Purple light excited cyan fluorescent material as well as preparation method and application thereof

By using Lu ions instead of Y ions to widen the band gap in cyan fluorescent materials excited by purple light, the problem of the cyan light gap under excitation of purple light chips in the existing technology is solved, the spectral continuity and color rendering index are improved, and the material's Quantum efficiency and thermal stability achieve efficient and healthy lighting effects.

CN118853166APending Publication Date: 2024-10-29SHANGHAI INST OF CERAMIC CHEM & TECH CHINESE ACAD OF SCI
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
CN202310463574.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-04-26
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing violet-excited cyan fluorescent materials have performance defects when excited by violet chips. They are difficult to effectively match violet chips with a wavelength of 400-410nm. They cannot effectively solve the cyan light gap bottleneck problem in sun-like full-spectrum white LEDs, and they cannot be used in room temperature atmospheric environments. Medium unstable.

Method used

Purple light with the chemical formula Ca2Y1-y-xLuyZr2Al3O12:xCe is used to excite cyan fluorescent materials. Lu ions partially replace Y ions to broaden the band gap of the matrix, increase the ionization energy of Ce ions, reduce the probability of non-radiative transitions, and enhance luminous intensity and thermal stability. , the preparation method includes calcining once in an air atmosphere and then calcining twice in a reducing atmosphere.

Benefits of technology

It improves the continuity and color rendering index of the spectrum, enhances the fluorescence quantum efficiency and thermal stability, is suitable for large-scale production, and the preparation process is clean and pollution-free.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118853166A_ABST
    Figure CN118853166A_ABST
Patent Text Reader

Abstract

The invention relates to a purple light excited cyan fluorescent material as well as a preparation method and application thereof. The chemical formula of the purple light excited cyan fluorescent material is CaaY (3-a-y-x) LuyAaB (5-a) O12: xCe, wherein A is selected from at least one of Zr and Hf, and B is selected from at least one of Al and Ga; 1.5 < = a < = 2.5, 0 < x < = 0.50, and 0 < y < = 0.10.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a purple light excited cyan fluorescent material and a preparation method and application thereof, belonging to the field of luminescent materials and preparation thereof. Background Art

[0002] White light LED is a green lighting technology with great development potential. It has many advantages such as energy saving, environmental protection, ultra-long life, green and high efficiency. It has become the fourth generation of energy-saving and environmentally friendly lighting source after incandescent lamps, fluorescent lamps, and high-intensity discharge lamps. At present, the mainstream commercial white light LED on the market is usually InGaN blue light (λ em =440-470nm) chip combined with YAG:Ce(Y3Al5O 12 :Ce 3+ ) yellow powder, but due to the lack of some blue light, cyan light and a large amount of red light, it shows disadvantages such as low color rendering index (Ra<80) and high color temperature (CCT>4000K); at the same time, the white light LED excited by the blue light chip with sharp peak shape and high intensity will cause blue light damage to human body rhythm and eyes to a certain extent. In order to obtain high-quality white light, researchers have proposed a full-spectrum pc-LED strategy in recent years: using purple light chips combined with blue, green and red phosphors, and encapsulating a full-spectrum lighting source with a high color rendering index by adjusting the proportion of light in each band, but there is a cyan gap (480-520nm) between blue and green in the spectrum. Therefore, the development of high-performance purple light-excited cyan phosphors is of great significance for the continuous and uniform spectrum and improving the color rendering index.

[0003] Regarding violet light-excited cyan fluorescent materials, relevant research at home and abroad is still developing. Pei et al. (ECS Journal of Solid State Science and Technology, 2021, 10(9):096005) reported a hexagonal Li2BaSiO4:Ce 3+ ,Eu 2+ , Ce 3+ and Eu 2+ The ions successfully replaced the Ba in the Li2BaSiO4 matrix. 2+ , produces 500nm emission under 340nm excitation, and studies the Ce 3+ and Eu 2+ The dipole-dipole interaction of ion energy transfer in Li2BaSiO4 matrix is ​​studied by changing the Eu 2+ion doping concentration, a series of phosphors with continuously changing colors from blue (0.1297, 0.3912) to cyan (0.1660, 0.0343) were obtained. Liu et al. (Advanced Optical Materials, 2020, 8(22):2001037) reported the orthorhombic structure Ca3Ga4O9:Bi 3+ ,Zn 2+ Under the excitation of 370nm wavelength near-ultraviolet light, the emission peak is located at 486nm cyan light, and the transition metal ion Zn 2+ The co-doping of Bi 3+ The cyan emission intensity of the ions is enhanced by four times, combining the 370nm near-ultraviolet chip with the cyan powder Ca3Ga4O9:Bi 3+ ,Zn 2+ Combined with commercial red, green and blue powders, a full-spectrum white light LED prototype device was obtained, with a color rendering index of up to 97.4 and a lumen efficiency of 69.72lm / W. The excitation wavelengths of the cyan fluorescent materials reported above are mostly concentrated in the ultraviolet or near-ultraviolet region of the 340-380nm band, which is difficult to effectively match with the 400-410nm wavelength purple light chip, and still cannot effectively solve the cyan light gap bottleneck problem encountered in the sunlight-like full-spectrum white light LED excited by the purple light chip.

[0004] Zhao et al. (Light: Science & Applications, 2019, 8(1):38) reported a cubic UCr4C4 structured Na 0.5 K 0.5 Li3SiO4:Eu 2+ Under the excitation of 400nm wavelength violet light, the emission peak is located at 486nm cyan light. The matrix structure is rigid and has high cubic symmetry. The half-height width is only 20.7nm. Combining the 455nm blue light chip with the cyan powder Na 0.5 K 0.5 Li3SiO4:Eu 2+ , yellow powder YAG:Ce, red powder K2SiF6:Mn 4+ The combination of the two materials resulted in a white light LED prototype device with a color rendering index of 95.2, color coordinates of (0.3835, 0.3910), and a color temperature of 4021K. However, the cyan powder was unstable in the room temperature atmosphere. At the same time, some garnet-structured cyan fluorescent materials have attracted widespread attention. Wang et al. (J Mater Chem C, 2016, 4(48): 11396-11403) reported a garnet-structured Ca2LuHf2Al3O 12 :Ce 3+The bandgap width is 4.15 eV. Under the excitation of 410 nm wavelength violet light, it emits cyan light with a main peak at 484 nm, with a quantum efficiency of 50.3%. At 150 ° C, the luminescence intensity remains at 87% of that at room temperature. Sun et al. (J Mater Chem C, 2020, 8 (3): 1095-1103) reported a new garnet structure Ca2LuZr2Al3O 12 :Ce 3+ Under the excitation of 408nm wavelength violet light, the emission peak is located at 483nm cyan light, the half-width is 91nm, the internal quantum efficiency is 58%, and the luminous intensity at 150℃ remains 48% of that at room temperature. Sun et al. (Materials Today Energy, 2020, 17: 100448) reported a new garnet structure Ca2GdHf2Al3O 12 :Ce 3+ Under the excitation of 408nm wavelength violet light, the emission peak is located at 489nm cyan light, the half-width is 103nm, the internal quantum efficiency is 80%, and the cyan powder Ca2GdHf2Al3O 12 :Ce 3+ By filling the cyan gap in the white light LED prototype device obtained by combining a 400nm purple light chip with red, green and blue powders, the color rendering index was improved from 80.5 to 91.6.

[0005] The sunlight-like full-spectrum healthy lighting excited by the violet light chip requires excellent violet light-excited cyan fluorescent materials to fill the cyan gap to improve the continuity and color rendering of the spectrum. However, the violet light-excited cyan fluorescent materials reported so far all have performance defects to a certain extent. Therefore, it is very important to develop high-quality cyan fluorescent materials with high quantum efficiency, good structure and thermal stability, and low cost suitable for violet light chip excitation. Summary of the invention

[0006] To this end, the purpose of the present invention is to provide a violet light-excited cyan fluorescent material and a preparation method and application thereof, aiming to improve the continuity of the spectrum and enhance the color rendering index of the white light LED.

[0007] In a first aspect, the present invention provides a violet light-excited cyan fluorescent material, wherein the chemical formula of the violet light-excited cyan fluorescent material is Ca a Y 3-a-y-x Lu y A a B 5-a O 12 :xCe; wherein A is selected from at least one of Zr and Hf, and B is selected from at least one of Al and Ga; 1.5≤a≤2.5, 0<x≤0.50, 0<y≤0.10.

[0008] In the present invention, the luminescent center of the violet light-excited cyan fluorescent material is a positive trivalent Ce ion, which emits cyan light with a central wavelength of 487nm under the excitation of violet light with a wavelength of 405nm. Moreover, based on energy band engineering, the present invention partially replaces the Y ions with Lu ions to widen the band gap of the matrix, thereby increasing the ionization energy of the Ce ions, reducing the probability of non-radiative transitions, effectively enhancing the luminous intensity of the material, improving the fluorescence quantum efficiency, and improving thermal stability. The violet light-excited cyan powder CYLZA:Ce has significant advantages in improving the continuity of the violet light-excited white light LED spectrum and improving the color rendering index. It is an efficient cyan phosphor for healthy lighting full-spectrum white light LEDs.

[0009] Preferably, 1.8≤a≤2.1, preferably x=2; 0.01≤x≤0.1, preferably 0.06; y=0.04 to 0.08, preferably 0.06.

[0010] Preferably, the violet light-excited cyan fluorescent material is in powder form with a particle size of 5 μm to 10 μm.

[0011] Preferably, the luminescent center of the cyan fluorescent material excited by the purple light is Ce 3+ The ions emit cyan light with a central wavelength of 487nm when excited by 405nm violet light.

[0012] In a second aspect, the present invention provides a method for preparing a violet light-excited cyan fluorescent material, comprising: mixing a Ca source, a Y source, a Lu source, a Zr source, an Al source and a Ce source, first calcining them in an air atmosphere, and then calcining them in a reducing atmosphere to obtain the violet light-excited cyan fluorescent material.

[0013] Preferably, the Ca source is selected from at least one of CaCO3 and Ca(NO3)2; The Y source is selected from at least one of Y2O3, yttrium carbonate and yttrium nitrate; The Lu source is selected from at least one of Lu2O3, lutetium carbonate and lutetium nitrate; The Zr source is selected from at least one of ZrO2, zirconium carbonate and zirconium nitrate; The Al source is selected from at least one of Al2O3, aluminum carbonate and aluminum nitrate The Ce source is selected from at least one of CeO2, cerium carbonate and cerium nitrate.

[0014] Preferably, the primary calcination is carried out at a temperature of 400-800°C and for a time of 1-5 hours.

[0015] Preferably, the secondary calcination is carried out at a temperature of 1300 to 1600° C. and for a time of 2 to 6 hours.

[0016] Preferably, the reducing atmosphere is a mixed atmosphere of at least one of nitrogen and argon and hydrogen, and the hydrogen content does not exceed 10 Vol%.

[0017] In a third aspect, the present invention provides an application of the above-mentioned purple light excited cyan fluorescent material in the preparation of white light LED materials.

[0018] In a fourth aspect, the present invention provides a white light LED, comprising: a purple light chip and a resin coating coated on the surface of the purple light chip containing red phosphor, green phosphor, blue phosphor and the above-mentioned purple light-excited cyan fluorescent material.

[0019] Preferably, the mass ratio of the red phosphor, the green phosphor, the blue phosphor and the violet light excited cyan phosphor is 1:(0.8-2):(2-3):(2-4); The thickness of the resin coating is 1 mm to 1.5 mm; The ratio of the total mass of the red phosphor, the green phosphor, the blue phosphor and the violet light excited cyan phosphor material to the mass of the resin is 1:(2-4); The composition of the red phosphor is (Ca, Sr)AlSiN3:Eu 2+ ; The composition of the green phosphor is (Ba, Sr)2SiO4:Eu 2+ ; The composition of the blue phosphor is Sr(PO4)3Cl:Eu 2+ .

[0020] Furthermore, preferably, the mass ratio of the red phosphor, the green phosphor, the blue phosphor and the violet light excited cyan phosphor is 1:2:2:2; The ratio of the total mass of the red phosphor, the green phosphor, the blue phosphor and the violet light excited cyan phosphor material to the mass of the resin is 1:4; The particle sizes of the red phosphor, green phosphor and blue phosphor are all 5 μm to 30 μm. The purple light chip is a 395-400nm purple light lamp bead with a power of 3W.

[0021] In a fifth aspect, the present invention provides a method for preparing the white light LED as described in claim 11 or 12, wherein red phosphor, green phosphor, blue phosphor and purple light excited cyan fluorescent material are weighed and mixed according to a mass ratio, and then evenly mixed with a resin, and then evenly coated on a purple light chip to obtain the white light LED.

[0022] Beneficial effects of the present invention: In the present invention, starting from the garnet structural material with low price and good stability (such as Ca2YZr2Al3O 12 ) is started, Ce ions are doped as the luminescent center, and band engineering is used to partially replace Y ions by Lu ions, broadening the matrix Ca2Y 1-y Lu y Zr2Al3O 12 The band gap of Ce ions is increased, thereby increasing the ionization energy of Ce ions, reducing the probability of non-radiative transitions, effectively enhancing the luminescence intensity of the material, improving the fluorescence quantum efficiency, and improving the thermal stability. The purple light-excited cyan fluorescent material obtained in the present invention (for example, Ca2Y 1-y-x Lu y Zr2Al3O 12 :xCe) When excited by 405nm wavelength violet light, it emits cyan light with a central wavelength of 487nm, which has significant advantages in improving spectral continuity and color rendering index. The preparation process is clean and pollution-free, and is suitable for large-scale production. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 The series of Ce ions Ca doped with different concentrations in Example 1 2-x YZr2Al3O 12 :xCe(0≤x≤0.50) sample library high-throughput photography results; Figure 2 The samples Ca2Y with different concentrations of Lu ions in Example 2 are replaced by 0.94-y Lu y Zr2Al3O 12 :Emission spectrum of 0.06Ce (0≤y≤0.10) excited by 405nm violet light; Figure 3 The samples Ca2Y with different concentrations of Lu ions in Example 2 are replaced by 0.94-y Lu y Zr2Al3O 12 : Excitation spectrum of 0.06Ce (0≤y≤0.10) monitored at 487nm wavelength; Figure 4 The samples Ca2Y with different concentrations of Lu ions in Example 2 are replaced by 0.94-y Lu y Zr2Al3O 12 : PL integrated intensity histogram of 0.06Ce (0≤y≤0.10) under 405nm excitation; Figure 5 The samples Ca2Y with different concentrations of Lu ions in Example 2 are replaced by 0.94-y Lu y Zr2Al3O 12: X-ray diffraction pattern of 0.06Ce (0≤y≤0.10) and pure phase Ca3Fe2Si as reference 1.15 O 4.6 (OH) 7.4 Standard X-ray diffraction patterns of CaZrO3 (X-ray diffraction standard card PDF No.75-0553) and CaZrO3 (X-ray diffraction standard card PDF No.75-0358); Figure 6 Ca2Y 0.94 Zr2Al3O 12 :0.06Ce and Ca2Y 0.88 Lu 0.06 Zr2Al3O 12 :Comparison of quantum efficiency of 0.06Ce; Figure 7 Ca2Y 0.94 Zr2Al3O 12 :0.06Ce and Ca2Y 0.88 Lu 0.06 Zr2Al3O 12 :0.06Ce thermal stability comparison; Figure 8 Ca2Y 0.94 Zr2Al3O 12 :0.06Ce and Ca2Y 0.88 Lu 0.06 Zr2Al3O 12 :Comparison of thermal activation energy of 0.06Ce; Fig. 9 The spectrum of a white LED made by combining a purple chip with blue, green, and red phosphors (above), and the spectrum of a white LED made by combining a purple chip with blue, green, and red phosphors and Ca2Y 0.88 Lu 0.06 Zr2Al3O 12 : Spectrum of white light LED made of 0.06Ce cyan powder (below); Fig.10 for Fig. 9 Color coordinates and device photos of neutral white LED devices; Fig.11 Ca 1.88 Y 0.06 Zr 1.88 Al 3.12 O 12 :PL and PLE spectra of 0.06Ce. DETAILED DESCRIPTION

[0024] The present invention is further described below by the following embodiments. It should be understood that the following embodiments are only used to illustrate the present invention, but not to limit the present invention.

[0025] In the present disclosure, the chemical formula of the cyan fluorescent material excited by violet light is Ca2Y 1-y-x Lu y Zr2Al3O 12 :xCe, abbreviated as CYLZA:Ce, where 0<x≤0.50, 0<y≤0.10, the luminescence center is the trivalent Ce ion, which emits cyan light with a central wavelength of 487nm under the excitation of 405nm violet light.

[0026] The present invention adopts a high temperature solid phase method to prepare a violet light excited cyan fluorescent material. The following is an exemplary description of the preparation method of the violet light excited cyan fluorescent material provided by the present invention.

[0027] Commercially available CaCO3, Y2O3, Lu2O3, ZrO2, Al2O3, CeO2 powders, or other carbonates and nitrates containing Ca, Y, Lu, Zr, Al, Ce sources are weighed as raw materials according to the corresponding stoichiometric ratio, ground in an agate mortar for half an hour, and mixed evenly to prepare raw material powders.

[0028] As an example, the raw materials used include: commercially available CaCO3 (99.99%), Y2O3 (99.99%), Lu2O3 (99.99%), ZrO2 (analytical grade), Al2O3 (99.99%), CeO2 (99.99%) powders, etc.

[0029] The raw material powder is calcined at 400-800° C. in an air atmosphere for 1-5 hours to decompose the carbonate or nitrate into oxides to obtain a calcined powder.

[0030] The calcined powder is calcined at 1300-1600°C in a reducing atmosphere for 2-10 hours to allow the oxide to react fully. When cooled to room temperature, the powder is taken out to obtain a cyan phosphor excited by violet light.

[0031] The following further examples are given to illustrate the present invention in detail. It should also be understood that the following examples are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made by those skilled in the art based on the above content of the present invention belong to the scope of protection of the present invention. The specific process parameters and the like in the following examples are also only examples within a suitable range, that is, those skilled in the art can make a selection within a suitable range through the description herein, and are not limited to the specific values ​​​​exemplified below.

[0032] Example 1 (Determining the Optimal Concentration of Ce Ion Doping) Using commercially available Ca(NO3)2·4H2O, YN3O9·6H2O, Zr(NO3)4·5H2O, Al(NO3)3·9H2O, and CeN3O9·6H2O as raw materials, 2mol / L Ca(NO3)2 solution, 1mol / L YN3O9 solution, 0.5mol / L Zr(NO3)4 solution, 1.5mol / L Al(NO3)3 solution, and 0.2mol / L CeN3O9 solution were prepared in 50ml volumetric flasks respectively. 3+ The doping concentration ranges from 0% to about 50%. The solution is connected to the high-throughput screening equipment in turn for rinsing and machine dripping. The sample is then ultrasonically dried and sintered at 1450°C in a reducing atmosphere to obtain Ca 2-x YZr2Al3O 12 :xCe (0≤x≤0.416, 54 samples in total, the first sample x=0, each sample is arranged in an arithmetic sequence of d=0.008) (at this time a=2-x) sample library.

[0033] like Figure 1 A series of samples doped with different concentrations of Ce ions Ca 2-x YZr2Al3O 12 The high-throughput photography results of :xCe (0<x≤0.416) show that the cyan luminescence is strongest when the Ce ion doping concentration is about 6%. Therefore, the Ce ion doping concentration is determined to be 6% to study the regulation of Lu ion substitution on performance.

[0034] Example 2: Lu ion substitution increases the luminescence intensity of the material Weigh the commercially available CaCO3, Y2O3, Lu2O3, ZrO2, Al2O3, CeO2 powders in a molar ratio of 2:1-x:x:2:3:0.06 (where x = 0, 0.01, 0.02, 0..04, 0.06, 0.08, 0.10, 0.12 or 0.14). Grind in an agate mortar for half an hour, mix well and use as raw powder. Calcine the raw powder at 400-800°C in an air atmosphere for 1 to 5 hours; then calcine at 1300-1600°C in a reducing atmosphere for 2 to 6 hours, and take it out when cooled to room temperature to obtain a cyan phosphor excited by violet light, Ca2Y 0.94-x Lu x Zr2Al3O 12 :0.06Ce.

[0035] like Figure 2 and Figure 3 A series of samples with different concentrations of Lu ions replacing Ca2Y 0.94-x Lu x Zr2Al3O 12The emission spectrum of 0.06Ce under 405nm violet light excitation and the excitation spectrum monitored by 487nm wavelength light show that Lu ion substitution enhances the 0.94- x Lu x Zr2Al3O 12 : The PL intensity and PLE intensity of 0.06Ce reach the maximum value when the substitution concentration is 6%. 3+ Ions are Lu 3+ When ions are substituted, the lattice constant decreases, resulting in a denser crystal structure. 3+ Excessive ion doping (0.12 or 0.14) is not conducive to the PL intensity and PLE intensity. In addition, due to the shortening of the average distance of the activator, the local Ce 3+ As the concentration increases, the energy transfer is more active. Figure 4 A series of samples with different concentrations of Lu ions replacing Ca2Y 0.94-y Lu y Zr2Al3O 12 :0.06Ce (0≤y≤0.10) under 405nm excitation PL integrated intensity bar graph, with Ca2Y 0.94 Zr2Al3O 12 :0.06Ce compared to Ca2Y 0.88 Lu 0.06 Zr2Al3O 12 The emission intensity of 0.06Ce was significantly improved, about 1.4 times. Among them, the emission intensities of 1%, 2%, 4%, 8%, 10%, 12%, and 14% were increased by 1.15 times, 1.16 times, 1.23 times, 1.4 times, 1.29 times, and 1.18 times, respectively.

[0036] like Figure 5 As shown, a series of samples with different concentrations of Lu ions replacing Ca2Y 0.94-x Lu x Zr2Al3O 12 :0.06Ce X-ray diffraction pattern, all consistent with the garnet structure of Ca3Fe2Si 1.15 (OH) 7.4 The standard diffraction pattern is basically consistent with that of the standard diffraction pattern, and there is also a weak peak of trace perovskite structure CaZrO3.

[0037] like Figure 6 The quantum efficiency of Ca2Y 0.94 Zr2Al3O 12 :0.06Ce has a quantum efficiency of 58.3%, Ca2Y 0.88 Lu 0.06 Zr2Al3O 12: The quantum efficiency of 0.06Ce is 58.6%, indicating that the substitution of Lu ions improves the quantum efficiency of the material.

[0038] like Figure 7 As shown, Ca2Y 0.94 Zr2Al3O 12 :0.06Ce and Ca2Y 0.88 Lu 0.06 Zr2Al3O 12 :0.06Ce PL spectrum with temperature changes, with the increase of temperature, the luminescence intensity gradually decreases. 0.88 Lu 0.06 Zr2Al3O 12 : The emission intensity of 0.06Ce at 373K remains at 70.6% of the initial intensity, which is higher than that of Ca2Y 0.94 Zr2Al3O 12 : 69.7% of 0.06Ce. Figure 8 As shown, Ca2Y was calculated by fitting the experimental data. 0.88 Lu 0.06 Zr2Al3O 12 : The thermal activation energy of 0.06Ce is 0.294eV, Ca2Y 0.94 Zr2Al3O 12 The thermal activation energy of 0.06Ce is 0.281eV. To a certain extent, the thermal quenching originates from the electrons from Ce 3+ Therefore, using band engineering, Lu 3+ Ion substitution Y 3+ ions, and also increased Ca2Y 0.88 Lu 0.06 Zr2Al3O 12 : Thermal stability of 0.06Ce.

[0039] Example 3 (white light LED application demonstration) To verify that Ca2Y 0.88 Lu 0.06 Zr2Al3O 12 :0.06Ce application potential, two white light LEDs were made for comparison: White light LED (1): Red phosphor, green phosphor and blue phosphor are weighed and mixed according to the mass ratio, and then mixed with epoxy resin and evenly coated on the purple light chip, and the coating thickness is controlled to be 1.5mm. The particle size of the blue, green and red phosphors is 5μm-30μm; the mass ratio of the red phosphor, green phosphor and blue phosphor is 1:2:2; the (Ca, Sr)AlSiN3:Eu of the red phosphor is 1:2:2; the (Ca, Sr)AlSiN3:Eu of the red phosphor is 1:2:2; the (Ca, Sr)AlSiN3:Eu of the red phosphor is 1:2:2; the (Ca, Sr)AlSiN3:Eu of the blue ... 2+; The composition of green phosphor is (Ba, Sr)2SiO4:Eu 2+ ; The composition of blue phosphor is Sr(PO4)3Cl:Eu 2+ ). And, the total mass of phosphor powder: epoxy resin = 1:4. The manufacturer and model of the purple light chip used is Shenzhen Rongcheng Microelectronics, 3W 395-400nm purple light lamp beads; White light LED (2): Red phosphor, green phosphor, blue phosphor and Ca2Y 0.88 Lu 0.06 Zr2Al3O 12 :0.06Ce cyan powder (particle size is 5μm-10μm) is weighed and mixed according to the mass ratio, and then evenly mixed with epoxy resin, and evenly coated on the purple light chip, and the coating thickness is controlled to be 1.5mm. The mass ratio of red phosphor, green phosphor, blue phosphor and purple light excited cyan fluorescent material is 1:2:2:2; the mass ratio of red phosphor (Ca, Sr)AlSiN3:Eu 2+ ; The composition of green phosphor is (Ba, Sr)2SiO4:Eu 2+ ; The composition of blue phosphor is Sr(PO4)3Cl:Eu 2+ ). And, the total mass of phosphor powder: epoxy resin = 1:4. The manufacturer and model of the purple light chip used is Shenzhen Rongcheng Microelectronics, 3W 395-400nm purple light lamp beads.

[0040] like Fig. 9 As shown, the spectrum of a white light LED made by combining a purple chip with blue, green, and red phosphors (above), and the spectrum of a white light LED made by combining a purple chip with blue, green, and red phosphors and Ca2Y 0.88 Lu 0.06 Zr2Al3O 12 : The spectrum of a white LED made of 0.06Ce cyan powder (below). It can be seen that the addition of cyan fluorescent material Ca2Y 0.88 Lu 0.06 Zr2Al3O 12 :0.06Ce, the cyan gap in the spectrum of white light LED is effectively filled, and Ra is also increased from 84.1 to 87.3. Fig.10 As shown in the figure, the CIE chromaticity coordinates and corresponding digital photos of the two LED devices at 40mA current and 3V driving voltage. The CIE chromaticity coordinates of LED1 are (0.4668, 0.3922), and the chromaticity coordinates of LED2 are (0.4149, 0.4168).

[0041] Example 4 Weigh the commercially available CaCO3, Y2O3, Lu2O3, ZrO2, Al2O3, CeO2 powders in a molar ratio of 1.88:1:0.06:1.88:3.12:0.06. Grind in an agate mortar for half an hour and mix well as raw powder. Calcine the raw powder at 400-800℃ in air atmosphere for 1-5 hours; then calcine at 1300-1600℃ in a reducing atmosphere for 2-6 hours, and take it out when cooled to room temperature to obtain cyan phosphor excited by purple light, Ca 1.88 Y 0.06 Zr 1.88 Al 3.12 O 12 :0.06Ce.

[0042] Industrial applicability: From the low-cost and stable garnet structure Ca2YZr2Al3O 12 Starting from Ce ion doping as the luminescent center, using band engineering, Lu ions partially replaced Y ions to broaden the matrix Ca2Y 1-y Lu y Zr2Al3O 12 The band gap of Ca2Y increases the ionization energy of Ce ions, reduces the probability of non-radiative transitions, effectively enhances the luminescence intensity of the material, improves the fluorescence quantum efficiency, and improves thermal stability. 1-y Lu y Zr2Al3O 12 : Ce emits cyan light with a central wavelength of 487nm when excited by 405nm violet light, which has significant advantages in improving spectral continuity and color rendering index. The preparation process is clean and pollution-free, making it suitable for large-scale production.

Claims

1. A cyan fluorescent material excited by violet light, characterized in that: The chemical formula of the violet light excited cyan fluorescent material is Ca a Y 3-a-y-x Lu y A a B 5-a O 12 :xCe; wherein A is selected from at least one of Zr and Hf, and B is selected from at least one of Al and Ga; 1.5≤a≤2.5, 0<x≤0.50, 0<y≤0.

10.

2. The violet light excited cyan fluorescent material according to claim 1, characterized in that: 1.8≤a≤2.1, preferably x=2; 0.01≤x≤0.1, preferably 0.06; y=0.04 to 0.08, preferably 0.

06.

3. The violet light excited cyan fluorescent material according to claim 1 or 2, characterized in that: The purple light excited cyan fluorescent material is in powder form, and the particle size is 5 μm to 10 μm.

4. The violet light excited cyan fluorescent material according to any one of claims 1 to 3, characterized in that: The luminescent center of the purple light-excited cyan fluorescent material is Ce 3+ The ions emit cyan light with a central wavelength of 487nm when excited by 405nm violet light.

5. A method for preparing a violet light excited cyan fluorescent material as claimed in any one of claims 1 to 4, characterized in that: include: After the Ca source, Y source, Lu source, Zr source, Al source and Ce source are mixed, they are first calcined in an air atmosphere and then calcined again in a reducing atmosphere to obtain the purple light excited cyan fluorescent material.

6. The preparation method according to claim 5, characterized in that: The Ca source is selected from at least one of CaCO3 and Ca(NO3)2; The Y source is selected from at least one of Y2O3, yttrium carbonate and yttrium nitrate; The Lu source is selected from at least one of Lu2O3, lutetium carbonate and lutetium nitrate; The Zr source is selected from at least one of ZrO2, zirconium carbonate and zirconium nitrate; The Al source is selected from at least one of Al2O3, aluminum carbonate and aluminum nitrate; The Ce source is selected from at least one of CeO2, cerium carbonate and cerium nitrate.

7. The preparation method according to claim 5, characterized in that: The primary calcination is carried out at a temperature of 400-800° C. and for a time of 1-5 hours.

8. The preparation method according to claim 5, characterized in that: The secondary calcination is carried out at a temperature of 1300 to 1600° C. and for a time of 2 to 6 hours.

9. The preparation method according to any one of claims 5 to 8, characterized in that: The reducing atmosphere is a mixed atmosphere of at least one of nitrogen and argon and hydrogen, and the hydrogen content is preferably no more than 10 Vol%.

10. Use of the violet light excited cyan fluorescent material according to any one of claims 1 to 4 in preparing white light LED materials.

11. A white light LED, characterized in that: include: A purple light chip and a resin coating coated on the surface of the purple light chip containing red phosphor, green phosphor, blue phosphor and the purple light excited cyan fluorescent material described in any one of claims 1 to 4; Preferably, the mass ratio of the red phosphor, the green phosphor, the blue phosphor and the violet light excited cyan fluorescent material is 1:(0.8-2):(2-3):(2-4); Preferably, the thickness of the resin coating is 1 mm to 1.5 mm; Preferably, the ratio of the total mass of the red phosphor, the green phosphor, the blue phosphor and the violet light excited cyan fluorescent material to the mass of the resin is 1:(2-4); Preferably, the composition of the red phosphor is (Ca, Sr)AlSiN3:Eu 2+ ; Preferably, the composition of the green phosphor is (Ba, Sr)2SiO4:Eu 2+ ; Preferably, the composition of the blue phosphor is Sr(PO4)3Cl:Eu 2+ .

12. The white light LED according to claim 11, characterized in that: The mass ratio of the red phosphor, the green phosphor, the blue phosphor and the violet light excited cyan phosphor material is 1:2:2:2; The ratio of the total mass of the red phosphor, the green phosphor, the blue phosphor and the violet light excited cyan phosphor material to the mass of the resin is 1:4; The particle sizes of the red phosphor, green phosphor and blue phosphor are all 5 μm to 30 μm; The purple light chip is a 395-400nm purple light lamp bead with a power of 3W.

13. A method for preparing a white light LED according to claim 11 or 12, characterized in that: The red phosphor, green phosphor, blue phosphor and purple light excited cyan fluorescent material are weighed and mixed according to the mass ratio, and then evenly mixed with resin, and then evenly coated on the purple light chip to obtain the white light LED.

Citation Information

Patent Citations

  • Fluorescent powder capable of emitting cyan light and preparation method thereof

    CN106520119A