056] It can be seen from the above three parameter tables that the Young's modulus of the product of this embodiment is within the optimal range of 30-50Mpa, which not only avoids the deformation of low-modulus adhesive due to its low hardness (lower than 15HD), thereby changing the stress distribution of the optical fiber ring and changing the accuracy of the optical fiber gyroscope; at the same time, the modulus is not too high (greater than 100Mpa) which will produce a large external stress on the optical fiber ring and affect its performance.

[0057] In addition, the viscosity (25°C) of the product of this embodiment is between 5200-5350 cPs, the refractive index (23°C) is between 1.12-1.16, and its curing conditions and other parameters all meet the process requirements and can exactly match the performance requirements of the fiber ring production.

[0058] The adhesive is very suitable for the preparation of optical fiber rings and optical fiber gyroscopes, can meet the technical requirements of the optical fiber ring production process, and can improve the performance of the optical fiber rings and optical fiber gyroscopes.

[0059] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. An adhesive, characterized in that , by weight, including the following components: Polyurethane modified acrylic adhesive 20-30 parts Epoxy acrylate 70-80 parts Hydroxyethyl methacrylate 0.3-0.9 parts 0.1-0.3 parts of di-o-chlorodiphenylamine Photoinitiator 0.1-0.3 parts Polyethoxysiloxane 0.1-0.3 parts.

2. An adhesive according to claim 1, characterized in that: The photoinitiator adopts TPO type.

3. A preparation method comprising the following steps: S10, heating dichlorodiphenylamine to boiling point, distilling, cooling and testing the water content, and setting aside after passing; heating polyethoxysiloxane to boiling point, distilling, cooling and testing the water content, and setting aside after passing; S20, first weigh the polyurethane modified acrylic adhesive and epoxy acrylate in proportion, put them into a mixer and stir them under vacuum; then add hydroxyethyl methacrylate and di-o-chlorodiphenylamine obtained in step S10 in sequence and stir; then add a photoinitiator and the polyethoxysiloxane obtained in step S10 and stir; S30, turning on the vacuum, gradually increasing the vacuum degree, and performing a defoaming process until there are no bubbles; S40, putting the mixture into a container.

4. An adhesive according to claim 3, characterized in that: In step S10, the o-chlorodiphenylamine methane is distilled for 8-12 hours.

5. An adhesive according to claim 3 or 4, characterized in that: In step S10, the polyethoxysiloxane is treated for 1-3 hours.

6. An adhesive according to any one of claims 3 to 5, characterized in that: In step S20, the stirring technical requirements of the polyurethane modified acrylic adhesive and epoxy acrylate are: Temperature 60-80°C, vacuum, stirring speed 10-50 rpm, stirring time 2-4 hours.

7. An adhesive according to any one of claims 3 to 6, characterized in that: In step S20, a photoinitiator and the polyethoxysiloxane obtained in step S10 are added and stirred for 20-40 minutes.

8. An adhesive according to any one of claims 3 to 7, characterized in that: In step S20, hydroxyethyl methacrylate and di-o-chlorodiphenylamine obtained in step S10 are added in sequence and stirred for 8-15 minutes.

9. An adhesive as claimed in claim 3, characterized in that: The container is a black container.

10. An adhesive as claimed in claim 3, characterized in that: The defoaming treatment time in step S30 is 8-12 minutes.