A single crystal positive electrode material with defective phase and its preparation method and application

By constructing a single-crystal-like positive electrode material with defective phases, combined with the advantages of single-poly crystals, the problem of insufficient capacity and cycle stability of single-poly crystal materials in the prior art is solved, and the improvement of high capacity and good cycle performance is achieved.

CN118854455BActive Publication Date: 2024-11-22SHENZHEN BTR NEW ENERGY TECH RES INST CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411276594.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-22
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

The existing single-poly crystal positive electrode materials have shortcomings in improving capacity and cycling stability, especially the lack of effective technical means for increasing capacity of single-crystal materials.

Method used

By constructing a single crystal positive electrode material with defective phases, co-precipitation method and multi-stage sintering process are used to form a complex secondary particle structure, and the defective phase is distributed on the particle surface, which improves ion conductivity and enhances material stability, and combines single-poly crystalline Advantages improve capacity.

Benefits of technology

It achieves high capacity and good cycling performance of the material, combines the high particle strength of single crystals and the high rate performance of poly crystals, and improves the electrochemical performance of sodium ion batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118854455B_ABST
    Figure CN118854455B_ABST
Patent Text Reader

Abstract

The present invention discloses a quasi-single crystal positive electrode material with a defective phase, and a preparation method and application thereof. The quasi-single crystal positive electrode material includes a plurality of secondary particles, and the secondary particles are formed by assembling 5-12 primary particles. The quasi-single crystal positive electrode material has a defective phase, and the defective phase is distributed on the surface of each primary particle assembled with each other; wherein, when the quasi-single crystal positive electrode material is charged, dQ / dV≥1.5mAh / V within the voltage range of 4.0-4.1V. The quasi-single crystal positive electrode material provided by the present invention has the characteristics of high rate and high capacity in battery applications. At the same time, the quasi-single crystal positive electrode material of the present invention fully combines the advantages of single and polycrystalline materials, and uniquely constructs defective phases to further improve the material capacity.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of sodium ion batteries, and in particular relates to a single-crystal-like positive electrode material with a defective phase, and a preparation method and application thereof. Background Art

[0002] Due to the constraints of factors such as the shortage of traditional fossil energy and energy security, as well as the enhancement of people's awareness of ecological and environmental protection, the sustainable development and storage of energy have received great attention. Among various energy storage systems, electrochemical energy storage systems (EES) are considered to be an effective way to balance the cycle characteristics of renewable energy due to their long service life, low cost, low investment, and easy installation. Secondary battery energy storage has great potential in electrochemical energy storage. Among them, lithium-ion batteries dominate the energy storage market due to their high theoretical specific capacity and specific energy density. However, due to the limited reserves and uneven distribution of lithium (Li) resources and the multi-faceted consumption of lithium, subject to objective factors such as lithium extraction technology, geographical environment, and traffic conditions, there is still a bottleneck in lithium resources in the field of power batteries. The insufficient supply of lithium resources has led to an increase in prices, and the continued rise in lithium prices will accelerate the process of companies looking for more cost-effective alternatives. In order to alleviate this problem, relevant fields have proposed to replace lithium with abundant elements such as sodium (Na), potassium (K), magnesium (Mg), aluminum (Al), calcium (Ca), etc. to prepare a new generation of low-cost and environmentally friendly secondary ion batteries. Among them, sodium-ion batteries have received more and more attention and support.

[0003] Sodium-based layered oxide cathode material is one of the most critical materials for sodium-ion batteries. Similar to lithium cobalt oxide and ternary structure of lithium batteries, the layered oxide structure has good ion channels. The cycle performance may have certain shortcomings, but the average maturity is relatively high. XMeO2 is an embedded or intercalated compound, which theoretically has a high discharge specific capacity, but poor cycle performance. The shortcomings can be improved by introducing active or inert elements for doping or substitution. Layered oxides are mainly divided into two types according to their morphology: polycrystalline and single crystal. Among them, polycrystalline refers to the material particles being secondary particles composed of primary particles, and the primary particles are often relatively small, and one secondary particle is composed of at least dozens or even hundreds of primary particles. Polycrystalline materials have a larger specific surface area and a shorter ion conduction path, so that this type of material often has better ion and electron conductivity, which is reflected in the electrochemical performance, that is, the capacity and rate performance are relatively better. The material particles of single crystal materials are only primary particles, but the particles are larger. The characteristic of this material is that its single particle has a higher strength, so it is reflected in the application end, that is, better cycle capacity, less gas production, and better safety performance. Single and polycrystalline have their own significant advantages, but their disadvantages are also obvious, and can be regarded as the two ends of a seesaw. Therefore, the industry has also proposed some methods to improve the performance of single and polycrystalline materials: for example, patent CN202311642639.5 discloses a single crystal sodium ion battery positive electrode material and a preparation method thereof, and a sodium ion battery, which achieves high compaction and suitable particle size distribution single crystal preparation by limiting the roundness and size distribution concentration of the single crystal particles of the material, but it does not get rid of the disadvantage of low capacity of single crystal materials, and only further improves the strength of its macroscopic particles; patent CN202311817379.0 provides a sodium ion battery mixed phase polycrystalline positive electrode material and a preparation method thereof and a sodium ion battery, which regulates the P2 / O3 ratio by sodium matching and element doping to obtain a polycrystalline layered positive electrode material with high capacity, high rate and long cycle; but it does not get rid of the disadvantages of polycrystalline materials, and does not make up for its shortcomings.

[0004] At present, the known single-crystal and polycrystalline positive electrode materials and their improved technical solutions have the following defects: no corresponding improvements have been made to the disadvantages of their respective material systems, especially single-crystal materials, and their capacity has not been improved through effective technical means. Therefore, providing sodium battery positive electrode materials with both single-crystal and polycrystalline advantages is of great significance for improving material capacity and cycle stability. Summary of the invention

[0005] The main purpose of the present invention is to provide a single-crystal-like positive electrode material with a defective phase and a preparation method and application thereof, so as to overcome the deficiencies of the prior art.

[0006] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0007] An embodiment of the present invention provides a single-crystal-like positive electrode material with a defective phase, wherein the single-crystal-like positive electrode material includes a plurality of secondary particles, wherein the secondary particles are assembled from 5-12 primary particles, wherein the single-crystal-like positive electrode material has a defective phase, and the defective phase is distributed on the surfaces of each primary particle assembled from each other; wherein, when the single-crystal-like positive electrode material is charged, the battery voltage differential capacity dQ / dV≥1.5mAh / V is within the voltage range of 4.0-4.1V.

[0008] The embodiment of the present invention further provides a method for preparing the aforementioned single-crystal-like positive electrode material having a defective phase, which comprises:

[0009] A precursor is prepared by a coprecipitation method using a nickel source, a manganese source, and an iron source as raw materials, or using a nickel source, a manganese source, an iron source, and an M source as raw materials;

[0010] Furthermore, the precursor is subjected to a first sintering treatment at a first temperature, then rapidly heated to a second temperature in a humid air atmosphere and subjected to a second sintering treatment, and then slowly cooled to the first temperature and subjected to a third sintering treatment, to obtain a single crystal-like positive electrode material with a defective phase.

[0011] The embodiments of the present invention also provide the use of the aforementioned single-crystal-like positive electrode material with defective phase in preparing a positive electrode of a sodium battery or a sodium ion battery.

[0012] An embodiment of the present invention further provides a sodium battery positive electrode, which includes a positive electrode material, a conductive agent, a binder and a current collector; wherein the positive electrode material includes the aforementioned single-crystal-like positive electrode material with a defective phase.

[0013] An embodiment of the present invention further provides a sodium ion battery, which includes the aforementioned single-crystal-like positive electrode material with a defective phase or a sodium battery positive electrode.

[0014] Compared with the prior art, the present invention has the following beneficial effects:

[0015] (1) The quasi-single crystal positive electrode material in this application exists in a quasi-single crystal form in terms of morphology, that is, multiple small single crystal particles are assembled together to form a larger quasi-single crystal particle. Particles of this morphology have the high particle strength and low specific surface area characteristics unique to single crystals, which makes them also have the characteristics of less gas production, less powdering, and better cycle performance in battery applications of traditional single-particle single crystals; secondly, they also have the short ion conduction path characteristics unique to polycrystalline particles, which makes them have the characteristics of higher rate and higher capacity in battery applications of traditional polycrystalline materials;

[0016] (2) The present invention constructs a defect phase with lower energy. On the one hand, the existence of the defect phase improves the ion conductivity of this area, so that when the material is charged to the same voltage, a portion of sodium ions can be released, which significantly improves the capacity compared with traditional single crystals. On the other hand, through special process methods, the defect phases are combined with each other during sintering and are located on the contact surface of each primary particle that is not exposed to the outside, avoiding the poor stability of the defect phase itself and the wider ion channel. The worse material stability and water resistance; in summary, the present invention fully combines the advantages of single and polycrystalline materials, and uniquely constructs defect phases to further improve the material capacity. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0018] Figure 1 is a SEM electron microscope image of the positive electrode material prepared in Example 1 of the present invention;

[0019] Figure 2 is a charge and discharge curve diagram of the battery in Example 1 of the present invention;

[0020] Figure 3 is a battery voltage differential capacity dQ / dV curve diagram of the battery in Example 1 of the present invention;

[0021] Figure 4 is a SEM electron microscope image of the positive electrode material prepared in Example 2 of the present invention;

[0022] Figure 5 is a SEM electron microscope image of the positive electrode material prepared in Example 3 of the present invention;

[0023] Figure 6 is a SEM electron microscope image of the positive electrode material prepared in Example 4 of the present invention;

[0024] Figure 7 This is a SEM electron microscope image of the positive electrode material prepared in Comparative Example 1 of the present invention;

[0025] Figure 8 is a SEM electron microscope image of the positive electrode material prepared in Comparative Example 3 of the present invention;

[0026] Fig. 9 It is a SEM electron microscope image of the positive electrode material prepared in Comparative Example 4 of the present invention. DETAILED DESCRIPTION

[0027] In view of the defects of the prior art, the inventors of this case have proposed the technical solution of the present invention after long-term research and extensive practice. The present invention mainly achieves that the intermediate material has the respective advantages of single and polycrystalline materials and introduces additional capacity by regulating the material morphology and the mutual assembly of defective phases. At the process end, by adding an ultra-high temperature interval and supplemented by the introduction of humid air, the sodium in the higher energy surface at the interface quickly exchanges protons with water molecules and evaporates to form a sodium-deficient defective phase. The slow cooling section introduced next causes the material particles that are partially melted at high temperature to undergo a recrystallization process under slow cooling. Since the defective phases have higher energy and react more violently, they assemble with each other during the recrystallization process to form single-crystal-like particles with defective phases inside. The quasi-single crystals formed by this method have the advantages of both single and polycrystalline particles, and the presence of defective phases can increase the additional capacity.

[0028] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Specifically, as one aspect of the technical solution of the present invention, a single-crystal-like positive electrode material with a defective phase comprises a plurality of secondary particles, wherein the secondary particles are assembled from 5-12 primary particles, the single-crystal-like positive electrode material has a defective phase, and the defective phase is distributed on the surface of each primary particle assembled with each other; wherein, when the single-crystal-like positive electrode material is charged, the battery voltage differential capacity dQ / dV≥1.5mAh / V is within the voltage range of 4.0-4.1V.

[0030] In some preferred embodiments, the chemical formula of the single-crystal-like positive electrode material is Na x Ni a Fe b Mn c M d O2, wherein (a+b+c+d)=1, 0.6≤x≤0.9, 0.1≤a≤0.4, 0.1≤b≤0.4, 0.2≤c≤0.8, 0.01≤d≤0.2; M is selected from any one or more combinations of K, Li, Ca, Cu, Mg, Zn, Sr, B, Y, Sn, Al, Nb, Ti, Zr, W, Sr, Co, and Mo elements.

[0031] In some preferred embodiments, the secondary particles have a particle size of 5-12 μm.

[0032] In some preferred embodiments, the particle size of the primary particles is 0.2-5 μm.

[0033] Another aspect of the embodiments of the present invention further provides a method for preparing the aforementioned single-crystal-like positive electrode material having a defective phase, which comprises:

[0034] A precursor is prepared by a coprecipitation method using a nickel source, a manganese source, and an iron source as raw materials, or using a nickel source, a manganese source, an iron source, and an M source as raw materials;

[0035] Furthermore, the precursor, sodium source, and M source are subjected to a first sintering treatment at a first temperature, and then rapidly heated to a second temperature in a humid air atmosphere and subjected to a second sintering treatment, and then slowly cooled to the first temperature and subjected to a third sintering treatment, to obtain a single-crystal-like positive electrode material with a defective phase.

[0036] In some preferred embodiments, the nickel source, manganese source, and iron source are independently selected from any one or more combinations of sulfates, hydrochlorides, nitrates, carbonates, acetates, oxides, sulfides, nitrides, and hydroxides of the corresponding metal ions, and are not limited thereto.

[0037] In some preferred embodiments, the sodium source includes any one or more combinations of anhydrous sodium carbonate, sodium carbonate monohydrate, sodium carbonate decahydrate, sodium bicarbonate, and sodium sulfate, but is not limited thereto.

[0038] In some preferred embodiments, the M source is selected from sulfates, hydrochlorides, nitrates, carbonates, acetates, oxides, sulfides, nitrides or hydroxides corresponding to any one or more combinations of K, Li, Ca, Cu, Mg, Zn, Sr, B, Y, Sn, Al, Nb, Ti, Zr, W, Sr, Co, and Mo, and is not limited thereto.

[0039] In some preferred embodiments, the preparation method specifically includes: subjecting the precursor sodium source and M source to a first sintering treatment at 800-1000°C in a dry gas atmosphere, followed by a second sintering treatment at 1000-1200°C in a humid air atmosphere, and then switching to dry gas and slowly cooling the temperature to 800-1000°C for a third sintering treatment to obtain a single-crystal-like positive electrode material with a defective phase; wherein the rate of introducing humid air is 2-50L / min.

[0040] Furthermore, the first sintering treatment time is 6-18 hours.

[0041] Further, the dry gas atmosphere includes a dry air atmosphere and / or a dry oxygen atmosphere, but is not limited thereto.

[0042] Furthermore, the humidity of the humid air atmosphere at room temperature is 50-99%.

[0043] Furthermore, the second sintering treatment time is 0.1-3h.

[0044] Furthermore, the temperature is lowered to the first temperature at a rate of 0.1-5°C / min.

[0045] Furthermore, the third sintering treatment takes 1-9 hours.

[0046] Another aspect of the embodiments of the present invention further provides the use of the aforementioned single-crystal-like positive electrode material with a defective phase in the preparation of a sodium battery positive electrode or a sodium ion battery.

[0047] Another aspect of an embodiment of the present invention further provides a sodium battery positive electrode, which includes a positive electrode material, a conductive agent, a binder and a current collector; wherein the positive electrode material includes the aforementioned single-crystal-like positive electrode material with a defective phase.

[0048] In some preferred embodiments, the positive electrode material, the conductive agent and the binder form a positive electrode slurry, and the positive electrode slurry is coated on the surface of the current collector to form a positive electrode of a sodium battery.

[0049] In some preferred embodiments, the mass ratio of the positive electrode material, the conductive agent and the binder is 90-99:0.5-5:0.5-5.

[0050] In some preferred embodiments, the conductive agent includes conductive carbon black, but is not limited thereto.

[0051] In some preferred embodiments, the binder includes any one or more combinations of sodium carboxymethyl cellulose, styrene-butadiene latex, and polyvinylidene fluoride, but is not limited thereto.

[0052] In some preferred embodiments, the current collector is a metal foil, which includes aluminum foil and / or copper foil, but is not limited thereto.

[0053] Another aspect of an embodiment of the present invention further provides a sodium ion battery, which includes the aforementioned single-crystal-like positive electrode material with a defective phase or a sodium battery positive electrode.

[0054] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments and drawings. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.

[0055] The experimental materials used in the following examples can be purchased from conventional biochemical reagent companies unless otherwise specified. Unless otherwise specified, "room temperature" used in this application refers to the temperature measured by a Celsius thermometer in an ordinary laboratory, generally 20-30°C, preferably 25°C (Kelvin temperature is 298.15K) ± 2°C.

[0056] Example 1

[0057] A spherical hydroxide precursor with a ratio of Ni:Fe:Mn = 1:1:2 was prepared by coprecipitation. The precursor, sodium carbonate, and copper oxide were mixed according to the chemical formula Na 0.75 Ni 0.23 Fe 0.23 Mn 0.46 Cu 0.08 O2 is weighed and mixed evenly, and then put into a box furnace for sintering, kept at 850°C for 12 hours, and then kept at 1100°C for 2 hours with humid air passing at a rate of 20L / min, and then dry air is passed through at a rate of 1°C / min to cool down to 850°C and keep for 6 hours, and finally cooled naturally to obtain a single-crystal positive electrode material with a defective phase.

[0058] The high-magnification SEM electron microscope image of the single-crystal-like positive electrode material with defective phase prepared in this embodiment is as follows: Figure 1 As shown, it presents a single crystal morphology, and each secondary particle is composed of 5-12 primary block particles. The positive electrode material is prepared into a positive electrode sheet and the electrochemical performance of the battery is tested. The mass percentage of the positive electrode material, binder, and conductive agent in the positive electrode slurry is 90:5:5. The conductive agent used is conductive carbon black, the binder is PVDF, the current collector used is aluminum foil, the battery shell model is CR2032, and the electrolyte is NaPF6-diethylene glycol dimethyl ether (DIGLYME) electrolyte. Its charge and discharge curve and the corresponding dQ / dV curve are shown in Figure 2 , 3 The rest of the test results are shown in Table 1.

[0059] Example 2

[0060] A spherical hydroxide precursor with a ratio of Ni:Fe:Mn = 2:3:4 was prepared by coprecipitation. The precursor, sodium carbonate and zinc oxide were mixed according to the chemical formula Na 0.9 Ni 0.2 Fe 0.3 Mn 0.4 Zn 0.1 O2 is weighed and mixed evenly, and then put into a box furnace for sintering, kept at 900°C for 12 hours, and then kept at 1200°C for 1 hour by passing humid air at a rate of 30L / min, and then dry air is passed in and cooled to 900°C at a rate of 0.5°C / min and kept for 4 hours, and finally cooled naturally to obtain a single-crystal positive electrode material with a defective phase.

[0061] The SEM image of the single-crystal-like positive electrode material with defect phase prepared in this embodiment is as follows: Figure 4 shown.

[0062] Example 3

[0063] A spherical hydroxide precursor with a ratio of Ni:Fe:Mn:Ti = 2:1:6:1 was prepared by coprecipitation. The precursor, sodium carbonate, magnesium oxide, calcium oxide, and zirconium oxide were mixed according to the chemical formula Na 0.7 Ni 0.2 Fe 0.1 Mn 0.6 Ti 0.1 Mg 0.04 Zr 0.04 Ca 0.02 O2 is weighed and mixed evenly, and then put into a box furnace for sintering, kept at 1000℃ for 10 hours, and then kept at 1200℃ for 1 hour at a rate of 50L / min for humid air, and then dry air is passed through at a rate of 2℃ / min to cool down to 1000℃ and keep for 3 hours, and finally cooled naturally to obtain a single-crystal positive electrode material with a defect phase.

[0064] The SEM image of the single-crystal-like positive electrode material with defect phase prepared in this embodiment is as follows: Figure 5 shown.

[0065] Example 4

[0066] A spherical hydroxide precursor with a ratio of Ni:Fe:Mn = 1:1:1 was prepared by coprecipitation. The precursor, sodium carbonate, magnesium oxide, niobium oxide, and boric acid were mixed according to the chemical formula Na 0.9 Ni 0.3 Fe 0.3 Mn 0.3 Mg 0.08 Nb 0.01 B 0.01 O2 is weighed and mixed evenly, and then placed in a box furnace for sintering, kept at 800°C for 16 hours, and then kept at 1000°C for 3 hours with humid air passing at a rate of 40L / min, and then dry air is passed through at a rate of 5°C / min to cool down to 800°C and keep for 9 hours, and finally cooled naturally to obtain a single-crystal positive electrode material with a defective phase.

[0067] The SEM image of the single-crystal-like positive electrode material with defect phase prepared in this embodiment is as follows: Figure 6 shown.

[0068] Comparative Example 1

[0069] The method is the same as that of Example 1, except that after the second sintering treatment, dry air is introduced to cool the temperature to 850°C at a rate of 10°C / min and kept at this temperature for 6 hours. The SEM image of the prepared positive electrode material is as follows: Figure 7In this comparative example, the temperature is lowered too fast, resulting in insufficient melting of the particles, and the morphology is closer to dispersed single crystals, that is, the secondary particles are composed of fewer primary particles (≤5), resulting in the surface of the defective phase being exposed. Since the defective phase is exposed and the single crystal is more dispersed, the cycle and rate are poor.

[0070] Comparative Example 2

[0071] The method is the same as Example 1, except that the second sintering process is performed in dry air. In this comparative example, since the second sintering process is not performed in humid air, it is difficult to form a defect phase, which ultimately leads to a lower capacity ratio.

[0072] Comparative Example 3

[0073] The method is the same as that of Example 1, except that the raw materials are placed in a box furnace for sintering and kept at 850°C for 20 hours (i.e., prepared using a conventional polycrystalline process). The SEM image of the positive electrode material prepared in this comparative example is shown in FIG. Figure 8 As shown in the figure, the prepared cathode material is not single crystal but polycrystalline, and does not have the advantages of high safety and low gas production of single crystal.

[0074] Comparative Example 4

[0075] The method is the same as that of Example 1, except that the second sintering treatment is performed at 850°C. The SEM image of the positive electrode material prepared in this comparative example is shown in FIG. Fig. 9 As shown, the prepared positive electrode material is not a single crystal but a polycrystalline one, and does not have the advantages of high safety and low gas production of single crystals. In addition, due to the introduction of humid air, sodium salt precipitates on the surface of the material, further deteriorating the material performance.

[0076] Table 1 Characterization data of positive electrode materials obtained in Examples 1-4 and Comparative Examples 1-4

[0077]

[0078] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0079] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.

Claims

1. A single-crystal-like cathode material with defective phase, Features: The quasi-single-crystal positive electrode material comprises a plurality of secondary particles, wherein the secondary particles are formed by assembling 5-12 primary particles, the quasi-single-crystal positive electrode material has defective phases, and the defective phases are distributed on the surfaces of the mutually assembled primary particles; wherein when the quasi-single-crystal positive electrode material is charged, dQ / dV≥1.5mAh / V in the voltage range of 4.0-4.1V; the chemical formula of the quasi-single-crystal positive electrode material is Na x Ni a Fe b Mn c M d O 2 , wherein (a+b+c+d)=1, 0.6≤x≤0.9, 0.1≤a≤0.4, 0.1≤b≤0.4, 0.2≤c≤0.8, 0.01≤d≤0.2; M is selected from any one or more combinations of K, Li, Ca, Cu, Mg, Zn, Sr, B, Y, Sn, Al, Nb, Ti, Zr, W, Sr, Co, and Mo elements; The method for preparing the single-crystal-like positive electrode material having a defective phase comprises: A precursor is prepared by a coprecipitation method using a nickel source, a manganese source, and an iron source as raw materials, or using a nickel source, a manganese source, an iron source, and an M source as raw materials; And, the precursor, sodium source and M source are subjected to a first sintering treatment at 800-1000°C in a dry gas atmosphere for 6-18h, and then a second sintering treatment is carried out at 1000-1200°C in a humid air atmosphere for 0.1-3h, and then the dry gas is switched and the temperature is reduced to 800-1000°C at a decreasing rate of 0.1-5°C / min for a third sintering treatment for 1-9h to obtain a single-crystal-like positive electrode material with a defective phase; wherein the dry gas atmosphere includes a dry air atmosphere and / or a dry oxygen atmosphere; the humidity of the humid air atmosphere at room temperature is 50-99%; the rate of introducing humid air is 2-50L / min.

2. The single-crystal-like positive electrode material according to claim 1, Features: The particle size of the secondary particles is 5-12 μm; and / or the particle size of the primary particles is 0.2-5 μm.

3. The single-crystal-like positive electrode material according to claim 1, Features: The nickel source, manganese source, and iron source are independently selected from any one or more combinations of sulfates, hydrochlorides, nitrates, carbonates, acetates, oxides, sulfides, nitrides, and hydroxides of the corresponding metal ions; And / or, the sodium source includes any one or more combinations of anhydrous sodium carbonate, sodium carbonate monohydrate, sodium carbonate decahydrate, sodium bicarbonate, and sodium sulfate; And / or, the M source is selected from sulfates, hydrochlorides, nitrates, carbonates, acetates, oxides, sulfides, nitrides or hydroxides corresponding to any one or more combinations of K, Li, Ca, Cu, Mg, Zn, Sr, B, Y, Sn, Al, Nb, Ti, Zr, W, Sr, Co and Mo.

4. Use of the single-crystal-like positive electrode material with defective phase according to any one of claims 1 to 3 in preparing a positive electrode for a sodium battery or a sodium ion battery.

5. A sodium battery positive electrode, It is characterized in that It comprises a positive electrode material, a conductive agent, a binder and a current collector; wherein the positive electrode material comprises the single-crystal-like positive electrode material with a defective phase as described in any one of claims 1 to 3.

6. The sodium battery positive electrode according to claim 5, Features: The positive electrode material, the conductive agent and the binder form a positive electrode slurry, and the positive electrode slurry is coated on the surface of the current collector to form a positive electrode of a sodium battery; And / or, the mass ratio of the positive electrode material, the conductive agent and the binder is 90-99:0.5-5:0.5-5; and / or, the conductive agent comprises conductive carbon black; And / or, the binder includes a combination of one or more of sodium carboxymethyl cellulose, styrene-butadiene latex, and polyvinylidene fluoride; And / or, the current collector is a metal foil, and the metal foil includes aluminum foil and / or copper foil.

7. A sodium ion battery, It is characterized in that The invention comprises the single-crystal-like positive electrode material with defective phase according to any one of claims 1 to 3 or the positive electrode of a sodium battery according to any one of claims 5 to 6.

Citation Information

Patent Citations

  • Sodium-ion battery mixed-phase polycrystalline positive electrode material, preparation method thereof and sodium-ion battery

    CN117594774A

  • Single crystal type sodium ion battery positive electrode material, preparation method thereof and sodium ion battery

    CN117810437A

  • High-capacity monocrystalline high-nickel positive electrode material for lithium battery and preparation method of high-capacity monocrystalline high-nickel positive electrode material for lithium battery

    CN107768619A

  • High-entropy composite-phase positive electrode material with monocrystal-like morphology and preparation method of high-entropy composite-phase positive electrode material

    CN117174895A

  • Modified polycrystalline positive electrode material, preparation method thereof and secondary battery

    CN118579853A