Structures including photoresist adhesive layers and

By using photoresist adhesion layers in electronic device manufacturing, the metal contamination and defect control problems of MOR in high numerical aperture extreme ultraviolet lithography are solved, achieving higher pattern transfer resolution and stability, reducing Radiation dose during photolithography process.

CN118859631APending Publication Date: 2024-10-29ASM IP HLDG BV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410494609.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2023-04-27
Filing Date
2024-04-24
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

In the manufacturing process of electronic devices, the metal oxide resist (MOR) used in high numerical aperture extreme ultraviolet lithography technology has challenges such as metal contamination control, line width roughness and defect control, making it difficult to form fine and stable feature patterns. .

Method used

A photoresist adhesive layer is used to form a non-metallic adhesive layer through a cyclic deposition process to reduce metal pollution. Nitrogen is included in the adhesive layer to improve the etching selectivity and exposure efficiency of the photolithography process and promote carbon hardening. Bonding between mask and MOR.

Benefits of technology

It reduces metal contamination and defects in the photolithography process, improves the resolution and stability of pattern transfer, reduces the radiation dose requirements of the photolithography process, and increases the throughput of the manufacturing process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118859631A_ABST
    Figure CN118859631A_ABST
Patent Text Reader

Abstract

A method of forming a structure including an adhesive layer and a structure including an adhesive layer are disclosed. The adhesive layer may include nitrogen. The method may include forming a metal oxide resist overlying and in contact with the adhesive layer. The example method also includes forming a bottom layer of photoresist.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates generally to structures and methods of forming structures using photoresists. More particularly, the present disclosure relates to structures including a photoresist adhesion layer and methods of forming such structures. Background Art

[0002] In the manufacture of electronic devices, fine patterns of features can be formed on a substrate surface by patterning the substrate surface and etching material from the substrate surface using, for example, a vapor phase etching process. As the density of devices on a substrate increases, it is increasingly desirable to form features of smaller size.

[0003] Prior to etching, photoresists are often used to pattern the surface of a substrate. A pattern can be formed in a photoresist by applying a photoresist layer to a substrate surface, masking the surface of the photoresist, exposing unmasked portions of the photoresist to radiation, such as ultraviolet light, and removing a portion of the photoresist (e.g., the unmasked or masked portion) while leaving a portion of the photoresist on the substrate surface.

[0004] High numerical aperture (high NA) extreme ultraviolet (EUV) lithography can provide relatively high resolution for smaller pitch patterns. However, this lithography usually uses relatively thin photoresist (PR) films and relatively thin carbon hard mask (CHM) films. Studies on chemically amplified resists (CARs) have shown that thinner PR films lead to increased line edge and line width roughness (LER / LWR). Recently, metal oxide resists (MORs) have attracted attention. Compared with traditional organic CARs, MORs show better resolution on line / space and pillar patterns, and better local critical dimension (CD) uniformity (LCDU) on pillar patterns. Better resolution should expand the single patterning approach, which in turn will reduce process complexity and cost. Robust refractory metal oxide etch barrier layers make MOR more suitable for pattern transfer of smaller features and thinner resists, and provide better etching durability and sensitivity. MOR is considered to be the most suitable candidate PR for high NA EUV lithography. However, there are still some challenges when considering the use of MOR, including metal contamination control, CD control, and defect control.

[0005]

[0006] Therefore, there is a need for improved methods and structures suitable for forming fine patterns of features on substrate surfaces.

[0006] Any discussion of problems and solutions set forth in this section has been included in the present disclosure merely to provide context for the present disclosure, and should not be considered an admission that any or all of the discussion was known at the time the present invention was made. Summary of the invention

[0007] Various embodiments of the present disclosure relate to methods of forming structures including an adhesion layer, and more specifically, to methods of forming structures including a metal oxide resist (MOR) or suitable for use therewith. Although the manner in which various embodiments of the present disclosure address the shortcomings of existing methods is discussed in more detail below, in general, various embodiments of the present disclosure provide a method that includes using a photoresist adhesion layer to promote adhesion between, for example, a carbon hard mask (CHM) and a MOR. The adhesion layer can be non-metallic to reduce metal contamination and can have tunable surface properties so that the adhesion layer can be used with various MORs. In addition, the adhesion layer can have a relatively high etch selectivity to an underlying layer (e.g., silicon oxide) compared to, for example, a silicon oxycarbide photoresist underlying layer. In addition, the inclusion of nitrogen in the adhesion layer can increase the secondary electron source during the lithography process, which can allow for a reduction in radiation dose during the exposure step of the lithography process.

[0008] According to an example of the present disclosure, a method for forming a structure including an adhesive layer includes providing a substrate including a substrate surface in a reaction chamber, and forming an adhesive layer using a (e.g., first) cyclic deposition process covering the substrate surface. The step of forming the adhesive layer may include providing a silicon precursor to the reaction chamber, providing one or more of an inert gas and a nitrogen-containing reactant gas into the reaction chamber, and forming a plasma to form an active substance that reacts with the silicon precursor or its derivative to form an adhesive layer. In some cases, the silicon precursor includes nitrogen. In some cases, the silicon precursor may not include nitrogen—that is, the silicon precursor may include a nitrogen-free precursor. The adhesive layer may include silicon, oxygen, carbon, and nitrogen. According to a further example, the method may include forming a metal oxide resist (MOR) covering the adhesive layer. The exemplary method may further include forming a photoresist bottom layer covering the substrate, wherein the photoresist bottom layer is between the substrate surface and the adhesive layer. The bottom layer may include, for example, an oxide, a nitride, or a nitride oxide. The photoresist bottom layer may be formed using a second cyclic deposition process.

[0009] According to an exemplary embodiment of the present disclosure, a structure is formed using the method described herein.

[0010] According to a further example of the present disclosure, a system for forming an adhesion layer is provided. The exemplary system includes a reaction chamber, a silicon precursor source fluidly coupled to the reaction chamber, an inert and / or nitrogen source fluidly coupled to the reaction chamber, and a controller configured to perform a method or a portion thereof as described herein.

[0011] These and other embodiments will become readily apparent to those skilled in the art from the following detailed description of certain embodiments, which proceeds by reference to the attached figures; the invention is not limited to any particular embodiment disclosed. BRIEF DESCRIPTION OF THE DRAWINGS

[0012] A more complete understanding of exemplary embodiments of the present disclosure may be obtained by referring to the detailed description and claims when considered in conjunction with the following illustrative drawings.

[0013] Figure 1 A method according to an exemplary embodiment of the present disclosure is shown.

[0014] Figure 2 A cyclic deposition process according to an exemplary embodiment of the present disclosure is shown.

[0015] Figure 3 Another cyclic deposition process according to an exemplary embodiment of the present disclosure is shown.

[0016] Figure 4 The structure of an exemplary embodiment according to the present disclosure is shown.

[0017] Figure 5 A system configured for performing the methods described herein is shown.

[0018] Figure 6 Systems according to other examples of the present disclosure are shown.

[0019] It should be understood that the elements in the drawings are shown for simplicity and clarity and are not necessarily drawn to scale. For example, the size of some elements in the drawings may be exaggerated relative to other elements to help improve the understanding of the illustrated embodiments of the present disclosure. DETAILED DESCRIPTION

[0020] Although certain embodiments and examples are disclosed below, it should be understood that the invention extends beyond the specifically disclosed embodiments and / or their uses and their obvious modifications and equivalents. Therefore, it is intended that the scope of the disclosed invention should not be limited by the specifically disclosed embodiments described below.

[0021] The present disclosure generally relates to methods of forming structures including adhesion layers and structures including adhesion layers. As described in more detail below, exemplary methods can be used to form structures suitable for use with or including metal oxide resists (MORs). Use of the adhesion layers described herein can reduce defects that may occur during photolithography and can mitigate metal contamination that may occur when using a metal underlayer. In addition, use of the adhesion layers described herein can provide relatively high etch selectivity—for example, compared to an underlayer that does not contain nitrogen, which improves pattern transfer, particularly for patterns or features with high aspect ratios. In addition, use of the adhesion layers described herein can reduce the amount of radiation required during the exposure step of the photolithography process, thereby increasing the yield of the manufacturing process.

[0022] As used herein, the term "substrate" may refer to any one or more underlying materials including and / or on which one or more layers may be deposited. The substrate may include a bulk material, such as silicon (e.g., single crystal silicon), other Group IV materials, such as germanium, or a compound semiconductor material, such as GaAs, and may include one or more layers overlying or beneath the bulk material. For example, the substrate may include a multilayer patterned stack overlying the bulk material. The patterned stack may vary depending on the application. In addition, the substrate may additionally or alternatively include various features, such as grooves, lines, etc. formed in or on at least a portion of the substrate layer. According to an example of the present disclosure, the substrate may include a carbon hard mask (CHM) on the surface.

[0023] In some embodiments, a film refers to a layer extending in a direction perpendicular to the thickness direction. In some embodiments, a layer refers to a synonym for a material or a film or non-film structure having a certain thickness formed on a surface. A film or layer may be composed of a discrete single film or layer or multiple films or layers having certain properties, and the boundaries between adjacent films or layers may be clear or unclear, and may be established or not established based on physical, chemical and / or any other properties, formation process or sequence and / or the function or purpose of adjacent films or layers. In addition, a layer or film may be continuous or discontinuous.

[0024] In the present disclosure, a gas may include a material that is a gas at normal temperature and pressure, a vaporized solid, and / or a vaporized liquid, and may consist of a single gas or a gas mixture, depending on the context. Gases other than process gases, i.e., gases that are not introduced through a gas distribution component (e.g., a showerhead, other gas distribution devices, etc.), may be used, for example, to seal a reaction space, and may include sealing gases, such as rare gases.

[0025] In some cases, such as in the case of material deposition, the term precursor can refer to a compound that participates in a chemical reaction to produce another compound, particularly a compound that constitutes the membrane matrix or the main skeleton of the membrane, while the term reactant can refer to a compound that activates the precursor, modifies the precursor, or catalyzes the reaction of the precursor, and in some cases is different from the precursor; the reactant can provide elements (such as O, N and / or C) to the membrane matrix and become part of the membrane matrix. In some cases, the terms precursor and reactant can be used interchangeably. The term inert gas refers to a gas that does not participate in the chemical reaction to an appreciable extent and / or a gas that excites or splits the precursor when, for example, RF or microwave power is applied, but unlike the reactant, it may not become part of the membrane matrix to an appreciable extent.

[0026] The term cyclic deposition process or cyclic deposition process can refer to the sequential introduction of precursors (and / or reactants) into a reaction chamber to deposit layers on a substrate, and includes processing techniques such as atomic layer deposition (ALD), cyclic chemical vapor deposition (cyclic CVD), and hybrid cyclic deposition processes that include an ALD component and a cyclic CVD component and can be plasma enhanced.

[0027] The term atomic layer deposition may refer to a vapor deposition process in which a deposition cycle (typically multiple consecutive deposition cycles) is performed in a processing chamber. Typically, for an ALD process, during each cycle, a precursor is introduced into the reaction chamber and chemically adsorbed onto a deposition surface (e.g., a substrate surface that may include previously deposited material or other material from a previous ALD cycle), forming a monolayer or sub-monolayer of material that is not easily reacted with additional precursors (i.e., a self-limiting reaction). Thereafter, in some cases, a reactant (e.g., another precursor or a reactive gas or an inert gas) may subsequently be introduced into the processing chamber for converting the chemically adsorbed precursor onto the deposition surface into a desired material. The reactant / inert gas is capable of further reacting or interacting with the precursor. During one or more cycles, such as during each step of each cycle, a purge step may be utilized to remove any excess precursor from the processing chamber and / or to remove any excess reactant and / or reaction byproducts from the reaction chamber.

[0028] In the present disclosure, any two numbers of a variable may constitute a feasible range of the variable, and any range indicated may include or exclude endpoints. In addition, any value of the variable indicated (whether or not they are expressed as "about") may refer to an exact value or an approximate value, and include equivalents, and in some embodiments may refer to an average value, a median, a representative value, a majority value, etc. In addition, in the present disclosure, the terms "include", "consist of" and "have" and related words may independently refer to "usually or broadly include", "comprise", "essentially consist of" or "consist of" in some embodiments. According to various aspects of the present disclosure, the meaning of any definition of a term does not necessarily exclude the common and customary meaning of the term.

[0029] Now turning to the attached figure, Figure 1 A method 100 of forming a structure including an adhesion layer according to an exemplary embodiment of the present disclosure is shown. The method 100 includes the steps of providing a substrate (step 102), optionally forming a photoresist bottom layer (step 104), and forming an adhesion layer (step 106).

[0030] Step 102 includes providing a substrate, such as a substrate described herein. The substrate may include one or more layers to be etched, including one or more material layers. For example, the substrate may include a deposited oxide, a native oxide, or an amorphous carbon layer to be etched and a carbon hard mask. The substrate may include several layers below the material layer to be etched.

[0031] During step 104, a photoresist bottom layer is formed on the substrate surface. The photoresist bottom layer can be formed using a variety of techniques, including spin coating, chemical vapor deposition, and cyclic processing techniques. Plasma-treated SiO and SiOC materials are considered promising candidates for photoresist bottom layer materials due to their ability to sustain thinner thicknesses and lower dry etching rates compared to conventional spin-on glass (SoG). In general, PEALD is suggested as a method to obtain higher (lower) film thickness non-uniformity (%NU).

[0032] According to exemplary aspects of method 100, a photoresist bottom layer is formed using a cyclic deposition process, such as an ALD process (e.g., PEALD). The cyclic deposition process may include the use of an active substance (e.g., formed by one or more of a precursor, a reactant, and / or an inert gas) that is formed using one or more of a direct plasma and a remote plasma. Alternatively, step 104 may include a thermal cyclic deposition process. The use of cyclic deposition processes may be desirable because they allow the formation of a photoresist bottom layer having a desired thickness within and between substrates—e.g., less than 10 nm or less than or approximately equal to 5 nm, with improved thickness uniformity. The use of a plasma enhanced process may be desirable because it allows the deposition of a photoresist bottom layer material at a relatively low temperature and / or a relatively high rate compared to thermal treatments.

[0033] According to examples of the present disclosure, the temperature within the reaction chamber during step 104 may be less than 500° C., less than 300° C., less than 100° C., or between about 50° C. and about 500° C., or between about 150° C. and about 300° C. The pressure within the reaction chamber during step 104 may be about 1 Torr to about 100 Torr, about 2 Torr to about 20 Torr, or about 3 Torr to about 10 Torr.

[0034] According to an exemplary embodiment of the present disclosure, step 104 includes forming or depositing one or more of silicon or metal oxides, silicon or metal nitrides, and silicon or metal oxynitrides. Such oxides, nitrides, and / or oxynitrides may also include carbon.

[0035] The photoresist bottom layer may include, for example, one or more of the following: silicon oxide, silicon oxycarbide, silicon nitride, silicon oxynitride, silicon carbon nitride, silicon oxycarbon nitride, metal oxide, metal nitride, metal carbon oxide, metal nitride oxide, metal oxycarbon nitride and metal carbon nitride. The metal may include, for example, one or more metals selected from titanium, tantalum, tungsten, tin and hafnium. In some cases, the photoresist bottom layer includes carbon. When the photoresist bottom layer is deposited, carbon may be incorporated into the photoresist bottom layer, and / or the surface of the photoresist bottom layer may be subjected to carbon treatment. Additionally or alternatively, a carbon-containing layer or other layers may be deposited on the surface of the photoresist bottom layer. The thickness of the photoresist bottom layer may be less than 10nm, less than 5nm, or greater than 0nm and less than 10nm.

[0036] Figure 3 A cyclic process 300 for forming a photoresist bottom layer suitable for step 104 is shown. The cyclic process 300 may include (A) pulsing a first precursor containing a metal or silicon into a reaction chamber (step 302), and (B) pulsing or continuously providing a reactant (e.g., an oxidant and / or a nitriding agent and / or an inert gas) into the reaction chamber (step 310). In the illustrated example, the cyclic process 300 also includes forming a plasma (step 306) by providing a plasma power (step 312) to form a plasma. The cyclic process 300 may also include purging the reaction chamber (steps 304, 306). During the purging steps 304, 306, any excess precursor and / or reactant and / or any reaction byproducts may be purged from the reaction chamber. Purging may be performed by supplying an inert gas to the reaction chamber and / or using a vacuum source. The cyclic process 300 may be repeated—for example, between about 10 and about 50 times or between about 200 and about 500 times—before the method 100 proceeds to step 106. The cyclic deposition process 300 may be a plasma enhanced atomic layer deposition process.

[0037] In some cases, a cyclic process for forming a photoresist bottom layer may include (A) pulsing a metal-containing precursor into a reaction chamber, (B) pulsing or continuously providing a reactant (e.g., comprising an oxidant and / or a nitriding agent and / or an inert gas) into the reaction chamber, and (C) pulsing a carbon precursor into the reaction chamber. One or more pulses may be separated by a purge step. In addition, each pulse step or a combination of pulse steps (e.g., pulse steps (A) and (B)) may be repeated multiple times before proceeding to the next step to adjust the composition of the photoresist bottom layer. For example, the ratio of (AB):C may range from about 1:1 to about 1:10. Unless otherwise indicated, steps (A) and (B) or steps (A), (B), and (C) may be performed in any order, and various combinations of these steps may be repeated.

[0038] According to an exemplary aspect of the present disclosure, a precursor comprising silicon is provided during step 302. In some cases, the silicon precursor may also include carbon. Exemplary silicon precursors suitable for forming the photoresist bottom layer include the silicon precursors mentioned below in conjunction with step 202.

[0039] According to other exemplary aspects of the present disclosure, the precursor includes a metal. In these cases, the precursor may include a transition metal, such as one or more metals selected from titanium, tantalum, tungsten, tin and hafnium. The precursor comprising the metal may also include carbon, such as one or more organic groups directly or indirectly bonded to the metal atom. As a specific example, the precursor comprising the metal may include a metal halide or a metal organic compound or an organometallic compound, such as one or more of the following: tetrakis(dimethylamino)titanium (TDMAT), titanium isopropoxide (TTIP), titanium chloride (TiCl), tetrakis(ethylmethylamino)hafnium (TEMAHf), hafnium chloride (HfCl), trimethylaluminum (TMA), triethylaluminum (TEA), other metal halides or other metal-containing compounds.

[0040] The reactants may include oxidizing reactants, nitriding reactants, or reducing agents, such as hydrogen-containing reactants. Oxidizing and / or nitriding reactants include reactants containing one or more of oxygen and nitrogen. In some cases, the reactants may include nitrogen and oxygen. And, in some cases, two or more oxidizing and / or nitriding reactants may be contained in a single pulse or continuous flow. Exemplary oxidizing and nitriding agents include oxygen (O2), water (H2O), ozone (O3), hydrogen peroxide (H2O2), ammonia (NH3), diazene (N2H2), CO2, nitrous oxide (N2O); exemplary hydrogen-containing reactants include hydrogen (H2), etc.

[0041] As described above, the oxidizing and / or nitriding reactants may be exposed to (e.g., directly) plasma during step 306 / 312 to form excited species for a PEALD process or a cyclic plasma process. The power at which the plasma is formed during step 312 / 306 may be about 20 W to about 1000 W. The frequency of the power at which the plasma is formed may be between about 200 kHz and about 2.45 GHz. The duration of step 312 may be between about 0.01 seconds and about 5 seconds.

[0042] When used, the carbon precursor may include any suitable organic compound, such as a compound comprising carbon and oxygen. In some cases, the carbon precursor may also include nitrogen. The carbon precursor may be selected to react with, for example, the -OH-terminated surface of a metal oxide and / or the -NH2-terminated surface of a metal nitride. Examples of suitable carbon precursors include one or more of the following: organic compounds, such as anhydrides (e.g., acetic anhydride), toluene, diethylene glycol, triethylene glycol, acetaldehyde; and organosilicon compounds, such as silanes and siloxanes. Exemplary organosilicon compounds include (n,n-dimethylamino)trimethylsilane, trimethoxy(octadecyl)silane, hexamethyldisilazane, trimethoxy(3,3,3-trifluoropropyl)silane, trimethoxyphenylsilane, trichloro(3,3,3-trifluoropropyl)silane and hexamethyldisilazane.

[0043] Once the photoresist bottom layer is formed, an adhesion layer is formed during step 106. Step 106 may be performed in-situ within the same reaction chamber and without air and / or vacuum breaks.

[0044] Figure 2 An exemplary cyclic deposition process 200 for forming an adhesion layer is shown. The cyclic deposition process 200 includes pulsing or providing a silicon precursor to a reaction chamber (step 202), purging any unreacted precursor and / or byproducts (step 204), providing one or more of an inert gas and a nitrogen-containing reactant gas into the reaction chamber (step 210); and forming a plasma using the inert gas and / or the nitrogen-containing reactant gas, and providing plasma power (step 212) to form a plasma (step 206) that produces reactive species that react with the silicon precursor or a derivative thereof to form an adhesion layer, and purging any excess reactive species and / or byproducts from the reaction chamber (step 208). As shown, steps 202-208 may be repeated—e.g., between about 5 and about 50 times, or about 200 or about 500 times. The temperature and pressure during step 106 may be the same or similar to steps 102 and / or 104.

[0045] During step 202, a silicon precursor is provided to a reaction chamber. According to an example of the present disclosure, the silicon precursor includes nitrogen. In some cases, the silicon precursor does not contain nitrogen. When the silicon precursor is a nitrogen-free precursor, the reactants may include nitrogen so that the adhesion layer includes silicon, oxygen, carbon, and nitrogen.

[0046] According to further examples, the silicon precursor consists of or consists essentially of Si, C, H and O or Si, C, H, O and N, which can be provided to the reaction chamber with the help of a carrier gas. For example, the silicon precursor can be selected from one or more of the following:

[0047] (a)

[0048] (b)

[0049] (c)

[0050] (d)

[0051] According to further examples, the silicon precursor is selected from one or more of the following: 3-methoxypropyltrimethoxysilane, bis(trimethoxysilyl)methane, 1,2-bis(methyldimethoxysilyl)ethane, 1,2-bis(triethoxysilyl)ethane, 1,2-bis(diethoxymethylsilyl)ethane, 1,2-bis(trimethoxysilyl)ethane, 1,1,3,3-tetramethoxy-1,3-disilacyclobutane, 1,1,3,3-tetraethoxy-1,3-disilacyclobutane, 1,1,3,3,5,5-hexamethoxy-1,3,5-trisilylcyclohexane, 1,1,3,3,5,5-hexaethoxy-1,3,5-trisilylcyclohexane and 3-(trimethoxysilyl)propylamine. As a specific example, the silicon precursor may be or include 3-methoxypropyltrimethoxysilane or 3-(trimethoxysilyl)propylamine. The flow rate of the silicon precursor during step 202 may be between about 100 sccm and about 150 sccm. The duration of step 202 may be between about 0.1 s and about 0.3 s. According to an example of the present disclosure, the silicon precursor used during process 300 (step 104) is the same as the silicon precursor used during process 200 (step 106). In other cases, the silicon precursor may be different.

[0052] Any excess silicon precursor and / or any reaction byproducts may be purged from the reaction chamber during step 204. Purging may be performed by supplying an inert gas to the reaction chamber and / or using a vacuum source.

[0053] During step 206, a plasma is formed using an inert gas and / or a nitrogen-containing reactant gas. The inert gas may be or include one or more of the following: Ar, He, Ne, Kr, Xe, O2, CO, CO2, CxH y and H2 or mixtures thereof. The nitrogen-containing reactant gas may be or include N2, N2O, NH3 or mixtures thereof. The flow rate of one or more of the inert gas and the nitrogen-containing reactant gas may be between about 5 and about 100 sccm or between about 0.1 and about 10 slm.

[0054] The power used to form the plasma during step 206 / 212 may be between about 20 W and about 1000 W. The duration of step 312 may be between about 0.01 s and about 5 s. The frequency of the power used to form the plasma may be between about 200 kHz and about 2.45 GHz.

[0055] During step 208, the plasma power is turned off and any excess reactive species and / or byproducts are purged. Steps 202-208 may be repeated multiple times to form a silicon-based adhesion layer of a desired thickness—eg, greater than 0 and less than about 2 nm.

[0056] The method according to the present disclosure may also include the step of forming a photoresist layer covering and contacting the adhesive layer. According to an example of the present disclosure, the photoresist layer is or includes a metal oxide resist (MOR). Exemplary MOR materials include oxides of tin, titanium, tantalum, indium and / or zirconium. MOR can be deposited using, for example, a spin coating technique or a vapor deposition technique. The thickness of MOR can be greater than 0 and less than 100 nm.

[0057] Table 1 below shows specific process conditions, which show that the amount of nitrogen and carbon in the bonding layer can be controlled by controlling the process conditions. The precursor used in the examples of Table 1 is a nitrogen-free precursor, and the reactant is nitrogen (N2).

[0058]

[0059] As can be observed by the table, the nitrogen content and the carbon content can be controlled, with samples having high carbon and low nitrogen on the one hand and high carbon and nitrogen on the other.

[0060] These analyses from XPS consider depths up to 10 nm, so one must consider that the actual nitrogen and carbon content will be much higher, since the layers have 1.4 to 2.4 nm. In any case, the relative elemental composition can be inferred.

[0061] By using a nitrogen plasma in this way, it is possible to introduce relevant nitrogen contents without eliminating carbon in the adhesion-promoting layer. It also has advantages over using different precursors, as this allows easier processing (using the same precursor for the adhesion layer and the bottom layer) and higher nitrogen contents.

[0062] Figure 4 A structure 400 is shown according to an exemplary embodiment of the present disclosure. The structure 400 can be formed using the method 100, for example.

[0063] As shown, structure 400 includes a substrate 402 , a material layer 404 , a photoresist bottom layer 406 , a photoresist layer 408 , and an adhesive layer 410 interposed between and in contact with the photoresist bottom layer 406 and the photoresist layer 408 .

[0064] Substrate 402 may include a substrate as described above. For example, substrate 402 may include a semiconductor substrate, such as a bulk material, such as silicon (e.g., single crystal silicon), other IV semiconductor materials, III-V semiconductor materials, and / or II-VI semiconductor materials, and may include one or more layers (e.g., a patterned stack) covering the bulk material. In addition, as described above, substrate 402 may include various topological structures, such as grooves, lines, etc. formed in or on at least a portion of the substrate layer.

[0065] As described herein, a photoresist base layer and a photoresist layer can be used to pattern and etch the material layer 404. Exemplary materials suitable for the material layer 404 include, for example, oxides, such as native oxides or field oxides. Other exemplary material layer 404 materials include carbon hardmask, amorphous carbon, nitrides, other oxides, silicon, and additional films such as self-assembled monolayers such as hexamethyldisilazane (HMDS).

[0066] The photoresist bottom layer 406 may include a photoresist bottom layer formed according to the methods described herein (e.g., method 100 / process 300) and / or have the properties and / or materials described herein. Exemplary photoresist bottom layers include one or more of silicon or metal oxides, silicon or metal nitrides, and silicon or metal oxynitrides—any of which may or may not include carbon. For example, the photoresist bottom layer 406 may include one or more of silicon oxide, silicon oxycarbide, silicon nitride, silicon oxynitride, silicon carbonitride, silicon oxycarbonitride, metal oxide, metal nitride, metal oxycarbide, metal oxynitride, metal oxycarbonitride, and metal carbonitride.

[0067] The thickness of the photoresist bottom layer 406 may depend on the composition of the material layer 404, the thickness of the material layer 404, the type of photoresist, etc. According to an example of the present disclosure, the photoresist bottom layer 406 has a thickness less than 10 nm, or less than or about 5 nm, or between about 0.1 nm and about 10 nm.

[0068] As described herein, the adhesive layer 410 ideally exhibits good adhesion and other properties. As described above, according to an example of the present disclosure, the adhesive layer 410 includes nitrogen. According to an example of the present disclosure, the adhesive layer includes silicon, oxygen, carbon, and nitrogen. The thickness of the adhesive layer can be greater than 0nm and less than 2nm.

[0069] In order to provide the desired adhesion between the photoresist layer 408 and the photoresist bottom layer 406, the adhesive layer 410 can have or be adjusted to have the desired surface chemical properties, such as quantified as surface energy, which is further classified into the polar part of the surface energy and the dispersed part of the surface energy. The polar part of the surface energy and the dispersed part of the surface energy of the photoresist bottom layer 406 can be calculated by measuring the contact angle of a liquid such as water or CH2I2 and determining the polar part and the dispersed part of the surface energy using the Owens, Wendt, Rabel and Kaelble (OWRK) method. The same characteristics of the photoresist layer 408 can be measured and calculated.

[0070] According to further examples of the present disclosure, the photoresist layer 408 is or includes MOR. Exemplary MOR materials and thicknesses are described above.

[0071] Figure 5 A system 500 configured to perform the methods described herein is shown. System 500 includes at least one reaction chamber configured to deposit an underlayer and / or form an adhesion layer as described herein. System 500 may include a first reaction chamber 511 and a second reaction chamber 512, both of which may be configured to deposit an underlayer and form an adhesion layer or a portion thereof as described herein. If desired, system 500 may include a third reaction chamber 513, in which another process, such as thermal or plasma enhanced post-processing, may be performed.

[0072] Figure 6 An exemplary reaction system is shown that includes a chamber suitable for use as reaction chamber 511 or 512. Reactor system 600 can be used to perform one or more steps or sub-steps described herein and / or form one or more structures described herein or portions thereof.

[0073] The reactor system 600 includes a pair of conductive plate electrodes 4, 2 parallel and facing each other in the interior 11 (reaction zone) of the reaction chamber 3. Plasma can be ignited in the reaction chamber 3 by applying HRF power (e.g., 13.56 MHz or 27 MHz) from, for example, a power source 25 to one electrode (e.g., electrode 4) and electrically grounding the other electrode (e.g., electrode 2). A temperature regulator can be provided in the lower platform 2 (lower electrode), and the temperature of the substrate 1 placed thereon can be maintained at a desired temperature. The electrode 4 can be used as a gas distribution device, such as a shower plate. Reactant gas, dilution gas (if any), precursor gas, etc. can be introduced into the reaction chamber 3 through the shower plate 4 using one or more of the gas pipeline 20, the gas pipeline 21, and the gas pipeline 22, respectively. Although three gas pipelines are illustrated, the reactor system 600 can include any suitable number of gas pipelines. The gas pipeline 20 can be connected to a silicon precursor source 29, the gas pipeline 21 can be connected to an inert gas source 27, and the gas pipeline 22 can be connected to another (e.g., reactant) gas source 28.

[0074] In the reaction chamber 3, a circular duct 13 having an exhaust line 7 is provided, through which the gas in the interior 11 of the reaction chamber 3 can be exhausted. In addition, the transfer area 5 arranged below the reaction chamber 3 is provided with a sealing gas line 24 to introduce the sealing gas into the interior 11 of the reaction chamber 3 via the interior 16 (transfer zone) of the transfer area 5, wherein a partition plate 14 for separating the reaction zone and the transfer zone is provided (the figure omits the gate valve through which the wafer is transferred into or out of the transfer area 5). The transfer area is also provided with an exhaust line 6. In some embodiments, the deposition and treatment steps are performed in the same reaction space, so that two or more (e.g., all) (e.g., the base layer and the bonding layer) steps can be performed continuously without exposing the substrate to air or other oxygen-containing atmospheres.

[0075] In some embodiments, the continuous flow of the inert gas or carrier gas to the reaction chamber 3 can be achieved using a flow system (FPS), wherein the carrier gas line is provided with a detour line having a precursor reservoir (bottle), and the main line and the detour line are switched, wherein when only the carrier gas is intended to be supplied to the reaction chamber, the detour line is closed, and when both the carrier gas and the precursor gas are intended to be supplied to the reaction chamber, the main line is closed, the carrier gas flows through the detour line, and flows out of the bottle together with the precursor gas. In this way, the carrier gas can flow continuously into the reaction chamber, and the precursor gas can be delivered in pulses by switching between the main line and the detour line without significantly fluctuating the pressure of the reaction chamber.

[0076] Reactor system 600 also includes one or more controllers 26, which are programmed or otherwise configured to implement one or more method steps described herein. Controller 26 is communicated with various power supplies, heating systems, pumps, robots, and gas flow controllers or valves of the reactor, as will be understood by those skilled in the art. For example, controller 26 can be configured to control the gas flow of silicon precursors and inert gases to form an adhesive layer on the photoresist bottom layer. Additionally or alternatively, the controller can be configured to perform steps to form a photoresist bottom layer as described herein.

[0077] In some embodiments, a dual chamber reactor (two portions or compartments for processing a wafer positioned close to each other) may be used, wherein reactant gases and noble gases may be supplied through shared lines, while precursor gases are supplied through non-shared lines.

[0078] The exemplary embodiments disclosed above do not limit the scope of the present invention, because these embodiments are merely examples of embodiments of the present invention. Any equivalent embodiments are within the scope of the present invention. In fact, in addition to the embodiments shown and described herein, various modifications of the present disclosure, such as the useful alternative combinations of the described elements, will become apparent to those skilled in the art from the description. Such modifications and embodiments are also intended to fall within the scope of the appended claims.

Claims

1. A method of forming a structure comprising an adhesive layer, the method comprising: The following steps are involved: providing a substrate including a substrate surface within a reaction chamber; and The bonding layer is formed using a first cycle deposition process covering the surface of the substrate, the steps of forming the bonding layer comprising: providing a silicon precursor to the reaction chamber; providing one or more of an inert gas and a nitrogen-containing reactant gas into the reaction chamber; and forming a plasma to form a reactive species that reacts with the silicon precursor or a derivative thereof to form an adhesion layer, The bonding layer contains silicon, oxygen, carbon and nitrogen. 2 . The method according to claim 1 , further comprising forming a metal oxide resist (MOR) covering the adhesion layer.

3. The method according to claim 1 or 2, further comprising forming a photoresist bottom layer covering the substrate, wherein the photoresist bottom layer is interposed between the substrate surface and the adhesive layer.

4. The method according to claim 3, in, The photoresist bottom layer includes one or more of the following: silicon oxide, silicon oxycarbide, silicon nitride, silicon oxynitride, silicon carbon nitride, silicon oxycarbon nitride, metal oxide, metal nitride, metal oxycarbide, metal oxynitride, metal oxycarbon nitride and metal carbon nitride.

5. The method according to claim 4, in, The metal includes one or more metals selected from titanium, tantalum, tungsten, tin and hafnium.

6. The method according to any one of claims 3 to 5, in, The thickness of the photoresist bottom layer is greater than 0.1 nm and less than 10 nm.

7. The method according to any one of claims 1 to 6, in, The first cyclic deposition process is an atomic layer deposition process.

8. The method according to any one of claims 1 to 7, in, The silicon precursor includes nitrogen.

9. The method according to any one of claims 1 to 7, in, The silicon precursor includes a nitrogen-free precursor.

10. The method according to any one of claims 1 to 9, in, The silicon precursor is selected from one or more of the following:

11. The method according to any one of claims 1 to 10, in, The silicon precursor is selected from one or more of the following: 3-methoxypropyltrimethoxysilane, bis(trimethoxysilyl)methane, 1,2-bis(methyldimethoxysilyl)ethane, 1,2-bis(triethoxysilyl)ethane, 1,2-bis(diethoxymethylsilyl)ethane, 1,2-bis(trimethoxysilyl)ethane, 1,1,3,3-tetramethoxy-1,3-disilacyclobutane, 1,1,3,3-tetraethoxy-1,3-disilacyclobutane, 1,1,3,3,5,5-hexamethoxy-1,3,5-trisilylcyclohexane, 1,1,3,3,5,5-hexaethoxy-1,3,5-trisilylcyclohexane and 3-(trimethoxysilyl)propylamine.

12. The method according to any one of claims 3 to 11, in, The photoresist bottom layer is formed using a second cyclic deposition process.

13. The method according to any one of claims 3 to 12, in, The photoresist bottom layer is formed using the silicon precursor.

14. The method according to any one of claims 1 to 8, in, The chemical formula of the silicon precursor consists of Si, C, H, O and N.

15. The method according to any one of claims 1 to 14, in, The first cyclic deposition process is repeated between about 5 and about 50 times or about 200 times or about 500 times.

16. The method according to any one of claims 1 to 15, in, The thickness of the adhesive layer is greater than 0.1 nm and less than 10 nm.

17. The method according to any one of claims 11 to 16, in, The second cyclic deposition process is repeated between about 5 and about 50 times or between about 200 and about 500 times.

18. A structure formed by the method of any one of claims 1-17.

19. The structure according to claim 18, in, The photoresist bottom layer includes one or more of the following: silicon oxide, silicon oxycarbide, silicon nitride, silicon oxynitride, silicon carbon nitride, silicon oxycarbon nitride, metal oxide, metal nitride, metal oxycarbide, metal oxynitride, metal oxycarbon nitride and metal carbon nitride.

20. The structure according to claim 18 or 19, in, The thickness of the adhesive layer is greater than 0.1 nm and less than about 10 nm.

21. The structure of any one of claims 17-20, further comprising a MOR overlying and in contact with the adhesive layer.