Garment
By using a laminated non-woven structure and belt member design in the clothes, combined with an appropriate amount of antistatic agent, the problem of insufficient liquid protection and dust protection in the existing technology is solved, and efficient protection and comfort are improved.
Patent Information
- Application Number
- CN202380023494.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-29
- Filing Date
- 2023-03-23
- Publication Date
- 2024-10-29
AI Technical Summary
Existing clothing has deficiencies in liquid protection and dust protection, cannot take into account both properties, and has poor production efficiency and comfort.
It adopts a laminated non-woven fabric structure, in which the first outermost layer contains 0.02 to 0.50 mass% of antistatic agent, and the second outermost layer contains less than 0.01 mass% of antistatic agent. The combined belt member and the adhesive resin layer are stitched together. The design of the welded part provides excellent dust protection and liquid protection.
It achieves efficient dust protection and liquid protection, improves the overall performance and comfort of clothing, and meets sufficient performance requirements.
Smart Images

Figure CN118871003A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to clothing. Background Art
[0002] Conventionally, various clothes formed by joining a plurality of fiber fabric pieces together are commercially available. As joining techniques for these clothes, sewing with a sewing machine, or a method of melting and solidifying overlapping fabric pieces and bonding or welding them together is mainly adopted.
[0003] As clothing in patent literature, there is disclosed clothing made by inserting a hot melt adhesive containing a polyurethane, acrylic, silicone or other resin between overlapping fabric sheets and performing heat compression bonding, thereby melting and solidifying the hot melt adhesive to join multiple fiber fabric sheets (Patent Literature 1) and the like.
[0004] As clothing that imparts liquid protection to the raw fabric and the joints, there is disclosed clothing that uses a raw fabric with high water resistance and moisture-permeable liquid protection formed by laminating a base fabric and a liquid-protective membrane or a moisture-permeable waterproof membrane, and a sealing tape, and after the raw fabric pieces are sewn or welded together by a sewing machine, the joints are covered with a sealing tape (patent documents 2, 3, 4, 5), etc.
[0005] As clothing having washing durability and sterilization durability imparted to the grey fabric and the joints, clothing using polyester fabric as the base fabric of the grey fabric and polycarbonate-based polyurethane resin as the moisture-permeable waterproof film and the adhesive is disclosed (Patent Document 6).
[0006] As clothing that imparts liquid protection and fire resistance to the grey fabric and the joints, there are disclosed clothing in which the surface of the grey fabric blended with heat-resistant and flame-retardant fibers is treated with aluminum, the grey fabric pieces are sewn together with a sewing machine, and the front and back surfaces of the seamed portion are sealed with a flame-retardant waterproof tape (waterproofing tape) (Patent Document 7); and raincoats in which multiple pieces of multi-layer non-woven fabric are sewn together, an antistatic agent is applied to the outer surface, and an open-pore tape is sealed at the seamed portion (Patent Document 8).
[0007] Prior art literature
[0008] Patent Literature
[0009] Patent Document 1: Japanese Patent Application Publication No. 2017-186695
[0010] Patent Document 2: International Publication No. 2007 / 034837
[0011] Patent Document 3: Japanese Patent Application Publication No. 2009-183849
[0012] Patent Document 4: International Publication No. 2016 / 006418
[0013] Patent Document 5: Japanese Patent Application No. 2007-508870
[0014] Patent Document 6: Japanese Patent Application Publication No. 2013-047397
[0015] Patent Document 7: Japanese Patent Application Publication No. 2015-168889
[0016] Patent Document 8: Japanese Patent Application Publication No. 2014-009954 Summary of the invention
[0017] Problems to be solved by the invention
[0018] However, in the clothing of Patent Document 1, in which overlapping grey fabric pieces are joined by inserting an adhesive between each other, one side of the overlapping grey fabric pieces is the grey fabric surface and the other side is the grey fabric back. When the compositions of the surface and back of the grey fabric pieces are different, there is a problem that the liquid protection of the joint becomes poor.
[0019] Patent Documents 2 to 6 use a highly water-resistant and liquid-permeable grey fabric formed by laminating a base fabric and a moisture-permeable waterproof film and a sealing tape to form a joint, and the clothing can easily suppress the intrusion of humidity and water in the clothing by virtue of moisture permeability and liquid protection. However, when dust charged by friction on the surface of the clothing or charged by static electricity approaches the surface of the clothing, static electricity is easily charged on the surface of the clothing due to electrostatic induction, which easily causes dust adhesion, that is, there is a problem of poor dust protection.
[0020] Patent document 7 discloses a garment in which the surface of a grey cloth blended with heat-resistant flame-retardant fibers is treated with aluminum, the grey cloth pieces are sewn together using a sewing machine, and then the inner and outer surfaces of the seamed portion are sealed with a flame-retardant waterproof tape. However, since the inner and outer surfaces of the seamed portion are sealed with a waterproof tape, the production efficiency is poor, and the sealed portion becomes hard, resulting in poor comfortability as a garment.
[0021] Patent document 8 discloses a garment in which an antistatic agent is applied to the outer surface of the garment and the opening tape is sealed at the seam portion. Regarding the water pressure resistance of the garment in the embodiment, no antistatic agent is applied, and no disclosure is made about the reduction in water pressure resistance after the antistatic agent is applied. In addition, no disclosure is made about the specific manner of the ridge and tape in the seam portion. In addition, the water pressure resistance of the SMS nonwoven fabric is as low as 500 mmH. 2 O is weak and has the problem of poor liquid protection.
[0022] Thus, the conventional clothes cannot take into account both liquid protection and dust protection and cannot satisfy sufficient performance.
[0023] Therefore, an object of the present invention is to solve the problems of the prior art and provide clothing having excellent dust protection and liquid protection.
[0024] Means for solving problems
[0025] The clothing of the present invention that can achieve the above-mentioned subject includes the following structures. That is:
[0026] 1) A garment comprising a laminated nonwoven fabric and a member including a rectangular belt member and having a joint portion, wherein:
[0027] The first outermost layer of the laminated nonwoven fabric is a nonwoven fabric containing 0.02 to 0.50% by mass of an antistatic agent relative to the entire layer, and is located on the outside of the garment;
[0028] The second outermost layer of the laminated nonwoven fabric is a nonwoven fabric containing 0.01% by mass or less of an antistatic agent relative to the entire layer, and is located on the inner side of the garment;
[0029] The aforementioned joint portion has a rim located on the inner side of the aforementioned garment and the aforementioned belt member;
[0030] The aforementioned nest edge has one or more laminated portions formed by laminating a portion of the aforementioned laminated nonwoven fabric;
[0031] The laminated portion has at least one of a stitched portion and a welded portion;
[0032] The aforementioned nest edge is covered by the aforementioned belt member;
[0033] The belt member is located on the inner side of the garment;
[0034] At least two ends of the belt member in the short-side direction are fixed to the second outermost layer;
[0035] The water pressure resistance (A) of the laminated nonwoven fabric measured according to JIS L 1092 (2009) A method is 1000 to 10000 mmH 2 The scope of O;
[0036] The ratio of the water pressure resistance (B) measured by JIS L 1092 (2009) Method A to the water pressure resistance (A) (water pressure resistance (B) / water pressure resistance (A)) of the joint is 0.4 to 1.0.
[0037] 2) A garment comprising a laminated nonwoven fabric and a member including a rectangular belt member and having a joint portion, wherein:
[0038] The first outermost layer of the laminated nonwoven fabric is a nonwoven fabric containing 0.02 to 0.50% by mass of an antistatic agent relative to the entire layer, and is located on the outside of the garment;
[0039] The second outermost layer of the laminated nonwoven fabric is a nonwoven fabric containing 0.01% by mass or less of an antistatic agent relative to the entire layer, and is located on the inner side of the garment;
[0040] The joining portion includes at least one of a sewing portion and a welding portion, and the belt member;
[0041] In at least one of the stitched portion and the welded portion, horizontal surfaces in the thickness direction of two ends of at least one of the laminated nonwoven fabrics face each other;
[0042] At least one of the stitched portion and the welded portion is covered by the belt member;
[0043] The belt member is located on the inner side of the garment;
[0044] At least two ends of the belt member in the short-side direction are fixed to the second outermost layer;
[0045] The water pressure resistance (A) of the laminated nonwoven fabric measured according to JIS L 1092 (2009) A method is 1000 mm to 10000 mmH 2 The scope of O;
[0046] The ratio of the water pressure resistance (B) measured by JIS L 1092 (2009) Method A to the water pressure resistance (A) (water pressure resistance (B) / water pressure resistance (A)) of the joint is 0.4 to 1.0.
[0047] 3) More preferably, the aforementioned laminated nonwoven fabric comprises a first spunbond nonwoven fabric, a meltblown nonwoven fabric and a second spunbond nonwoven fabric in sequence;
[0048] The weight per unit area of the first spunbonded nonwoven fabric is 20 to 50 g / m 2 The second spunbonded nonwoven fabric has a unit area weight of 5 to 30 g / m 2 ;
[0049] The second spunbonded nonwoven fabric has a smaller basis weight than the first spunbonded nonwoven fabric.
[0050] 4) More preferably, the belt member is a laminate comprising a base material layer and an adhesive resin layer;
[0051] The thickness of the adhesive resin layer is 10 to 200 μm 100 to 200 μm;
[0052] The adhesive resin layer is in contact with the second outermost layer.
[0053] 5) More preferably, the air permeability of the laminated nonwoven fabric measured according to JIS L1913 (2010) 6.8 (Frazier method) is 2.0 to 40.0 cm 3 / cm2 / sec.
[0054] Effects of the Invention
[0055] According to the present invention, clothes having excellent dust protection and liquid protection can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 : is a cross-sectional view of a portion including a joining portion of the garment according to Embodiment 1 of the present invention.
[0057] Figure 2 : is a cross-sectional view of a portion including a joining portion of a garment according to a second embodiment of the present invention.
[0058] Figure 3 : is a cross-sectional view of a portion including a joining portion of a garment according to a modified example of embodiment 2 of the present invention.
[0059] Figure 4 : This is a partial cross-sectional view of a laminated nonwoven fabric.
[0060] Figure 5 : It is a partial cross-sectional view of a belt component.
[0061] Figure 6 : Is Figure 1 A perspective view of the garment shown as viewed from the outside.
[0062] Figure 7 :yes Figure 6 Exploded view of the garment shown. DETAILED DESCRIPTION
[0063] Hereinafter, the clothes of the present invention will be described in detail with reference to the drawings.
[0064] (Implementation Method 1)
[0065] Figure 1 This is a cross-sectional view of a portion of the garment 1 including the joining portion 3 according to the first embodiment of the present invention. Figure 4 This is a cross-sectional view of a portion of the laminated nonwoven fabric 2 . Figure 5 It is a cross-sectional view of a part of the belt member 4 . Figure 6 Is Figure 1 The garment 1 is shown in a perspective view, viewed from its outer side 1 a . Figure 7 yes Figure 6 An exploded view of the garment 1 is shown.
[0066] The garment 1 according to the first embodiment of the present invention comprises a laminated nonwoven fabric 2, a rectangular belt member 4, and a joining portion 3. Here, the inside of the garment refers to the wearer's side when the garment is worn, and the outside of the garment refers to the opposite side of the inside of the garment.
[0067] The laminated nonwoven fabric 2 includes a first outermost layer 2 a and a second outermost layer 2 b . The first outermost layer 2 a is located on the outer side 1 a of the garment 1 , and the second outermost layer 2 b is located on the inner side 1 b of the garment 1 .
[0068] The laminated nonwoven fabric 2 is cut into components for each portion of the garment 1 , and the components are joined at the joining portions 3 to form the garment 1 .
[0069] The aforementioned joining portion 3 has a welt 5 and a belt member 4. In addition, the welt 5 has a laminated portion 5a formed by laminating a portion of one or more laminated nonwoven fabrics 2, and the laminated portion 5a has at least one of a sewing portion and a fusion portion 5b (in this application, "at least one of a sewing portion and a fusion portion" is sometimes referred to as "sewing portion, etc.").
[0070] The laminated portion 5a mentioned here refers to the minimum distance side from at least one of the sewing portion and the welding portion 5b (in this application, "at least one of the sewing portion and the welding portion" will sometimes be referred to as "sewing portion, etc.") to the cutting end in the area where more than one laminated non-woven fabrics 2 overlap.
[0071] Here, as the mode of the laminated portion, the following modes are exemplified. For example, in the case where there is one rectangular laminated nonwoven fabric, a mode in which a part of the laminated nonwoven fabric is the two ends in the length direction of the laminated nonwoven fabric, and the two ends overlap to form the laminated portion. In this case, the laminated nonwoven fabric becomes a cylindrical shape. In addition, for example, in the case where there are two rectangular laminated nonwoven fabrics, a mode in which one end of one laminated nonwoven fabric overlaps with one end of another laminated nonwoven fabric to form the laminated portion can be cited.
[0072] As a method for forming the sewn portion, there are sewing with a sewing machine or sewing by hand, and sewing with a sewing machine is preferred from the viewpoint of productivity. As a method for sewing with a sewing machine, a method such as flat stitching, lock stitching, staggered stitching, double lock stitching, flat stitching, etc. can be appropriately used, and any one of them can be used, and more preferably, as Figure 1 As shown, the flat seam is straight, with a small exposed area and thickness, and excellent hand feel and strength. In addition, as a method for forming the welded portion, welding using any of ultrasonic heating, high-frequency heating, and resistance heating can be appropriately used. Any one of them can be used, and more preferably, the ultrasonic processing method is excellent in quality stability and productivity.
[0073] <Provision of dust protection>
[0074] As a method of imparting dust protection to the garment 1 of the present invention, the first outermost layer 2a of the laminated nonwoven fabric 2 located on the outer side 1a of the garment 1 contains 0.02 to 0.50% by mass of an antistatic agent 7 relative to the entire layer. Here, the first outermost layer 2a is located on the outer side 1a of the garment 1, so that the surface of the outer side 1a of the garment 1 is charged. Thereby, the adhesion of dust in the external air environment to the outer side 1a of the garment 1 is suppressed, and as a result, the dust protection of the garment 1 becomes excellent. It should be noted that the content of the antistatic agent in the first outermost layer is the content relative to the entire first outermost layer.
[0075] It should be noted that even if the charging of the inner side 1b of the garment 1 is suppressed, the dust adsorption of the inner side 1b of the garment 1 is suppressed, and the dust protection of the garment 1 is certainly not improved. On the other hand, as described later, for the reason that the liquid protection of the garment becomes excellent, in the garment of the present invention, the content of the antistatic agent in the second outermost layer is 0.01% by mass, and the second outermost layer does not contain the antistatic agent, or even if it contains it, it is a very small amount. It should be noted that the content of the antistatic agent in the second outermost layer is the content relative to the entire second outermost layer.
[0076] The factors causing dust to adhere to the clothes 1 include the charging of the dust and electrostatic induction to the surface of the clothes 1 .
[0077] Dust floating in the air usually carries positive or negative static electricity and is in a charged state. Due to the charge of the dust near the clothes 1, the opposite polarity of electricity is attracted to the surface of the clothes 1, causing electrostatic induction. When electrostatic induction occurs, Coulomb force acts between the dust and the clothes 1, and the dust is attracted to the clothes 1 and adheres.
[0078] In the present invention, in order to inhibit charged dust from adhering to the surface of clothing 1 due to electrostatic attraction, it is preferred to apply the antistatic agent 7 within the above-mentioned preferred range relative to the side where the dust and clothing 1 are in contact, that is, relative to the first outermost layer 2a of the laminated non-woven fabric 2 located on the outer side 1a of the clothing 1.
[0079] When the content of antistatic agent 7 is less than 0.02 mass%, the antistatic effect cannot be fully obtained and the dust protection is poor. On the contrary, when it is more than 0.50 mass%, the hydrophilicity of the fiber surface becomes high and the water pressure resistance decreases. The more preferred range is 0.20 to 0.50 mass%.
[0080] The antistatic effect, i.e., the dust protection of the laminated nonwoven fabric 2 can be measured based on the surface resistance value of EN 1149-1-2006, with the first outermost layer 2a of the laminated nonwoven fabric 2 as the measurement surface. The preferred range of the surface resistance value of the garment 1 of the present invention is 2.5×10 9 Ω or less. Surface resistance value is higher than 2.5×10 9When the antistatic effect is insufficient, the dust protection is poor. More preferably, it is 1.5×10 9 The following range.
[0081] As the type of antistatic agent 7, cationic antistatic agents, amphoteric antistatic agents and anionic antistatic agents can be cited. Then, quaternary ammonium salt compounds and acetate compounds of aliphatic amines are equivalent to cationic antistatic agents, betaine compounds, carboxymethylamine compounds and imidazolinium compounds are equivalent to amphoteric antistatic agents, and sulfate compounds, sulfonic acid compounds and phosphate compounds are equivalent to anionic antistatic agents. Among them, from the aspect of being able to reduce the surface resistance as an index of antistatic performance, anionic antistatic agents are more preferred, and phosphate compounds are further preferred.
[0082] The processing method of the antistatic agent 7 may be any of a method of immersing the fibers of the first outermost layer 2a of the laminated nonwoven fabric 2 in a treatment solution containing the antistatic agent 7, a method of mixing the antistatic agent 7 into the fibers of the first outermost layer 2a of the laminated nonwoven fabric 2 and subjecting the fibers themselves to antistatic treatment, and a method of subjecting the fibers of the first outermost layer 2a of the laminated nonwoven fabric 2 to antistatic treatment by coating the fibers with a coating agent containing the antistatic agent 7. Among these, the immersion treatment is preferred because it is easy to control the amount of adhesion and has excellent productivity.
[0083] The agent adhesion rate of the antistatic agent 7 on the laminated nonwoven fabric is obtained by the following method. That is, as a first step, the layers other than the first outermost layer 2a of the laminated nonwoven fabric are removed using No. 1000 sandpaper, the first outermost layer 2a of the obtained laminated nonwoven fabric is cut into 15 cm×15 cm, and the weight of the first outermost layer 2a of the obtained laminated nonwoven fabric is measured in g to the fifth decimal place.
[0084] As a second step, the first outermost layer 2a of the laminated nonwoven fabric whose weight was measured was put into a beaker with 100 ml of methanol and subjected to ultrasonic extraction for 10 minutes. The extract obtained by ultrasonic cleaning was dried at 40°C, concentrated to 1 ml, filtered with a 0.45 μm PTFE disk filter, and the obtained extract filtrate was diluted 10 times and measured with LC / MS / MS and LC20A manufactured by Shimadzu Corporation. The antistatic agent used was identified based on the obtained results, and the area of the peak portion corresponding to the identified antistatic agent was calculated respectively.
[0085] As a third step, in order to calculate the drug adhesion rate, a composition identical to the antistatic agent identified by the first outermost layer 2a of the laminated nonwoven fabric is prepared again, and a 10-fold dilution solution, a 100-fold dilution solution, and a 1000-fold dilution solution are prepared with methanol, respectively, and the measurement is performed in the same manner as the extraction filtrate. The peak area corresponding to the identified antistatic agent is calculated, and a calibration curve of the identified antistatic dose and the obtained peak area is prepared. The obtained peak area is compared with the calibration curve to calculate the antistatic dose attached to the first outermost layer 2a of the laminated nonwoven fabric.
[0086] As a fourth step, the amount of antistatic agent attached to the first outermost layer 2a of the aforementioned laminated nonwoven fabric is divided by the weight of the first outermost layer 2a of the laminated nonwoven fabric measured in advance, and the obtained value is rounded to the second decimal place to be set as the agent adhesion rate (mass %) of the antistatic agent 7.
[0087] The joint 3 of the garment 1 of the present invention has the hem 5 located on the inner side 1b of the garment. This is important in making the outer side 1a of the garment 1 flat to suppress dust adhesion and snagging of objects in contact with the garment 1.
[0088] As a method for arranging the hem 5 on the inner side 1b of the garment 1, it is preferable to use a method of processing in a state where the outer sides 1a of the garment 1 of the joined plurality of components are in contact with each other, that is, in a state where the first outermost layers 2a of the laminated nonwoven fabrics 2 are in contact with each other.
[0089] <Provision of liquid protection>
[0090] As a preferred way to impart liquid protection to the garment 1 of the present invention, the welt 5 of the joint 3 is covered with the belt member 4, which blocks the path for liquids in the external air environment to intrude from the welt 5, which is necessary for liquid protection.
[0091] exist Figure 1 In the example of FIG. 1 , the liquid attached to the outer side 1a of the garment 1 enters the inner side 1b of the garment 1 through the following paths: first reaching the sewing portion 5b of the hem 5, then reaching the end of the hem, or through the sewing portion 5b of the hem 5 to reach the outermost layer of the laminated nonwoven fabric 2. The present invention covers the hem 5 with the belt member 4, thereby preventing the liquid from entering the garment 1 through the above-mentioned paths.
[0092] When the belt member 4 is not covered with the dimple 5, the aforementioned path is not blocked, and liquid intrudes from the dimple 5, which shows a tendency of poor liquid protection.
[0093] As a method for covering the dimple 5 of the joint portion 3 with the tape member 4 , a method of placing the tape member 4 on the dimple 5 of the joint portion 3 and performing bonding processing can be preferably used.
[0094] As the bonding method, hot air heating, resistance heating, high frequency heating, ultrasonic heating, etc. can be preferably used. Any of them may be used, and more preferably, hot air heating is excellent in productivity and followability to the joining portion 3 having a curve.
[0095] In the garment 1 of the present invention, the hem 5 is located on the inner side of the garment, and the belt member 4 is also located on the inner side 1b of the garment 1. As a result, the number of components on the outer side of the outer side 1a of the garment 1 that can accumulate dust is reduced, and as a result, the dust protection of the garment becomes excellent. In addition, by the belt member 4 being located on the inner side 1b of the garment, the adhesive resin layer 4b of the belt member 4 is in contact with the second outermost layer of the laminated nonwoven fabric, which is the raw fabric of the garment. The second outermost layer does not contain an antistatic agent, or even if it contains an antistatic agent, it is only a very small amount, so the affinity with the above-mentioned adhesive resin layer 4b is high, and the fixing of the belt member 4 and the laminated nonwoven fabric 2 becomes firm, and as a result, the liquid protection performance of the joint becomes selected. On the other hand, when the belt member 4 is located on the outer side 1a of the garment 1, due to the antistatic agent contained in the first outermost layer, the belt member 4 is difficult to bond with the laminated nonwoven fabric, which is the raw fabric of the garment, and as a result, it can be seen that the liquid protection of the garment tends to be poor.
[0096] As a method of arranging the tape member 4 on the inner side 1b of the garment 1, it is preferable to use a method of making the inner side 1b of the garment 1, that is, the second outermost layer 2b of the laminated nonwoven fabric 2, and the tape member 4 face each other and bond them together.
[0097] At least the two ends of the belt member 4 in the short side direction are fixed to the second outermost layer 2b of the laminated nonwoven fabric 2, which blocks the path of liquids existing in the external air environment from the nest edge 5, which is necessary in terms of liquid protection. When the two ends of the belt member 4 in the short side direction are not fixed to the second outermost layer 2b of the laminated nonwoven fabric 2, liquid penetrates from the joint 3, and the liquid protection is poor.
[0098] As a method for fixing both ends of the short side direction of the belt member 4 to the second outermost layer 2b of the laminated nonwoven fabric 2, it is preferable to use a method of designing in such a way that the dimension of the short side direction of the belt member 4 is larger than the minimum dimension from the sewing portion 5b of the serge 5 to the end of the laminated portion 5a. More preferably, when the minimum distance from one end of the short side direction of the belt member 4 to the end of the laminated portion 5a of the serge 5 is set as the first dimension, and the minimum distance from the other end of the short side direction of the belt member 4 to the sewing portion 5b of the serge 5 is set as the second dimension, a method of arranging in such a way that the first dimension and the second dimension become equal is preferable. This is because the intrusion path of the liquid object can be evenly covered, and the unevenness of the liquid protection is reduced.
[0099] The garment 1 of the present invention may be provided with an opening for putting on and taking off the garment formed by combining the laminated nonwoven fabric 2 and the zipper, and a pocket for storage, in addition to the aforementioned joint 3. In this case, the hem 5 at this position has a laminated portion 5a of the laminated nonwoven fabric 2 and a portion of an auxiliary material. The hem 5 has multiple interlayer boundaries, and the intrusion path of liquids covers multiple ranges, so it is sometimes necessary to add or change the position of the belt member 4. In this way, in the portion of the hem 5 having a laminated portion 5a of the laminated nonwoven fabric 2 and an auxiliary material, the belt member 4 can be positioned on the outside 1a of the garment 1, or on both the inside and the outside. Figure 6 , Figure 7 In the example, the entire central portion of the garment 1 is provided with an opening for wearing and taking off with a zipper, and the belt member 4 at this location can be arranged on both the inner side 1b and the outer side of the garment 1. Therefore, the belt member 4 provided on the outer side 1a of the garment 1 can be seen.
[0100] The content of the antistatic agent 7 in the second outermost layer 2b of the laminated nonwoven fabric 2 located on the inner side 1b of the garment 1 is 0.01% by mass or less relative to the entire second outermost layer, which is important from the viewpoint of the adhesion between the layer and the belt member 4. That is, the second outermost layer, unlike the first outermost layer, does not contain an antistatic agent, or even if it contains an antistatic agent, it is a very small amount. The content of the antistatic agent in the second outermost layer is 0.02% by mass, etc. When the content of the antistatic agent exceeds 0.01% by mass, the adhesion between the second outermost layer and the belt member 4 becomes low, and the liquid protection of the garment is poor.
[0101] As a method for applying the antistatic agent 7, the same method as the processing of the first outermost layer 2a of the laminated nonwoven fabric 2 can be used.
[0102] The laminated nonwoven fabric 2 constituting the garment 1 of the present invention has a water pressure resistance of 1,000 mmH as measured by JIS L 1092 (2009) A method. 2 O~1,0000mmH 2 The range of 0 is preferred because the liquid protection of the garment 1 is excellent. Water pressure resistance is less than 1,000 mmH 2 When the pressure is 0, liquids can easily penetrate through the laminated nonwoven fabric 2 when the garment 1 is worn, resulting in poor liquid protection. When the pressure exceeds 1,0000 mmH2, the temperature inside the garment 1 is likely to rise due to the airtightness of the laminated nonwoven fabric 2, resulting in poor comfort. More preferably, the pressure is 1,000 mmH2. 2 O~4000mmH 2 The scope of O.
[0103] The ratio of the water pressure resistance (A) of the aforementioned laminated non-woven fabric 2 to the water pressure resistance (B) of the joint 3 (water pressure resistance (B) / water pressure resistance (A)) is 0.4 to 1.0, which is preferred in terms of balancing the water pressure resistance of the laminated non-woven fabric 2 and the joint 3 and providing excellent stability in the liquid protection of the clothing 1.
[0104] When the ratio is less than 0.4 or exceeds 1, the pressure of liquid intrusion is concentrated on the side of the laminated nonwoven fabric 2 or the joint 3 where the water pressure resistance is low, which easily causes local contamination and poor liquid protection.
[0105] As a method for setting the ratio of the water pressure resistance (A) of the laminated nonwoven fabric 2 to the water pressure resistance (B) of the joint 3 to the above-mentioned preferred range, there are methods such as selecting a belt member 4 having a structure with the same water pressure resistance as the laminated nonwoven fabric 2, or adjusting the adhesion of the two ends of the belt member 4 in the short side direction fixed to the second outermost layer 2b of the laminated nonwoven fabric 2 according to the bonding conditions. Any of them is acceptable, and a combination of these methods is more preferred.
[0106] <More preferred embodiment of laminated nonwoven fabric>
[0107] Examples of fiber raw materials constituting the first outermost layer 2a of the laminated nonwoven fabric 2 and the second outermost layer 2b of the laminated nonwoven fabric 2 include polyolefin resins (e.g., polyethylene, polypropylene, copolymers of ethylene and α-olefin, copolymers of propylene and α-olefin, etc.), styrene resins (e.g., polystyrene, acrylonitrile styrene resin, etc.), polyether resins (e.g., polyetheretherketone, polyacetal, modified polyphenylene ether, aromatic polyetherketone, etc.), polyester resins (e.g., polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, etc.), and polyester resins (e.g., polyethylene terephthalate, polytrimethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polybutylene naphthalate, etc.). esters, polycarbonates, polyarylates, aromatic polyester resins, etc.), polyimide resins, polyamideimide resins, polyamide resins (for example, aromatic polyamide resins, aromatic polyetheramide resins, nylon resins, etc.), polyurethane resins, epoxy resins, polysulfone resins (for example, polysulfone, polyethersulfone, etc.), fluorine resins (for example, polytetrafluoroethylene, polyvinylidene fluoride, etc.), cellulose resins, polybenzimidazole resins, acrylic resins (for example, polyacrylonitrile resins obtained by copolymerizing acrylic acid esters or methacrylates, modified acrylic resins obtained by copolymerizing acrylonitrile with vinyl chloride or vinylidene chloride, etc.).
[0108] Among them, polyolefin resins are preferred from the viewpoint of productivity and excellent hand feel of the laminated nonwoven fabric 2. Polyolefin resins are particularly preferred because polyethylene and polypropylene have low hygroscopicity, excellent skin separation between the fabric and the skin surface after sweating, and higher comfort can be obtained during handling.
[0109] The clothing 1 of the present invention can be used by directly laminating the fibers of the first outermost layer 2a of the laminated nonwoven fabric 2 and the fibers of the second outermost layer 2b of the laminated nonwoven fabric 2. Here, in order to impart strength and various functionalities, it is preferred that another nonwoven fabric layer is included as an intermediate layer between the first outermost layer 2a of the laminated nonwoven fabric 2 and the second outermost layer 2b of the laminated nonwoven fabric 2.
[0110] As the structure of the laminated nonwoven fabric 2, for example, a laminate of one or more nonwoven fabrics selected from spunlace nonwoven fabrics, spunbond nonwoven fabrics, meltblown nonwoven fabrics 6c and needle-punched nonwoven fabrics can be exemplified. Among them, a laminate of a spunbond nonwoven fabric having high productivity, high strength and high air permeability and a meltblown nonwoven fabric 6c having high water pressure resistance is preferred.
[0111] A more preferred structure of the laminated nonwoven fabric 2 is a structure including a first spunbonded nonwoven fabric 6a, a meltblown nonwoven fabric 6c, and a second spunbonded nonwoven fabric 6b in this order. This is preferred in terms of strength, productivity, and cost, and the aforementioned preferred water pressure resistance of the laminated nonwoven fabric 2 can be easily obtained.
[0112] The first spunbonded nonwoven fabric 6 a described here corresponds to the first outermost layer 2 a of the laminated nonwoven fabric 2 , and the second spunbonded nonwoven fabric 6 b corresponds to the second outermost layer 2 b of the laminated nonwoven fabric 2 .
[0113] The first spunbonded nonwoven fabric 6a has a unit area weight of 20 to 50 g / m 2 This makes it easy to make the amount of antistatic agent 7 attached to the first outermost layer 2a of the laminated nonwoven fabric 2 within the aforementioned preferred range, so it is preferred. The unit area weight of the first spunbonded nonwoven fabric 6a is less than 20g / m 2 When the antistatic agent 7 of the first outermost layer 2a of the laminated nonwoven fabric 2 is difficult to adhere, the dust protection is poor. 2 When the weight of the garment 1 increases, it is more preferably 25 to 40 g / m 2 range.
[0114] The weight per unit area of the second spunbonded nonwoven fabric 6b is 5 to 30 g / m 2 , which makes it easy to make the amount of antistatic agent 7 attached to the second outermost layer 2b of the laminated nonwoven fabric 2 within the above-mentioned preferred range. In addition, it is easy to fix the two ends of the belt member 4 in the short side direction to the second outermost layer 2b of the laminated nonwoven fabric 2, so it is preferred. The unit area weight of the second spunbonded nonwoven fabric 6b is 5g / m 2 When it is above, the strength is excellent. 30g / m 2 When the thickness is less than 10 g / m, the tape member 4 and the second outermost layer 2b of the laminated nonwoven fabric 2 are easily adhered to each other, and the aforementioned water pressure resistance is easily obtained in the joint 3, that is, the liquid protection is excellent. More preferably, the thickness is 10 to 25 g / m 2 range.
[0115] The weight per unit area is measured according to JIS L 1096 (2010) 8.3.2-A method, and the weight per 1m2 under standard conditions is calculated. 2 Mass (g / m 2 ).
[0116] As a method for adjusting the basis weight of the first spunbonded nonwoven fabric 6a and the second spunbonded nonwoven fabric 6b, it is preferable to adjust the spinning flow rate or the stretching rate of the fibers from the spinneret, adjust the speed of the collecting conveyor, or a combination thereof.
[0117] The unit area weight of the second spunbonded nonwoven fabric 6b is smaller than the unit area weight of the first spunbonded nonwoven fabric 6a, which makes it easy to fix the two ends of the short side direction of the belt component 4 to the second outermost layer 2b of the laminated nonwoven fabric 2 which is the low unit area weight side, and the water pressure resistance of the joint 3 is excellent, so it is preferred.
[0118] Since the weight per unit area of the second spunbonded nonwoven fabric 6b is lower than the weight per unit area of the first spunbonded nonwoven fabric 6a, the antistatic agent 7 of the first outermost layer 2a of the laminated nonwoven fabric 2 is easily attached, and the dust protection is excellent. In addition, the adhesion between the belt member 4 and the second outermost layer 2b of the laminated nonwoven fabric 2 is increased, and it is easy to obtain the water pressure resistance of the joint 3, that is, the liquid protection is excellent.
[0119] <More preferred embodiment of belt member>
[0120] As a more preferred embodiment of the belt member 4, the belt member 4 is a laminate including a base material layer and an adhesive resin layer, and due to the impregnation and permeability of the adhesive resin layer 4b of the belt member 4, it is easy to fix both ends of the belt member 4 in the short side direction to the second outermost layer 2b of the laminated nonwoven fabric 2. In addition, the base material layer 4a of the belt member 4 plays the role of a waterproof layer, and it is easy to improve the water pressure resistance, that is, liquid protection of the joint 3, so it is preferred.
[0121] As the material of the substrate layer, fiber knitted fabrics, nonwoven fabrics, or films alone or in a laminate are mainly used, which are excellent in flexibility and are therefore preferred. Films or high-density fabrics are more preferred, which are difficult to see in terms of thickness and have excellent appearance quality.
[0122] The thickness of the adhesive resin layer 4b of the belt member 4 is 10 to 200 μm, and the adhesive resin layer is in contact with the second outermost layer, which makes it easy to seal the height difference formed by the nest edge 5 located on the second outermost layer side of the laminated nonwoven fabric 2 in the joint 3 and the laminated portion 5a of the laminated nonwoven fabric 2. That is, the water pressure resistance, i.e., liquid protection of the joint 3 is excellent, so it is preferred.
[0123] When the thickness of the adhesive resin layer is 10 μm or more, it is easy to fill the gap between the height difference between the belt member 4 and the nest 5, that is, the laminated portion 5a of the laminated nonwoven fabric 2, and it is easy to obtain water pressure resistance in the joint 3, that is, excellent liquid protection. When the thickness of the adhesive resin layer is 200 μm or less, the thickness of the adhesive resin layer is reduced, the joint 3 is easy to soften, and the adhesive resin is difficult to overflow around the belt member 4 and the nest 5, that is, the laminated portion 5a of the laminated nonwoven fabric 2, and the appearance quality is excellent. The range of 30 to 100 μm is more preferred.
[0124] The thickness of the adhesive portion is measured based on JIS K 7130:1999 Plastic Film and Sheet Thickness Measurement Method. The thickness of the adhesive portion may be adjusted by any method, such as various molding methods such as T-die, injection, blow molding, knife coating, gravure coating, etc., although it depends on the manufacturing method. T-die molding is preferred in terms of suitable thickness, shape, etc.
[0125] As the formation method of the adhesive resin layer, a coating method or a lamination method can be preferably used. In the coating method, any method can be used as long as the method of forming a film by dry bonding or wet coagulation of the resin on the substrate layer. In addition, in order to adjust the static friction coefficient or lightweight, microporous formation caused by dry foaming with the addition of silicon dioxide, the addition of a foaming agent, the wet coagulation of polyurethane, and the use of an embossing roller to give concave and convex, etc. can also be suitably contained in the resin film. Titanium oxide, carbon black, pigment, antioxidant, ultraviolet absorber, light stabilizer, flame retardant, etc.
[0126] As the type of resin constituting the adhesive resin layer, an organic adhesive is mainly used, and the types of organic adhesives are roughly divided into natural resin systems such as natural rubber casein, semi-synthetic systems such as cellulose acetate, and synthetic resin systems using polyolefins, polyurethanes, acrylic acids, etc. Preferably, synthetic resin systems are preferred in terms of processability and cost.
[0127] The resin component of the synthetic resin system is subdivided into resin systems using polyurethane, polyester, PVA, vinyl chloride, acrylic resin, polyethylene, ethylene-vinyl acetate polymer, polyamide system, polyolefin system, etc., and elastic systems using silicone rubber, nitrile rubber, etc., nylon·epoxy resin, vinyl·phenol resin, etc. Composite systems. More preferably, polyolefin systems have high processability and are excellent in heat resistance, bonding strength, and durability by cross-linking reaction with water (humidity) contained in the air, so they are preferred.
[0128] For the curing and reaction modes of synthetic resins, there are dry curing types such as water-soluble, latex, and dispersion types; chemical reaction types that cure by causing a cross-linking reaction through the mixing of a main agent and a curing agent; hot melt types that are solid at room temperature but melt when heated and solidify when cooled; pressure sensitive types that pressurize and bond high-viscosity fluid liquids; and moisture curing types that cure by reacting with moisture in the air.
[0129] More preferably, a heat-fusible (thermoplastic hot melt) or moisture-curable adhesive resin layer is excellent in adhesive strength at the interface with the second outermost layer 2b of the laminated nonwoven fabric 2 and is therefore preferred.
[0130] <Providing breathability>
[0131] The air permeability of the laminated nonwoven fabric 2 measured according to JIS L1913 (2010) 6.8 (Frazier method) is 2.0 to 40.0 cm 3 / cm 2 / sec, the breathability of the garment 1 is excellent, which is preferred.
[0132] Air permeability: 2.0cm 3 / cm 2 / sec or more, the temperature inside the garment 1 is unlikely to rise when the garment 1 is worn, and the air permeability is excellent. 3 / cm 2 / sec or less, dust-like scattered matter is unlikely to flow into the laminated nonwoven fabric 2, and the protective property is excellent. More preferably, it is 4.0 to 20.0 cm 3 / cm 2 / sec range.
[0133] As a method of imparting air permeability, any of a method of adjusting the fiber diameter, unit weight, and density of the laminated nonwoven fabric 2, and a method of changing them according to the layers of the laminated nonwoven fabric 2 may be used. However, from the viewpoint of being able to achieve both the aforementioned dust protection and liquid protection, a method of adjusting the unit weight of the laminated nonwoven fabric 2 is preferred. More preferably, it is set to the preferred range of the unit weight of the first spunbonded nonwoven fabric 6a and the second spunbonded nonwoven fabric 6b.
[0134] (Implementation Method 2)
[0135] Next, the garment 1 according to the second embodiment will be described.
[0136] Figure 2 This is a cross-sectional view of a garment 1 according to a second embodiment of the present invention. Figure 3 It is a cross-sectional view of a garment 1 according to a modified example of the second embodiment of the present invention. Figure 6 Is Figure 1 The garment 1 is shown in a perspective view, viewed from its outer side 1 a . Figure 7 yes Figure 6 An exploded view of the garment 1 is shown.
[0137] The garment 1 of the second embodiment of the present invention is composed of a laminated nonwoven fabric 2 and a member including a rectangular belt member 4, similarly to the first embodiment, and further includes a joining portion 3. The main differences between the garment 1 of the second embodiment and the garment 1 of the first embodiment will be described below.
[0138] The laminated nonwoven fabric 2 is cut into components for each part of the garment 1, and the components are joined at the joining portion 3 to form the garment 1. The joining portion 3 is composed of at least one of a sewn portion and a welded portion 5b and a belt member 4.
[0139] In the second embodiment, the joining portion 3 is different from the sewing portion of the clothes of the first embodiment, and the horizontal surfaces in the thickness direction of the two ends of at least one laminated nonwoven fabric face each other in at least one of the sewing portion and the fusion portion. That is, the joining portion 3 in the second embodiment does not have the dimpled edge 5 having the laminated portion 5a formed by laminating a part of the laminated nonwoven fabric 2 as the clothes of the first embodiment have.
[0140] Here, the two ends of one laminated nonwoven fabric, for example, when the laminated nonwoven fabric is rectangular, can be exemplified as the two ends in the length direction, and in a manner in which the horizontal surfaces of the two ends in the thickness direction are opposite to each other, the laminated nonwoven fabric is cylindrical. In addition, the two ends of two laminated nonwoven fabrics, for example, when both laminated nonwoven fabrics are rectangular, can be exemplified as one end of one laminated nonwoven fabric and one end of the other laminated nonwoven fabric, and the horizontal surfaces of the two ends in the thickness direction are opposite to each other.
[0141] The horizontal surface in the thickness direction of the laminated nonwoven fabric is a concept including surfaces substantially horizontal to the thickness direction, and is a concept including common sense surfaces that are cut surfaces of the laminated nonwoven fabric.
[0142] Figure 2 In the example, the joint 3 is formed by butting the ends of the laminated nonwoven fabric 2 components together, forming a sewn portion by sewing or a welded portion by welding in the butted area, and covering the sewn portion 5b with a belt member 4.
[0143] In addition, similar to the clothes of the first embodiment, the belt member in the clothes of the second embodiment is also located on the inside of the clothes. The reason is the same as that described for the clothes of the first embodiment. That is, in order to make the clothes excellent in dust protection, the first outermost layer needs to contain a specific content of antistatic agent. For the second outermost layer, there is no need to suppress static electricity, and on the other hand, in order to make the adhesion with the belt member excellent, no antistatic agent is contained, or even if it is contained, it is only a very small amount. Therefore, by locating the belt member on the inside of the clothes, the adhesive resin layer of the belt member is inevitably in contact with the second outermost layer, and the fixing of the laminated nonwoven fabric and the belt member becomes firm.
[0144] In this embodiment, the liquid enters the garment 1 through the sewing or welding parts of the butted laminated nonwoven fabrics 2. The present invention covers the sewing parts 5b with the tape member 4 to prevent the liquid from entering the garment 1 through the above-mentioned paths.
[0145] exist Figure 3 In the example, the joining portion 3 is formed by overlapping a portion of the laminated nonwoven fabric 2 components in parallel, forming a sewn portion by sewing or a fused portion by welding in the overlapping area, and covering the sewn portion 5b with a belt member 4.
[0146] The intrusion path of liquid into the garment 1 in this embodiment includes, as a first path, a path from the stitching or welding part located on the upper side of the overlapping laminated nonwoven fabric 2 parts, i.e., the outermost laminated nonwoven fabric 2 side of the garment 1, to the stitching or welding part located on the lower side of the laminated nonwoven fabric 2 parts, i.e., the innermost laminated nonwoven fabric 2 side of the garment 1. As a second path, a path is intruded from the stitching or welding part of the boundary surface between the overlapping laminated nonwoven fabric 2 parts. The present invention covers the stitching part etc. 5b with the belt member 4, thereby suppressing the intrusion of liquid into the garment 1 through the aforementioned path.
[0147] The second embodiment of the clothing of the present invention can be the same as the first embodiment except for the above-mentioned difference.
[0148] Example
[0149] The present invention will be described in more detail below with reference to Examples and Comparative Examples, but the present invention is not limited thereto. Evaluation of clothing used in Examples and Comparative Examples was carried out by the following method.
[0150] [Measurement method]
[0151] (1) Weight per unit area
[0152] Based on JIS L1096-2010, two test pieces of 200 mm × 200 mm were taken from the first outermost layer 2a of the laminated nonwoven fabric and the second outermost layer 2b of the laminated nonwoven fabric, and their respective masses were weighed to find the mass per unit area, and the average value of each was used. The unit is g / m 2 .
[0153] (2) Water pressure resistance
[0154] The water pressure resistance of the laminated nonwoven fabric 2 and the joint 3 is measured based on the low water pressure resistance method of JIS L1092-2009. Water pressure is applied to the test piece at a pressure increase rate of 60 cm / min, and the water pressure when three drops of water are dropped is measured. The average value of the three measurements is used. The unit is mmH 2 O.
[0155] (3) Water pressure resistance ratio
[0156] The ratio of the water pressure resistance (A) of the laminated nonwoven fabric to the water pressure resistance (B) of the joint portion measured in the previous paragraph is calculated by the following formula (water pressure resistance (B) ÷ water pressure resistance (A)) and is expressed as a value to two decimal places.
[0157] (4) Antistatic agent content
[0158] The content of the antistatic agent relative to the first outermost layer 2a of the laminated nonwoven fabric and the content of the antistatic agent relative to the second outermost layer 2b of the laminated nonwoven fabric are obtained by layer through the following steps. As a first step, use No. 1000 sandpaper to remove the layers other than the first outermost layer 2a of the laminated nonwoven fabric, cut the first outermost layer 2a of the obtained laminated nonwoven fabric into 15cm×15cm, and measure the weight of the first outermost layer 2a of the obtained laminated nonwoven fabric in g units to the fifth decimal place. As a second step, the first outermost layer 2a of the laminated nonwoven fabric whose weight was measured was put into a beaker with 100ml of methanol added, and ultrasonic extraction was performed for 10 minutes. The extract obtained by ultrasonic cleaning was dried at 40°C, concentrated to 1ml, filtered with a 0.45μm PTFE disc filter, and the obtained extract filtrate was diluted 10 times and measured with LC / MS / MS and LC20A made by Shimadzu Corporation. The antistatic agent used was identified based on the obtained results, and the area of the peak portion corresponding to the identified antistatic agent was calculated.
[0159] As a third step, in order to calculate the drug adhesion rate, a composition identical to the antistatic agent identified by the first outermost layer 2a of the laminated nonwoven fabric is prepared again, and a 10-fold dilution solution, a 100-fold dilution solution, and a 1000-fold dilution solution are prepared with methanol, respectively, and the measurement is performed in the same manner as the extraction filtrate. The peak area corresponding to the identified antistatic agent is calculated, and a calibration curve of the identified antistatic dose and the obtained peak area is prepared. The obtained peak area is compared with the calibration curve to calculate the antistatic dose attached to the first outermost layer 2a of the laminated nonwoven fabric.
[0160] As a fourth step, the amount of antistatic agent attached to the first outermost layer 2a of the laminated nonwoven fabric is divided by the weight of the first outermost layer 2a of the laminated nonwoven fabric measured in advance, and the obtained value is rounded to the second decimal place, and the value is set as the content of the antistatic agent in the first outermost layer 2a of the laminated nonwoven fabric. The unit is set to mass %. For the second outermost layer 2b of the laminated nonwoven fabric, the content of the antistatic agent is also calculated in the same manner as above.
[0161] (5) Surface resistance
[0162] The surface resistance of the antistatic dust protection fabric is measured by using the first outermost layer 2a of the laminated nonwoven fabric as the measurement surface, and using a surface resistance value obtained from a test piece of 12 cm×12 cm in size based on EN1149-1-2006. The unit is Ω.
[0163] (6) Thickness of the adhesive resin layer of the tape member
[0164] The thickness of the adhesive resin layer 4b of the belt member is measured as follows: a cross section of the belt member 4 is cut out, a platinum-palladium alloy is vapor-deposited on the cross section, and the overall thickness of the belt member 4 is measured from a photographic image taken with a scanning electron microscope (SEM) (S-4000 model manufactured by Hitachi, Ltd.), and then the thickness of the base material layer 4a of the belt member is measured, and the thickness of the base material layer is subtracted from the overall thickness of the belt member 4 obtained previously, and the result is taken as the thickness of the adhesive resin layer 4b of the belt member. The unit is μm.
[0165] (7) Air permeability
[0166] The air permeability of the laminated nonwoven fabric 2 was measured based on the Frazier method of JIS L1913-2010, and was determined as the amount of air passing through a test piece of 15 cm×15 cm in size. The average value of the amount of air passing through was used after three measurements. The unit is cm 3 / cm 2 / sec, the first decimal place is set to be effective.
[0167] [evaluate]
[0168] (8) Liquid protection of laminated nonwoven fabric 2
[0169] The liquid repellency of the front and back parts of the garment, that is, the laminated nonwoven fabric 2, was evaluated according to the criteria in Table 1. The higher the parameter score, the better the liquid repellency.
[0170] (9) Liquid protection of joints
[0171] The liquid repellency of the joints 3, where the parts of the garment are joined together, was evaluated according to the criteria shown in Table 1. The higher the parameter score, the better the liquid repellency.
[0172] (10) Dust protection
[0173] The dust protection of the clothes was evaluated according to the criteria in Table 1. The higher the parameter score, the better the dust protection.
[0174] (11) Comprehensive evaluation
[0175] The total of the evaluation scores of the liquid protection, dust protection, and air permeability of the evaluation items was calculated and used as a comprehensive evaluation. The higher the evaluation score, the better the comprehensiveness, and the case of an evaluation result of 4 points or more was considered as a good garment. The evaluation criteria are shown in Table 2.
[0176] [Table 1]
[0177]
[0178] [Table 2]
[0179] Fraction Comprehensive evaluation 7 or more Very good 4~6 Excellent 0~4 Difference Less than 0 Very bad
[0180] (Example 1)
[0181] Figure 1 and 4 The clothes shown in ~7, that is,
[0182] As the structure of the laminated nonwoven fabric 2, a nonwoven fabric with a unit weight of 45 g / m 2 A polypropylene spunbonded nonwoven fabric was prepared by mixing an anionic antistatic agent in pure water as the antistatic agent 7, and the antistatic agent 7 was calendered to adjust the coating amount of the antistatic agent 7 to 0.135 g / m 2 The antistatic agent was applied so that the content of the antistatic agent was 0.3% by mass. The calendered polypropylene spunbonded nonwoven fabric was dried at 135° C. for 1 minute using a pin tenter to form the outermost layer 2 a of the laminated nonwoven fabric 2 .
[0183] Next, use a weight per unit area of 25g / m 2 The polypropylene spunbonded nonwoven fabric was coated with an antistatic agent 7 at a coating amount of 0 g / m 2 , thereby setting the content of the antistatic agent to 0 mass %, and using this as the second outermost layer 2 b of the laminated nonwoven fabric 2 .
[0184] Next, as the middle layer of the laminated nonwoven fabric 2, a nonwoven fabric having an average fiber diameter of 1.6 μm and a unit weight of 15 g / m 2 Polypropylene meltblown nonwoven fabric 6c.
[0185] The first outermost layer 2a, the middle layer, and the second outermost layer 2b of the laminated nonwoven fabric are laminated in this order and embossed by an embossing device at a temperature of 120°C and a pressure of 60 kg / m 2 The laminated nonwoven fabric 2 was obtained by laminating and integrating the two layers at a speed of 10 m / min.
[0186] In the construction of the belt member 4, a polyolefin-based thermoplastic hot melt resin, that is, a resin mainly composed of a polyolefin-based resin having a melting point of 85° C. and having hot melt adhesiveness, is used. The resin is discharged in a sheet form on release paper by an extrusion method in such a manner that the film thickness is 150 μm, the stress is 3.4 MPa at an elongation of 50%, and the breaking strength is 26.7 MPa. After the resin is stretched, an adhesive resin layer separated from the release paper is obtained, which is used as the adhesive resin layer 4b of the belt member 4.
[0187] Next, as the base material layer 4a of the belt component 4, a resin mainly composed of polypropylene resin with a softening point of 60°C and a melting point of 115°C is used as a raw material, and is discharged and stretched in a sheet form in such a manner that the film thickness is 50 μm, the stress is 0.5 MPa at an elongation of 50%, and the breaking strength is 26 MPa to obtain a film.
[0188] The adhesive resin layer 4b was laminated on the base layer 4a of the obtained tape member 4 to obtain a tape member 4 including the base layer 4a and the adhesive resin layer 4b. The slit molding was performed so that the width of the tape member 4, that is, the dimension between the ends 4c in the short side direction, was 22 mm.
[0189] Next, the laminated nonwoven fabric 2 is cut into Figures 6-7 The parts of the garment shown in the figure are cut and sewn together by a sewing machine to form a hem 5 including a sewn portion 5b and a laminated portion 5a. The hem 5 is exposed in the direction of the inner side of the garment 1.
[0190] Next, the belt member 4 is arranged on the inner side of the garment, and the hem 5 is covered with the adhesive resin layer 4b of the belt member 4, and the adhesive process is performed using a hot air heating heat sealer under the conditions of a roller heating temperature of 90°C, a pressure of 0.4 MPa, and a speed of 2 m / min. The two end portions 4c of the belt member 4 in the short side direction are connected and fixed to the second outermost layer 2b of the laminated nonwoven fabric 2, and the belt member 4 extends along the length direction of the hem 5 to form a joint portion 3 having a rectangular belt member 4, thereby obtaining the garment 1.
[0191] The water pressure resistance of the laminated nonwoven fabric 2 of the obtained clothing 1, the ratio of the water pressure resistance of the joining portion 3 to the laminated nonwoven fabric 2, the content of the antistatic agent 7, the surface resistance, the air permeability, and the thickness 4d of the adhesive resin layer of the belt member 4 were measured.
[0192] Next, dust repellency, liquid repellency of the laminated nonwoven fabric, and liquid repellency of the joint were evaluated according to Table 1, and overall evaluation was evaluated according to the evaluation criteria in Table 2. Table 3 shows the respective numerical values and evaluation results.
[0193] (Example 2)
[0194] In the garment of Example 1, the coating amount of the antistatic agent 7 of the first outermost layer 2a of the laminated nonwoven fabric 2 was set to 0.135 g / m 2 , thereby making the content of the antistatic agent 0.3 mass %, and by setting the coating amount of the antistatic agent 7 of the second outermost layer 2b of the laminated nonwoven fabric 2 to 0 g / m 2 , thereby making the content of the antistatic agent 0 mass %. The film thickness of the adhesive resin layer 4b of the belt member 4 was set to 40 μm.
[0195] Next, the laminated nonwoven fabric 2 is cut into Figures 6-7 The parts of the clothes shown in the figure are welded together by ultrasonic welding machine to form Figure 2 Next, the belt member 4 is arranged on the inner side of the garment, the fusion bond 5b is covered with the adhesive resin layer 4b of the belt member 4, and the same bonding process as in Example 1 is performed. The two ends 4c of the belt member 4 in the short side direction are in contact with and fixed to the second outermost layer 2b of the laminated nonwoven fabric 2, and the belt member 4 extends in the longitudinal direction of the fusion bond 5b to form a junction 3 having a rectangular belt member 4, and the garment 1 is obtained. It should be noted that in the junction 3, in the fusion bond, the horizontal surfaces of the two ends of the two laminated nonwoven fabrics in the thickness direction are opposite to each other.
[0196] The garment 1 was obtained under the same conditions as in Example 1 except for the configuration of the laminated nonwoven fabric 2, the joining portion 3, and the belt member 4. Table 3 shows the numerical values and the evaluation results.
[0197] (Example 3)
[0198] In the garment of Example 1, the weight per unit area of the first outermost layer 2a of the laminated nonwoven fabric 2 is set to 25 g / m 2 The coating amount of the antistatic agent 7 is set to 0.05 g / m 2 The content of the antistatic agent was set to 0.2 mass %, and the weight per unit area of the second outermost layer 2b of the laminated nonwoven fabric 2 was set to 10 g / m 2 , the coating amount of antistatic agent 7 is set to 0g / m 2, the content of the antistatic agent is set to 0% by mass. As the composition of the belt member 4, a polyester fabric is used as follows: the base material layer 4a uses a polyester taffeta fabric, that is, the fibers of the warp yarn and the fibers of the weft yarn are both 33dtex-26f polyester filaments, woven into a plain fabric with a warp density of 207 yarns / inch and a weft density of 147 yarns / inch, and then relaxed and refined and circulated liquid dyed at 130°C, and after drying, calendered at 180°C / 60°C. The film thickness of the adhesive resin layer 4b of the belt member 4 is set to 40μm.
[0199] The garment 1 was obtained under the same conditions as in Example 1 except for the configuration of the laminated nonwoven fabric 2 and the belt member 4. Table 3 shows the numerical values and the evaluation results.
[0200] (Example 4)
[0201] In the garment of Example 1, the weight per unit area of the first outermost layer 2a of the laminated nonwoven fabric 2 is set to 55 g / m 2 The coating amount of antistatic agent 7 is set to 0.0825 g / m 2 The content of the antistatic agent was set to 0.15% by mass, and the weight per unit area of the second outermost layer 2b of the laminated nonwoven fabric 2 was set to 35 g / m 2 , the coating amount of antistatic agent 7 is set to 0g / m 2 The content of the antistatic agent was set to 0% by mass. A polypropylene film was used as the base material layer 4a of the belt member 4. The film thickness of the adhesive resin layer 4b of the belt member 4 was set to 150 μm.
[0202] The garment 1 was obtained under the same conditions as in Example 1 except for the configuration of the laminated nonwoven fabric 2 and the belt member 4. Table 3 shows the numerical values and the evaluation results.
[0203] (Example 5)
[0204] In the garment of Example 1, the weight per unit area of the first outermost layer 2a of the laminated nonwoven fabric 2 is set to 18 g / m 2 The coating amount of antistatic agent 7 is set to 0.081 g / m 2 The content of the antistatic agent is set to 0.45% by mass, and the weight per unit area of the second outermost layer 2b of the laminated nonwoven fabric 2 is set to 4 g / m 2 , the coating amount of antistatic agent 7 is set to 0g / m 2 The content of the antistatic agent was set to 0% by mass. A polypropylene film was used as the base material layer 4a of the belt member 4. The film thickness of the adhesive resin layer 4b of the belt member 4 was set to 9 μm.
[0205] The garment 1 was obtained under the same conditions as in Example 1 except for the configuration of the laminated nonwoven fabric 2 and the belt member 4. Table 3 shows the numerical values and the evaluation results.
[0206] (Example 6)
[0207] In the garment of Example 1, the weight per unit area of the first outermost layer 2a of the laminated nonwoven fabric 2 is set to 55 g / m 2 The coating amount of antistatic agent 7 is set to 0.0825 g / m 2 The content of the antistatic agent is set to 0.15% by mass, and the weight per unit area of the second outermost layer 2b of the laminated nonwoven fabric 2 is set to 4 g / m 2 , the coating amount of antistatic agent 7 is set to 0g / m 2 The content of the antistatic agent was set to 0% by mass. As the middle layer of the laminated nonwoven fabric 2, a polyethylene microporous film having a thickness of 14 μm, a melting point of 137° C., a microporous pore size of 32 μm, and a moisture permeability of 380 g / m 2 h, tensile strength (warp) 40N / 50mm, tensile strength (weft) 40N / 50mm, tensile elongation (warp) 10%, tensile elongation (weft) 8%, water pressure resistance 65kPa, puncture strength 370N / mm. The thickness of the adhesive resin layer 4b of the belt member 4 is set to 250μm.
[0208] The garment 1 was obtained under the same conditions as in Example 1 except for the configuration of the laminated nonwoven fabric 2 and the belt member 4. Table 4 shows the numerical values and the evaluation results.
[0209] (Comparative Example 1)
[0210] In the joint portion 3 of the garment of Example 1, the sewn portion 5b and the laminated portion 5a are arranged so that the exposed direction of the hem 5 is on the outside of the garment 1. The tape member 4 is arranged on the outside of the garment, the hem 5 is covered with the adhesive resin layer 4b of the tape member 4, and the two end portions 4c of the tape member 4 in the short side direction are fixed to the first outermost layer 2a of the laminated nonwoven fabric 2 so as to form the joint portion 3.
[0211] The garment 1 was obtained under the same conditions as in Example 1 except for the configuration of the aforementioned joining portion 3. Table 4 shows the numerical values and the evaluation results.
[0212] (Comparative Example 2)
[0213] In the garment of Example 1, the coating amount of the antistatic agent 7 of the first outermost layer 2a of the laminated nonwoven fabric 2 was set to 0.0045 g / m 2, thereby making the content of the antistatic agent 7 0.01 mass %, and setting the coating amount of the antistatic agent 7 of the second outermost layer 2b of the laminated nonwoven fabric 2 to 0.075 g / m 2 , thereby making the content of the antistatic agent 0.3 mass %.
[0214] The garment 1 was obtained under the same conditions as in Example 1 except for the configuration of the laminated nonwoven fabric 2. Table 4 shows the numerical values and the evaluation results.
[0215] (Comparative Example 3)
[0216] In the garment of Example 1, the coating amount of the antistatic agent 7 of the first outermost layer 2a of the laminated nonwoven fabric 2 was set to 0.0045 g / m 2 , thereby making the content of the antistatic agent 7 0.01 mass %, and setting the coating amount of the antistatic agent 7 of the second outermost layer 2b of the laminated nonwoven fabric 2 to 0.075 g / m 2 , thereby making the content of the antistatic agent 0.3% by mass. The joining portion 3 does not contain the tape member 4, and is formed by sewing the parts formed by cutting and laminating the nonwoven fabric 2 together by a sewing machine, and is formed only by the welt 5 including the sewn portion 5b and the laminated portion 5a.
[0217] The garment 1 was obtained under the same conditions as in Example 1 except for the configuration of the laminated nonwoven fabric 2 and the joining portion 3 and the configuration of not using the tape member 4. Table 4 shows the numerical values and the evaluation results.
[0218] (Comparative Example 4)
[0219] In the garment of Comparative Example 3, a single-layer nonwoven fabric is used instead of the laminated nonwoven fabric 2, that is, the weight per unit area is 45 g / m 2 , the coating amount of antistatic agent 7 is 0.0045g / m 2 The spunbonded nonwoven fabric having an antistatic agent content of 0.01 mass % was prepared under the same conditions as in Comparative Example 3 except for the above-mentioned configuration to obtain clothing 1. Table 4 shows the numerical values and evaluation results.
[0220] [Table 3]
[0221]
[0222] [Table 4]
[0223]
[0224] In the clothes of Examples 1 to 6, in the first outermost layer 2a and the second outermost layer 2b of the laminated nonwoven fabric 2, the content of the respective antistatic agent 7 is within a preferred range, and the configuration of each layer in the clothes and the joint 3 is preferably arranged, so that the water pressure resistance of the laminated nonwoven fabric 2 and the ratio of the water pressure resistance of the laminated nonwoven fabric 2 to the joint 3 are within a preferred range, thereby forming clothes with excellent dust protection and liquid protection.
[0225] The clothes of Examples 1 to 4 are clothes with better liquid protection of the joint portion by setting the configuration of the tape member 4 and the thickness 4d of the adhesive resin layer 4b to be within the preferred range.
[0226] The clothes of Examples 1 to 3 have air permeability in addition to dust protection and liquid protection by setting the nonwoven fabric structure and basis weight per layer of the laminated nonwoven fabric 2 within the preferred range.
[0227] The garment of Comparative Example 1 has poor liquid protection at the joint portion by arranging the welt 5 and the tape member 4 of the joint portion 3 on the outer side of the first outermost layer 2a of the laminated nonwoven fabric 2 having a high antistatic agent content, that is, the garment 1.
[0228] The clothes of Comparative Example 2 are formed by setting the content of the antistatic agent 7 in the first outermost layer 2a and the second outermost layer 2b of the laminated nonwoven fabric 2 and the ratio of the water pressure resistance of the joint 3 to the laminated nonwoven fabric 2 to a range different from the preferred range, thereby forming clothes with poor dust protection and liquid protection of the joint.
[0229] The garment of Comparative Example 3 is further configured such that no tape member is used in the joint 3 , thereby resulting in poor dust protection and poor liquid protection of the joint.
[0230] The clothing of Comparative Example 4 further used a single-layer nonwoven fabric instead of the laminated nonwoven fabric 2 and did not use a tape member, resulting in poor dust protection, liquid protection of the laminated nonwoven fabric, and liquid protection of the joints.
[0231] That is, the more the clothing of the present invention satisfies the requirements of the invention, the more comprehensive the clothing becomes.
[0232] Industrial Applicability
[0233] The present invention can be used as clothing with dust protection and liquid protection.
[0234] Explanation of symbols
[0235] 1. Clothes
[0236] 1a: Outside of the garment
[0237] 1b: Inside of the garment
[0238] 2: Laminated non-woven fabric
[0239] 2a: The first outermost layer of laminated nonwoven fabric
[0240] 2b: The second outermost layer of laminated nonwoven fabric
[0241] 3: Joint
[0242] 4: With components
[0243] 4a: Base material layer with components
[0244] 4b: Adhesive resin layer of the belt member
[0245] 4c: End of the short side of the belt member
[0246] 4d: Thickness of the adhesive resin layer of the tape member
[0247] 5: Nest
[0248] 5a: Lamination section
[0249] 5b: At least one of a stitched portion and a welded portion
[0250] 6a: First spunbond nonwoven fabric
[0251] 6b: Second spunbond nonwoven fabric
[0252] 6c: Meltblown nonwoven fabric
[0253] 7: Antistatic agent
Claims
1. A garment comprising a laminated nonwoven fabric and a member including a rectangular belt member and having a joint portion, wherein: The first outermost layer of the laminated nonwoven fabric is a nonwoven fabric containing 0.02 to 0.50% by mass of an antistatic agent relative to the entire layer, and is located on the outside of the garment; The second outermost layer of the laminated nonwoven fabric is a nonwoven fabric containing 0.01% by mass or less of an antistatic agent relative to the entire layer, and is located on the inner side of the garment; The aforementioned joint portion has a rim located on the inner side of the aforementioned garment and the aforementioned belt member; The aforementioned nest edge has one or more laminated portions formed by laminating a portion of the aforementioned laminated nonwoven fabric; The laminated portion has at least one of a stitched portion and a welded portion; The aforementioned nest edge is covered by the aforementioned belt member; The belt member is located on the inner side of the garment; At least two ends of the belt member in the short-side direction are fixed to the second outermost layer; The water pressure resistance (A) of the laminated nonwoven fabric measured based on JIS L 1092 (2009) A method is in the range of 1,000 mmH2O to 1,0000 mmH2O; The ratio of the water pressure resistance (B) measured by JIS L 1092 (2009) Method A to the water pressure resistance (A) (water pressure resistance (B) / water pressure resistance (A)) of the joint is 0.4 to 1.
0.
2. A garment comprising a laminated nonwoven fabric and a member including a rectangular belt member and having a joint portion, wherein: The first outermost layer of the laminated nonwoven fabric is a nonwoven fabric containing 0.02 to 0.50% by mass of an antistatic agent relative to the entire layer, and is located on the outside of the garment; The second outermost layer of the laminated nonwoven fabric is a nonwoven fabric containing 0.01% by mass or less of an antistatic agent relative to the entire layer, and is located on the inner side of the garment; The joining portion includes at least one of a sewing portion and a welding portion, and the belt member; In at least one of the stitched portion and the welded portion, horizontal surfaces in the thickness direction of two ends of at least one of the laminated nonwoven fabrics face each other; At least one of the stitched portion and the welded portion is covered by the belt member; The belt member is located on the inner side of the garment; At least two ends of the belt member in the short-side direction are fixed to the second outermost layer; The water pressure resistance (A) of the laminated nonwoven fabric measured based on JIS L 1092 (2009) A method is in the range of 1,000 mmH2O to 1,0000 mmH2O; The ratio of the water pressure resistance (B) measured by JIS L 1092 (2009) Method A to the water pressure resistance (A) (water pressure resistance (B) / water pressure resistance (A)) of the joint is 0.4 to 1.
0.
3. The garment according to claim 1 or 2, wherein: The aforementioned laminated nonwoven fabric comprises, in sequence, a first spunbond nonwoven fabric, a meltblown nonwoven fabric, and a second spunbond nonwoven fabric; The weight per unit area of the first spunbonded nonwoven fabric is 20 to 50 g / m 2 The second spunbonded nonwoven fabric has a unit area weight of 5 to 30 g / m 2 ; The second spunbonded nonwoven fabric has a smaller basis weight than the first spunbonded nonwoven fabric.
4. The clothing according to claim 1 or 2, wherein: The belt member is a laminate comprising a base material layer and an adhesive resin layer; The thickness of the adhesive resin layer is 100 to 200 μm; The adhesive resin layer is in contact with the second outermost layer.
5. The clothing according to claim 1 or 2, wherein: The air permeability of the laminated nonwoven fabric measured in accordance with JIS L1913 (2010) 6.8 (Frazier method) is 2.0 to 40.0 cm 3 / cm 2 / sec.