Short-process and high-Zr-element-yield ZM6 alloy smelting method
By using technical means such as Mg-20wt.%Zr master alloy and argon gas protection in the smelting of ZM6 alloy, the problem of low Zr yield was solved, the uniform distribution of high Zr elements and the improvement of mechanical properties were achieved, significantly improving the alloy The tensile strength and yield strength simplify the process and reduce costs.
Patent Information
- Application Number
- CN202410900475.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-05
- Publication Date
- 2024-10-29
AI Technical Summary
The yield of Zr during the traditional smelting process of ZM6 alloy is low, which makes it difficult to improve the mechanical properties and the cost is high. The existing technology cannot effectively solve the problem of improving the yield and mechanical properties of zirconium.
Adopting a short process method, by using pure Mg, pure Zn, Mg-30wt.%Nd and Mg-20wt.%Zr master alloy as ingredients, combined with argon protection and RJ-5 refining agent, smelting and stirring at a specific temperature , shorten the smelting time, increase the diffusion speed and uniform distribution of Zr, reduce melt oxidation, and achieve high Zr element yield.
The zirconium content and mechanical properties of ZM6 alloy are significantly improved, the tensile strength is increased by more than 14%, the yield strength is increased by more than 20%, and the elongation is increased by more than 66.7%, while reducing process complexity and cost.
Smart Images

Figure CN118854097A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of magnesium alloy smelting, in particular to a method for smelting a ZM6 alloy with a short process and high Zr element yield. Background Art
[0002] ZM6 is one of the "magnesium-rare earth metal-zirconium alloys" and one of the three major series of cast magnesium alloys. ZM6 is composed of four alloying elements and has a high degree of alloying. Its mechanical properties: in HB7780-2005, it is required to reach σb≥225MPa, σ0.2≥135MPa, and δ5≥3% in the T6 state. With the rapid development of aerospace technology, aviation standards can no longer meet the needs, and it is necessary to further improve the mechanical indicators of materials. Among them, Zr can refine the grains and improve the mechanical properties. Therefore, improving the yield of Zr plays a very important role.
[0003] In the traditional Zr-containing ZM6 alloy smelting process, Zr is often added directly into the smelting furnace. The solubility of Zr in magnesium is very low, and the Zr yield is very low. In addition, since the density of Mg is lower than that of Zr, it is easy to sink to the bottom of the ZM6 alloy melt after being added, resulting in the segregation of the ZM6 alloy melt composition. The Zr yield is low and its content cannot be stably controlled, which ultimately leads to the ZM6 alloy failing to meet its chemical composition, slag and other index requirements, and the product quality fluctuates greatly. If it is unqualified, the entire furnace will be scrapped, causing significant economic losses.
[0004] At present, the research and development of ZM6 has received extensive attention and great attention at home and abroad, and ZM6 alloys with higher mechanical properties have been developed. Among these ZM6 alloys that have been trial-produced and studied, they are mainly divided into:
[0005] (1) Use recycled ingots and Mg-30wt.% Zr and other materials as ingredients. The smelting process requires adjusting the temperature before adding each metal material. Some also require lowering the smelting furnace temperature after the magnesium ingot is melted, and some require lowering the smelting furnace temperature before adding Mg-Nd alloy. The smelting process is relatively cumbersome and takes a long time.
[0006] (2) Some studies have also added all the raw materials of Mg, Al, Zn, Zr, Nd, Fe, Si, Cu and Ni elements into the smelting process at one time, tested the composition after smelting, and refined them after passing the test. This process is relatively simple and is considered to be a promising new generation of ZM6 alloy material.
[0007] For example: Patent application CN 115386747A (method for preparing ZM5 and ZM6 magnesium alloys) obtains good room temperature mechanical properties by adding Al, Zn, Zr, Nd, Fe, Si, Cu and Ni elements, but the cost is high and the composition is uneven, and the yield of zirconium is not involved. Patent application CN104550863A (sand casting process for producing magnesium alloy ZM6) prepares ZM6 alloy by adding recycled ingots and rare earth metals (referring to magnesium alloys containing rare earth) other than magnesium zirconium master alloy and magnesium neodymium master alloy, but does not involve the improvement of the mechanical properties of the alloy and the yield of zirconium. Patent CN 104165789A (casting method for ZM6 alloy spectral standard) requires multiple adjustments to the temperature of the resistance furnace to prepare the ZM6 alloy, but the operation process is complicated, and does not involve the yield of zirconium in the ZM6 alloy, and improve the mechanical properties of the casting.
[0008] In summary, with the development of the industry, new requirements have been put forward for the yield and mechanical properties of ZM6 materials. When ZM6 alloy is prepared through traditional MgZr30 alloy, Zr diffuses slowly, unevenly, is easily burned and easily sinks to the bottom, resulting in a low yield of Zr, insufficient grain refinement, and difficulty in improving the mechanical properties of castings. The current commonly used method of refining grains by greatly increasing or even multiplying the content of expensive heavy rare earths such as zirconium and neodymium to improve the mechanical properties of alloys is bound to increase costs sharply and only obtain tensile strength performance benefits of about 10 to 20 MPa, making it difficult to achieve industrial application. And there is no research on improving the yield of Zr and the mechanical properties of castings by using Mg-20wt.%Zr and a short process.
[0009] Therefore, in order to improve the Zr recovery rate during ZM6 alloy smelting, especially for magnesium alloys with strict Zr content requirements, it is of great engineering significance to find a method of using low-cost pure Mg, pure Zn, Mg-30wt.% Nd and Mg-20wt.% Zr intermediate alloys as ingredients and then using a new smelting process to prepare ZM6 alloy. Summary of the invention
[0010] In order to solve the above-mentioned technical problems existing in the prior art, the present invention provides a method for smelting ZM6 alloy with a short process and high Zr element yield, which is specifically achieved through the following technical scheme.
[0011] A method for smelting ZM6 alloy with a short process and high Zr element yield, comprising the following steps:
[0012] (1) Composition determination: ZM6 alloy, the components and their mass percentages of the alloy are: 0.4-0.6wt.% Zn, 2.-2.8wt.% Nd, 1.25-1.3wt.% Zr, and Mg as the balance;
[0013] (2) Ingredient preparation: Ingredients are prepared according to the ZM6 alloy composition determined in step (1), wherein Mg and Zn are added in the form of pure Mg and pure Zr, and Nd and Zr are added in the form of Mg-30wt.%Nd and Mg-20wt.%Zr master alloys, respectively, and the pure Mg, pure Zn, Mg-30wt.%Nd and Mg-20wt.%Zr master alloys are preheated;
[0014] (3) Preparation of auxiliary materials: argon gas and RJ-5 refining agent;
[0015] (4) Melting: Under the protection of argon, when the temperature of the melting furnace reaches 300-350°C, add preheated pure Mg and Mg-30wt.%Nd master alloy, continue to heat the melt until the temperature reaches 770-780°C, add preheated pure Zn and Mg-20wt.%Zr master alloy, stir the alloy melt and keep it warm for 10-20min, remove the scum on the surface of the alloy liquid, keep it warm at 770-780°C, stir it with RJ-5 refining agent for 5-10min, remove the scum on the alloy liquid, cool it to 725-740°C after treatment, and let it stand for 10-15min, then inject the smelted alloy liquid into the sand core and cast it into an ingot with a diameter of ≤120 and a height of ≤240;
[0016] (5) Solution treatment: Heat the ingot obtained by casting to 520-535°C, keep it at this temperature for 13-14 hours, and cool it.
[0017] (6) Aging treatment: The alloy after solution treatment is aged at a temperature of 190 to 215°C for 12 to 14 hours, followed by cooling.
[0018] Furthermore, the preheating in step (2) is specifically to preheat the pure Mg, pure Zn, Mg-30wt.% Nd and Mg-20wt.% Zr master alloys in an oven at 250°C to 360°C for 1.5h to 2h.
[0019] Furthermore, the argon gas is 99.99% argon gas.
[0020] Furthermore, in step (4), the alloy melt is stirred and kept warm for 15 minutes.
[0021] Furthermore, in step (4), the smelted alloy liquid is poured into the sand core for casting, specifically by using differential pressure casting equipment.
[0022] Furthermore, the cooling method used in steps (5) and (6) is air cooling.
[0023] Compared with the prior art, the technical effects created by the present invention are embodied in:
[0024] (1) The Zr particles in the ZM6 alloy obtained by the method of the present application are dispersedly distributed, the zirconium content is high, the component segregation is small, and the inclusions are less.
[0025] (2) The present application adopts a method of adding multiple components simultaneously, which can shorten the smelting time and improve the smelting efficiency. In addition, the simultaneous addition of multiple components helps to ensure the uniform distribution of various components in the melt, which helps to obtain high-quality ZM6 alloy.
[0026] (3) The method of the present application requires fewer times of adding alloy ingots, which can reduce melt oxidation and thus reduce material consumption.
[0027] (4) The temperature change of the molten metal in the smelting process of the present application only needs to be heated to 770-780°C for refining, and then cooled to 725-740°C for waiting for casting. There is no need to heat up or cool down. During the smelting process, it is only necessary to increase the temperature of the molten metal, and then close the smelting furnace after the refining is completed. When the temperature of the molten metal reaches the temperature required for the casting by differential pressure casting, casting can be performed. This makes the process have the advantages of simple operation, short process, and high efficiency.
[0028] (5) The present application uses a Mg-20wt.% Zr master alloy. Compared with the traditional Mg-30wt.% Zr master alloy, Zr has the advantages of fast diffusion speed, less burning loss, less sinking to the bottom, and higher yield.
[0029] (6) The zirconium yield of the ZM6 alloy ingot prepared in the present application is 44%. The mechanical properties of the ZM6 alloy are improved by increasing the Zr yield.
[0030] (7) The mechanical properties of the ZM6 alloy prepared by the magnesium alloy preparation method of the present invention are significantly improved. Compared with the ZM6 alloy prepared by the prior art process, the tensile strength of the prepared ZM6 alloy is increased by more than 14%, the yield strength is increased by more than 20%, and the elongation is increased by more than 66.7%. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is a photograph of the entirety of the obtained ZM6 alloy ingot.
[0032] Figure 2 It is the microstructure diagram of Mg-20wt.%Zr master alloy.
[0033] Figure 3 It is the microstructure diagram of the obtained ZM6 alloy ingot.
[0034] Figure 4 It is a structural diagram of the pouring casting used. DETAILED DESCRIPTION
[0035] The technical solution of the present invention is further defined below in conjunction with specific implementation methods, but the scope of protection required is not limited to the description.
[0036] Example 1
[0037] Pouring preparation: Use differential pressure pouring, 6 slot runners, such as Figure 4 As shown,
[0038] Pouring: The outer mold and sand core are made of resin sand, and the end chiller is placed in the middle of the runner. Pouring is performed at 725-740℃.
[0039] The pouring parameters are: tank pressure 500-520Mpa, liquid rising speed 38-40mm / s, liquid rising pressure 18-20Kpa, filling pressure 41-43Kpa, boosting pressure 10-11Kpa, boosting speed 1.5-2Kpa / s, crystallization time 210-220s, unpacking time 1.5-2h. The pouring effect is better at this time.
[0040] The smelting steps are as follows:
[0041] (1) Composition determination: ZM6 alloy, the weight of each component of the alloy is as follows:
[0042] Material Name Actual mass / kg Mg-20%Zr 12.92 Zn 0.87 Mg-30wt.%Nd 21.74 Mg 164.47
[0043] (2) Material preparation: The materials are prepared according to the ZM6 alloy composition determined in step (1), wherein Mg and Zn are added in the form of pure Mg and pure Zr, and Nd and Zr are added in the form of Mg-30wt.%Nd and Mg-20wt.%Zr master alloys, respectively (the specific raw material types are as described in step (1), and the pure Mg, pure Zn, Mg-30wt.%Nd and Mg-20wt.%Zr master alloys are preheated in an oven at 250°C to 360°C for 1.5h to 2h;
[0044] (3) Preparation of auxiliary materials: argon gas and RJ-5 refining agent;
[0045] (4) Melting: under the protection of 99.99% argon, when the temperature of the melting furnace reaches 300-350°C, add preheated pure Mg and Mg-30wt.%Nd master alloy, continue to heat the melt until the temperature reaches 770-780°C, add preheated pure Zn and Mg-20wt.%Zr master alloy, stir the alloy melt and keep it warm for 15 minutes, remove the scum on the surface of the alloy liquid, keep it warm at 770-780°C, stir it with RJ-5 refining agent for 5-10 minutes, remove the scum on the alloy liquid, cool it to 725-740°C after treatment, and let it stand for 10-15 minutes, then inject the smelted alloy liquid into the sand core and cast it into an ingot with a diameter of ≤120 and a height of ≤240;
[0046] (5) Solution treatment: Heat the ingot obtained by casting to 520-535°C, keep it at this temperature for 13-14 hours, and air cool it.
[0047] (6) Aging treatment: The alloy after solution treatment is aged at a temperature of 190 to 215°C for 12 to 14 hours and air cooled.
[0048] Comparative Example 1
[0049] Conventional technology smelting solution:
[0050] Melting materials: pure Mg, pure Zn, Mg-30wt.%Nd and Mg-30wt.%Zr master alloys. The chemical composition by mass percentage is: Al: 8.5%, Zn: 0.5%, Mn: 0.35, and the balance is Mg.
[0051] Melting steps:
[0052] Step 1: Preheat the cleaned crucible until the material turns dark red, sprinkle a proper amount of flux into the crucible, and then add the recycled material and magnesium ingot into the crucible in sequence;
[0053] Step 2: Continue heating the crucible, and when the temperature of the alloy material in the crucible rises to 700° C. to 720° C., add zinc into the crucible;
[0054] Step 3: Continue to heat the crucible, and when the temperature of the alloy material in the crucible rises to 760° C. to 770° C., add the magnesium-neodymium master alloy into the crucible;
[0055] Step 4: Continue to heat the crucible, and when the temperature of the alloy material in the crucible rises to 780°C to 810°C, add magnesium-zirconium master alloy into the crucible;
[0056] Step 5: Sprinkle a proper amount of flux into the crucible, control the temperature of the alloy material in the crucible at 770° C. to 780° C., and continuously stir all the alloy materials in the crucible for 4 to 5 minutes, so that the alloy materials in the crucible are refined during the stirring process;
[0057] Step 6: controlling the temperature of the alloy material in the crucible at 770° C. to 780° C., continuously feeding argon gas into the alloy material in the crucible, and continuously stirring all the alloy materials in the crucible for 1 min to 2 min, so that the alloy material in the crucible is refined during the stirring process;
[0058] Step 7: The alloy material in the crucible is heated to 780° C. to 810° C., kept at this temperature and allowed to stand for 20 min to 30 min, and the refining is completed.
[0059] Preheating the alloy: In step 3 or step 4, preheat the magnesium-neodymium master alloy or the magnesium-zirconium master alloy to above 450°C.
[0060] Casting method: gravity casting.
[0061] Chemical composition test report of magnesium alloy ingot cast by the technology of the present invention (Example 1)
[0062]
[0063] The zirconium yield of the prepared ZM6 alloy ingot is 44%
[0064] Comparison of mechanical properties of the prepared ZM6 alloy ingot after heat treatment with those of conventional technology:
[0065]
[0066] It can be seen from the above table that the mechanical properties of the ZM6 alloy prepared by the magnesium alloy preparation method of the present invention are significantly improved. Specifically, the ZM6 alloy prepared by the magnesium alloy preparation method of the present invention has a tensile strength increased by more than 14%, a yield strength increased by more than 20%, and an elongation increased by more than 66.7% compared with the ZM6 alloy prepared by the prior art process.
[0067] In summary, the ZM6 magnesium alloy preparation method of the present invention effectively improves the zirconium recovery rate in the magnesium alloy melt by adjusting the alloy composition, preparing the Mg-20wt.% Zr alloy ingot in advance and formulating a new smelting method, and the inclusions are small, and through reasonable heat treatment, the mechanical properties of the ZM6 magnesium alloy product are significantly improved. At the same time, the ZM6 magnesium alloy preparation method of the present invention also has the advantages of easy operation, short process and low cost.
[0068] Finally, it should be pointed out that the above embodiments are only representative examples of the present invention. Obviously, the technical solution of the present invention is not limited to the above embodiments, and there are many variations. All variations that can be directly derived or associated with the content disclosed by ordinary technicians in this field should be considered as the protection scope of the present invention.
Claims
1. A method for smelting ZM6 alloy with a short process and high Zr element yield, characterized in that: The following steps are involved: (1) Composition determination: ZM6 alloy, the components and their mass percentages of the alloy are: 0.4-0.6wt.% Zn, 2.-2.8wt.% Nd, 1.25-1.3wt.% Zr, and Mg as the balance; (2) Ingredient preparation: Ingredients are prepared according to the ZM6 alloy composition determined in step (1), wherein Mg and Zn are added in the form of pure Mg and pure Zr, and Nd and Zr are added in the form of Mg-30wt.%Nd and Mg-20wt.%Zr master alloys, respectively, and the pure Mg, pure Zn, Mg-30wt.%Nd and Mg-20wt.%Zr master alloys are preheated; (3) Preparation of auxiliary materials: argon gas and RJ-5 refining agent; (4) Melting: Under the protection of argon, when the temperature of the melting furnace reaches 300-350°C, add preheated pure Mg and Mg-30wt.%Nd master alloy, continue to heat the melt until the temperature reaches 770-780°C, add preheated pure Zn and Mg-20wt.%Zr master alloy, stir the alloy melt and keep it warm for 10-20min, remove the scum on the surface of the alloy liquid, keep it warm at 770-780°C, stir it with RJ-5 refining agent for 5-10min, remove the scum on the alloy liquid, cool it to 725-740°C after treatment, and let it stand for 10-15min, then inject the smelted alloy liquid into the sand core and cast it into an ingot with a diameter of ≤120 and a height of ≤240; (5) Solution treatment: Heat the ingot obtained by casting to 520-535°C, keep it at this temperature for 13-14 hours, and cool it. (6) Aging treatment: The alloy after solution treatment is aged at a temperature of 190 to 215°C for 12 to 14 hours, followed by cooling.
2. The method for smelting ZM6 alloy with a short process and high Zr element yield according to claim 1, characterized in that: The preheating in step (2) is specifically to preheat the pure Mg, pure Zn, Mg-30wt.% Nd and Mg-20wt.% Zr master alloys in an oven at 250°C to 360°C for 1.5h to 2h.
3. The method for smelting ZM6 alloy with a short process and high Zr element yield according to claim 1, characterized in that: The argon gas is 99.99% argon gas.
4. The method for smelting ZM6 alloy with a short process and high Zr element yield according to claim 1, characterized in that: In the step (4), the alloy melt is stirred and kept warm for 15 minutes.
5. The method for smelting ZM6 alloy with a short process and high Zr element yield according to claim 1, characterized in that: In the step (4), the smelted alloy liquid is injected into the sand core for casting, which is specifically carried out by using differential pressure casting equipment.
6. The method for smelting ZM6 alloy with a short process and high Zr element yield according to claim 1, characterized in that: The cooling method used in steps (5) and (6) is air cooling.