Dissimilar steel welded joint creep damage quantitative diagnosis and life evaluation method and system

Through creep accelerated fracture experiments and electron backscatter diffraction experiments, characteristic parameters are obtained and analyzed, which solves the accuracy problem of creep damage diagnosis of dissimilar steel welded joints and achieves accurate life span of materials such as T92/HR3C in high temperature and high pressure environments. Assessment and early injury identification.

CN118864360APending Publication Date: 2024-10-29CHINA SPECIAL EQUIP INSPECTION & RES INST
View PDF 0 Cites 6 Cited by

Patent Information

Application Number
CN202410841223.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing creep damage diagnosis methods are difficult to accurately reveal the full picture of creep damage at high temperatures for dissimilar steel welded joints, especially T92/HR3C dissimilar steel welded joints, resulting in inaccurate and unreliable monitoring results, which affects their performance in extreme working conditions. reliability and security.

Method used

By conducting creep accelerated rupture experiments and electron backscatter diffraction experiments on dissimilar steel welded joints, creep rupture images and diffraction data are obtained, and quantitative processing is performed to obtain characteristic parameters, such as pore size, volume fraction, precipitate phase size, and grain size. Size, geometric dislocation density, etc., combined with these parameters to determine its life stage and remaining life.

Benefits of technology

It improves the accuracy of creep tissue damage diagnosis of dissimilar steel welded joints and provides a more reliable life assessment. It is suitable for new materials and long-term service in high-temperature and high-pressure environments. It can identify damage early and provide key information for management.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118864360A_ABST
    Figure CN118864360A_ABST
Patent Text Reader

Abstract

The invention discloses a creep damage quantitative diagnosis and life evaluation method and system for a dissimilar steel welded joint, and relates to the field of welding damage detection.The method comprises the steps that first experimental data of the dissimilar steel welded joint are obtained; performing quantification processing on the first experimental data to obtain first quantitative characteristic parameters including the size of a hole, the volume fraction and the size of a precipitated phase; acquiring second experimental data of the dissimilar steel welded joint; performing quantification processing on the second experimental data to obtain second quantification characteristic parameters including the grain size, the geometric dislocation density, the grain boundary angle, the recrystallization fraction, the recovery grain proportion and the deformation grain proportion; and according to the first quantitative characteristic parameter and the second quantitative characteristic parameter, the current life stage and the creep residual life of the dissimilar steel welded joint are determined. According to the method, the accuracy of quantitative diagnosis of the creep structure damage of the dissimilar steel welded joint can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of welding damage detection, and in particular to a method and system for quantitatively diagnosing creep damage and evaluating life of a dissimilar steel welded joint. Background Art

[0002] In order to improve the efficiency of thermal power generation and save fossil fuels, many countries are developing ultra-supercritical (USC) thermal power generating units with steam temperatures of up to 600°C and above. In recent years, a new generation of heat-resistant steels such as HR3C austenitic steel and T92 ferritic steel have been developed for use in high-temperature components of ultra-supercritical boilers. Generally speaking, austenitic stainless steel is often used for high-temperature parts of the heating surface tubes of power station boilers, while martensitic heat-resistant steel is generally used for parts with relatively low temperatures from an economic point of view. Therefore, many dissimilar metal welded joints such as T92 / HR3C have appeared in ultra-supercritical boilers. Most of these dissimilar steel joints are in high-temperature, high-pressure environments for a long time, and the use conditions are very harsh. They are the parts with many accidents during boiler operation. Creep failure is the most common failure form of high-temperature service components. Therefore, creep damage diagnosis and remaining life prediction for dissimilar steel welded joints have become one of the urgent problems that power plants need to solve.

[0003] For ferrite / austenite dissimilar welded joints, the creep strength of the weld nickel-based alloy and the parent material on the austenite side is higher than that of the ferrite steel, so the ferrite side becomes the weakest link in the entire joint during service. In particular, the heat-affected zone on the ferrite side becomes the first area of ​​the joint to be damaged due to the most serious structural aging. Studies have shown that when T92 / HR3C steel is in service in a power plant, failure fracture occurs in the fine-grained heat-affected zone of T92, which is a relatively weak link in the creep process.

[0004] Creep damage is a key factor affecting material performance and structural integrity under high-temperature working environments. Especially in the energy industry, such as power plants and petrochemical facilities, materials are prone to creep when working under high temperature and high stress conditions for a long time. This slow and continuous deformation process can lead to a decrease in material performance and even sudden structural failure, bringing safety risks and economic losses. Current methods for diagnosing creep damage, such as microstructural analysis and physical property testing, often have limitations in accuracy and efficiency. These methods may require a lot of time and resources, and have limited effectiveness in detecting early damage. Therefore, for dissimilar steel welded joints, especially T92 / HR3C dissimilar steel welded joints, due to their complex microstructural changes at high temperatures, traditional creep tissue damage quantitative diagnosis methods are difficult to fully reveal the full picture of creep damage, and the obtained creep damage monitoring results are inaccurate and unreliable. Therefore, a more sophisticated and comprehensive method is needed for the creep damage diagnosis of such materials to ensure their reliability and safety under extreme working conditions.

[0005] Based on this, how to provide a more accurate and reliable method for quantitative diagnosis of creep structure damage and life assessment of dissimilar steel welded joints to determine the current life stage and creep remaining life of dissimilar steel welded joints is a technical problem that urgently needs to be solved in this field. Summary of the invention

[0006] The purpose of the present invention is to provide a method and system for quantitative diagnosis of creep damage and life assessment of dissimilar steel welded joints, which can effectively improve the accuracy of damage diagnosis of creep structure of dissimilar steel welded joints.

[0007] To achieve the above object, the present invention provides the following solutions:

[0008] In a first aspect, the present invention provides a method for quantitatively diagnosing creep damage and assessing life of a dissimilar steel welded joint, the method comprising:

[0009] Acquire first experimental data of a dissimilar steel weld joint; the first experimental data is a creep rupture image of the dissimilar steel weld joint after creep rupture occurs during a creep accelerated rupture experiment, wherein the creep rupture image includes a microstructure aging image and a precipitation phase image.

[0010] The first experimental data is quantitatively processed to obtain first quantitative characteristic parameters; the first quantitative characteristic parameters include the size, volume fraction and size of pores in the creep rupture image and the size of precipitated phases.

[0011] Acquire second experimental data of the dissimilar steel weld joint; the second experimental data is electron backscatter diffraction experimental data obtained by performing an electron backscatter diffraction experiment after creep rupture of the dissimilar steel weld joint.

[0012] The second experimental data is quantitatively processed to obtain second quantitative characteristic parameters; the second quantitative characteristic parameters include grain size, geometric dislocation density, grain boundary angle, recrystallization fraction, recovery grain ratio and deformation grain ratio.

[0013] The current life stage and the creep residual life of the dissimilar steel weld joint are determined according to the first quantitative characteristic parameter and the second quantitative characteristic parameter.

[0014] Optionally, obtaining first experimental data of a dissimilar steel weld joint specifically includes:

[0015] A creep accelerated fracture experiment was carried out based on the dissimilar steel welded joint to obtain a creep fracture sample.

[0016] The creep rupture sample is observed by using an optical microscope, and the tissue aging image of the creep rupture sample is output.

[0017] The creep rupture sample is observed by using a scanning electron microscope, and the precipitation phase image of the creep rupture sample is output.

[0018] Optionally, before observing the creep rupture sample with an optical microscope and outputting the tissue aging image of the creep rupture sample, the method further includes:

[0019] The sample surface of the creep rupture region of the creep rupture sample is ground and polished respectively to obtain a ground and polished creep rupture sample.

[0020] The polished creep rupture sample is placed in an erosion solution for erosion to obtain an eroded creep rupture sample.

[0021] The eroded creep rupture sample is rinsed and dried to obtain a rinsed creep rupture sample, and the rinsed creep rupture sample is used as the creep rupture sample observed by the optical microscope and the scanning electron microscope.

[0022] Optionally, before performing quantitative processing on the first experimental data to obtain a first quantitative characteristic parameter, the method further includes:

[0023] The creep rupture image is processed by automatic threshold segmentation, edge detection and image denoising in sequence using Image-J software to obtain a preprocessed creep rupture image; the preprocessed creep rupture image is used as the first experimental data for quantitative processing.

[0024] Optionally, the first experimental data is quantitatively processed to obtain a first quantitative characteristic parameter, specifically including:

[0025] Image-J software was used to determine the size and volume fraction of each hole in the tissue aging image.

[0026] According to the precipitation phase image, the type of each precipitation phase in the precipitation phase image is determined.

[0027] The size of each type of precipitated phase in the precipitated phase image was determined using Image-J software.

[0028] Optionally, performing quantitative processing on the second experimental data to obtain a second quantitative characteristic parameter specifically includes:

[0029] The electron backscatter diffraction experimental data are imported into Channel 5 software, and the grain size, geometric dislocation density, grain boundary angle, recrystallization fraction, recovered grain ratio and deformed grain ratio corresponding to the electron backscatter diffraction experimental data are output using Channel 5 software.

[0030] Optionally, before obtaining the second experimental data of the dissimilar steel weld joint, the method further includes:

[0031] The sample surface of the creep rupture sample is polished to obtain a polished creep rupture sample.

[0032] The sample surface of the polished creep rupture sample is electrolytically polished to obtain an electropolished creep rupture sample; the electropolished creep rupture sample is used as the creep rupture sample for the electron backscatter diffraction experiment.

[0033] Optionally, determining the current life stage and creep residual life of the dissimilar steel weld joint according to the first quantitative characteristic parameter and the second quantitative characteristic parameter specifically includes:

[0034] According to the first quantitative characteristic parameter and the second quantitative characteristic parameter, a relationship curve between the characteristic parameters of the dissimilar steel weld joint and the creep life loss is established.

[0035] According to the relationship curve between the characteristic parameters of the dissimilar steel welded joint and the creep life loss, the current life stage and the creep remaining life of the dissimilar steel welded joint are determined.

[0036] In a second aspect, the present invention provides a system for quantitative diagnosis and life assessment of creep damage of dissimilar steel welded joints, the system comprising:

[0037] The first experimental data acquisition module is used to acquire the first experimental data of the dissimilar steel welded joint; the first experimental data is a creep rupture image of the dissimilar steel welded joint after creep rupture occurs during a creep accelerated rupture experiment, and the creep rupture image includes a tissue aging image and a precipitation phase image.

[0038] The first quantitative characteristic parameter acquisition module is used to perform quantitative processing on the first experimental data to obtain first quantitative characteristic parameters; the first quantitative characteristic parameters include the size, volume fraction and size of pores in the creep rupture image.

[0039] The second experimental data acquisition module is used to acquire the second experimental data of the dissimilar steel weld joint; the second experimental data is the electron backscatter diffraction experimental data obtained by performing an electron backscatter diffraction experiment after the dissimilar steel weld joint undergoes creep rupture.

[0040] The second quantitative characteristic parameter acquisition module is used to perform quantitative processing on the second experimental data to obtain second quantitative characteristic parameters; the second quantitative characteristic parameters include grain size, geometric dislocation density, grain boundary angle, recrystallization fraction, recovered grain ratio and deformed grain ratio.

[0041] The diagnosis module is used to determine the current life stage and creep residual life of the dissimilar steel weld joint according to the first quantitative characteristic parameter and the second quantitative characteristic parameter.

[0042] According to the specific embodiments provided by the present invention, the present invention discloses the following technical effects:

[0043] The present invention provides a method for quantitative diagnosis and life assessment of creep damage of a dissimilar steel welded joint. The method sequentially performs creep accelerated fracture experiment and electron backscatter diffraction experiment on the dissimilar steel welded joint, collects creep fracture images and electron backscatter diffraction experimental data after the experiment, and quantitatively analyzes the size, volume fraction and size of the pores in the creep fracture image, as well as parameters such as grain size, geometric dislocation density, grain boundary angle, recrystallization fraction, recovery grain ratio and deformation grain ratio, so as to combine the two parameters (i.e., the first quantitative characteristic parameter and the second quantitative characteristic parameter) analyzed in the creep accelerated fracture experiment and the electron backscatter diffraction experiment, and is used to determine the current life stage and creep remaining life of the creep structure of the dissimilar steel welded joint, thereby improving the accuracy of damage diagnosis of the creep structure of the dissimilar steel welded joint. In addition, the method can be widely applied to new materials, long-term service materials, and dissimilar steel welded joints that experience high temperature and high pressure creep accelerated fracture materials, has universality, and can provide key information for early diagnosis and effective management of creep damage. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0045] Figure 1 This is a flow chart of a method for quantitative diagnosis of creep damage and life assessment of dissimilar steel welded joints provided in Example 1 of the present invention.

[0046] Figure 2 A schematic diagram of the relationship between the pore volume fraction and time provided in Example 1 of the present invention.

[0047] Figure 3 A schematic diagram of the relationship between hole size and time provided in Example 1 of the present invention.

[0048] Figure 4 This is a schematic diagram of the relationship between the size of the Laves phase and time provided in Example 1 of the present invention.

[0049] Figure 5 M provided in Example 1 of the present invention 23 Schematic diagram of the relationship between the size of the C6 phase and time.

[0050] Figure 6 This is a schematic diagram of the relationship between the change of grain size and time provided in Example 1 of the present invention.

[0051] Figure 7 This is a schematic diagram of the relationship between dislocation density and time provided in Example 1 of the present invention.

[0052] Figure 8 This is a schematic diagram of the relationship between the grain boundary angle and time provided in Example 1 of the present invention.

[0053] Fig. 9 A schematic diagram showing the relationship between the proportions of the three types of grains provided in Example 1 of the present invention and the changes over time. DETAILED DESCRIPTION

[0054] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0055] The purpose of the present invention is to provide a method and system for quantitative diagnosis of creep damage and life assessment of dissimilar steel welded joints, which can be applicable to the damage diagnosis of any metal welded joint during the creep process, and can determine the current life stage and creep remaining life of the dissimilar steel welded joint, thereby effectively improving the accuracy of damage diagnosis of the creep structure of the dissimilar steel welded joint.

[0056] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0057] Example 1

[0058] like Figure 1 As shown, a method for quantitative diagnosis of creep damage and life assessment of a dissimilar steel welded joint in this embodiment includes the following steps:

[0059] Step S1, obtaining first experimental data of a dissimilar steel weld joint; the dissimilar steel weld joint is a joint formed by welding dissimilar steels, and the material is a new material, a long-term service material, or a material that has undergone high temperature and high pressure creep accelerated fracture; the first experimental data is a creep fracture image of the dissimilar steel weld joint after creep fracture occurs during a creep accelerated fracture test, and the creep fracture image includes a tissue aging image and a precipitation phase image.

[0060] Step S2, quantitatively processing the first experimental data to obtain first quantitative characteristic parameters; the first quantitative characteristic parameters include the size, volume fraction and size of the pores in the creep rupture image.

[0061] Step S3, obtaining second experimental data of the dissimilar steel weld joint; the second experimental data is electron backscatter diffraction experimental data obtained by performing an electron backscatter diffraction experiment after creep rupture of the dissimilar steel weld joint.

[0062] Step S4, quantitatively process the second experimental data to obtain second quantitative characteristic parameters; the second quantitative characteristic parameters include grain size, geometric dislocation density, grain boundary angle, recrystallization fraction, recovery grain ratio and deformation grain ratio. The recrystallization fraction refers to the ratio of the volume portion of the material that undergoes recrystallization to the total volume, also known as the recrystallized grain ratio.

[0063] Step S5: determining the current life stage and creep residual life of the dissimilar steel weld joint according to the first quantitative characteristic parameter and the second quantitative characteristic parameter.

[0064] In this embodiment, step S1 obtains first experimental data of a dissimilar steel weld joint, specifically including:

[0065] Step S11: conducting a creep accelerated fracture experiment based on the dissimilar steel weld joint to obtain a creep fracture sample.

[0066] Step S12: observing the creep rupture sample with an optical microscope, and outputting the tissue aging image of the creep rupture sample.

[0067] Step S13: observing the creep rupture sample using a scanning electron microscope, and outputting the precipitation phase image of the creep rupture sample.

[0068] In this embodiment, before observing the creep rupture sample with an optical microscope in step S12 and outputting the tissue aging image of the creep rupture sample, the method further includes:

[0069] Step S111, grinding and polishing the sample surface of the creep rupture region of the creep rupture sample to obtain a grinded and polished creep rupture sample.

[0070] Step S112, placing the polished creep rupture sample in an erosion solution for erosion to obtain an eroded creep rupture sample.

[0071] Step S113, rinsing the eroded creep rupture sample, and obtaining the rinsed creep rupture sample after drying, wherein the rinsed creep rupture sample is used as the creep rupture sample observed by the optical microscope and the scanning electron microscope.

[0072] In this embodiment, before performing quantitative processing on the first experimental data to obtain the first quantitative characteristic parameter in step S2, the method further includes:

[0073] Step S14, using Image-J software to perform automatic threshold segmentation processing, edge detection processing and image denoising processing on the creep rupture image in sequence to obtain a preprocessed creep rupture image; the preprocessed creep rupture image is used as the first experimental data for quantitative processing.

[0074] In this embodiment, step S2 performs quantitative processing on the first experimental data to obtain a first quantitative characteristic parameter, which specifically includes:

[0075] Step S21, using Image-J software to determine the size and volume fraction of each hole in the tissue aging image.

[0076] Step S22: determining the type of each precipitated phase in the precipitated phase image according to the precipitated phase image.

[0077] Step S23: using Image-J software to determine the size of each type of precipitated phase in the precipitated phase image.

[0078] In this embodiment, step S4 performs quantitative processing on the second experimental data to obtain a second quantitative characteristic parameter, which specifically includes:

[0079] The electron backscatter diffraction experimental data are imported into Channel 5 software, and the grain size, geometric dislocation density, grain boundary angle, recrystallization fraction, recovered grain ratio and deformed grain ratio corresponding to the electron backscatter diffraction experimental data are output using Channel 5 software.

[0080] In this embodiment, before obtaining the second experimental data of the dissimilar steel welded joint in step S3, the method further includes:

[0081] Step S24, grinding the sample surface of the creep rupture sample to obtain a ground creep rupture sample.

[0082] Step S25, electrolytically polishing the sample surface of the polished creep rupture sample to obtain an electrolytically polished creep rupture sample; the electrolytically polished creep rupture sample is used as the creep rupture sample for the electron backscatter diffraction experiment.

[0083] In this embodiment, step S5 determines the current life stage and creep residual life of the dissimilar steel weld joint according to the first quantitative characteristic parameter and the second quantitative characteristic parameter, specifically including:

[0084] Step S51: establishing a relationship curve between the characteristic parameters of the dissimilar steel weld joint and the creep life loss according to the first quantitative characteristic parameter and the second quantitative characteristic parameter.

[0085] Step S52: determining the current life stage and the creep remaining life of the dissimilar steel weld joint according to the relationship curve between the characteristic parameters of the dissimilar steel weld joint and the creep life loss.

[0086] The following examples are given in the form of examples to make the specific operation process of this embodiment clearer.

[0087] This embodiment uses computer-aided image processing and data analysis methods to diagnose and quantify the creep failure process of dissimilar steel welded joints (especially martensite / austenite heterogeneous welded joints, such as T92 / HR3C and other materials) under high temperature and high pressure environments. The key steps of this embodiment include image acquisition, image processing, feature extraction, data analysis and creep residual life prediction, specifically including the following steps

[0088] Step (1) A creep accelerated fracture test at 650°C and 50MPa is performed on the welded joints that have been in service for a long time in the power plant until they fracture. A precise temperature and pressure control system is used to ensure stable experimental conditions. After the experiment is completed, the location of the creep fracture is accurately recorded, and the fracture is located in the fine grain area of ​​the heat affected zone of T92. Subsequently, the microstructure evolution characteristic quantities that affect creep fracture based on the creep damage mechanism research are extracted, that is, the creep damage mechanism research found that the creep damage fracture is mainly due to the fine grain area of ​​the T92 heat affected zone on one side of the martensitic steel, and microstructure aging occurs, thereby generating creep holes. The microstructure aging characteristics include an increase in the size of the precipitated phase, an increase in the grain size, a decrease in the proportion of small-angle grain boundaries, and the formation of large-angle grain boundaries, a decrease in the average dislocation density, and an increase in the recrystallization ratio.

[0089] In this embodiment, the creep acceleration test of the welded joint is carried out at a temperature of 650°C and a pressure of 50MPa, wherein 650°C and 50MPa are selected to ensure that the fracture position is in the heat affected zone of T92, which is the same as the failure position of high temperature and low stress service in an actual power plant, so as to ensure that the fracture position is located in the fine grain heat affected zone of T92, and the observed position is located in the area near the fracture position, and the observed characteristic quantities include the size of the precipitated phase, the grain size, the grain boundary angle distribution, the average dislocation density and the recrystallization fraction. In addition, based on the study of the failure mechanism, the organizational characteristic parameters that cause the failure of the dissimilar steel welded joint are quantitatively detected, and the quantitative diagnosis provides a new method for evaluating the creep damage and remaining life of the dissimilar steel welded joint, which is of great significance to the development of material creep performance evaluation.

[0090] Step (2) The sample surface near the fracture area before and after creep fracture is ground and polished respectively, then etched with FeCl3 and HCl solution for 10 to 15 seconds, rinsed with alcohol and blown dry.

[0091] In this embodiment, grinding and polishing are usually performed using sandpaper and a polishing machine, and the grinding is gradually performed from coarse sandpaper to fine sandpaper, generally in the order of 60 mesh, 200 mesh, 400 mesh, 1000 mesh, 1500 mesh, and 2000 mesh; then the surface scratches are polished away with a polishing machine, in order to make the sample surface flat and smooth, which is convenient for subsequent microscopic observation and analysis. After grinding and polishing, the surface is cleaned by using solution etching and alcohol rinsing to better observe the changes in the microstructure.

[0092] In this embodiment, the etching solution can use FeCl3 and HCl solution, and other solutions can also be used. However, considering that the etching solution prepared by FeCl3 and HCl solution has a better effect on sample corrosion for T92 / HR3C welding joints, therefore, FeCl3 and HCl solution are preferably used for sample corrosion in this embodiment, and the ratio of the solution reagent is: FeCl3 1g, HCl 10ml, water 20ml.

[0093] Step (3) The etched sample is observed under an optical microscope and a scanning electron microscope, and the photographed photos are processed using Image-J software, including the application of image preprocessing technology, including automatic threshold segmentation, edge detection and denoising, to optimize the image quality, followed by quantitative processing to obtain the size of the pores, volume fraction and size of the precipitated phase.

[0094] An optical microscope was used to take photos of the microstructure aging of the T92 fine-grained heat-affected zone. Photos of the T92 fine-grained heat-affected zone containing precipitates were taken in the SEM scattering BSE (Back Scattered Electron) mode. At least 30 photos were taken for each sample at a magnification of 10,000 times. 23 C6, Laves, MX, etc., while M 23 The size and area ratio of C6 and Laves phases changed greatly after creep rupture, so it was judged that these two precipitated phases may cause the failure rupture on the T92 side of the welded joint.

[0095] Due to M 23 The sizes of C6 and Laves phases are generally larger than 50 nm. Therefore, in this embodiment, the precipitated phases larger than 50 nm were first screened for statistics using Image-J software, and then the M phases were distinguished by the color of the BSE images. 23 Two precipitated phases, C6 and Laves, were identified and quantified.

[0096] It should be noted that in the BSE mode of the scanning electron microscope, the elements with larger atomic numbers are brighter. The main chemical components of Laves include W, M 23 The main components of C6 are Cr, and the main components of MX are Nb and V. Therefore, the Laves phase will be brighter in the BSE mode and appear bright white in the image; 23 The C6 phase and MX phase appear gray in the image, but the MX phase is smaller and easier to distinguish.

[0097] In this embodiment, due to Laves and M 23 The excessive growth of the size of the C6 precipitate is one of the reasons for the failure and fracture of the material. Therefore, in this embodiment, the precipitate is first identified in the BSE mode, and then the size is screened and counted using Image J software, so that the Laves and M 23 The two precipitated phases of C6 were quantified and counted for use in the diagnosis and evaluation of tissue damage.

[0098] Step (4) grinds the sample surface before and after creep rupture respectively, and then uses perchloric acid and alcohol to electropolish the sample surface for 15 seconds to remove surface stress.

[0099] In this embodiment, step (4) polishes the sample surface before and after creep rupture respectively, using 60 mesh, 200 mesh, 400 mesh, 1000 mesh, 1500 mesh and 2000 mesh sandpaper for polishing in sequence, and each polishing direction is perpendicular to the direction of the previous scratch, and finally polishes to a state where the scratches are fine and consistent in direction.

[0100] In this embodiment, the solution used for electrolytic polishing can be perchloric acid and alcohol, or other solutions can be used. However, the electrolytic polishing solution prepared with perchloric acid and alcohol solution for this material has a better electrolytic polishing effect. The ratio of the perchloric acid alcohol solution is: 10ml perchloric acid, 90ml alcohol; the voltage of the electrolytic polishing is 15V, and the electrolytic polishing time is 15s, so as to ensure the effect of electrolytic polishing and effectively remove surface stress.

[0101] Step (5) The electro-polished sample is subjected to an Electron Back Scatter Diffraction (EBSD) experiment, and the experimental data are processed using Channel 5 software to quantitatively analyze the microstructural characteristics of the material.

[0102] In this embodiment, the electron backscatter diffraction experimental data of the sample is first collected and imported into the Channel 5 software. Then, the data is cleaned to remove noise and non-indexed areas to ensure the accuracy of the analysis. The grain size distribution is calculated through the analysis tools in the software. This step involves identifying grain boundaries and counting the frequency distribution of grains of various sizes. The grain boundary angle is automatically identified by the software according to the orientation difference between the grains. In this process, the angle threshold 2°-10° is set as a small angle grain boundary, and >10° is set as a large angle grain boundary. Subsequently, the software will calculate and count the angles of all identified grain boundaries to form a distribution map of grain boundary angles. The geometrically necessary dislocation density (GND) value can be estimated by calculating the local orientation gradient. After the calculation is completed, the software will provide a distribution map and statistical data of the GND value. Finally, by comparing the size, orientation and shape of the grains, the software can identify recrystallized grains and calculate the recrystallization fraction.

[0103] In this embodiment, after the electron backscatter diffraction experiment, it is usually necessary to use professional software such as Channel 5 for data processing, mainly because the data generated by the electron backscatter diffraction experiment is very rich and complex, including crystallographic orientation, grain boundaries, phase information, etc., which need to be analyzed and interpreted in detail by professional software. Channel 5 software is a powerful tool specially designed to process and analyze EBSD data, providing functions from basic data processing to advanced material property analysis. In this embodiment, Channel 5 is mainly used to determine parameters such as grain size, geometric dislocation density, grain boundary angle, recrystallization fraction, recovered grain ratio and deformed grain ratio.

[0104] In this embodiment, step (6) divides the creep rupture time into 10 stages by conducting a durability test on the material after service to obtain the rupture time t, and then divides the rupture time into 10 time points in equal proportion, such as 0.1t, 0.2t, 0.3t, 0.4t, 0.5t, 0.6t, 0.7t, 0.8t, 0.9t, t, etc., wherein t is any preset time length value, thereby realizing the division of 10 creep rupture time stages. According to the first quantitative test method based on the first quantitative characteristic parameter and the second quantitative test method based on the second quantitative characteristic parameter, the pore size, pore volume fraction, Laves phase size, M at each time point are measured respectively. 23 C6 size and grain size, dislocation density, large and small grain boundary angle ratio, recovery grain ratio, recrystallization fraction, and deformed grain ratio are quantitatively counted, and a suitable fitting method is selected to establish a relationship curve related to creep time. The fitting equation can be used to predict the creep stage by one or more microstructural parameters that are strongly correlated with time. The accuracy of the prediction can be improved by multiple sets of parallel tests.

[0105] In this embodiment, since the creep rupture time is divided into 10 stages, when establishing the relationship curve between the characteristic parameters and the creep life loss, the Origin software is used to associate the quantified parameters with the creep rupture times, so that a relationship curve between the microstructure and the creep time can be drawn.

[0106] When determining the current life stage of the dissimilar steel welded joint, this embodiment uses Origin software to perform statistical analysis and curve fitting through experimental data (such as precipitate phase size, grain size, grain boundary angle distribution, etc.) and corresponding data of creep time. The fitted curve may be in the form of linear, logarithmic, exponential or other mathematical models. Then analyze the above curve, especially to find the parameter change trend that is obviously related to the creep life. For example, if a specific microstructural parameter (such as precipitate phase size) increases with time and is strongly correlated with the decline in material properties (such as hardness reduction), the change of this parameter can be used as a key indicator for predicting material failure.

[0107] When calculating the remaining life, this embodiment uses the relationship curve between the characteristic parameter and the creep life loss, and inputs the currently measured microstructure parameters (from the prepared new sample or the component in service) into the remaining life prediction model (the remaining life prediction model can be any model in the prior art that has the function of predicting the remaining life of the equipment) to predict the time required to reach the critical damage state. For example, if it is known that the critical size of a specific precipitated phase is closely related to material failure, the time to reach this critical size can be predicted based on the current size and growth rate. If the life under the temperature and stress of the persistent creep experiment different from that of this embodiment is to be calculated, the Larson-Miller parameter model of the material can be combined. This Larson-Miller parameter model is a model of temperature and time, so that the remaining life under the desired temperature and stress can be predicted by the microstructure.

[0108] The following shows some experimental results obtained by this method: Figure 2 is a schematic diagram of the relationship between the pore volume fraction and time. Figure 3 is a schematic diagram of the relationship between the change of hole size and time. Figure 4 This is a schematic diagram of the relationship between the size of the Laves phase and time. Figure 5 It is M 23 Schematic diagram of the relationship between the size of the C6 phase and time. Figure 6 is a schematic diagram of the relationship between grain size and time. Figure 7 is a schematic diagram of the relationship between dislocation density and time. Figure 8 is a schematic diagram of the relationship between the change of grain boundary angle and time. Fig. 9 This is a schematic diagram of the relationship between the proportion of three types of grains: recrystallized grains, recovered grains, and deformed grains over time. Figures 2 to 9The variation patterns of different quantitative data and creep time can be intuitively seen, and microstructural parameters that are strongly correlated with time can be obtained through fitting. After the creep time reaches 0.7t, the material undergoes obvious pore merging and growth, precipitate phase coarsening, and dislocation density decrease in this area, which will lead to a decrease in material performance. Therefore, after this stage, the material may be more prone to failure and fracture, and prevention of material failure should be strengthened after this stage.

[0109] This embodiment uses advanced image processing technology and detailed quantitative analysis methods, and realizes accurate evaluation of creep damage through careful observation and quantification of the microstructure characteristics of actual materials. Combined with optical microscope and scanning electron microscope observation, image analysis is performed with Image-J software to accurately quantify the key damage characteristics in the creep process, such as the size of the precipitated phase, grain size, grain boundary angle distribution, average dislocation density and recrystallization fraction. This quantitative analysis method provides a more accurate damage assessment than traditional methods. Therefore, this method focuses on quantitative analysis through various detailed microstructure evolution characteristics to provide a creep damage diagnosis method for welded joints (T92 / HR3C). Its principles and technical frameworks are generally applicable and can be extended to other materials and different industrial application scenarios, providing technical support for creep damage diagnosis and life prediction of various materials. Since this method can identify early signs of creep damage at the microscopic level, it provides an earlier warning, which helps to take necessary maintenance or replacement measures in time, avoid possible equipment failures, and reduce economic losses and safety risks. In contrast, the traditional evaluation methods of creep damage and fatigue damage factors only focus on the carbide M in creep damage. 23 C6 size change focuses more on life prediction through theoretical and physical models combined with damage mechanism. In actual service, it is the result of various microstructural changes. Various changes such as Laves phase size, grain size, dislocation density, etc. will have a great impact on the creep process.

[0110] The present embodiment provides a method for quantitative diagnosis of creep damage and life assessment of dissimilar steel welded joints, which is actually a set of comprehensive technical methods for creep damage diagnosis and remaining life prediction of new materials of dissimilar steel welded joints and long-term service materials under high temperature and high pressure environments, including detailed quantification of the microstructure evolution characteristics of the creep damage process of dissimilar steel welded joints, and the use of advanced image processing technology, including optical microscope and scanning electron microscope observation, and Image-J software for image analysis, to quantify key damage characteristic parameters, including the size of the precipitated phase, grain size, grain boundary angle distribution, average dislocation density and recrystallization fraction, and establish a correlation between these damage characteristic parameters and creep life time.

[0111] The traditional analysis method for damage and remaining life assessment of ferrite / austenite dissimilar steel welded joints in power plants mainly conducts qualitative analysis of metallographic structures and compares the structures before and after failure to analyze the degree of damage. This method is highly subjective and cannot reflect the comprehensive performance of each area. In this embodiment, the creep damage diagnosis method has the following advantages:

[0112] (1) Enhanced accuracy. This embodiment can provide a more comprehensive and in-depth understanding of the creep damage process by comprehensively analyzing the microstructural changes of new materials, long-term service materials, and materials undergoing high temperature and high pressure creep, such as grain size, grain boundary angle distribution, dislocation density, etc. This comprehensive analysis provides more accurate damage diagnosis, especially in the early stages of damage.

[0113] (2) Early damage identification. This embodiment can identify subtle changes in the early stages of creep damage by quantifying microstructural changes. Early detection helps to take timely repair or replacement measures to prevent potential large-scale equipment failures.

[0114] (3) Wide applicability. This embodiment is not only applicable to the specific T92 / HR3C dissimilar steel weld joints, but can also be applied to creep damage diagnosis of various other industrial materials, metal materials working at high temperatures, such as other types of steel and alloys, and especially heat-resistant materials used in the power, petrochemical and other industries. This makes this method an important tool for material performance evaluation and maintenance decision-making in a variety of industrial applications.

[0115] (4) Data-driven decision support. The quantitative data provided by this embodiment supports more scientific decision-making, such as maintenance planning, life prediction, and risk assessment. It enhances the decision-making ability of enterprises in material maintenance and replacement strategies, and improves operational efficiency and cost-effectiveness.

[0116] (5) Promote industry research and development. The development and application of the new method of this embodiment can stimulate further industry research and promote the development of materials science and engineering technology. The method and data results can be used to develop or improve creep damage prediction models. These models can help power plants predict the life and maintenance requirements of key components, thereby planning maintenance and replacement in advance and reducing the risk of unexpected downtime.

[0117] This embodiment provides a method for quantitative diagnosis and life assessment of creep damage in dissimilar steel welded joints, which combines advanced quantitative technology and microstructure analysis to accurately assess the degree of damage of materials under different creep states, including new materials, long-term service materials, and materials that experience high temperature and high pressure creep accelerated fracture. Through detailed analysis of microstructure evolution characteristics, such as quantification of characteristic parameters such as precipitation phase size, grain size, grain boundary angle distribution, dislocation density, and recrystallization fraction, this method will provide key information for early diagnosis and effective management of creep damage.

[0118] This embodiment achieves the effect of improving the creep damage prediction model by establishing the correlation between multiple microstructures, such as precipitate phase size, grain size, dislocation density, etc. and life. According to the prediction model, a regular inspection plan based on the model prediction results can be formulated to timely identify and deal with potential damage. According to the results of the prediction model, the maintenance and replacement plan is optimized to avoid premature or late maintenance activities, save costs and reduce downtime.

[0119] The creep damage diagnosis method of this embodiment provides important improvements for the maintenance and life management of industrial materials by providing more comprehensive and accurate damage analysis and earlier damage identification. These advantages are derived from its comprehensive and in-depth microstructure analysis method, making it an indispensable tool in industrial applications. The method extracts the mean of the characteristic quantity around the fracture area, and the result has a great reference value. Quantitative evaluation of creep damage at the fracture location is of great significance for reducing power plant equipment accidents and ensuring the long-term operation of equipment.

[0120] Example 2

[0121] This embodiment provides a system for quantitative diagnosis of creep damage and life assessment of dissimilar steel welded joints. The system is a system corresponding to the method for quantitative diagnosis of creep damage and life assessment of dissimilar steel welded joints in Embodiment 1. The system includes:

[0122] The first experimental data acquisition module is used to acquire the first experimental data of the dissimilar steel welded joint; the first experimental data is a creep rupture image of the dissimilar steel welded joint after creep rupture occurs during a creep accelerated rupture experiment, and the creep rupture image includes a tissue aging image and a precipitation phase image.

[0123] The first quantitative characteristic parameter acquisition module is used to perform quantitative processing on the first experimental data to obtain first quantitative characteristic parameters; the first quantitative characteristic parameters include the size, volume fraction and size of pores in the creep rupture image.

[0124] The second experimental data acquisition module is used to acquire the second experimental data of the dissimilar steel weld joint; the second experimental data is the electron backscatter diffraction experimental data obtained by performing an electron backscatter diffraction experiment after the dissimilar steel weld joint undergoes creep rupture.

[0125] The second quantitative characteristic parameter acquisition module is used to perform quantitative processing on the second experimental data to obtain second quantitative characteristic parameters; the second quantitative characteristic parameters include grain size, geometric dislocation density, grain boundary angle, recrystallization fraction, recovered grain ratio and deformed grain ratio.

[0126] The diagnosis module is used to determine the current life stage and creep residual life of the dissimilar steel weld joint according to the first quantitative characteristic parameter and the second quantitative characteristic parameter.

[0127] It should be noted that the object information (including but not limited to object device information, object personal information, etc.) and data (including but not limited to data used for analysis, stored data, displayed data, etc.) involved in the present invention are all information and data authorized by the object or fully authorized by all parties, and the collection, use and processing of relevant data need to comply with relevant laws, regulations and standards of relevant countries and regions.

[0128] The technical features of the above embodiments may be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0129] The principles and implementation methods of the present invention are described in this article using specific examples. The description of the above embodiments is only used to help understand the method and core idea of ​​the present invention. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as limiting the present invention.

Claims

1. A method for quantitative diagnosis of creep damage and life assessment of dissimilar steel welded joints. It is characterized in that The method comprises: Acquire first experimental data of a dissimilar steel weld joint; the first experimental data is a creep fracture image of the dissimilar steel weld joint after creep fracture occurs during a creep accelerated fracture experiment, wherein the creep fracture image includes a microstructure aging image and a precipitation phase image; Performing quantitative processing on the first experimental data to obtain first quantitative characteristic parameters; the first quantitative characteristic parameters include the size, volume fraction and size of pores in the creep rupture image; Acquire second experimental data of the dissimilar steel weld joint; the second experimental data is electron backscatter diffraction experimental data obtained by performing an electron backscatter diffraction experiment after creep rupture of the dissimilar steel weld joint; Quantitatively processing the second experimental data to obtain second quantitative characteristic parameters; the second quantitative characteristic parameters include grain size, geometric dislocation density, grain boundary angle, recrystallization fraction, recovery grain ratio and deformation grain ratio; The current life stage and the creep residual life of the dissimilar steel weld joint are determined according to the first quantitative characteristic parameter and the second quantitative characteristic parameter.

2. The method for quantitative diagnosis and life assessment of creep damage of dissimilar steel welded joints according to claim 1, It is characterized in that Obtain the first experimental data of dissimilar steel welded joints, including: Conducting a creep accelerated fracture experiment based on the dissimilar steel welded joint to obtain a creep fracture sample; Observing the creep rupture sample using an optical microscope, and outputting the tissue aging image of the creep rupture sample; The creep rupture sample is observed by using a scanning electron microscope, and the precipitation phase image of the creep rupture sample is output.

3. The method for quantitative diagnosis and life assessment of creep damage of dissimilar steel welded joints according to claim 2, It is characterized in that Before observing the creep rupture sample with an optical microscope and outputting the tissue aging image of the creep rupture sample, the method further includes: Grinding and polishing the sample surface of the creep rupture region of the creep rupture sample to obtain a grinded and polished creep rupture sample; Placing the polished creep rupture sample in an erosion solution for erosion to obtain an eroded creep rupture sample; The eroded creep rupture sample is rinsed and dried to obtain a rinsed creep rupture sample, and the rinsed creep rupture sample is used as the creep rupture sample observed by the optical microscope and the scanning electron microscope.

4. The method for quantitative diagnosis of creep damage and life assessment of dissimilar steel welded joints according to claim 1, It is characterized in that Before performing quantitative processing on the first experimental data to obtain the first quantitative characteristic parameter, the method further includes: The creep rupture image is processed by automatic threshold segmentation, edge detection and image denoising in sequence using Image-J software to obtain a preprocessed creep rupture image; the preprocessed creep rupture image is used as the first experimental data for quantitative processing.

5. The method for quantitative diagnosis of creep damage and life assessment of dissimilar steel welded joints according to claim 1, It is characterized in that The first experimental data is quantitatively processed to obtain a first quantitative characteristic parameter, which specifically includes: Using Image-J software to determine the size and volume fraction of each hole in the tissue aging image; According to the precipitation phase image, determining the type of each precipitation phase in the precipitation phase image; The size of each type of precipitated phase in the precipitated phase image was determined using Image-J software.

6. The method for quantitative diagnosis of creep damage and life assessment of dissimilar steel welded joints according to claim 1, It is characterized in that The second experimental data is quantitatively processed to obtain a second quantitative characteristic parameter, which specifically includes: The electron backscatter diffraction experimental data are imported into Channel 5 software, and the grain size, geometric dislocation density, grain boundary angle, recrystallization fraction, recovered grain ratio and deformed grain ratio corresponding to the electron backscatter diffraction experimental data are output using Channel 5 software.

7. The method for quantitative diagnosis of creep damage and life assessment of heterogeneous steel welded joints according to claim 2, It is characterized in that Before obtaining the second experimental data of the dissimilar steel welded joint, the method further includes: Grinding the sample surface of the creep rupture sample to obtain a grinded creep rupture sample; The sample surface of the polished creep rupture sample is electrolytically polished to obtain an electropolished creep rupture sample; the electropolished creep rupture sample is used as the creep rupture sample for the electron backscatter diffraction experiment.

8. The method for quantitative diagnosis of creep damage and life assessment of dissimilar steel welded joints according to claim 1, It is characterized in that Determining the current life stage and creep residual life of the dissimilar steel weld joint according to the first quantitative characteristic parameter and the second quantitative characteristic parameter specifically includes: Establishing a relationship curve between the characteristic parameters of the dissimilar steel weld joint and the creep life loss according to the first quantitative characteristic parameter and the second quantitative characteristic parameter; According to the relationship curve between the characteristic parameters of the dissimilar steel welded joint and the creep life loss, the current life stage and the creep remaining life of the dissimilar steel welded joint are determined.

9. A system for quantitative diagnosis and life assessment of creep damage of dissimilar steel welded joints. It is characterized in that The system comprises: A first experimental data acquisition module is used to acquire first experimental data of a dissimilar steel weld joint; the first experimental data is a creep rupture image of the dissimilar steel weld joint after creep rupture occurs during a creep accelerated rupture experiment, and the creep rupture image includes a microstructure aging image and a precipitation phase image; A first quantitative characteristic parameter acquisition module, used for performing quantitative processing on the first experimental data to obtain first quantitative characteristic parameters; the first quantitative characteristic parameters include the size, volume fraction and size of pores in the creep rupture image; A second experimental data acquisition module is used to acquire second experimental data of the dissimilar steel weld joint; the second experimental data is electron backscatter diffraction experimental data obtained by performing an electron backscatter diffraction experiment after creep rupture of the dissimilar steel weld joint; A second quantitative characteristic parameter acquisition module, used for performing quantitative processing on the second experimental data to obtain second quantitative characteristic parameters; the second quantitative characteristic parameters include grain size, geometric dislocation density, grain boundary angle, recrystallization fraction, recovery grain ratio and deformation grain ratio; The diagnosis module is used to determine the current life stage and creep residual life of the dissimilar steel weld joint according to the first quantitative characteristic parameter and the second quantitative characteristic parameter.

Citation Information

Cited By

  • Method for quantitatively analyzing creep mechanism of high-temperature alloy based on subboundary

    CN119959263A

  • A method for quantitatively analyzing high-temperature alloy creep mechanism based on subgrain boundaries

    CN119959263B

  • Creep experiment data analysis processing method for power station boiler

    CN120043879A

  • Aging analysis method for dissimilar steel welded joint of boiler

    CN120121807A

  • Aging Analysis Method for Boiler Dissimilar Steel Welded Joints

    CN120121807B