Light breathable high-strength vamp fabric
By using a combination of low-temperature shaping skin-core structure thermal bonding yarn and ultra-high molecular weight polyethylene fiber in sports shoe upper materials, the challenges of cost-effectiveness and shaping stability of lightweight, breathable and high-strength shoe upper fabrics are solved, and high-performance Shoe upper material production.
Patent Information
- Application Number
- CN202410981197.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-22
- Publication Date
- 2024-10-29
AI Technical Summary
Existing sports shoe upper materials are difficult to balance cost performance when pursuing lightweight, breathable, strength, wear resistance and bending properties, and the application of ultra-high molecular weight polyethylene fiber in the field of civilian textiles is limited by high cost and styling stability issues.
It is woven using the perforated twisted heddle weaving method, combined with low-temperature shaping skin-core structure thermal bonding yarn and ultra-high molecular weight polyethylene fiber. By controlling the ratio of the skin and core layers and the weaving process, the shaping temperature and speed are reduced to achieve a lightweight, breathable and high-strength upper. Fabric production.
We have obtained a shoe upper material that is lightweight, breathable, high-strength, wear-resistant, and cool-feeling, which is superior to existing technology, has improved cost performance, and expanded the application potential of ultra-high molecular weight polyethylene fiber in the field of civilian textiles. .
Smart Images

Figure BDA0004956116790000061 
Figure BDA0004956116790000071 
Figure BDA0004956116790000081
Abstract
Description
Technical Field
[0001] The invention belongs to the field of textile technology, and in particular relates to a lightweight, breathable and high-strength shoe upper fabric. Background Art
[0002] Existing sports shoe mesh materials usually use polyester (PET), nylon (PA), spandex (PU), polyolefin elastic fiber (PP), thermoplastic polyurethane elastic yarn (TPU), etc. With the growing enthusiasm for national fitness, consumers' requirements for the comfort and functionality of sports shoes are increasing day by day. Whether it is running shoes, basketball shoes, table tennis shoes, badminton shoes and other categories with a large audience base, wearers hope that the upper can have functions such as lightness and breathability.
[0003] Therefore, functional sports shoes are turning towards lightweight, but in order to maintain the requirements of the upper for strength, wear resistance, bending and other performance, the weight of the upper is still relatively high, making it difficult to achieve the ultimate pursuit of lightweight.
[0004] Patent application CN114908453A discloses a lightweight and breathable upper that is woven using an openwork twisted weave method and uses PEBA fiber in the ground warp of the warp yarn. Only 18% of the fiber is needed to achieve the advantages of excellent wrapping, lightness, comfort, and low temperature resistance.
[0005] However, as a pursuit of upper performance and cost-effectiveness, further improving the upper's lightness, strength, wear resistance and bending performance is still a problem that needs to be solved. Summary of the invention
[0006] In view of the fact that the lightness, breathability, strength, wear resistance, bending and other properties of sports shoe uppers in the prior art still need to be continuously improved, and the cost-effectiveness needs to be taken into account, the present invention provides a lightweight, breathable and high-strength upper fabric.
[0007] The technical scheme of the present invention is as follows: a lightweight, breathable, high-strength upper fabric is woven by an open-hole twisted heald weaving method, the ground warp in the warp yarn includes one or more of polyester fibers, polyamide fibers, polyolefin fibers, polyurethane fibers, and thermoplastic elastomer fibers, and the twisted warp is a core-sheath structure hot-bonded wire; the weft yarn includes a core-sheath structure hot-bonded wire and an ultra-high molecular weight polyethylene fiber; the weight of the core-sheath structure hot-bonded wire in the lightweight, breathable, high-strength upper fabric accounts for 15-75%, and the weight of the ultra-high molecular weight polyethylene fiber accounts for 15%-85%; the heat setting temperature of the lightweight, breathable, high-strength upper fabric is 110-140°C, and the heat setting speed is 12-21m / min.
[0008] Furthermore, the thermoplastic elastomer fibers in the ground warp yarns include PEBA fibers; and the polyolefin fibers include ultra-high molecular weight polyethylene fibers.
[0009] Furthermore, the skin-core structure hot-adhesive wire includes a skin layer and a core layer, the skin layer is 88A thermoplastic polyurethane elastomer, and the core layer is 70A hardness thermoplastic polyurethane; the mass ratio of the skin layer to the core layer is 2:8-8:2.
[0010] Preferably, the mass ratio of the skin layer to the core layer is 6:4.
[0011] Preferably, the heat setting temperature of the lightweight, breathable and high-strength upper fabric is 120° C., and the heat setting speed is 15 m / min.
[0012] Furthermore, in the lightweight, breathable and high-strength upper fabric, the weight of the skin-core structure hot-bonded yarn accounts for 25-50%, and the mass fraction of the ultra-high molecular weight polyethylene fiber is 40-75%.
[0013] Furthermore, the twisted warp in the warp yarn is 1 low-temperature qualitative hot-bonded yarn, and the ground warp is 6 ultra-high molecular weight polyethylene fibers; the weft yarn is 6 ultra-high molecular weight polyethylene fibers and 1 low-temperature hot-bonded yarn.
[0014] Furthermore, the twisted warp in the warp yarn is 1 low-temperature qualitative hot-bonded yarn, the ground warp is 3 ultra-high molecular weight polyethylene fibers and 3 PEBA monofilaments; the weft yarn is 3 ultra-high molecular weight polyethylene fibers, 3 PEBA monofilaments and 1 low-temperature hot-bonded yarn.
[0015] Furthermore, the twisted warp in the warp yarn is 1 low-temperature qualitative hot-bonded yarn, and the ground warp is 6 PEBA monofilaments; the weft yarn is 6 ultra-high molecular weight polyethylene fibers and 1 low-temperature hot-bonded yarn.
[0016] Furthermore, the skin layer and core layer materials of the skin-core structure hot-bonded yarn are prepared through multiple processes including raw material drying, melt extrusion, ice water molding, hot water stretching, hot air stretching, primary fiber setting, secondary fiber setting, oiling to increase lubrication, and winding.
[0017] The advantages of the present invention are: the proportion of the low-temperature hot-adhesive silk cortex and the core layer is controlled, the content of the low-temperature hot-adhesive silk in the cloth piece is controlled, and the use method and content of the ultra-high molecular weight polyethylene fiber are regulated in all directions. The present invention finds that the purpose of enhancing the upper can be achieved by adding a small amount of high molecular weight polyethylene in a single direction or in multiple directions. The lightweight weight reduction requirements of the cloth piece can be met by controllable adjustment of the content of ultra-high molecular weight polyethylene fibers in the cloth piece and in combination with different weaving processes. The upper material finally obtained has the performance advantages of light weight, breathability, high strength, wear resistance, and cool feeling, and these advantages are better than the existing technology, and the comprehensive cost performance is the best. DETAILED DESCRIPTION
[0018] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0019] The main goal of the present invention is to provide a lightweight, high-strength, wear-resistant and cost-effective upper fabric. In the selection of upper fibers, in addition to conventional thermoplastic elastomer fibers, polyester fibers, polyamide fibers and polyurethane fibers, ultra-high molecular weight polyethylene fibers (UHMW-PE) among polyolefin fibers are introduced.
[0020] As one of the three major special fibers, ultra-high molecular weight polyethylene fiber (UHMW-PE) has excellent physical and chemical properties. Low density, high specific strength, large specific modulus, wear resistance, cut resistance, excellent chemical stability, non-absorbent, strong acid, strong alkali, organic solvent resistance, UV resistance are all advantageous features of ultra-high molecular weight polyethylene, so it is the preferred material for high-performance ropes, bulletproof vests, deep-sea fishing nets, cut-resistant gloves and other industrial and protective fields.
[0021] Although ultra-high molecular weight polyethylene fiber has great application potential, it also faces many obstacles in its application in the field of civil textiles due to its high price and heat resistance. Ultra-high molecular weight polyethylene fiber textiles are often expensive and difficult to effectively heat-set (which will lead to poor shaping stability of textile fabrics or loss of ultra-high molecular weight polyethylene fiber performance, etc.).
[0022] Heat setting is an essential part of fabric production. It has the function of releasing fiber stress and stabilizing fabric size. Fabrics that are not heat set will have negative effects such as slippage and wrinkling during use. At the same time, the heat setting temperature of commonly used materials for uppers is not less than 160°C. The melting point of ultra-high molecular weight polyethylene fiber is 144°C. If it is kept above 70°C for a long time or above 130°C for a short time, its performance will be greatly attenuated.
[0023] Therefore, the present invention adopts low-temperature setting skin-core structure hot-bonded silk and ultra-high molecular weight polyethylene fiber as main raw materials, which are mixed with other yarns to obtain a lightweight shoe upper under low-temperature hot pressing setting conditions.
[0024] The low temperature setting skin-core structure hot-adhesive yarn includes: one or more of thermoplastic polyurethane elastomer, thermoplastic polyester elastomer, thermoplastic nylon elastomer, and the skin / core ratio is 2:8-8:2, preferably 6:4. The Shore hardness of the skin layer is 50-100A, preferably 85-90A. The Shore hardness of the core layer is 40-80A, preferably 55-70A.
[0025] The other yarns are one or more of thermoplastic elastomer fibers, polyester fibers, polyamide fibers, polyolefin fibers, and polyurethane fibers; preferably, PEBA fibers among polyamide fibers.
[0026] The cortex of the low-melting-point core-skin structure hot-bonded yarn can be shaped below 130°C, which is lower than the melting point of ultra-molecular-weight polyethylene fibers. The cortex material that is shaped, melted, cooled and solidified is firmly bonded to the surface of the filaments or monofilaments of polyester, polyamide, polyolefin and its elastomers in contact, so that the fabric has good mechanical properties and wrapping properties while maintaining good air permeability. With the help of low-temperature shaped hot-bonded yarn, the shaping temperature of fabrics containing ultra-high molecular weight polyethylene fibers can be effectively reduced, and low-temperature shaping of ultra-high molecular weight polyethylene fibers can be achieved. After shaping, there is no problem of yarn slippage in the fabric.
[0027] The mass fraction of the low temperature setting skin-core structure hot-adhesive yarn in the fabric is 15-75%, the mass fraction of the ultra-high molecular weight polyethylene fiber is 15-85%, and the mass fraction of other yarns is 0-75%. Preferably, the mass fraction of the low temperature setting skin-core structure hot-adhesive yarn in the fabric is 25-50%, the mass fraction of the ultra-high molecular weight polyethylene fiber is 40-75%, and the mass fraction of other yarns is 0-25%.
[0028] Taking 88A hardness thermoplastic polyurethane elastomer as the skin material and 70A hardness thermoplastic polyurethane as the core material as an example, the skin and core layer materials are subjected to multiple processes of raw material drying, melt extrusion, ice water molding, hot water stretching, hot air stretching, primary fiber setting, secondary fiber setting, oiling to enhance lubrication, and winding to prepare skin-core structure low-temperature shaping hot adhesive wire.
[0029] During the melt extrusion process, low-temperature setting hot-bonded yarns with skin-core ratios of 2:8, 4:6, 6:4 and 8:2 were obtained by proportion control, and the four skin-core ratio hot-bonded yarns were used in combination with polyester fibers to weave twisted heald cloth pieces; there was one hot-bonded yarn in the warp direction and one in the weft direction, and the hot-bonded yarn in the warp direction was used as a twisted warp, the fabric setting temperature was 110°C, and the setting speed was 12m / min.
[0030] Table 1 Effect of skin-core ratio on fabric properties
[0031] Skin-to-core ratio 2:8 4:6 6:4 8:2 Tensile force (warp / weft) (kg / 2.54cm) 36.8 / 33.1 36.1 / 32.6 35 / 30.6 30.2 / 29.7 Tear (warp / weft) (kg / 2.54cm) 2.5 / 2.8 3.0 / 3.4 5.9 / 6.1 4.1 / 4.3 Elongation (warp / weft) (%) 25.8 / 26.1 27.3 / 27.9 29.2 / 31.8 33.2 / 34.3 Bursting strength (kg / 2.54cm) 16.7 17.9 18.6 15.3
[0032] As shown in Table 1, the above example mainly examines the effect of the ratio of the hot-bonded silk skin layer to the core layer on the shaping effect of the overall twisted heald cloth piece. It can be seen that with the increase in the ratio of the hot-bonded silk skin layer, the shaping firmness of the twisted heald cloth piece increases, but the tensile strength of the cloth piece decreases. When the skin-core ratio of the low-temperature shaping hot-bonded silk is 6:4, good shaping firmness can be obtained, and at the same time, the tensile strength of the cloth piece can meet the use requirements of the upper.
[0033] The following continues to use ultra-molecular weight polyethylene fiber and low-temperature setting hot-bonded silk with a skin-core ratio of 6:4 as cloth material, and uses the twisted heddle weaving method to weave the cloth, to further illustrate the influence of setting temperature and setting speed on fabric performance.
[0034] It should be noted that in the conventional openwork twisted weaving method, the number of fibers in the weft direction varies from about 1 to 15, depending on the thickness of the fibers or the difference in monofilament or multifilament. In order to unify the differences, in the embodiment, 7 weft fibers are selected (6 ultra-high molecular weight polyethylene fibers + 1 low-temperature hot-bonding yarn), and the warp fibers are fixed with 1 twisted warp + 6 ground warps; these are used as cloth fibers.
[0035] Example 1
[0036] In the weaving process of the fabric, the above-mentioned low-temperature setting hot-bonded yarn and ultra-high molecular weight polyethylene fiber are used in the warp direction, wherein the twisted warp is 1 low-temperature setting hot-bonded yarn and the ground warp is 6 ultra-high molecular weight polyethylene fibers; after weaving 6 ultra-high molecular weight polyethylene fibers and 1 low-temperature hot-bonded yarn in the weft direction, the twisted warp and the ground warp are twisted once to form a uniformly distributed porous breathable twisted heald fabric. The fabric setting temperature is 110°C and the setting speed is 12m / min.
[0037] Example 2
[0038] In the weaving process of the fabric, the above-mentioned low-temperature qualitative hot-bonding yarn and ultra-high molecular weight polyethylene fiber are used in the warp direction, wherein the twisted warp is 1 low-temperature qualitative hot-bonding yarn and the ground warp is 6 ultra-high molecular weight polyethylene fibers. After weaving 6 ultra-high molecular weight polyethylene fibers and 1 low-temperature hot-bonding yarn in the weft direction, the twisted warp and the ground warp are twisted once to form a uniformly distributed porous breathable twisted heald fabric. The fabric setting temperature is 120°C and the setting speed is 15m / min.
[0039] Example 3
[0040] In the weaving process of the fabric, the above-mentioned low-temperature qualitative hot-bonding yarn and ultra-high molecular weight polyethylene fiber are used in the warp direction, wherein the twisted warp is 1 low-temperature qualitative hot-bonding yarn and the ground warp is 6 ultra-high molecular weight polyethylene fibers. After weaving 6 ultra-high molecular weight polyethylene fibers and 1 low-temperature hot-bonding yarn in the weft direction, the twisted warp and the ground warp are twisted once to form a uniformly distributed porous breathable twisted heald fabric. The fabric setting temperature is 130°C and the setting speed is 18m / min.
[0041] Example 4
[0042] In the weaving process of the fabric, the above-mentioned low-temperature qualitative hot-bonding yarn and ultra-high molecular weight polyethylene fiber are used in the warp direction, wherein the twisted warp is 1 low-temperature qualitative hot-bonding yarn and the ground warp is 6 ultra-high molecular weight polyethylene fibers. After weaving 6 ultra-high molecular weight polyethylene fibers and 1 low-temperature hot-bonding yarn in the weft direction, the twisted warp and the ground warp are twisted once to form a uniformly distributed porous breathable twisted heald fabric. The fabric setting temperature is 140°C and the setting speed is 21m / min.
[0043] Comparative Example 1
[0044] In the weaving process of the fabric, the above-mentioned low-temperature qualitative hot-bonding yarn and ultra-high molecular weight polyethylene fiber are used in the warp direction, wherein the twisted warp is 1 low-temperature qualitative hot-bonding yarn and the ground warp is 6 ultra-high molecular weight polyethylene fibers. After weaving 6 ultra-high molecular weight polyethylene fibers and 1 low-temperature hot-bonding yarn in the weft direction, the twisted warp and the ground warp are twisted once to form a uniformly distributed porous breathable twisted heald fabric. The fabric setting temperature is 160°C and the setting speed is 27m / min.
[0045] In the above examples, the influence of the shaping conditions (shaping temperature and speed) on the shaping effect and the performance of the spun heald fabric containing ultra-high molecular weight polyethylene fibers is mainly investigated. The test results are shown in Table 2.
[0046] Table 2 Effect of shaping conditions on fabric properties
[0047]
[0048]
[0049] Ultra-high molecular weight polyethylene fiber is abbreviated as UPE
[0050] As shown in Table 2, with the increase of the setting temperature and setting speed of the cloth piece, the physical properties of the cloth piece first increase and then decrease. After setting at 120℃ and 15m / min, the tensile strength, tearing, bursting and other properties of the cloth piece are the highest. When the setting temperature is lower than 120℃, although the demand for low-temperature use of ultra-high molecular weight polyethylene fiber is met, the cortex of the low-temperature hot-bonding yarn fails to fully melt during the setting process to play the role of evenly bonding the warp and weft materials, so the tensile strength, tearing and bursting values of the cloth piece are low. When the setting temperature is higher than 120℃, as the setting temperature increases, the feel of the cloth piece becomes harder and harder and the comprehensive performance begins to decline, especially when the setting temperature of the cloth piece reaches 160℃ for conventional setting, the ultra-high molecular weight polyethylene filaments in the cloth piece are melted and the cloth piece is damaged, and the cloth piece structure cannot be maintained. This shows that it is impossible to use ultra-high molecular weight polyethylene filaments under conventional setting conditions to obtain a functional shoe upper that is both extremely light, breathable and comfortable.
[0051] The setting temperature of ultra-high molecular weight polyethylene fiber should not be too high. In order to expand its applicable setting temperature as much as possible, while increasing the setting temperature, the setting speed is increased to reduce the finishing process of the cloth piece at high temperature as much as possible, which is helpful to protect the mechanical properties of the ultra-high molecular weight polyethylene filament. Therefore, the setting speed of 15m / min combined with the setting temperature of 120℃ in Example 2 can achieve a better setting effect while protecting the mechanical properties of the ultra-high molecular weight polyethylene filament.
[0052] Continue to use ultra-molecular weight polyethylene fiber and low-temperature setting hot-bonded silk with a skin-core ratio of 6:4 as the cloth material, combined with a setting temperature of 120℃ and a setting speed of 15m / min, to further investigate the influence of different material ratios in the warp and weft directions and the content of ultra-molecular weight polyethylene fiber on the performance of the overall cloth.
[0053] Example 5
[0054] In the weaving process of the fabric, the above-mentioned low-temperature qualitative hot-bonding yarn, ultra-high molecular weight polyethylene fiber and PEBA monofilament are used in the warp direction, wherein the twisted warp is 1 low-temperature qualitative hot-bonding yarn, and the ground warp is 3 ultra-high molecular weight polyethylene fibers and 3 PEBA monofilaments. After weaving 3 ultra-high molecular weight polyethylene fibers, 3 PEBA monofilaments and 1 low-temperature hot-bonding yarn in the weft direction, the twisted warp and the ground warp are twisted once to form a uniformly distributed porous breathable twisted heald fabric. The fabric setting temperature is 120°C and the setting speed is 15m / min.
[0055] Example 6
[0056] In the weaving process of the fabric, the above-mentioned low-temperature qualitative hot-bonding yarn, ultra-high molecular weight polyethylene fiber and PEBA monofilament are used in the warp direction, wherein the twisted warp is 1 low-temperature qualitative hot-bonding yarn and the ground warp is 6 PEBA monofilaments. After weaving 6 ultra-high molecular weight polyethylene fibers and 1 low-temperature hot-bonding yarn in the weft direction, the twisted warp and the ground warp are twisted once to form a uniformly distributed porous breathable twisted heald fabric. The fabric setting temperature is 120°C and the setting speed is 15m / min.
[0057] Comparative Example 2
[0058] In the weaving process of the fabric, the above-mentioned low-temperature qualitative hot-bonding yarn and polyester filament are used in the warp direction, wherein the twisted warp is 1 low-temperature qualitative hot-bonding yarn and the ground warp is 6 polyester filaments. After weaving 6 polyester filaments and 1 low-temperature hot-bonding yarn in the weft direction, the twisted warp and the ground warp are twisted once to form a uniformly distributed porous breathable twisted heald fabric. The fabric setting temperature is 120°C and the setting speed is 15m / min.
[0059] Comparative Example 3
[0060] In the weaving process of the fabric, the above-mentioned low-temperature qualitative hot-bonding yarn and ultra-high molecular weight polyethylene fiber are used in the warp direction, wherein the twisted warp is 1 low-temperature qualitative hot-bonding yarn and the ground warp is 6 ultra-high molecular weight polyethylene fibers. After weaving 6 ultra-high molecular weight polyethylene fibers and 2 low-temperature hot-bonding yarns in the weft direction, the twisted warp and the ground warp are twisted once to form a uniformly distributed porous breathable twisted heald fabric. The fabric setting temperature is 120°C and the setting speed is 15m / min.
[0061] Table 3 Effect of fabric material ratio on performance
[0062]
[0063]
[0064] Air permeability standard: GB / T 5453-1997
[0065] Table 3 shows the performance comparison results of the open-hole twisted heald fabrics obtained by weaving the low-temperature shaped hot-bonded yarn obtained by melt spinning and ultra-high molecular weight polyethylene filaments, PEBA monofilaments, polyester filaments, etc. It can be seen that when the content of low-temperature hot-bonded yarn is 25%-50%, the samples containing ultra-high molecular weight polyethylene filaments, PEBA monofilaments, and polyester filaments have good adhesion, and the fabric will not slip. The scheme can also be applied to conventional materials such as polyester to expand the application range of ultra-high molecular weight polyethylene fibers.
[0066] By comparing Examples 2, 5, and 6 with Comparative Example 2, it can be seen that the higher the content of ultra-high molecular weight polyethylene filaments in the cloth piece after being shaped by low-temperature hot-bonding yarn, the lighter the weight of the cloth piece and the higher the bursting strength and tear strength, and the cloth piece exhibits excellent comprehensive performance. In addition, the twisted heald cloth piece using the low-temperature shaped hot-bonding yarn has good air permeability, that is, the use of the low-temperature shaped hot-bonding yarn does not affect the air permeability of the cloth piece.
[0067] In particular, in Example 6, after the PEBA monofilament and ultra-high molecular weight polyethylene fiber are used in the warp and weft directions respectively, the cloth pieces show significant differences in the elongation in the warp and weft directions, which is more beneficial to the upper in the process of wearing without affecting the radial movement performance while making the wearer feel a good wrapping feeling. At the same time, compared with the ordinary polyester in Comparative Example 1, the cloth pieces of Examples 2, 5, and 6 have the characteristic of being cool to the touch due to the ultra-high molecular weight polyethylene filament cloth pieces.
[0068] Since ultra-high molecular weight polyethylene fiber is the most expensive compared to other fibers, the higher the proportion of ultra-high molecular weight polyethylene fiber in the cloth, the higher the cost. In Example 6, ultra-high molecular weight polyethylene fiber is only used in the weft direction, which not only reduces the amount of ultra-high molecular weight polyethylene fiber (only 44%), but also achieves a significant difference in elongation between the warp and weft directions to provide a good wrapping feeling. In addition, the cloth is light in weight and its low-temperature bending performance does not decrease, making it the application form with the highest actual cost performance.
[0069] At the same time, it can be seen from Example 2 and Comparative Example 3 that although increasing the content of low-temperature hot-melt yarn in the weft direction has a certain improvement on the tearing performance, the increase in the content of hot-melt yarn will lead to a significant increase in the weight of the cloth and a significant decrease in the low-temperature bending performance of the cloth. Moreover, under the same shaping conditions, the higher the content of hot-melt yarn in the cloth, the harder the feel of the cloth will be, and the wearing comfort of the upper or clothing product will be significantly reduced. Therefore, controlling the content (mass percentage) of hot-melt yarn to not more than 34% is more conducive to exerting the performance of ultra-high molecular weight polyethylene and other fibers and improving the comprehensive performance of the cloth.
[0070] Thus, the present invention has obtained a shoe fabric which is superior to the prior art and has the best comprehensive cost performance by controlling the ratio of the low-temperature hot-bonding silk skin layer and the core layer, controlling the content of the low-temperature hot-bonding silk in the cloth piece, and regulating the use mode and content of the ultra-high molecular weight polyethylene fiber.
[0071] The above is only a preferred embodiment of the present invention, and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment, it is not used to limit the present invention. Any technician familiar with this patent can make some changes or modify the technical contents suggested above into equivalent embodiments without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the solution of the present invention.
Claims
1. A lightweight, breathable, high-strength upper fabric, characterized in that: The light-weight, breathable and high-strength upper fabric is woven by an open-hole twisted heald weaving method. The ground warp in the warp yarn includes one or more of polyester fibers, polyamide fibers, polyolefin fibers, polyurethane fibers, and thermoplastic elastomer fibers. The twisted warp is a core-skin structure hot-bonded yarn; the weft yarn includes a core-skin structure hot-bonded yarn and ultra-high molecular weight polyethylene fiber. The weight of the skin-core structure hot-bonded yarn in the lightweight, breathable and high-strength upper fabric is 15-75%, and the weight of the ultra-high molecular weight polyethylene fiber is 15%-85%; The heat setting temperature of the lightweight, breathable and high-strength upper fabric is 110-140℃, and the heat setting speed is 12-21m / min.
2. The lightweight, breathable, high-strength upper fabric according to claim 1, characterized in that: The thermoplastic elastomer fibers in the ground warp of the warp yarn include PEBA fibers; the polyolefin fibers include ultra-high molecular weight polyethylene fibers.
3. The lightweight, breathable and high-strength upper fabric according to claim 1, characterized in that: The skin-core structure hot-adhesive wire includes a skin layer and a core layer, the skin layer is 88A thermoplastic polyurethane elastomer, and the core layer is 70A hardness thermoplastic polyurethane; the mass ratio of the skin layer to the core layer is 2:8-8:
2.
4. The lightweight, breathable, high-strength upper fabric according to claim 3, characterized in that: The mass ratio of the skin layer to the core layer is 6:
4.
5. The lightweight, breathable, high-strength upper fabric according to claim 1 or 3, characterized in that: The lightweight, breathable and high-strength upper fabric has a heat setting temperature of 120°C and a heat setting speed of 15m / min.
6. The lightweight, breathable, high-strength upper fabric according to claim 1, characterized in that: In the lightweight, breathable and high-strength upper fabric, the weight of the skin-core structure hot-bonded yarn accounts for 25-50%, and the mass fraction of the ultra-high molecular weight polyethylene fiber is 40-75%.
7. The lightweight, breathable, high-strength upper fabric according to claim 5, characterized in that: The twisted warp in the warp yarn is 1 low-temperature qualitative hot-bonded yarn, and the ground warp is 6 ultra-high molecular weight polyethylene fibers; the weft yarn is 6 ultra-high molecular weight polyethylene fibers and 1 low-temperature hot-bonded yarn.
8. The lightweight, breathable, high-strength upper fabric according to claim 5, characterized in that: The warp yarn is composed of 1 low-temperature qualitative hot-bonded yarn, and the ground warp is composed of 3 ultra-high molecular weight polyethylene fibers and 3 PEBA monofilaments; the weft yarn is composed of 3 ultra-high molecular weight polyethylene fibers, 3 PEBA monofilaments and 1 low-temperature hot-bonded yarn.
9. The lightweight, breathable, high-strength upper fabric according to claim 5, characterized in that: The warp yarn is composed of 1 low-temperature qualitative hot-bonded yarn, and the ground warp is composed of 6 PEBA monofilaments; the weft yarn is composed of 6 ultra-high molecular weight polyethylene fibers and 1 low-temperature hot-bonded yarn.
10. The lightweight, breathable, high-strength upper fabric according to claim 1 or 3, characterized in that: The skin layer and core layer materials of the skin-core structure hot-bonded yarn are prepared through multiple processes including raw material drying, melt extrusion, ice water shaping, hot water stretching, hot air stretching, primary fiber setting, secondary fiber setting, oiling to increase lubrication, and winding.
Citation Information
Patent Citations
Sheath-core type low-melting-point copolyamide composite fiber and preparation method thereof
CN104894686A
Elastic composite fiber and preparation method thereof
CN109537076A
High-strength and high-toughness vamp
CN114128960A
Light breathable vamp fabric and light high-elastic fiber spinning process
CN114908453A
Core-spun yarn of polyester-coated ultra-high molecular weight polyethylene and preparation method of core-spun yarn
CN118048719A
Cited By
Wrapped yarn containing ultra-high molecular weight polyethylene fiber and preparation method and application thereof
CN120889080A