Preparation method and application of rare earth enhanced near-infrared phosphor luminescence and thermal stability
By doping rare earth elements in near-infrared phosphor and adopting specific sintering methods, the problem of insufficient luminescence efficiency and thermal stability of Cr3+ doped phosphor is solved, which significantly improves the quantum efficiency and thermal stability of fluorescent materials, and is suitable for high temperatures Lower eye care and eye protection device light source.
Patent Information
- Application Number
- CN202310469757.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-04-27
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-04-27
AI Technical Summary
The existing Cr3+ doped near-infrared phosphor has less than 30% luminescent quantum efficiency and poor thermal stability, making it difficult to meet the needs of eye care and repair at high temperatures.
By doping a variety of rare earth elements in the pyroxene structure substrate material, such as Ce3+, Pr3+ and Eu3+, surface mechanical activation and procedural temperature-raising sintering methods, the rare earth elements are uniformly embedded in the crystal lattice of the substrate material to form stable co-doping Oxides improve the thermal stability and emission intensity of fluorescent materials.
The internal quantum efficiency and thermal stability of near-infrared fluorescent materials were significantly improved. After incorporation of Pr3+, the internal quantum yield increased from 71.4% to 93%, and the external quantum yield increased from 13.5% to 33%, at a temperature of 150℃. The luminous intensity is increased to 74.1%, and it is suitable for near-infrared light sources of eye protection instruments.
Smart Images

Figure CN116536045B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a near-infrared phosphor, in particular to a preparation method and application of a rare earth-enhanced near-infrared phosphor with luminescence and thermal stability, belonging to the technical field of fluorescent materials. Background Art
[0002] Applications of near-infrared (NIR) light sources include night vision lighting, medical diagnosis, biometrics (including iris and vein image acquisition), near-infrared spectroscopy detection, and human eye care. Incandescent lamps, halogen lamps, and AlGaAs near-infrared light-emitting diodes (LEDs) are the main near-infrared light sources. Near-infrared light sources have irreplaceable advantages in the field of optical diagnosis and treatment, but there are also inevitable defects in practical applications. Near-infrared phosphor-converted light-emitting diodes (NIR pc-LEDs) have the advantages of small size, high efficiency, low cost, and long life, making them an ideal choice for current applications. Therefore, it is crucial to develop near-infrared phosphors with high quantum efficiency and thermal stability. Cr 3+ The doped near-infrared phosphor has 4 A1→ 4 The blue light absorption band of T1 energy level transition can be well matched with high-efficiency commercial blue light LED chips, but most of the Cr 3+ The external quantum efficiency of the doped phosphor is less than 30%, and the thermal stability is poor. 3+ The quantum yield and thermal stability of long-wave near-infrared phosphors are of paramount importance. Currently, crystal field regulation and doping are the main methods to optimize Cr 3+ An important method to improve the quantum yield and thermal stability of near-infrared phosphors.
[0003] In addition, near-infrared light irradiation has a repairing and caring effect on the eyes, but when acting on the eyes, near-infrared light needs to be continuously irradiated, which causes the temperature to rise. The existing near-infrared fluorescent materials are difficult to meet application requirements at a high temperature of 150°C, and the quantum yield is low, making it difficult to provide effective care and repair for the eyes. Summary of the invention
[0004] In view of the problems existing in the prior art, the first purpose of the present invention is to provide a near-infrared phosphor with rare earth enhanced luminous efficiency and thermal stability. By doping a variety of rare earth elements on a pyroxene structure base material, on the one hand, the thermal stability of the fluorescent material is improved, and on the other hand, the emission intensity of the fluorescent material can be significantly enhanced, thereby improving the internal quantum efficiency of the fluorescent material.
[0005] The second object of the present invention is to provide a method for preparing a near-infrared phosphor with rare earth enhanced luminous efficiency and thermal stability. The method embeds the rare earth elements uniformly into the lattice of the base material through surface mechanical activation and programmed temperature sintering. The preparation method is simple to operate, the yield rate of the obtained fluorescent material is high, and it is convenient for industrial production.
[0006] The third object of the present invention is to provide an application of a near-infrared phosphor with rare earth enhanced luminous efficiency and thermal stability for preparing a near-infrared light source for an eye protector. The near-infrared light source for an eye protector prepared based on the near-infrared fluorescent material provided by the present invention has excellent energy conversion efficiency. 3+ The absorption of blue light by the latter sample increased significantly, with the internal quantum yield increasing from 71.4 to 93%, and the external quantum yield also increasing from 13.5% to 33%. 3+ The change of the rigidity of the framework structure and the increase of the thermal activation energy due to doping also improve the thermal stability. At 150℃, the luminescence intensity of CMG:1Pr,2Cr and CMG:2Cr increased from 67.8% of room temperature to 74.1%.
[0007] In order to achieve the above technical objectives, the present invention provides a near-infrared phosphor with rare earth enhanced luminous efficiency and thermal stability, wherein the general structural formula of the fluorescent material is Ca 1-y Mg 1-x Ge2M x RE y Z y O6, where M is Cr 3+ , RE is Ce 3+ , Pr 3+ and Eu 3+ One of the following, Z is Na + and Li + One, 0.01≤x≤0.10, 0≤y≤0.05, 0≤z≤0.05.
[0008] The fluorescent material provided by the present invention is based on the synergistic effect between the various components. The selected rare earth elements can be embedded in the lattice of the pyroxene structure base material without lattice distortion, forming a stable co-doped oxide, which greatly improves the thermal stability of the material while ensuring the energy conversion efficiency of the fluorescent material.
[0009] As a preferred solution, M in the fluorescent material is Cr 3+ , RE is Pr 3+ ; The molar ratio of M to RE is 0.5-6:1. Cr 3+ and Pr 3+ The co-doping of 3d 3Structure of Cr 3+ It has a strong coupling effect on the host lattice, which is stronger than Pr 3+ has stronger non-radiative relaxation, so Pr 3+ Co-doping may improve the thermal stability of CMG:2Cr. On the other hand, due to the 3+ The incorporation of Cr 3+ The probability of non-radiative transition is reduced, which increases the internal quantum yield from 71.4% to 93%, and the absorbance also corresponds to the diffuse reflectance spectrum. After Pr is doped, the sample's absorption of blue light increases significantly. With the increase in internal quantum yield and absorbance, the external quantum yield also increases accordingly.
[0010] The present invention also provides a method for preparing near-infrared phosphor with rare earth enhanced luminous efficiency and thermal stability, which comprises uniformly mixing raw materials including calcium source, magnesium source, germanium source and M source, and sequentially subjecting the mixture to mechanical activation, sintering and crushing to obtain the near-infrared phosphor.
[0011] As a preferred embodiment, the calcium source is at least one of calcium carbonate, calcium oxide and calcium hydroxide.
[0012] As a preferred embodiment, the magnesium source is at least one of magnesium oxide, magnesium carbonate and magnesium hydroxide.
[0013] As a preferred solution, the germanium salt is at least one of germanium oxide, germanium carbonate and germanium hydroxide.
[0014] As a preferred solution, the M source is at least one of oxides, fluorides, hydroxides and carbonates containing the M element.
[0015] As a preferred solution, the Z source is a carbonate containing the M element.
[0016] The selection of raw materials follows the characteristics of high-temperature gas phase release, such as carbonates or hydroxides, which will be released in the form of carbon dioxide or water during the high-temperature sintering process, avoiding the formation of solid solution phase impurity ions during the sintering process, thereby improving the purity of the product.
[0017] As a preferred solution, the mechanical activation method is high-energy ball milling or grinding.
[0018] As a preferred solution, the mechanical activation is performed until the raw material particle size is 5-10 μm. Mechanical activation is used to refine and homogenize the raw material particle size on the one hand, and on the other hand, it can increase the surface activation energy of the material, which is convenient for embedding and doping of rare earth elements during subsequent sintering.
[0019] As a preferred solution, the sintering method is programmed temperature sintering, and the conditions are: in a protective atmosphere, the temperature is raised from room temperature to 1100-1200°C at 8-12°C / min, kept at this temperature for 4 hours, and cooled to room temperature with the furnace.
[0020] As a preferred solution, the protective atmosphere is high-purity nitrogen and / or high-purity argon.
[0021] The present invention also provides an application of a near-infrared phosphor with rare earth enhanced luminous efficiency and thermal stability, which is used for preparing a near-infrared light source for an eye protection device.
[0022] As a preferred solution, the near-infrared light source includes a monochromatic LED chip, a near-infrared fluorescent material coated on the surface of the monochromatic LED chip, and a silica gel packaging layer.
[0023] As a preferred solution, the wavelength of the near-infrared light source is 750-900 nm, and the optical power is 50-55 mW.
[0024] Compared with the prior art, the beneficial technical effects of the technical solution provided by the present invention are:
[0025] 1) The fluorescent material provided by the present invention is based on the synergistic effect between the various components. The selected rare earth elements can be embedded in the lattice of the pyroxene structure base material without lattice distortion, forming a stable co-doped oxide. On the one hand, the thermal stability of the fluorescent material is improved, and on the other hand, the emission intensity of the fluorescent material can be significantly enhanced, thereby improving the internal quantum efficiency of the fluorescent material.
[0026] 2) In the preparation method provided by the present invention, the rare earth elements are uniformly embedded into the lattice of the base material through surface mechanical activation and programmed temperature sintering. The preparation method is simple to operate, the yield rate of the obtained fluorescent material is high, and it is convenient for industrial production.
[0027] 3) In the technical solution provided by the present invention, Pr 3+ As a sensitizer for CaMgGe2O6:Cr with pyroxene structure 3+ The luminescence intensity was increased by 2 times by doping. 3+ The absorption of blue light by the latter sample increased significantly, with the internal quantum yield increasing from 71.4 to 93%, and the external quantum yield also increasing from 13.5% to 33%. 3+ The change of the rigidity of the framework structure and the increase of the thermal activation energy due to doping also improve the thermal stability. At 150℃, the luminescence intensity of CMG:1Pr,2Cr and CMG:2Cr increased from 67.8% of room temperature to 74.1%. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1The XRD patterns of the fluorescent materials obtained in Example 3 and Comparative Examples 1 to 3 of the present invention are shown below;
[0029] Figure 2 The diffuse reflection spectra of the fluorescent materials obtained in Example 3 and Comparative Examples 1 to 3 of the present invention are shown;
[0030] Figure 3 The excitation and emission spectra of the fluorescent materials obtained in Example 3 of the present invention and Comparative Examples 2 and 3;
[0031] Figure 4 The emission spectra of the fluorescent materials obtained in Examples 3 and 6 to 9 of the present invention;
[0032] Figure 5 The near-infrared emission spectra of the fluorescent materials obtained in Examples 1 to 5 of the present invention and Comparative Example 2;
[0033] Figure 6 This is a graph of the quantum yield of the fluorescent material obtained in Comparative Example 3 of the present invention;
[0034] Figure 7 This is a diagram of the quantum yield of the fluorescent material obtained in Example 3 of the present invention;
[0035] Figure 8 This is a temperature-dependent emission spectrum diagram of the fluorescent material obtained in Comparative Example 3 of the present invention;
[0036] Fig. 9 This is a temperature-dependent emission spectrum diagram of the fluorescent material obtained in Example 3 of the present invention;
[0037] Fig.10 It is a temperature-near infrared emission intensity correlation diagram of the fluorescent materials obtained in Example 3 of the present invention and Comparative Example 3. DETAILED DESCRIPTION
[0038] In the following description, it is obvious that the described embodiments are only a part of the embodiments of the present invention, rather than all the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Example 1
[0040] The raw materials used in this embodiment are CaCO3, MgO, GeO2, Li2CO3, Cr2O3 and PrF3, and the molar ratio thereof is 1:1:2:0.001:0.005:0.01.
[0041] The specific preparation process of the fluorescent material is as follows: accurately weigh each drug according to the above-mentioned ratio requirements, mix them evenly, and then grind them in an agate mortar for 30 minutes for mechanical empowerment to obtain a precursor powder; transfer the precursor powder into a crucible, and sinter it in a high-temperature box furnace, and the sintering parameters are set as follows: at a heating rate of 10°C / min, heat from room temperature to 1250°C, keep warm for 4 hours, and cool to room temperature with the furnace; the sintered sample is placed in an agate mortar again and ground and crushed to obtain the fluorescent material, which is recorded as CMG: 1Pr, 1Cr.
[0042] This embodiment also provides a preparation process of a near-infrared light source obtained by using the above fluorescent material: the obtained fluorescent material and silica gel are mixed and stirred at a mass ratio of 1:1 for 30 minutes, coated on a 460nm blue chip, and vacuum dried to obtain the result.
[0043] Example 2
[0044] This embodiment is exactly the same as the embodiment 1, except that the amount of Cr2O3 added is halved, and the obtained phosphor is recorded as CMG: 1Pr, 0.5Cr.
[0045] Example 3
[0046] This embodiment is exactly the same as the embodiment 1, except that the amount of Cr2O3 added is doubled, and the obtained phosphor is recorded as CMG: 1Pr, 2Cr.
[0047] Example 4
[0048] This embodiment is exactly the same as the embodiment 1, except that the amount of Cr2O3 added is increased by 3 times, and the obtained phosphor is recorded as CMG: 1Pr, 4Cr.
[0049] Example 5
[0050] This embodiment is exactly the same as the embodiment 1, except that the amount of Cr2O3 added is increased by 5 times, and the obtained phosphor is recorded as CMG: 1Pr, 6Cr.
[0051] Example 6
[0052] This embodiment is exactly the same as the embodiment 1, except that the addition amount of Cr2O3 is doubled and the addition amount of PrF3 is reduced by 70%. The obtained phosphor is recorded as CMG: 0.3Pr, 2Cr.
[0053] Example 7
[0054] This embodiment is exactly the same as the embodiment 1, except that the addition amount of Cr2O3 is doubled and the addition amount of PrF3 is reduced by 50%. The obtained phosphor is recorded as CMG: 0.5Pr, 2Cr.
[0055] Example 8
[0056] This embodiment is exactly the same as the embodiment 1, except that the addition amount of Cr2O3 is doubled and the addition amount of PrF3 is doubled. The obtained phosphor is recorded as CMG: 2Pr, 2Cr.
[0057] Example 9
[0058] This embodiment is exactly the same as the embodiment 1, except that the addition amount of Cr2O3 is doubled and the addition amount of PrF3 is doubled. The obtained phosphor is recorded as CMG: 3Pr, 2Cr.
[0059] Comparative Example 1
[0060] This comparative example is exactly the same as Example 1, except that Cr2O3 and PrF3 are not added.
[0061] Comparative Example 2
[0062] This embodiment is exactly the same as embodiment 1, except that Cr2O3 is not added.
[0063] Comparative Example 3
[0064] This comparative example is exactly the same as Example 3, except that PrF3 is not added.
[0065] In order to understand the near-infrared emission characteristics of CMG, a series of different Pr 3+ and Cr 3+ The typical XRD pattern of CMG doped with high concentration is as follows: Figure 1 shown.
[0066] Figure 2 The diffuse reflectance spectra of the samples obtained in Example 3 and Comparative Examples 1 to 3 of the present invention are shown in FIG. 3+ The incorporation of Cr 3+ The probability of non-radiative transition is reduced, which increases the internal quantum yield from 71.4% to 93%, and the absorptivity also corresponds to the diffuse reflectance spectrum. After Pr is doped, the sample's absorption of blue light increases significantly. With the increase in internal quantum yield and absorptivity, the external quantum yield also increases from 13.5% to 33%.
[0067] Under 468nm excitation, Pr 3+ With Cr 3+ can reach the excited state, for Pr 3+ For example, under blue light excitation, Pr 3+ The ground state 3 H4 reaches the excited state 3 P2, and then the electrons arrive in the form of thermal vibration 3 P0 excited state energy level. At this time, Pr 3+ exist 3 The P0 excited state energy level is 3P0→ 3 H J (J=5,4,6) and 3 P0→ 3 F J (J=2,4) transition, releasing energy in the form of luminescence to reach the ground state energy level, on the other hand, Pr 3+ exist 3 The P0 excited state energy level transfers energy to Cr 3+ Cr 3+ After absorbing the energy of blue light and the energy of energy transfer, it reaches the ground state in the form of emitting near-infrared light 4 A 2.
[0068] For pc-LED, since the pn junction in the blue LED will generate a lot of heat after power is turned on, the ambient temperature faced by the phosphor in the pc-LED is at least 150℃. 3 Structure of Cr 3+ It has a strong coupling effect on the host lattice, which is stronger than Pr 3+ has stronger non-radiative relaxation, so Pr 3+ Co-doping can effectively improve the thermal stability of CMG:2Cr. Figure 8 and Fig. 9 Temperature-dependent emission spectra of CMG:1Pr,2Cr and CMG:2Cr excited at 468 nm are shown. Fig.10 The luminescence intensity of CMG:1Pr,2Cr and CMG:2Cr excited at 468nm changes with temperature. 3+ Afterwards, the thermal quenching phenomenon of the phosphor was improved, and the luminous intensity increased from 67.8% of room temperature to 74.1% when the temperature was increased to 150°C.
[0069] The present invention also uses the sample obtained in Example 3 to prepare a near-infrared light source for an eye protector, and sequentially coats the red phosphor and the fluorescent material obtained in Example 3 on the surface of a blue LED chip and then uses silica gel to encapsulate the chip. The present invention tests the spectrum of the obtained near-infrared light source for an eye protector, and the light source has obvious characteristic peaks at 650nm and 850nm, which can meet the requirements of the eye protector for the light source band.
Claims
1. A near-infrared phosphor with rare earth enhanced luminous efficiency and thermal stability, characterized in that: The general structural formula of the fluorescent material is Ca 1-y Mg 1-x Ge2M x RE y Z y O6, where M is Cr 3+ , RE is Pr 3+ , Z is Na + and Li + , 0.01≤x≤0.10, 0≤y≤0.05, 0≤z≤0.05; the molar ratio of M to RE is 0.5~6:
1.
2. The method for preparing a near-infrared phosphor with rare earth enhanced luminous efficiency and thermal stability as claimed in claim 1, characterized in that: The raw materials including calcium source, magnesium source, germanium source, M source and Z source are mixed uniformly, and then mechanically activated, sintered and crushed in sequence to obtain the product.
3. The method for preparing a near-infrared phosphor with rare earth enhanced luminous efficiency and thermal stability according to claim 2, characterized in that: The calcium source is at least one of calcium carbonate, calcium oxide and calcium hydroxide; the magnesium source is at least one of magnesium oxide, magnesium carbonate and magnesium hydroxide; and the germanium salt is at least one of germanium oxide, germanium carbonate and germanium hydroxide.
4. The method for preparing a near-infrared phosphor with rare earth enhanced luminous efficiency and thermal stability according to claim 2, characterized in that: The M source is at least one of an oxide, a fluoride, a hydroxide and a carbonate containing the M element; and the Z source is a carbonate containing the Z element.
5. The method for preparing a near-infrared phosphor with rare earth enhanced luminous efficiency and thermal stability according to claim 2, characterized in that: The mechanical activation method is high-energy ball milling or grinding; the mechanical activation is performed until the raw material particle size is 5-10 μm.
6. The method for preparing a near-infrared phosphor with rare earth enhanced luminous efficiency and thermal stability according to claim 2, characterized in that: The sintering method is programmed temperature sintering, and the conditions are: in a protective atmosphere, the temperature is raised from room temperature to 1100-1200° C. at 8-12° C. / min, kept at that temperature for 4 hours, and cooled to room temperature along with the furnace.
7. The method for preparing a near-infrared phosphor with rare earth enhanced luminous efficiency and thermal stability according to claim 6, characterized in that: The protective atmosphere is high-purity nitrogen and / or high-purity argon.
8. The use of a near-infrared phosphor with rare earth enhanced luminous efficiency and thermal stability as claimed in claim 1, characterized in that: Used to prepare near-infrared light source for eye protection devices.
9. The use of a near-infrared phosphor with rare earth enhanced luminous efficiency and thermal stability according to claim 8, characterized in that: The near-infrared light source comprises a monochromatic LED chip, a near-infrared fluorescent material coated on the surface of the monochromatic LED chip, and a silica gel packaging layer; the wavelength of the near-infrared light source is 700-900nm, and the optical power is 10-130mW.