Preparation method of bis-benzimidazole derivative compounded corrosion inhibitor and product thereof

By preparing bisbenzimidazole derivative compound corrosion inhibitor HBH-A, the problem of insufficient performance of existing corrosion inhibitors in high temperature and high pressure environments has been solved, effective protection of metal pipe columns has been achieved, and corrosion inhibition performance has been significantly improved. and stability.

CN118854291APending Publication Date: 2024-10-29CHANGZHOU UNIV

Patent Information

Application Number
CN202410769866.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-14
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing corrosion inhibitors have problems such as low corrosion inhibition rate, poor solubility, easy coking, precipitation, stratification, and poor compatibility under high temperature and high pressure environments. It is difficult to effectively protect the metal pipe strings in oil wells, leading to corrosion damage and risk of structural collapse. .

Method used

A preparation method of a bisbenzimidazole derivative compound corrosion inhibitor is adopted, by reacting o-phenylenediamine and fatty acids under heating conditions, adding polyphosphoric acid and absolute ethanol, performing vacuum distillation and recrystallization to form a corrosion inhibitor with Stable and hydrophobic HBH is then compounded with surfactants to obtain HBH-A corrosion inhibitor.

Benefits of technology

HBH-A corrosion inhibitor maintains stability in high temperature and high pressure environments. It is firmly adsorbed on the metal surface by forming Fe-N bonds and Fe-C coordination bonds, blocking the contact with corrosive substances, significantly improving the metal protection effect, and The hydrophobic layer enhances the ability to isolate corrosive media and significantly improves corrosion inhibition performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854291A_ABST
    Figure CN118854291A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a bis-benzimidazole derivative compounded corrosion inhibitor and a product thereof, and the bis-benzimidazole derivative compounded corrosion inhibitor comprises o-phenylenediamine, fatty acid (oleic acid and isocaprylic acid), 1, 6-dichlorohexane and absolute ethyl alcohol. The novel bis-benzimidazole derivative (HBH) prepared by the invention contains a bis-benzimidazole ring, and can form a plurality of Fe-N bonds and a plurality of additional Fe-C coordinate bonds, so that the novel bis-benzimidazole derivative (HBH) is stably adsorbed on the surface of metal to form a protective film to isolate a corrosive medium and protect the metal; the compound corrosion inhibitor (HBH-A) is a mixed type corrosion inhibitor, and the inhibition of the cathode reaction is more obvious.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of corrosion inhibitor preparation, and specifically relates to a preparation method of a bisbenzimidazole derivative composite corrosion inhibitor and a product thereof. Background Art

[0002] In oil and gas exploration, development and production operations, oil pipes and casings play a vital role. Low-carbon steel and carbon steel are widely used due to their low cost. However, the high temperature, high pressure, acidic environment underground can easily lead to serious corrosion damage, which not only affects the mining efficiency, but also easily scratches the oil wells and even causes structural collapse, bringing huge challenges to the safe production of oil fields and causing huge impacts on the economy and the environment.

[0003] The earliest research on corrosion damage was to slow down corrosion through cathodic protection and injection of corrosion inhibitors. Currently, the main methods proposed to control corrosion include reasonable material selection, pipeline internal coating, and improvement of the corrosion environment. However, the application of corrosion inhibitors is still the most effective and convenient way to solve the corrosion problem.

[0004] However, as the exploration and development of oil and gas fields develops towards deep and ultra-deep layers, most of the corrosion inhibitors currently studied and developed have disadvantages such as low corrosion inhibition rate, poor solubility and dispersibility, easy coking, precipitation, stratification, and poor compatibility. They are not suitable for complex and extreme corrosion environments such as high temperature and high pressure.

[0005] Therefore, it is urgent to develop a corrosion inhibitor suitable for high temperature and high pressure conditions to protect metal pipes and ensure safety during mining and transportation. Summary of the invention

[0006] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.

[0007] In view of the above problems and / or the problems existing in the prior art, the present invention is proposed.

[0008] Therefore, the purpose of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a composite corrosion inhibitor of a bisbenzimidazole derivative.

[0009] In order to solve the above technical problems, the present invention provides the following technical solution: a method for preparing a composite corrosion inhibitor of a bisbenzimidazole derivative, comprising:

[0010] Heat o-phenylenediamine and fatty acid to reflux and stir for reaction, add polyphosphoric acid, heat to reflux and stir for reaction, and obtain a reaction mixture;

[0011] The obtained mixture was cooled and distilled under reduced pressure;

[0012] After the vacuum distillation is completed, add 1,6-dichlorohexane and anhydrous ethanol, heat under reflux and stir for 4 hours;

[0013] The reaction mixture was cooled and then distilled under reduced pressure and recrystallized to obtain the target product HBH;

[0014] The compound corrosion inhibitor HBH-A was obtained by compounding HBH with a surfactant.

[0015] As a preferred embodiment of the preparation method of the present invention, the fatty acid comprises oleic acid and isooctanoic acid.

[0016] As a preferred embodiment of the preparation method of the present invention, the molar ratio of o-phenylenediamine to fatty acid is 0.01-0.02:0.01-0.02.

[0017] As a preferred embodiment of the preparation method of the present invention, wherein: o-phenylenediamine and fatty acid are heated to reflux and stirred for reaction, wherein the heating reflux and stirring reaction time is 1 to 2 hours, and the reaction temperature is 150 to 160°C.

[0018] As a preferred embodiment of the preparation method of the present invention, the ratio of o-phenylenediamine to polyphosphoric acid is 0.02 mol: 0.3-0.5 mL.

[0019] As a preferred embodiment of the preparation method of the present invention, the temperature is raised to reflux and stirred for reaction, wherein the reaction time is 3 hours and the reaction temperature is 200-210°C.

[0020] As a preferred embodiment of the preparation method of the present invention, the obtained mixture is cooled and then distilled under reduced pressure, wherein the distillation temperature under reduced pressure is 110°C.

[0021] As a preferred embodiment of the preparation method of the present invention, the ratio of o-phenylenediamine, 1,6-dichlorohexane and anhydrous ethanol is 0.02 mol: 0.06 mol: 5-10 mL;

[0022] The heating reflux stirring is performed for 4 hours at a temperature of 80-85°C;

[0023] The vacuum distillation is carried out by step-by-step temperature increase, which is set at 50°C, 80°C, and 110°C respectively, and three consecutive vacuum distillations are carried out;

[0024] The recrystallization comprises: after cooling the crude product after three consecutive vacuum distillations, adding a mixed solvent of ethanol and water, stirring evenly until completely dissolved, then slowly heating and stirring until boiling, and obtaining the target product after boiling is completed, wherein the volume ratio of ethanol to water is 1:1.

[0025] As a preferred embodiment of the preparation method of the present invention, the surfactant includes AEO-5, and the HBH and the surfactant are compounded to include 85% HBH, 5% AEO-5 and 10% anhydrous ethanol in terms of mass percentage.

[0026] Another object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing a composite corrosion inhibitor of a bisbenzimidazole derivative, wherein the bisbenzimidazole derivative has a structure shown in Formula 1:

[0027]

[0028] Beneficial effects of the present invention:

[0029] (1) The HBH prepared by the present invention contains two benzimidazole structures, and there is a highly active N atom at the 1st and 3rd positions of the imidazole ring. The four N atom adsorption sites interact with the iron surface and form Fe-N bonds, which can be stably adsorbed on the metal surface, so that HBH is still stable under high temperature and high pressure environments.

[0030] (2) The two benzimidazole rings of HBH prepared in the present invention provide four aromatic rings (benzene ring, imidazole ring). The π electrons on the aromatic rings provide sufficient charge for the empty d orbitals of the iron atoms, forming additional multiple Fe-C coordination bonds, which enable the bibenzimidazole rings in the HBH molecule to be stably and firmly adsorbed on the metal surface to form a strong adsorption film, which can block the contact between the carbon steel surface and corrosive substances, thereby effectively protecting the metal.

[0031] (3) The HBH prepared in the present invention contains two long alkyl chains. With the firm adsorption of the two benzimidazole rings, the two long alkyl chains are drawn to the iron surface to form a hydrophobic layer, which has high hydrophobicity and further increases the ability of the protective film to isolate corrosive media.

[0032] (4) The HBH prepared in the present invention is quaternized on the basis of the bisbenzimidazole structure and compounded with the surfactant AEO-5. The obtained compound corrosion inhibitor HBH-A has good water solubility and excellent corrosion inhibition performance, and can effectively inhibit corrosion and protect metals. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:

[0034] Figure 1 FT-IR characterization of HBH in the embodiment of the present invention;

[0035] Figure 2 The Nyquist plot of N80 carbon steel in 1% NaCl solution without or with different concentrations of HBH-A in the embodiment of the present invention;

[0036] Figure 3 The Bode diagram of N80 carbon steel in 1% NaCl solution without or with different concentrations of HBH-A in the embodiment of the present invention;

[0037] Figure 4 is the electrochemical equivalent circuit for fitting the 1% NaCl solution without (a) and with (b) HBH-A;

[0038] Figure 5 The potentiodynamic polarization curves of N80 carbon steel in 1% NaCl solution without or with different concentrations of HBH-A added;

[0039] Figure 6 The corrosion rate and inhibition rate of N80 carbon steel after immersion in 1% NaCl solution with different concentrations of AEO-5 at 80℃ and 0.4Mpa for 72h.

[0040] Figure 7 N80 carbon steel at 80℃, 0.4Mpa, without additives and with 100mg·L -1 Corrosion rate and inhibition rate of different types of composite corrosion inhibitors after immersion in 1% NaCl solution for 72 hours. DETAILED DESCRIPTION

[0041] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0042] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0043] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0044] The principle of the generation of the bisbenzimidazole derivatives of the present invention:

[0045] At high temperature, o-phenylenediamine reacts with fatty acids to form amides through intermolecular condensation. The diamino structure of o-phenylenediamine provides two addition-elimination reaction interfaces. Then, the N atom and the lone pair of electrons react with the amides through intramolecular dehydration. Under acidic conditions, the ring is directly closed to form a benzimidazole ring, and finally quaternization is performed to form a bisbenzimidazole ring.

[0046] Example 1

[0047] This embodiment provides a preparation method of a novel bisbenzimidazole derivative (HBH) and a composite corrosion inhibitor (HBH-A):

[0048] ① Add 0.02 mol of o-phenylenediamine and 0.02 mol of fatty acid (0.01 mol each of oleic acid and isooctanoic acid) into a round-bottom flask in sequence, heat and reflux at 150°C in a magnetic stirrer for 2 h, then add 0.4 mL of polyphosphoric acid, heat to 210°C and reflux for 3 h;

[0049] ② The mixture obtained by the reaction was cooled to 110°C and distilled under reduced pressure;

[0050] ③Add 0.06mol 1,6-dichlorohexane and 10mL anhydrous ethanol, heat to 80℃ and reflux with stirring for 4h;

[0051] ④ After the reaction mixture is cooled, the temperature is set at 50°C, 80°C and 110°C respectively, and vacuum distillation is performed three times continuously, and recrystallization is performed to obtain the target product HBH;

[0052] ⑤ Compound HBH with a surfactant in a mass ratio of 85% HBH + 5% AEO-5 + 10% anhydrous ethanol to obtain a compound corrosion inhibitor HBH-A.

[0053] (1) The infrared spectrum of the target product HBH is shown in Figure 1 , we can see that at 741.90cm -1 The sharp peak at 878.32 cm is the absorption peak of -CH2+substituted on the benzene ring. -1 The stretching vibration absorption peak of imidazole ring C=CH is 1218.93cm -1 The in-plane bending and stretching vibration absorption peak of -CH is 1273.31cm-1 The stretching vibration absorption peak of CN- (aromatic hydrocarbon) is 1458.00cm -1 The vibration peak of the benzene ring skeleton is 1623.52cm -1 The vibration peak of C=N is 2922.25cm -1 and 2852.04cm -1 The peaks at the positions are the asymmetric stretching vibration absorption peaks of -CH3 and the symmetric stretching vibration absorption peaks of -CH2-. Analysis shows that the attribution of the infrared spectrum peaks of the product indicates that the synthetic product contains a benzene ring and an imidazole ring, and contains an alkyl chain. The presence of these functional group vibration peaks can confirm the synthesis of HBH.

[0054] at the same time, Figure 1 At 1373.99cm -1 The -CN stretching vibration absorption peak of the quaternary ammonium salt appears at the quaternary ammonium salt, indicating the quaternization transformation of the product.

[0055] (2) Electrochemical impedance spectroscopy (EIS) measurement

[0056] The traditional three-electrode system was used, the working electrode (WE) was an N80 carbon steel sample, and the test area was 1cm 2 The auxiliary electrode (CE) was a platinum electrode, and the reference electrode (SCE) was a saturated calomel electrode. Before the experiment, the working electrode was immersed in water without adding or adding different concentrations (10, 25, 50, 80, 100 mg·L -1 )HBH-A in 1% NaCl solution for 30 min to stabilize the corrosion potential.

[0057] (I) Electrochemical impedance spectroscopy (EIS) test

[0058] The AC excitation signal amplitude is 5mV, and the test frequency range is 0.01Hz~10 5 Hz, and use formula (1) to calculate the corrosion inhibition efficiency η of the sample EIS :

[0059]

[0060] Where R c1 (Ω) and R c0 (Ω) are the charge transfer resistance of the samples without and with corrosion inhibitors, respectively.

[0061] (II) Polarization curve test

[0062] The polarization curve was measured in the voltage range of -0.2V to 0.2V, with a scanning rate of 0.5mV / s, and the corrosion inhibition efficiency η of the sample was calculated using formula (2): p :

[0063]

[0064] Where i c0 (mA cm -2 ) and i c1 (mA cm -2 ) are the corrosion current densities of the samples without and with corrosion inhibitors, respectively.

[0065] Figure 2 , Figure 3 These are the Nyquist and Bode plots of N80 carbon steel in 1% NaCl solution without or with different concentrations of HBH-A.

[0066] like Figure 2 As shown, the Nyquist diagram shows a semicircular capacitance in the entire frequency range, indicating that the electrode reaction is controlled by the charge transfer process. In the solution containing corrosion inhibitor, the diameter of the semicircle is larger than that of the solution without corrosion inhibitor, and increases with the increase of corrosion inhibitor concentration. This is because the coverage of corrosion inhibitor molecules increases, indicating that the protectiveness of the adsorption film formed by the corrosion inhibitor gradually increases.

[0067] like Figure 3 As shown in the Bode diagram, the phase angle shows a single time constant over the entire test frequency. When the corrosion inhibitor is added and the concentration is gradually increased, the frequency range of the maximum phase angle becomes larger, indicating that the corrosion inhibitor is effectively adsorbed on the N80 carbon steel and becomes increasingly stable. The substantial increase in the low-frequency impedance modulus further proves the enhanced ability of the adsorption film formed by the corrosion inhibitor to isolate the corrosive medium, indicating that the corrosion inhibitor has efficient corrosion inhibition performance.

[0068] The electrochemical parameters were Figure 4 The equivalent circuits of (a) and (b) were fitted with the EIS data, and the fitting results are shown in Table 1.

[0069] In the equivalent circuit, R s is the solution resistance, R ct is the charge transfer resistance, Rf is the resistance of the corrosion inhibitor adsorption film on the surface of N80 carbon steel, CPE dl and CPE f are the constant phase angle elements of the double electric layer and the adsorption film respectively. The constant phase angle element CPE is defined by formula (3):

[0070] CPE=Y0(2πf max ) n-1 (3)

[0071] Where f is the frequency corresponding to the maximum imaginary value; Y0 and n are the amplitude and phase shift constant of CPE respectively.

[0072] Table 1 EIS fitting parameters of N80 carbon steel in 1% NaCl solution without and with different concentrations of HBH-A

[0073]

[0074]

[0075] As shown in Table 1, as the concentration of HBH-A increases, the charge transfer resistance R ct It gradually increases, which is due to the decrease in dielectric constant and / or the increase in the thickness of the double capacitance layer and the adsorption film capacitance layer, indicating that the exposed surface of the carbon steel gradually decreases and the number of corrosion inhibitor molecules adsorbed on the surface to form a film gradually increases;

[0076] Double capacitor layer C dl With the charge transfer resistance R ct This is because the substitution between the corrosion inhibitor molecules and the chloride ions and water molecules on the surface of carbon steel forms an effective adsorption film, which reduces the additional charge and mass transfer. This shows that the corrosion inhibitor molecules have good adsorption on the surface of carbon steel and have strong protection for carbon steel.

[0077] (3) Polarization curve test

[0078] Figure 5 Polarization curves of N80 carbon steel in 1% NaCl solution without or with different concentrations of HBH-A.

[0079] The corresponding electrochemical parameters of the polarization curves were obtained by Tafel extrapolation method, as shown in Table 2.

[0080] like Figure 5 As shown in the figure, when HBH-A is added to the corrosive medium, the current density of the cathode and the anode is reduced, which shows that the addition of the corrosion inhibitor has an inhibitory effect on both the cathode and anode reactions; generally speaking, if the corrosion potential change is greater than ±85mV, the corrosion inhibitor can be divided into cathode type or anode type, which affects the hydrogen evolution reaction (cathode) and metal dissolution (anode), respectively, otherwise it can be considered as a mixed corrosion inhibitor. In this study, the addition of HBH-A caused a change in corrosion potential of less than ±85mV, which is a mixed corrosion inhibitor.

[0081] Table 2 Polarization curve fitting parameters of N80 carbon steel in 1% NaCl solution without and with different concentrations of HBH-A

[0082] As shown in Table 2, with the increase of HBH-A concentration, the self-corrosion current density gradually decreases, indicating that the corrosion rate of the sample gradually decreases; after adding HBH-A, the Tafel slope (β c ,β a )

[0083]

[0084] Both of them have undergone small changes, but the anode slope has changed even less, indicating that the reduction of cathode current density is more important than that of anode. The reduction in cathode area is due to the reduction in exposed area of ​​carbon steel surface, indicating that compared with inhibiting anodic dissolution of carbon steel, the addition of corrosion inhibitor to form a stable adsorption film is more effective in inhibiting cathode hydrogen evolution reaction.

[0085] Comparative Example 1

[0086] ① Add 0.02 mol of o-phenylenediamine and 0.02 mol of fatty acid (0.01 mol each of oleic acid and isooctanoic acid) into a round-bottom flask in sequence, heat and reflux at 150°C in a magnetic stirrer for 2 h, then add 0.4 mL of polyphosphoric acid, heat to 210°C and reflux for 3 h;

[0087] ② The mixture obtained by the reaction was cooled to 110°C and distilled under reduced pressure;

[0088] ③Add 0.06mol 1,6-dichlorohexane and 10mL anhydrous ethanol, heat to 80℃ and reflux with stirring for 4h;

[0089] ④ After the reaction mixture is cooled, the temperature is set at 50°C, 80°C and 110°C respectively, and vacuum distillation is performed three times continuously, and recrystallization is performed to obtain the target product HBH;

[0090] ⑤ Compound HBH with a surfactant in a mass ratio of 86% HBH + 4% AEO-5 + 10% anhydrous ethanol to obtain a compound corrosion inhibitor HBH-A.

[0091] Comparative Example 2

[0092] ① Add 0.02 mol of o-phenylenediamine and 0.02 mol of fatty acid (0.01 mol each of oleic acid and isooctanoic acid) into a round-bottom flask in sequence, heat and reflux at 150°C in a magnetic stirrer for 2 h, then add 0.4 mL of polyphosphoric acid, heat to 210°C and reflux for 3 h;

[0093] ② The mixture obtained by the reaction was cooled to 110°C and distilled under reduced pressure;

[0094] ③Add 0.06mol 1,6-dichlorohexane and 10mL anhydrous ethanol, heat to 80℃ and reflux with stirring for 4h;

[0095] ④ After the reaction mixture is cooled, the temperature is set at 50°C, 80°C and 110°C respectively, and vacuum distillation is performed three times continuously, and recrystallization is performed to obtain the target product HBH;

[0096] ⑤ Compound HBH and surfactant in a mass ratio of 87% HBH + 3% AEO-5 + 10% anhydrous ethanol to obtain a compound corrosion inhibitor HBH-A.

[0097] Comparative Example 3

[0098] ① Add 0.02 mol of o-phenylenediamine and 0.02 mol of fatty acid (0.01 mol each of oleic acid and isooctanoic acid) into a round-bottom flask in sequence, heat and reflux at 150°C in a magnetic stirrer for 2 h, then add 0.4 mL of polyphosphoric acid, heat to 210°C and reflux for 3 h;

[0099] ② The mixture obtained by the reaction was cooled to 110°C and distilled under reduced pressure;

[0100] ③Add 0.06mol 1,6-dichlorohexane and 10mL anhydrous ethanol, heat to 80℃ and reflux with stirring for 4h;

[0101] ④ After the reaction mixture is cooled, the temperature is set at 50°C, 80°C and 110°C respectively, and vacuum distillation is performed three times continuously, and recrystallization is performed to obtain the target product HBH;

[0102] ⑤ Compound HBH with a surfactant in a mass ratio of 88% HBH + 2% AEO-5 + 10% anhydrous ethanol to obtain a compound corrosion inhibitor HBH-A.

[0103] Comparative Example 4

[0104] ① Add 0.02 mol of o-phenylenediamine and 0.02 mol of fatty acid (0.01 mol each of oleic acid and isooctanoic acid) into a round-bottom flask in sequence, heat and reflux at 150°C in a magnetic stirrer for 2 h, then add 0.4 mL of polyphosphoric acid, heat to 210°C and reflux for 3 h;

[0105] ② The mixture obtained by the reaction was cooled to 110°C and distilled under reduced pressure;

[0106] ③Add 0.06mol 1,6-dichlorohexane and 10mL anhydrous ethanol, heat to 80℃ and reflux with stirring for 4h;

[0107] ④ After the reaction mixture is cooled, the temperature is set at 50°C, 80°C and 110°C respectively, and vacuum distillation is performed three times continuously, and recrystallization is performed to obtain the target product HBH;

[0108] ⑤ Compound HBH with a surfactant in a mass ratio of 89% HBH + 1% AEO-5 + 10% anhydrous ethanol to obtain a compound corrosion inhibitor HBH-A.

[0109] Corrosion inhibition performance:

[0110] The corrosion rate was determined by weight loss method. The concentration of the fixed compound corrosion inhibitor was 100 mg·L -1When the surfactant (AEO-5) content was 1%, 2%, 3%, 4% and 5%, the polished and weighed N80 carbon steel specimens were immersed in 80℃, 0.4Mpa, 1% NaCl solution for 72h.

[0111] After taking out the sample, it was pickled with 10% dilute hydrochloric acid for 15s, and the corrosion products were removed at room temperature, washed with deionized water, dried with cold air and weighed. According to the corrosion loss of the sample before and after immersion, the corrosion rate υ and the corrosion inhibition rate η were calculated according to formula (4) and formula (5) respectively.

[0112]

[0113] Among them, corr (g·m -2 ·h -1 ) is the corrosion rate; Δw(g) is the mass difference of carbon steel before and after corrosion; ρ(g·cm -3 ) is the density of carbon steel; s(mm 2 ) is the surface area of ​​carbon steel; t(h) is the corrosion time; η(%) is the corrosion inhibition rate; υ1(mm·a -1 ) is the blank corrosion rate; υ2(mm·a -1 ) is the corrosion rate after adding corrosion inhibitor.

[0114] like Figure 6 It can be seen that with the increase of surfactant content, the corrosion rate gradually decreases. This is because as the surfactant concentration increases, the solubility and dispersion of HBH increases, and the water solubility of the compound corrosion inhibitor also gradually increases, which enables the corrosion inhibitor molecules to be more effectively and widely adsorbed on the metal surface. The protective film formed is denser and firmer, which effectively isolates the corrosive medium and reduces the corrosion rate.

[0115] like Figure 6 It can be seen that with the increase of surfactant content, the increase of corrosion inhibition rate shows a trend of first fast and then slow. This is because the degree of dissolution and dispersion of HBH increases with the increase of surfactant concentration. However, when the surfactant concentration is too high, HBH has basically been dissolved and dispersed, so the corrosion inhibition rate increases slowly.

[0116] like Figure 6 As shown, when 85% HBH, 5% AEO-5 and 10% anhydrous ethanol are added to 80°C, 0.4MPa and 1% NaCl solution, HBH has the best solubility and dispersibility and the best corrosion inhibition effect on the sample. Therefore, this system is selected to prepare the composite corrosion inhibitor (HBH-A).

[0117] Comparative Example 5

[0118] ① Add 0.02 mol of o-phenylenediamine and 0.02 mol of fatty acid (0.01 mol each of oleic acid and isooctanoic acid) into a round-bottom flask in sequence, heat and reflux at 150°C in a magnetic stirrer for 2 h, then add 0.4 mL of polyphosphoric acid, heat to 210°C and reflux for 3 h;

[0119] ② The mixture obtained by the reaction was cooled to 110°C and distilled under reduced pressure;

[0120] ③Add 0.06mol 1,6-dichlorohexane and 10mL anhydrous ethanol, heat to 80℃ and reflux with stirring for 4h;

[0121] ④ After the reaction mixture is cooled, the temperature is set at 50°C, 80°C and 110°C respectively, and vacuum distillation is performed three times continuously, and recrystallization is performed to obtain the target product HBH;

[0122] ⑤ Compound HBH and surfactant (polyethylene glycol 4000) in a mass ratio of 89% HBH + 1% polyethylene glycol 4000 + 10% anhydrous ethanol to obtain a compound corrosion inhibitor HBH-A.

[0123] Comparative Example 6

[0124] ① Add 0.02 mol of o-phenylenediamine and 0.02 mol of fatty acid (0.01 mol each of oleic acid and isooctanoic acid) into a round-bottom flask in sequence, heat and reflux at 150°C in a magnetic stirrer for 2 h, then add 0.4 mL of polyphosphoric acid, heat to 210°C and reflux for 3 h;

[0125] ② The mixture obtained by the reaction was cooled to 110°C and distilled under reduced pressure;

[0126] ③Add 0.06mol 1,6-dichlorohexane and 5-10mL anhydrous ethanol, heat to 80℃ and reflux with stirring for 4h;

[0127] ④ After the reaction mixture is cooled, the temperature is set at 50°C, 80°C and 110°C respectively, and vacuum distillation is performed three times continuously, and recrystallization is performed to obtain the target product HBH;

[0128] ⑤ Compound HBH and surfactant (C8-C10-fatty alcohol polyoxyethylene ether) in a mass ratio of 89% HBH + 1% C8-C10-fatty alcohol polyoxyethylene ether + 10% anhydrous ethanol to obtain a compound corrosion inhibitor HBH-A.

[0129] The concentration of the fixed compound corrosion inhibitor is 100 mg·L -1For the three surfactants, polyethylene glycol 4000, C8-C10-fatty alcohol polyoxyethylene ether, and fatty alcohol polyoxyethylene ether (AEO-5), three compound corrosion inhibitors were prepared according to the ratio of 89% HBH + 1% surfactant + 10% anhydrous ethanol.

[0130] The blank group without corrosion inhibitor was used as the reference standard. The static weight loss method was used to study the corrosion of N80 carbon steel at 80℃, 0.4Mpa, without corrosion inhibitor and with 100mg·L -1 The corrosion inhibition performance of different types of compound corrosion inhibitors in 1% NaCl solution after immersion for 72 hours, such as Figure 7 shown.

[0131] like Figure 7 As shown in the figure, the selected surfactants can improve the solubility and dispersibility of the corrosion inhibitor to a certain extent. The blank group is the corrosion rate without adding corrosion inhibitor. -1 Under these conditions, the three compound corrosion inhibitors all slowed down the corrosion rate to a certain extent, among which the AEO-5 surfactant group had the best corrosion inhibition effect and could be used as a surfactant for HBH.

[0132] The yield of the bisbenzimidazole derivative (HBH) prepared in Example 1 (actual yield / theoretical yield×100%) is higher than 77.82%, while in the patent CN 117865897 A, its yield is lower than 30.96%. The HBH preparation method provided in this example adopts the following method to improve the yield:

[0133] ① Since the product is relatively viscous, a large amount of adhesion will be produced and consumed during the transfer process. Therefore, the preparation method provided in this embodiment uses vacuum distillation as a purification method, omitting the transfer step, which can minimize unnecessary consumption of the product;

[0134] ② For multi-stage reactions, the preparation method provided in this embodiment optimizes different vacuum distillation schemes, which is more excellent in purifying the product. In comparison, the product contains fewer impurities;

[0135] ③ The preparation method provided in this embodiment optimizes the conditions such as the amount of catalyst and solvent added, thereby increasing the amount of product synthesized and the yield to a greater extent.

[0136] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.

Claims

1. A method for preparing a composite corrosion inhibitor of a bisbenzimidazole derivative, characterized in that: include, Heat o-phenylenediamine and fatty acid to reflux and stir for reaction, add polyphosphoric acid, heat to reflux and stir for reaction, and obtain a reaction mixture; The obtained mixture was cooled and distilled under reduced pressure; After the vacuum distillation is completed, add 1,6-dichlorohexane and anhydrous ethanol, heat under reflux and stir for 4 hours; The reaction mixture was cooled and then distilled under reduced pressure and recrystallized to obtain the target product HBH; The compound corrosion inhibitor HBH-A was obtained by compounding HBH with a surfactant.

2. The preparation method according to claim 1, characterized in that: The fatty acids include oleic acid and isooctanoic acid.

3. The preparation method according to claim 1 or 2, characterized in that: The molar ratio of o-phenylenediamine to fatty acid is 0.01-0.02:0.01-0.

02.

4. The preparation method according to claim 1 or 2, characterized in that: The o-phenylenediamine and fatty acid are heated to reflux and stirred for reaction, wherein the heating reflux and stirring reaction time is 1 to 2 hours and the reaction temperature is 150 to 160°C.

5. The preparation method according to claim 4, characterized in that: The ratio of o-phenylenediamine to polyphosphoric acid is 0.02 mol: 0.3-0.5 mL.

6. The preparation method according to any one of claims 1, 2 or 5, characterized in that: The temperature-raising, reflux-stirring reaction has a reaction time of 3 hours and a reaction temperature of 200-210°C.

7. The preparation method according to claim 6, characterized in that: The obtained mixture is cooled and then distilled under reduced pressure, wherein the distillation temperature under reduced pressure is 110°C.

8. The preparation method according to claim 1, characterized in that: The ratio of o-phenylenediamine, 1,6-dichlorohexane and anhydrous ethanol is 0.02 mol: 0.06 mol: 5-10 mL; The heating reflux stirring is 4h, and the temperature is 80-85°C; The vacuum distillation is carried out by step-by-step temperature increase, which is set at 50°C, 80°C, and 110°C respectively, and three consecutive vacuum distillations are carried out; The recrystallization comprises: after cooling the crude product after three consecutive vacuum distillations, adding a mixed solvent of ethanol and water, stirring evenly until completely dissolved, then slowly heating and stirring until boiling, and obtaining the target product after boiling is completed, wherein the volume ratio of ethanol to water is 1:

1.

9. The preparation method according to claim 1, characterized in that: The surfactant includes AEO-5, and the HBH is compounded with the surfactant, which includes 85% HBH, 5% AEO-5 and 10% anhydrous ethanol in terms of mass percentage.

10. The bisbenzimidazole derivative composite corrosion inhibitor prepared by the preparation method according to any one of claims 1 to 9, characterized in that: The bisbenzimidazole derivative has a structure shown in Formula 1: 。

Citation Information

Patent Citations

  • N, N-hexane bis (2-benzimidazolyl) n-octadecyl quaternary ammonium salt corrosion inhibitor and preparation method thereof

    CN117865897A

  • New special corrosion inhibitor for oil production

    CN101838811A

  • Metal decontaminating cleaning agent

    CN103510098A

  • Mixed fatty group di(benzimidazoline-ammonium-salt) as well as preparation method and application thereof

    CN106083727A

  • Bisbenzimidazolyl borate compound, preparation method thereof and corrosion inhibitor

    CN108129502A

Cited By

  • N, N-hexane bis (2-benzimidazolyl) n-octadecyl quaternary ammonium salt corrosion inhibitor and preparation method thereof

    CN117865897A

  • Environment-friendly compound constructed by function-integrated molecules, intermediate, preparation method and application

    CN120097920A

  • Cleaning method for double-sided polishing of lithium niobate wafer