Platinum group metal catalyst composition
By loading platinum on the composite material of alumina and magnesium oxide, a platinum-alumina-magnesia composite catalyst is formed, which solves the problem of sintering of the platinum catalyst under high-temperature hydrothermal conditions and improves the stability and performance of the catalyst. , enhancing the conversion ability of NOx and hydrocarbons.
Patent Information
- Application Number
- CN202280074013.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2021-11-05
- Filing Date
- 2022-10-20
- Publication Date
- 2024-10-29
AI Technical Summary
Existing platinum catalysts are prone to sintering under high-temperature hydrothermal aging conditions and are difficult to maintain stability at 900°C-1050°C, affecting their application in three-way conversion catalysts.
A composite material containing ceria, alumina and magnesia is used as a carrier, and platinum is supported in it to form a platinum-alumina-magnesia composite catalyst to improve its hydrothermal stability.
The stability and catalytic performance of the platinum catalyst under high-temperature hydrothermal conditions are improved, the conversion rate of NOx and hydrocarbons is enhanced, and the service life of the catalyst is extended.
Smart Images

Figure CN118871199A_ABST
Abstract
Description
Technical Field
[0001] The presently claimed invention relates to a catalyst composition for treating exhaust gas to reduce pollutants contained therein. Specifically, the presently claimed invention relates to a platinum group metal based catalyst composition. Background Art
[0002] Platinum (Pt) is prone to sintering under high temperature hydrothermal aging conditions, making it difficult to use Pt in conventional three-way conversion (TWC) formulations that require aging at 900°C-1050°C. Platinum deposited on conventional refractory alumina can grow to submicron sizes through the recognized Oswald ripening mechanism. Therefore, more research is needed on the use of appropriate support materials to stabilize platinum. When platinum is supported on alumina, the problem of platinum sintering can be solved by using ceria as a support. It has been found that platinum can form a monolayer, usually partially or completely oxidized on the surface of ceria due to strong Pt-CeO2 interactions. However, bulk ceria itself can undergo sintering when aged at high temperatures. Therefore, in the recent past, a ceria-alumina composite material as a platinum support for a TWC catalyst was proposed, in which platinum was selectively deposited on the ceria-alumina composite material. However, there is still a need for an improved support material that can provide high temperature hydrothermal stability to the catalyst at an aging temperature of>950°C, thereby improving catalyst performance. Summary of the invention
[0003] The present invention provides a catalyst composition, which comprises platinum; and at least one composite material, wherein the platinum is loaded on the composite material, wherein the composite material comprises: cerium dioxide (calculated as CeO2) in an amount of 5.0 wt% to 50 wt% based on the total weight of the composite material; aluminum oxide (calculated as Al2O3) in an amount of 10 wt% to 80 wt% based on the total weight of the composite material; and magnesium oxide (calculated as MgO) in an amount of 10 wt% to 80 wt% based on the total weight of the composite material.
[0004] The present invention also provides a method for preparing a catalyst composition. The present invention also provides a catalytic product and its preparation. BRIEF DESCRIPTION OF THE DRAWINGS
[0005] To provide an understanding of embodiments of the present invention, reference is made to the accompanying drawings, which are not necessarily drawn to scale, and in which reference numerals refer to components of exemplary embodiments of the present invention. The accompanying drawings are exemplary only and should not be construed as limiting the present invention. The above and other features of the presently claimed invention, their nature and various advantages will become more apparent when the following detailed description is considered in conjunction with the accompanying drawings:
[0006] FIG1 shows the CO, NO and HC conversions of aged samples 1-6.
[0007] FIG. 2 shows the CO, NO and HC conversions of aged samples 5, 8 and 9.
[0008] FIG. 3 shows the CO, NO and HC conversions of aged samples 1, 2, 5, 7 and 10.
[0009] FIG. 4 shows the CO, NO and HC conversions of aged samples 5, 7 and 10 before and after activation.
[0010] FIG. 5 shows the CO, NO and HC conversions of aged samples 11 , 13 , 14 , 16 , 17 and 18 .
[0011] FIG. 6 shows the CO, NO and HC conversions of aged samples 12, 15, 17 and 19.
[0012] Fig. 7A is a perspective view of a honeycomb type substrate support that may contain a catalyst composition according to one embodiment of the presently claimed invention.
[0013] Figure 7B is relative to Fig. 7A Zoom in and follow the Fig. 7A A partial cross-sectional view taken through a plane of the end surface of a substrate carrier, showing Fig. 7A An enlarged view of the multiple gas flow channels shown in FIG.
[0014] Figure 8 is relative to Fig. 7A A cross-sectional view of an enlarged section, wherein Fig. 7A The honeycomb-type substrate in ref. 3 represents a wall-flow filter substrate monolith.
[0015] Fig. 9 X-ray diffraction patterns of fresh Mg30 and Mg70 supports as well as X-ray diffraction patterns of aged Mg30 and Mg70 supports are shown.
[0016] Fig.10 X-ray diffraction patterns of Mg30-550 and Mg70-550 as well as aged samples of Mg30-550 and Mg70-550 are shown.
[0017] FIG. 11 shows X-ray diffraction patterns of a fresh Pt catalyst (A) and an aged Pt catalyst (B). DETAILED DESCRIPTION
[0018] The presently claimed invention will now be described more fully below. The presently claimed invention can be embodied in many different forms and should not be construed as limited to the embodiments described herein; rather, these embodiments are provided to make the presently claimed invention more complete and complete, and to fully convey the scope of the invention to those skilled in the art. Language in this specification should not be construed to indicate that any non-claimed element is essential to the practice of the materials and methods of the present disclosure.
[0019] Unless otherwise specified herein or clearly contradicted by context, all methods described herein can be performed in any suitable order. Unless otherwise stated, the use of any and all examples or exemplary language (e.g., "such as") provided herein is intended only to better illustrate materials and methods and is not intended to limit the scope.
[0020] definition :
[0021] The terms "a," "an," "the," and similar referents used in the context of describing the materials and methods discussed herein (especially in the context of the following claims) are to be construed to cover both the singular and the plural, unless otherwise indicated herein or clearly contradicted by context.
[0022] Recitation of ranges of values herein are merely intended to serve as a shorthand method of referring individually to each separate value falling within the range, unless otherwise indicated herein, and each separate value is incorporated into the specification as if it were individually recited herein.
[0023] In the context of the present invention, the term "first layer" is used interchangeably with "bottom layer" or "base coat", and the term "second layer" is used interchangeably with "top layer" or "top coat". The first layer is deposited on at least a portion of the substrate, and the second layer is deposited on at least a portion of the first layer.
[0024] The term "three-way conversion catalyst" refers to a catalyst that simultaneously promotes a) the reduction of nitrogen oxides to nitrogen and oxygen; b) the oxidation of carbon monoxide to carbon dioxide; and c) the oxidation of unburned hydrocarbons to carbon dioxide and water.
[0025] The term "NOx" refers to nitrogen oxide compounds, such as NO and / or NO2.
[0026] As used herein, the term "washcoat" has its ordinary meaning in the art, i.e., a thin, adherent coating of a catalytic material or other material applied to a substrate material. Typically, washcoats are formed by preparing a slurry of particles containing a certain solid content (e.g., 15 wt %-60 wt %) in a liquid vehicle, then coating the slurry on a substrate and drying to provide a washcoat layer.
[0027] The hydrothermal stability of the catalyst can be functionally defined as maintaining sufficient catalytic function after high temperature aging. Specifically, in this context, hydrothermal stability means that the catalyst should have lower and / or comparable NO after aging treatment with 10% steam at a temperature in the range of 950°C to 1050°C for about 5 hours. x and hydrocarbon ignition temperature.
[0028] As used herein, the term "stream" refers broadly to any combination of flowing gases that may contain solid or liquid particulate matter.
[0029] As used herein, the terms "upstream" and "downstream" refer to the relative directions of flow of engine exhaust gas from the engine to the tailpipe, with the engine being in the upstream position and the tailpipe and any pollutant abatement articles such as filters and catalysts being downstream of the engine.
[0030] The present invention focuses on solving the problem of platinum sintering under high temperature hydrothermal aging conditions. The solution proposed by the present invention is to stabilize the platinum dispersion and thereby effectively use platinum in TWC catalysts.
[0031] Catalyst composition :
[0032] The present invention provides a catalyst composition in a first aspect, the catalyst composition comprising a catalyst composition, the catalyst composition comprising:
[0033] a) platinum; and
[0034] b) at least one composite material,
[0035] Wherein platinum is loaded on the composite material,
[0036] The composite materials include:
[0037] i) cerium dioxide (calculated as CeO2) in an amount of 5.0 wt% to 50 wt%, based on the total weight of the composite material;
[0038] ii) aluminum oxide in an amount of 10 wt % to 80 wt % based on the total weight of the composite material (in
[0039] Al2O3 calculation); and
[0040] iii) magnesium oxide (calculated as MgO) in an amount of 10 to 80 wt.%, based on the total weight of the composite material.
[0041] Preferably, the total amount of cerium dioxide (calculated as CeO2); aluminum oxide (calculated as Al2O3); and magnesium oxide (calculated as MgO) is 80 wt% to 100 wt%, based on the total weight of the composite material.
[0042] Preferably, the amount of the composite material is from 80 wt% to 100 wt% of the total weight of the catalyst composition.
[0043] platinum:
[0044] Preferably, the total amount of platinum loaded on the composite material is in the range of 0.1 wt % to 10 wt % relative to the total weight of the composite material. More preferably, the total amount of platinum loaded on the composite material is in the range of 0.1 wt % to 5.0 wt % relative to the total weight of the composite material. Even more preferably, the total amount of platinum loaded on the composite material is in the range of 0.1 wt % to 3.0 wt % relative to the total weight of the composite material.
[0045] Carrier material :
[0046] The "support" in a catalytic material or catalyst composition or catalyst support coating refers to a material that receives metals (eg, PGMs), stabilizers, promoters, binders, etc. by precipitation, association, dispersion, impregnation or other suitable methods.
[0047] Composite Materials
[0048] The support material used to support platinum is a composite material comprising ceria, alumina and magnesium oxide.
[0049] The term "composite material" may refer to a mixture of oxides. Different metal oxides may be present in the mixture as different metal oxides in the form of solid solutions (also referred to as composite oxides), or may be present in the mixture as a mixture comprising different metal oxides, solid solutions and these two materials, each of which is in its different chemical and physical state, while interacting through their interface. In a preferred embodiment, the XRD results show that the catalyst composition has mixed CeO2, MgO, Al2O3 and MgAl2O4 phases. In a preferred embodiment, the composite material may be a bulk mixture, or there may be one or more separate oxides on the surface. An example is by CeO2 being deposited on the surface of the Mg / Al oxide and surface-modified.
[0050] The term "solid solution (or composite metal oxide)" refers to a mixed metal oxide containing oxygen anions and at least two different metal cations in a lattice structure. An example of a solid solution is spinel, in which Al 3+ and Mg 2+ Contained in a lattice structure.
[0051] Preferably, the composite material comprises a dopant selected from lanthanum oxide, titanium oxide, hafnium oxide, calcium oxide, strontium oxide, barium oxide, zirconium oxide or oxides of yttrium, praseodymium, neodymium, iron or any combination thereof.
[0052] Alumina :
[0053] The term "alumina" refers to either stable alumina or unstable alumina. Stable alumina and unstable alumina may exist in different phase transformations.
[0054] Preferably, the stable alumina comprises Al2O3 and one or more dopants selected from rare earth metal oxides, basic metal oxides, alkaline earth metal oxides, silicon dioxide or any combination of the foregoing substances. Preferred dopants are lanthanum oxide (La2O3), cerium oxide (CeO2), zirconium oxide (ZrO2), barium oxide (BaO), neodymium oxide (Nd2O3), strontium oxide (SrO), a combination of lanthanum oxide and zirconium oxide, a combination of barium oxide and lanthanum oxide, a combination of barium oxide, lanthanum oxide and neodymium oxide, or a combination of cerium oxide and zirconium oxide. Dopants can impart different properties to alumina. Dopants can delay undesirable phase changes of alumina, can stabilize surface regions, can introduce defect sites and / or change the acidity of the alumina surface. Dopant metals can be incorporated into the crystal structure of Al2O3 in cationic form to form a composite oxide, can be deposited on the surface of Al2O3 in oxidized form, or can exist as a blend of a mixture of both dopants and Al2O3 in oxidized form on a microscopic scale.
[0055] Exemplary stable aluminas and unstable aluminas may include macroporous boehmite, gamma-alumina, or delta / theta alumina. Available commercial aluminas include activated aluminas, such as high bulk density gamma-alumina, low or medium bulk density macroporous gamma-alumina, or low bulk density macroporous boehmite and gamma-alumina. Alumina materials are generally considered to impart durability to the resulting catalyst. High surface area alumina supports, also known as "gamma alumina" or "activated alumina," typically exhibit a BET surface area of more than 60 square meters per gram ("m2") of fresh material. 2 / g”), often up to about 300m 2 / g or more. Preferably, the BET surface area of the alumina is about 100 m 2 / g to about 150m 2 / g range. Activated alumina is generally a mixture of γ alumina phase and δ alumina phase, but may also contain a large amount of η alumina phase, κ alumina phase and θ alumina phase. Preferably, the alumina (calculated as Al2O3) in the composite material is present in an amount of 10 wt% to 80 wt%. More preferably, the alumina (calculated as Al2O3) in the composite material is present in an amount of 12 wt% to 32 wt%, based on the total weight of the composite material.
[0056] Cerium Oxide :
[0057] The term "cerium dioxide" refers to cerium oxide with a fluorite structure. Cerium oxide is preferably present as nanoparticles and / or cerium oxide crystallites. Cerium dioxide can be doped on the surface of an alumina-containing support by methods commonly used for catalyst preparation. The most commonly used preparation method is to impregnate a cerium precursor onto a support material using an incipient wetness technique, in which a cerium salt solution such as cerium nitrate is applied to the support material. After drying and calcining, the cerium material is converted into crystalline cerium oxide particles. Another cerium precursor is a colloidal cerium dioxide dispersion, typically as an aqueous suspension. Colloidal cerium dioxide can be purchased from commercial sources, and the average particle size of cerium dioxide in the colloidal suspension is typically between 5.0 nm and 100 nm. The average particle size of cerium dioxide on the final catalyst can be determined by X-ray diffraction (XRD) spectroscopy.
[0058] Colloidal suspension can be applied to support material in a manner similar to cerium salt solution. Because colloidal cerium oxide suspension has a specific average particle size, the final cerium oxide size on the catalyst after the calcination step is more predictable and can be better controlled. Cerium oxide doping and platinum deposition on the support can be carried out sequentially (for example, first cerium oxide, followed by platinum) or in one step (that is, co-impregnation). Preferably, the cerium oxide present in the composite material exists in the form of nanoparticles. More preferably, the cerium oxide present in the composite material has a particle size within the range of 5.0nm to 100nm. The average particle size of cerium oxide on the final catalyst can be measured by X-ray diffraction (XRD) spectrometry.
[0059] In a preferred embodiment, the ceria in the composite material is at least partially loaded on aluminum oxide, magnesium oxide, or loaded on both aluminum oxide and magnesium oxide. Based on the gross weight of the composite material, the amount of ceria (with CeO2calculated) in the composite material is 5.0 wt % to 50 wt %. Preferably, based on the gross weight of the composite material, the amount of ceria (with CeO2calculated) in the composite material is 20 wt % to 40 wt %.
[0060] Magnesium oxide :
[0061] The term "magnesium oxide" refers to magnesium oxide. The magnesium oxide in the composite material can be a bulk mixture of magnesium oxide and aluminum oxide prepared by coprecipitation of a magnesium and aluminum mixed salt solution, or is present on the surface of aluminum oxide. For a carrier with a high magnesium oxide / aluminum oxide ratio (e.g., 50:50), a bulk mixture is the only possibility. Magnesium oxide / aluminum oxide mixture carriers can be easily commercially available. Typically, by XRD measurement, the mixture has two different crystalline phases (magnesium oxide and aluminum oxide). If the magnesium oxide / aluminum oxide mixture is exposed to high temperature (>800°C), it can form a third phase magnesium aluminate (MgAl2O4), which is a spinel structure and can be easily identified by XRD. Based on the gross weight of the composite material, the amount of magnesium oxide (calculated as MgO) in the composite material is 10% to 80% by weight. Preferably, based on the gross weight of the composite material, the amount of magnesium oxide (calculated as MgO) in the composite material is 35% to 65% by weight.
[0062] The amount of oxide in the composite material
[0063] Based on the total weight of the composite material, the amount of cerium dioxide (calculated as CeO2) in the composite material is 5.0 wt% to 50 wt%. Preferably, based on the total weight of the composite material, the amount of cerium dioxide (calculated as CeO2) in the composite material is 20 wt% to 40 wt%. More preferably, based on the total weight of the composite material, the amount of cerium dioxide (calculated as CeO2) is 25 wt% to 35 wt%.
[0064] According to the present invention, the amount of aluminum oxide (calculated as Al2O3) in the composite material is 10 wt% to 80 wt% based on the total weight of the composite material. Preferably, the amount of aluminum oxide (calculated as Al2O3) in the composite material is 12 wt% to 32 wt% based on the total weight of the composite material.
[0065] According to the present invention, the amount of magnesium oxide (calculated as MgO) in the composite material is 10 wt % to 80 wt % based on the total weight of the composite material. Preferably, the amount of magnesium oxide (calculated as MgO) in the composite material is 35 wt % to 65 wt % based on the total weight of the composite material.
[0066] In the composite material, the weight ratio of magnesium oxide (calculated as MgO) to aluminum oxide (calculated as Al2O3) is preferably 1:4 to 4:1. More preferably, the weight ratio of magnesium oxide (calculated as MgO) to aluminum oxide (calculated as Al2O3) is 7:3.
[0067] In the composite material, a weight ratio of cerium oxide (calculated as CeO 2 ) to aluminum oxide (calculated as Al 2 O 3 ) is preferably in the range of 0.6 to 3.3.
[0068] The amount of the composite material is 80 wt % to 100 wt % based on the total weight of the catalyst composition.
[0069] Preparation of catalyst composition :
[0070] According to another aspect of the invention currently claimed for protection, a method for preparing the catalyst composition described herein above is also provided. The method includes mixing magnesium oxide and aluminum oxide to obtain a first composite material comprising magnesium oxide and aluminum oxide. In the next step, ceria is impregnated on the first composite material to obtain a second composite material. Finally, platinum is impregnated on the second composite material and then calcined to obtain a catalyst composition. The ceria used to prepare the catalyst composition is a cerium oxide nanoparticle or a cerium oxide microcrystal with a fluorite structure. Preferably, the ceria used is a colloidal ceria with an average particle size in the range of 10nm to 80nm. Alternatively, the method for preparing the catalyst composition includes mixing magnesium oxide and aluminum oxide to obtain a composite material comprising magnesium oxide and aluminum oxide, and then ceria and platinum are co-impregnated on the composite material and calcined to obtain a catalyst composition.
[0071] Catalytic products
[0072] According to another aspect of the presently claimed invention, there is provided a catalytic article wherein the catalyst composition described herein above is deposited on a substrate.
[0073] The catalyst composition comprises a) platinum; and b) at least one composite material, wherein platinum is supported on the composite material, wherein the composite material comprises: based on the total weight of the composite material, cerium dioxide (calculated as CeO2) in an amount of 5 wt% to 50 wt%; based on the total weight of the composite material, aluminum oxide (calculated as Al2O3) in an amount of 10 wt% to 80 wt%; and magnesium oxide (calculated as MgO) in an amount of 10 wt% to 80 wt% based on the total weight of the composite material. The composite material preferably comprises a dopant selected from lanthanum oxide, titanium oxide, hafnium oxide, calcium oxide, strontium oxide, barium oxide, zirconium oxide or oxides of yttrium, praseodymium, neodymium, iron or any combination thereof.
[0074] The total amount of platinum loaded on the composite material is in the range of 0.1 wt% to 10 wt% relative to the total weight of the composite material. Preferably, the amount of platinum loaded on the composite material is in the range of 0.1 wt% to 5.0 wt% relative to the total weight of the composite material.
[0075] Preferably, the ceria in the composite material is in the form of nanoparticles having an average particle size in the range of 5.0 nm to 100 nm.
[0076] Preferably, the amount of cerium dioxide (calculated as CeO2) in the composite material is 20 wt% to 40 wt% based on the total weight of the composite material.
[0077] Preferably, the amount of aluminum oxide (calculated as Al2O3) in the composite material is 12 to 32 wt% based on the total weight of the composite material. Preferably, the amount of magnesium oxide (calculated as MgO) in the composite material is 35 to 65 wt% based on the total weight of the composite material.
[0078] In the composite material, the weight ratio of magnesium oxide (calculated as MgO) to aluminum oxide (calculated as Al2O3) is preferably 1:4 to 4:1. More preferably, in the composite material, the weight ratio of magnesium oxide (calculated as MgO) to aluminum oxide (calculated as Al2O3) is 7:3.
[0079] The weight ratio of cerium dioxide (calculated as CeO2) to aluminum oxide (calculated as Al2O3) is in the range of 0.6 to 3.3.
[0080] In a preferred embodiment, the catalytic article is a monolayer catalytic article. That is, the catalyst composition described herein above is deposited on the substrate as a monolayer or single washcoat. Preferably, the washcoat coating covers 90% to 100% of the substrate surface. More preferably, the washcoat covers 95% to 100% of the substrate surface, and even more preferably, the washcoat covers the entire accessible surface of the substrate. The term "accessible surface" refers to the surface of the substrate that can be covered by conventional coating techniques used in the field of catalyst preparation (such as impregnation techniques).
[0081] In another preferred embodiment, the catalytic article is a two-layer article comprising a first layer; a second layer; and a substrate.
[0082] First floor :
[0083] The first layer (first washcoat) is deposited on at least a portion of the substrate. Preferably, the first washcoat coating covers 90% to 100% of the substrate surface. More preferably, the first washcoat covers 95% to 100% of the substrate surface, and even more preferably, the first washcoat covers the entire accessible surface of the substrate.
[0084] The first layer comprises a catalyst composition according to the presently claimed invention and optionally palladium. Preferably, the platinum loading is 5.0 gm / ft 3 Up to 200gm / ft 3 Preferably, the composite material has a loading of 0.5 gm / in 3 Up to 4gm / in 3 Preferably, the palladium loading is 5.0 gm / ft 3Up to 200gm / ft 3 .
[0085] Second floor :
[0086] The second layer (second washcoat) is deposited on at least a portion of the first layer, on at least a portion of the substrate, or on both. Preferably, the second washcoat coating covers 90% to 100% of the surface of the first layer. More preferably, the second washcoat covers 95% to 100% of the surface of the first layer, and even more preferably, the second washcoat covers the entire accessible surface of the first layer.
[0087] The second layer contains rhodium. Preferably, the rhodium loading is 1.0 gm / ft 3 Up to 40gm / ft 3 .
[0088] Alternatively, the first layer may comprise rhodium; and the second layer comprises the catalyst composition according to the presently claimed invention and optionally palladium.
[0089] Still alternatively, the first layer comprises a catalyst composition according to the presently claimed invention and optionally palladium; and the second layer comprises rhodium and a catalyst composition according to the presently claimed invention.
[0090] Partition structure :
[0091] The single-layer or double-layer catalytic article preferably has a partitioned structure. The partitioned structure includes a first zone and a second zone. The first zone, the second zone, or both contain a catalyst composition according to the invention claimed in the present invention.
[0092] The two-layer article preferably comprises a first layer and a second layer, wherein the first layer, the second layer or both have a partitioned structure, wherein the partitioned structure comprises a first zone and a second zone, wherein the first zone, the second zone or both comprise a catalyst composition according to the presently claimed invention.
[0093] In the context of the present invention, the term "first zone" may be used interchangeably with "inlet zone" or "front zone", and the term "second zone" may be used interchangeably with "outlet zone" or "rear zone". The terms "first zone" and "second zone" also describe the relative positioning of the catalytic article in the direction of flow, and the relative positioning of the catalytic article when placed in an exhaust gas treatment system, respectively. The first zone will be positioned upstream, while the second zone will be positioned downstream. The first zone covers at least some portion of the substrate from the inlet of the substrate, while the second zone covers at least some portion of the substrate from the outlet of the substrate. The inlet of the substrate is the first end that receives the flow of the engine exhaust gas flow from the engine, and the outlet of the substrate is the second end from which the treated exhaust gas flow exits.
[0094] Preferably, the first and second zones together cover 50% to 100% of the length of the substrate. More preferably, the first and second zones together cover 90% to 100% of the length of the substrate, and even more preferably, the first and second zones together cover the entire length of the substrate.
[0095] Preferably, the first zone covers 10% to 90% of the entire substrate length from the inlet, and the second zone covers 90% to 10% of the entire substrate length from the outlet, while the first zone and the second zone together cover 20% to 100% of the substrate length. More preferably, the first zone covers 20% to 80% of the entire substrate length from the inlet, and the second zone covers 80% to 20% of the entire substrate length from the outlet, while the first zone and the second zone together cover 40% to 100% of the substrate length. Even more preferably, the first zone covers 30% to 70% of the entire substrate length from the inlet, and the second zone covers 70% to 30% of the entire substrate length from the outlet, while the first zone and the second zone together cover 60% to 100% of the substrate length. Even most preferably, the first zone covers 40% to 50% of the entire substrate length from the inlet, and the second zone covers 50% to 60% of the entire substrate length from the outlet, while the first zone and the second zone together cover 90% to 100% of the substrate length.
[0096] Substrate :
[0097] The substrate of the catalytic article of the presently claimed invention may be composed of any material commonly used to prepare automotive catalysts. In a preferred embodiment, the substrate is a ceramic substrate, a metal substrate, a ceramic foam substrate, or a woven fiber substrate. Preferably, the substrate is a ceramic or metal monolithic honeycomb structure.
[0098] The substrate provides a plurality of wall surfaces onto which a washcoat comprising the catalyst composition described herein above is applied and adhered, thereby serving as a support for the catalyst composition.
[0099] Preferred metal substrates include heat-resistant metals and metal alloys, such as titanium and stainless steel, and other alloys in which iron is a substantial component or a major component. Such alloys may contain one or more nickel, chromium and / or aluminum, and the total amount of these metals may advantageously account for at least 15% by weight of the alloy. For example, 10% to 25% by weight of chromium, 3% to 8% by weight of aluminum, and up to 20% by weight of nickel. The alloy may also contain a small amount or trace amount of one or more metals, such as manganese, copper, vanadium, titanium, etc. The surface of the metal substrate may be oxidized at high temperatures (e.g., 1000° C. and higher) to form an oxide layer on the substrate surface, thereby improving the corrosion resistance of the alloy and promoting adhesion of the washcoat layer to the metal surface.
[0100] Preferred ceramic materials for constructing the substrate may include any suitable refractory material, for example, cordierite, mullite, cordierite-alumina, silicon nitride, zircon-mullite, spodumene, alumina-silica magnesia, zirconium silicate, sillimanite, magnesium silicate, zircon, petalite, alumina, aluminosilicates, and the like.
[0101] Any suitable substrate can be used, such as a monolithic flow-through substrate having a plurality of fine parallel gas flow channels extending from the inlet face of the substrate to the outlet face so that the channel is open to allow fluid to flow. The channel, which is essentially a straight path from the inlet to the outlet, is defined by a wall, and the walls are coated with a catalytic material as a carrier coating so that the gas flowing through the channel contacts the catalytic material. The flow channels of the monolithic substrate are thin-walled channels, which are in any suitable cross-sectional shape, such as trapezoidal, rectangular, square, sinusoidal, hexagonal, elliptical, circular, etc. Such structures contain about 60 to about 1200 or more gas inlet openings (i.e., "cells") per square inch of cross section (cpsi), more typically about 300 cpsi to 900 cpsi. The wall thickness of the flow-through substrate can vary, with a typical range of between 0.002 inches and 0.1 inches. A representative commercially available flow-through substrate is a cordierite substrate with 400 cpsi and 6 mil wall thickness or 600 cpsi and 4 mil wall thickness. However, it should be understood that the present invention is not limited to specific substrate types, materials or geometric shapes. In an alternative embodiment, the substrate can be a wall-flow substrate, wherein each channel is blocked with a non-porous plug at one end of the substrate body, wherein the alternating channels are blocked at the opposite end faces. This requires gas flow to reach the outlet through the porous wall of the wall-flow substrate. Such monolithic substrates can contain up to about 700 or higher cpsi, such as about 100 cpsi to 400 cpsi, and more typically about 200 cpsi to about 300 cpsi. The cross-sectional shape of the cell can be as described above. The wall thickness of the wall-flow substrate is usually between 0.008 inch and 0.012 inch. Representative commercially available wall-flow substrates are composed of porous cordierite, examples of which have 300 cpsi and a wall thickness of 12 mils (1 mil = 0.001 inches), or 300 cpsi and a wall thickness of 10 mils, or 300 cpsi and a wall thickness of 8 mils, and a wall porosity between 40% and 70%. Other ceramic materials (such as aluminum titanate, silicon carbide, and silicon nitride) are also used as wall-flow filter substrates. However, it should be understood that the present invention is not limited to a specific substrate type, material, or geometry. It should be noted that in the case where the substrate is a wall-flow substrate, the catalyst composition, in addition to being disposed on the surface of the wall, can also penetrate into the pore structure of the porous wall (i.e., partially or completely blocking the pore openings). In one embodiment, the substrate has a flow-through ceramic honeycomb structure, a wall-flow ceramic honeycomb structure, or a metal honeycomb structure.
[0102] Fig. 7A and Figure 7B An exemplary substrate 2 is shown in the form of a flow-through substrate coated with a washcoat composition as described herein. Fig. 7A , the exemplary substrate 2 has a cylindrical shape and a cylindrical outer surface 4, an upstream end face 6, and a corresponding downstream end face 8 that is identical to the end face 6. The substrate 2 has a plurality of fine parallel gas flow channels 10 formed therein. Figure 7B As shown, the flow channel 10 is formed by the wall 12 and extends through the substrate 2 from the upstream end face 6 to the downstream end face 8, and the channel 10 is unobstructed to allow a fluid (e.g., airflow) to flow longitudinally through the substrate 2 via its airflow channel 10. Figure 7B As can be more easily seen in the figure, the size and configuration of the wall 12 are such that the airflow channel 10 has a substantially regular polygonal shape. As shown, if desired, the washcoat composition can be applied in multiple, distinct layers. In the illustrated embodiment, the washcoat consists of a discrete first washcoat layer 14 adhered to the wall 12 of the substrate member and a second discrete second washcoat layer 16 coated on top of the first washcoat layer 14. In one embodiment, the presently claimed invention is also practiced with two or more (e.g., 3 or 4) washcoat layers and is not limited to the illustrated two-layer embodiment.
[0103] Figure 8 An exemplary substrate 2 is shown in the form of a wall flow filter substrate coated with a washcoat layer composition as described herein. Figure 8 As shown, the exemplary substrate 2 has a plurality of channels 52. These channels are tubularly surrounded by the inner wall 53 of the filter substrate. The substrate has an inlet end 54 and an outlet end 56. Alternating channels are plugged with inlet plugs 58 at the inlet end and plugged with outlet plugs 60 at the outlet end to form a relative checkerboard pattern at the inlet 54 and outlet 56. The gas flow 62 enters through the unblocked channel inlet 64, is blocked by the outlet plug 60, and diffuses to the outlet side 66 through the channel wall 53 (which is porous). The gas cannot return to the inlet side of the wall due to the inlet plug 58. The porous wall flow filter used in the present invention is catalyzed because the wall of the element has or contains one or more catalytic materials. The catalytic material may be present alone on the inlet side of the element wall, alone on the outlet side, on both the inlet side and the outlet side, or the wall itself may be composed of catalytic material in whole or in part. The present invention includes the use of one or more layers of catalytic material on the inlet and / or outlet wall of the element.
[0104] Preparation of catalytic products :
[0105] According to another aspect of the presently claimed invention, there is also provided a method for preparing a catalytic article according to the presently claimed invention. The method comprises preparing a first slurry comprising a catalyst composition according to the presently claimed invention; and depositing the first slurry on a substrate, followed by calcining at a temperature in the range of 400° C. to 700° C. The obtained catalytic article is a single layer.
[0106] Preferably, the double-layer catalytic article is prepared by a method comprising the following steps: preparing a first slurry comprising a catalyst composition according to the presently claimed invention and optionally palladium, preparing a second slurry comprising rhodium; depositing the first slurry on a substrate to obtain a first layer, followed by calcining at a temperature in the range of 400°C to 700°C; and depositing the second slurry on the first layer to obtain a second layer, followed by calcining at a temperature in the range of 400°C to 700°C.
[0107] Preferably, the double-layer catalytic article is prepared by a method comprising the following steps: preparing a first slurry comprising a catalyst composition according to the presently claimed invention and palladium; preparing a second slurry comprising rhodium and the catalyst composition according to the presently claimed invention; depositing the first slurry on a substrate to obtain a first layer, followed by calcining at a temperature in the range of 400°C to 700°C; and depositing the second slurry on the first layer to obtain a second layer, followed by calcining at a temperature in the range of 400°C to 700°C.
[0108] Preferably, the dual-layer catalytic article is prepared by a method comprising the following steps: preparing a first slurry comprising a catalyst composition according to the presently claimed invention and optionally palladium; preparing a second slurry comprising rhodium; depositing the second slurry on a substrate to obtain a first layer, followed by calcining at a temperature in the range of 400°C to 700°C; and depositing the first slurry on the first layer to obtain a second layer, followed by calcining at a temperature in the range of 400°C to 700°C.
[0109] The preparation of the catalytic article involves impregnating a support material in particulate form with an active metal solution, such as a palladium, platinum and / or rhodium precursor solution. As used herein, "impregnated" or "impregnation" refers to the penetration of the catalytic material into the porous structure of the support material. Techniques for performing the impregnation or preparing the slurry include the incipient wetness impregnation technique (A); the co-precipitation technique (B) and the co-impregnation technique (C).
[0110] The incipient wetness impregnation technique, also known as capillary impregnation or dry impregnation, is commonly used to synthesize heterogeneous materials, i.e., catalysts. Typically, a metal precursor is dissolved in an aqueous or organic solution, and the metal-containing solution is then added to a catalyst support that contains a pore volume equal to the volume of solution added. Capillary action draws the solution into the pores of the support. The volume of the added solution exceeding the pores of the support causes the transport of the solution to shift from a capillary action process to a much slower diffusion process. The catalyst is dried and calcined to remove the volatile components in the solution, depositing the metal on the surface of the catalyst support. The concentration profile of the impregnated material depends on the mass transfer conditions in the pores during impregnation and drying.
[0111] The support particles are typically dried enough to absorb substantially all of the solution to form a wet solid. An aqueous solution of a water-soluble compound or complex of an active metal is typically utilized, such as rhodium chloride, rhodium nitrate (e.g., Rh(NO)3 and its salts), rhodium acetate, or a combination thereof (where rhodium is the active metal); palladium nitrate, palladium tetraamine, palladium acetate, or a combination thereof (where palladium is the active metal); and platinum nitrate, platinum tetraamine nitrate, platinum acetate, or a combination thereof, where platinum is the active metal. After the support particles are treated with the active metal solution, the particles are dried, such as by heat treating the particles at an elevated temperature (e.g., 100°C-150°C) for a period of time (e.g., 1 hour-3 hours), and then calcined to convert the active metal to a more catalytically active form. An exemplary calcination method involves heat treatment in air at a temperature of about 400°C-550°C for 10 minutes to 3 hours. The above method may be repeated as needed to achieve the desired level of active metal impregnation.
[0112] Substrate coating :
[0113] The catalyst composition as described above is usually prepared in the form of catalyst particles as described above. These catalyst particles are mixed with water to form a slurry to coat a catalyst substrate such as a honeycomb substrate. In addition to the catalyst particles, the slurry may optionally contain a binder, an associative thickener and / or a surfactant (including anionic, cationic, nonionic or amphoteric surfactants) in the form of aluminum oxide, silicon dioxide, zirconium acetate, zirconium oxide or zirconium hydroxide. Other exemplary binders include boehmite, γ-alumina or δ / θ alumina and silica sol. When present, the binder is usually used in an amount of about 1.0 wt %-5.0 wt % of the total carrier coating loading. Acidic or alkaline substances are added to the slurry to adjust the pH accordingly. For example, in some embodiments, the pH of the slurry is adjusted by adding ammonium hydroxide, aqueous nitric acid solution or acetic acid. The typical pH range of the slurry is about 3.0 to 12.
[0114] The slurry may be ground to reduce particle size and enhance particle mixing. The grinding is done in a ball mill, a continuous mill or other similar equipment, and the solid content of the slurry may be, for example, about 20 wt% to 60 wt%, more specifically about 20 wt% to 40 wt%. In one embodiment, the grinding slurry is characterized by D 90 The particle size is about 3.0 microns to about 40 microns, preferably 10 microns to about 30 microns, and more preferably about 10 microns to about 15 microns. Use a dedicated particle size analyzer to determine D 90 The equipment used in this example uses laser diffraction to measure particle size in small volumes of slurry. Typically, D 90 In micrometers it is meant that 90% of the particles by number have a diameter smaller than this value.
[0115] The slurry is coated on the catalyst substrate using any carrier coating technology known in the art. In one embodiment, the catalyst substrate is dipped in the slurry or otherwise coated with the slurry one or more times. Thereafter, the coated substrate is dried for a period of time (e.g., 10 minutes-3.0 hours) at an elevated temperature (e.g., 100°C-150°C), and then calcined by, for example, heating at 400°C-700°C, typically for about 10 minutes to about 3 hours. After drying and calcining, the final carrier coating coating is considered to be substantially free of solvent. After calcining, the catalyst loading obtained by the above-mentioned carrier coating technology can be determined by calculating the difference between the coated and uncoated weights of the substrate. As is apparent to those skilled in the art, the catalyst loading can be modified by changing the slurry rheology. In addition, the coating / drying / calcining process of producing the carrier coating can be repeated as needed to construct the coating to the desired loading level or thickness, which means that more than one carrier coating may be applied.
[0116] Emission treatment system :
[0117] In another aspect of the present invention, an exhaust treatment system for an internal combustion engine is also provided, the system comprising the catalytic product described above. The system may include a catalytic product according to the invention currently claimed and an additional platinum group metal three-way conversion (TWC) catalytic product. The catalytic product of the present invention can be placed in a close-coupled position. The close-coupled catalysts are placed close to the engine so that they can reach the reaction temperature as quickly as possible. Typically, the close-coupled catalysts are placed within three feet of the engine, more specifically, within one foot of the engine, and even more specifically, less than six inches from the engine. The close-coupled catalysts are typically directly connected to the exhaust manifold. Since the close-coupled catalysts are close to the engine, they are required to be stable at high temperatures.
[0118] The catalytic articles of the present invention may also be used as part of an integrated exhaust system that includes one or more additional components for treating exhaust emissions.
[0119] For example, the exhaust system, also referred to as an emission treatment system, may also include a close-coupled TWC catalyst, an underfloor catalyst, a catalyzed soot filter (CSF) component, and / or a selective catalytic reduction (SCR) catalytic article. The preceding list of components is merely illustrative and should not be considered limiting the scope of the invention.
[0120] In another aspect of the invention, there is also provided a method for treating a gaseous exhaust stream comprising hydrocarbons, carbon monoxide and nitrogen oxides, the method comprising contacting the exhaust stream with a catalytic article according to the invention or an exhaust gas treatment system according to the invention.
[0121] The present invention also provides a method for reducing the levels of hydrocarbons, carbon monoxide and nitrogen oxides in a gaseous exhaust stream, the method comprising contacting the gaseous exhaust stream with a catalytic article according to the present invention or an exhaust gas treatment system according to the present invention to reduce the levels of hydrocarbons, carbon monoxide and nitrogen oxides in the exhaust gas.
[0122] In another aspect of the present invention, there is also provided the use of a catalytic article or an exhaust gas treatment system according to the presently claimed invention for purifying a gaseous exhaust stream comprising hydrocarbons, carbon monoxide and nitrogen oxides.
[0123] The present invention is further illustrated by the following embodiments. The features of each of these embodiments may be combined with any other embodiment where appropriate and practical.
[0124] Implementation 1 :
[0125] A catalyst composition comprising a) platinum; and b) at least one composite material, wherein the platinum is loaded on the composite material, wherein the composite material comprises: cerium dioxide (calculated as CeO2) in an amount of 5.0 wt% to 50 wt% based on the total weight of the composite material; aluminum oxide (calculated as Al2O3) in an amount of 10 wt% to 80 wt% based on the total weight of the composite material; and magnesium oxide (calculated as MgO) in an amount of 10 wt% to 80 wt% based on the total weight of the composite material.
[0126] Implementation 2 :
[0127] The catalyst composition according to Embodiment 1, wherein the cerium oxide is in the form of nanoparticles having an average particle size ranging from 5.0 nm to 100 nm.
[0128] Implementation 3 :
[0129] The catalyst composition according to any one of Embodiments 1-2, wherein the weight ratio of magnesium oxide (calculated as MgO) to aluminum oxide (calculated as Al2O3) is 1:4 to 4:1.
[0130] Implementation 4 :
[0131] The catalyst composition according to any one of Embodiments 1-3, wherein the weight ratio of magnesium oxide (calculated as MgO) to aluminum oxide (calculated as Al2O3) is 7:3.
[0132] Implementation 5 :
[0133] A catalyst composition according to any one of embodiments 1-4, wherein the total amount of platinum supported on the composite material is in the range of 0.1 wt% to 10 wt% relative to the total weight of the composite material.
[0134] Implementation 6 :
[0135] A catalyst composition according to any of embodiments 1-5, wherein the composite material comprises a dopant selected from lanthanum oxide, titanium oxide, hafnium oxide, calcium oxide, strontium oxide, barium oxide, zirconium oxide, or oxides of yttrium, praseodymium, neodymium, iron, or any combination thereof.
[0136] Implementation Plan 7 :
[0137] A catalyst composition according to any one of embodiments 1-6, wherein the amount of cerium oxide (calculated as CeO2) is 20 wt% to 40 wt% based on the total weight of the composite material.
[0138] Implementation 8 :
[0139] A catalyst composition according to any of Embodiments 1-7, wherein the amount of aluminum oxide (calculated as Al2O3) is 12 wt% to 32 wt% based on the total weight of the composite material.
[0140] Implementation Plan 9 :
[0141] A catalyst composition according to any one of embodiments 1-8, wherein the amount of magnesium oxide (calculated as MgO) is 35 wt% to 65 wt% based on the total weight of the composite material.
[0142] Implementation 10 :
[0143] A catalyst composition according to any one of embodiments 1-9, wherein the weight ratio of cerium dioxide (calculated as CeO2) to aluminum oxide (calculated as Al2O3) is in the range of 0.6 to 3.3.
[0144] Implementation Plan 11 :
[0145] A catalyst composition according to any of Embodiments 1-10, wherein the amount of the composite material is 80 wt% to 100 wt% of the total weight of the catalyst composition.
[0146] Implementation Plan 12 :
[0147] A catalyst composition according to any one of embodiments 1-11, wherein the total amount of cerium dioxide (calculated as CeO2); aluminum oxide (calculated as Al2O3); and magnesium oxide (calculated as MgO) is 80 wt% to 100 wt% based on the total weight of the composite material.
[0148] Implementation 13 :
[0149] A catalytic article comprising the catalyst composition according to any one of Embodiments 1 to 12 deposited on a substrate.
[0150] Implementation Plan 14 :
[0151] A catalytic article according to embodiment 13, wherein the catalytic article is a single layer catalytic article.
[0152] Implementation Plan 15 :
[0153] A catalytic article according to embodiment 13, wherein the catalytic article is a two-layer article, the two-layer article comprising a first layer; a second layer; and a substrate, wherein the first layer is deposited on at least a portion of the substrate, and the second layer is deposited on at least a portion of the first layer, on at least a portion of the substrate, or on both, wherein the first layer comprises the catalyst composition according to any one of embodiments 1 to 12 and optionally palladium, and wherein the second layer comprises rhodium.
[0154] Implementation Plan 16 :
[0155] A catalytic article according to embodiment 13, wherein the catalytic article is a two-layer article, the two-layer article comprising a first layer; a second layer; and a substrate, wherein the first layer is deposited on at least a portion of the substrate, and the second layer is deposited on at least a portion of the first layer, on at least a portion of the substrate, or on both, wherein the first layer comprises rhodium, and wherein the second layer comprises the catalyst composition according to any one of embodiments 1 to 12 and optionally palladium.
[0156] Implementation Plan 17 :
[0157] A catalytic article according to embodiment 13, wherein the catalytic article is a two-layer article, the two-layer article comprising a first layer; a second layer; and a substrate, wherein the first layer is deposited on at least a portion of the substrate, and the second layer is deposited on at least a portion of the first layer, on at least a portion of the substrate, or on both, wherein the first layer comprises the catalyst composition according to any one of claims 1 to 12 and palladium, and wherein the second layer comprises rhodium and the catalyst composition according to any one of embodiments 1 to 12.
[0158] Implementation Plan 18 :
[0159] A catalytic article according to any one of embodiments 13 to 14, wherein the catalytic article has a partitioned structure, wherein the partitioned structure includes a first zone and a second zone, wherein the first zone, the second zone, or both comprise the catalyst composition according to any one of embodiments 1 to 12.
[0160] Implementation Plan 19 :
[0161] A catalytic article according to any one of embodiments 15 to 17, wherein the catalytic article is a two-layer article including a first layer and a second layer, wherein the first layer, the second layer or both have a partitioned structure, wherein the partitioned structure includes a first zone and a second zone, wherein the first zone, the second zone or both contain the catalyst composition according to any one of embodiments 1 to 12.
[0162] Implementation Plan 20 :
[0163] The catalytic article according to any one of embodiments 13 to 19, wherein the substrate is selected from a ceramic substrate, a metal substrate, a ceramic foam substrate, a polymer foam substrate, or a woven fiber substrate.
[0164] Various aspects of the presently claimed invention are more fully illustrated by the following examples, which are set forth for the purpose of illustrating certain aspects of the invention and are not to be construed as limiting the invention.
[0165] Example 1: Catalyst composition
[0166] Table 1 lists the catalyst samples and their composition information.
[0167] The following five support materials are used to prepare various catalysts:
[0168] 1.Al2O3 is γ-alumina without MgO.
[0169] 2. Mg20 is a support material containing about 20 wt% MgO and about 80 wt% Al2O3.
[0170] 3. Mg30 is a support material containing about 30 wt% MgO and about 70 wt% Al2O3.
[0171] 4. Mg70 is a support material containing about 70 wt% MgO and about 30 wt% Al2O3.
[0172] 5. MgO is 100% MgO without any Al2O3.
[0173] Table 1: Catalyst samples
[0174] Sample No. Sample description Pt% <![CDATA[CeO2%]]> <![CDATA[CeO2 precursor]]> Carrier 1 <![CDATA[1.7Pt / Al2O3]]> 1.7 0 NA <![CDATA[Al2O3]]> 2 1.7Pt / Mg70 1.7 0 NA Mg70 3 1.7Pt_17Ce(20) / Mg70 1.7 17 <![CDATA[Colloidal CeO2 (20nm)]]> Mg70 4 1.7Pt_26Ce(20) / Mg70 1.7 26 <![CDATA[Colloidal CeO2 (20 nm)]]> Mg70 5 1.7Pt_34Ce(20) / Mg70 1.7 34 <![CDATA[Colloidal CeO2 (20 nm)]]> Mg70 6 1.7Pt_51Ce(20) / Mg70 1.7 51 <![CDATA[Colloidal CeO2 (20 nm)]]> Mg70 7 1.7Pt_34Ce / Mg70 1.7 34 Ce Nitrate Mg70 8 1.7Pt / 34Ce(20) / Mg70 1.7 34 <![CDATA[Colloidal CeO2 (20 nm)]]> Mg70 9 34Ce(20)_1.7Pt / Mg70 1.7 34 <![CDATA[Colloidal CeO2 (20 nm)]]> Mg70 10 1.7Pt_34Ce(80) / Mg70 1.7 34 <![CDATA[Colloidal CeO2 (80nm)]]> Mg70 11 <![CDATA[1Pt / Al2O3]]> 1 0 NA <![CDATA[Al2O3]]> 12 <![CDATA[1Pt-20Ce / Al2O3]]> 1 20 Cerium nitrate <![CDATA[Al2O3]]> 13 1Pt / Mg20 1 0 NA Mg20 14 1Pt / Mg30 1 0 NA Mg30 15 1Pt-20Ce / Mg30 1 20 Cerium nitrate Mg30 16 1Pt / Mg70 1 0 NA Mg70 17 1Pt-20Ce / Mg70 1 20 Cerium nitrate Mg70 18 1Pt / MgO 1 0 NA MgO 19 1Pt-20Ce / MgO 1 20 Cerium nitrate MgO
[0175] *The amount of carrier is the amount required to achieve 100% replenishment.
[0176] Sample preparation :
[0177] Samples 1, 2, 11, 13, 14, 16 and 18 were prepared by impregnating platinum nitrate solution on the support (Al2O3, Mg20, Mg30, Mg70 or MgO) using the incipient wetness impregnation technique. The impregnated samples were calcined at 550°C in air for 2 hours.
[0178] Samples 3-6 were prepared by sequentially impregnating a (first) colloidal CeO suspension (average diameter of CeO particles was about 20 nm) and a (second) platinum nitrate solution on a Mg70 support. After the first impregnation, the resulting material was dried at 120° C. for 15 minutes. After the second impregnation, the sample was calcined at 550° C. in air for 2 hours.
[0179] Sample 7 was prepared by sequentially impregnating a (first) Ce nitrate solution and a (second) platinum nitrate solution on a Mg70 support. After the first impregnation, the resulting material was dried at 120° C. for 15 minutes. After the second impregnation, the sample was calcined at 550° C. in air for 2 hours.
[0180] Sample 8 was prepared by sequentially impregnating a (first) colloidal CeO suspension (average diameter of CeO particles was about 20 nm) and a (second) platinum nitrate solution on a Mg70 support. After the first impregnation, the resulting material was calcined at 550° C. in air for 2 hours. After the second impregnation, the sample was again calcined at 550° C. in air for 2 hours.
[0181] Sample 9 was prepared by sequentially impregnating a (first) platinum nitrate solution and a (second) colloidal CeO2 suspension (average diameter of CeO2 particles was about 20 nm) on a Mg70 support. After the first impregnation, the resulting material was dried at 120°C for 15 minutes. After the second impregnation, the sample was again calcined in air at 550°C for 2 hours.
[0182] Sample 10 was prepared by sequentially impregnating a (first) colloidal CeO suspension (average diameter of CeO particles was about 80 nm) and a (second) platinum nitrate solution on a Mg70 support. After the first impregnation, the resulting material was dried at 120° C. for 15 minutes. After the second impregnation, the sample was calcined at 550° C. in air for 2 hours.
[0183] Samples 12, 15, 17, and 19 were prepared by co-impregnation of a mixed solution of platinum nitrate and cerium nitrate on a support (Al2O3, Mg30, Mg70, or MgO). The impregnated samples were calcined at 550°C in air for 2 hours.
[0184] Catalyst aging conditions :
[0185] Prior to activity evaluation, all catalysts were aged at 950°C with 10% H2O in air for 5 hours.
[0186] Catalyst evaluation conditions :
[0187] Two types of test runs (continuous heating and constant temperature) were performed for each sample. For the first run, the catalyst was tested by continuously heating from 100°C to 500°C at a heating rate of 10°C / min and maintaining at 500°C for 30 minutes. For the second run, a steady-state test was performed with a temperature step of 25°C from 125°C to 500°C and maintaining at each temperature for 15 minutes. Both tests used the same feed gas, which contained 1.5% CO, 0.5% H2, 667ppm C3H6, 333ppm C3H8, 1500ppm NO, 14% CO2, 10% H2O, 1.4% O2 and was balanced with Ar. The feed gas was equivalent to stoichiometric conditions, i.e., λ=1. The weight hourly space velocity for all tests was maintained at 400,000mL / (g cat .h). The outlet gas composition is measured by infrared spectroscopy (IR) and / or mass spectroscopy (MS).
[0188] result :
[0189] The second run data was used for activity comparison. The results are shown in Figures 1 to 6.
[0190] As shown in Figure 1, increasing CeO2 loading increases TWC activity to some extent. The HC conversion is highest when CeO2 loading is 26 wt%-34 wt%. Further increasing CeO2 loading to 51% leads to an activity lower than the maximum but still higher than that of the catalyst with 17% CeO2 or the Ce-free catalyst. x The optimal CeO2 loading was found to be 34%.
[0191] Figure 2 compares the change of TWC activity with the preparation method. The preparation method has a complex effect on the conversion rates of HC, NO x and CO. Calcination between the impregnation steps results in the lowest conversion rates of CO, NO x and HC. Without intermittent calcination, first Ce impregnation and then Pt impregnation result in higher activity of the catalyst towards HC and NO x , but not high activity towards CO. On the other hand, impregnation in the reverse order results in better activity of the catalyst towards HC and CO, but not high activity towards NO x .
[0192] Figure 3 shows the influence of the CeO2 precursor (Ce nitrate relative to colloidal CeO2) and the particle size (colloidal CeO2) on the TWC activity. It is found that sample 5 is the most active catalyst, followed by sample 10. The activity of the catalyst prepared with Ce nitrate - sample 7 is lower than that of the catalyst prepared with colloidal CeO2, and even worse than sample 2.
[0193] Figure 4 shows the activation of samples 5, 7 and 10. The sample activation is carried out by reduction treatment with 10% H2 in Ar at 250 °C for 1 hour. The activation treatment has various promoting effects on the conversion rates of CO, NO x and HC of these samples. The most significant activation effect is found on the aged sample 7. After activation, the most active catalyst is sample 5.
[0194] Figure 5 shows that the Pt catalyst supported on Mg70 (sample 16) is more active towards HC and NO compared to the Pt catalysts supported on Al2O3, Mg20, Mg30 or MgO.
[0195] Figure 6 shows that sample 17 (1Pt - 20Ce / Mg70) is more active towards the conversion rates of NO and HC compared to samples 12 or 15 (Al2O3 or Mg30 supported catalysts). The MgO supported catalyst (sample 19) has comparable activity to sample 17 in terms of HC conversion rate, but has lower activity towards NO conversion rate.
[0196] The specific surface area and average crystallite size of the sample catalysts were also evaluated. The results are shown in Table 2:
[0197] Table 2: BET surface area a and CeO2 crystallite size of fresh and aged catalysts ( D ) b
[0198]
[0199] a Calculated by using the BET method, based on the adsorption isotherm in the pressure interval of 0.05 < P / P0 < 0.3.b The XRD results were used to determine the CeO2(111) peak using the FWHM according to the Scherrer equation.
[0200] Table 2 shows the specific surface areas of samples 5, 7 and 10 and the average CeO2 crystallite size of both fresh and aged samples measured by XRD. The average CeO2 crystallite size of the fresh catalyst decreases in the order of sample 10 > sample 5 > sample 7. For each catalyst, aging increases the CeO2 crystallite size by 2 to 5 times.
[0201] The average CeO2 crystallite size of samples 12, 15 and 17 before and after aging is shown in Table 3:
[0202] Table 3: Average CeO2 crystallite size of fresh and aged catalysts ( D )
[0203]
[0204] a The XRD results were used to determine the CeO2(111) peak using the FWHM according to the Scherrer equation.
[0205] For the fresh samples, the CeO2 crystallite size follows the order of sample 12 > sample 15 > sample 17. That is, the CeO2 size decreases with the increase of MgO content on the support. After aging, the CeO2 size of all samples increases significantly, and the order of CeO2 crystallite size becomes sample 17 > sample 12 > sample 15.
[0206] The X-ray diffraction patterns of fresh Mg30 and Mg70 supports and the X-ray diffraction patterns of aged Mg30 and Mg70 supports are shown in Fig. 9 Aged at 950°C with 10% H2O in air for 5 hours.
[0207] Fig. 9 It is shown that: i) the fresh Mg30 sample is a mixture of layered binary hydroxide (LDH) phase and g-alumina phase. There is no obvious boundary between the two phases, ii) the aged Mg30 sample is a mixture of MgAl2O4 spinel phase and MgO phase, and there is no alumina phase in the aged Mg30, iii) the fresh Mg70 sample has a LDH phase with a clear boundary, iv) the aged Mg70 sample is a mixture of MgAl2O4 phase and MgO phase. There is no alumina phase in the aged Mg70.
[0208] The X-ray diffraction patterns of Mg30-550 and Mg70-550 as well as the aged samples of Mg30-550 and Mg70-550 are shown in Fig.10The Mg30-550 and Mg70-550 materials were calcined at 550°C for 2 hours in air. The Mg30-550 was aged and the Mg70-550 was aged at 950°C with 10% H2O in air for 5 hours.
[0209] Fig.10 It is shown that: i) the Mg30-550 sample is a mixture of MgO phase and g-Al2O3 phase, ii) the Mg70-550 sample has a major MgO phase and a minor g-Al2O3 phase, iii) the Mg30-550 aged sample consists of MgAl2O4 phase and a trace amount of MgO phase, iv) the Mg70-550 aged sample consists of MgAl2O3 phase and MgO phase, and v) there is no alumina phase in any of the aged samples.
[0210] FIG. 11 shows X-ray diffraction patterns of a fresh Pt catalyst (A) and an aged Pt catalyst (B).
[0211] For fresh samples, the following observations were found:
[0212] -1Pt-20Ce / Mg30 sample contains CeO2 phase and MgAl2O4 phase, and no g-
[0213] Al2O3 phase.
[0214] The -1Pt-20Ce / Mg70 sample contained CeO2 phase and MgO phase, and no g-Al2O3 phase was detected.
[0215] -1Pt-20Ce / Al2O3 sample contains CeO2 phase and g-Al2O3 phase.
[0216] - No crystalline Pt was detected on all fresh samples.
[0217] For the aged samples, the following observations were found:
[0218] The aged sample of -1Pt-20Ce / Mg30 contains CeO2 phase and MgAl2O4 phase, but no Al2O3 phase.
[0219] Pt was detected.
[0220] -1Pt-20Ce / Mg70 aged sample contains CeO2 phase, MgO phase and MgAl2O4 phase, but no Al2O3 phase. Pt was detected.
[0221] -1Pt-20Ce / Al2O3 aged sample contains CeO2 phase and g-Al2O3 phase. Pt was detected.
[0222] - The Pt diffraction peak (2θ = about 40°) with the highest intensity was found on the 1Pt20Ce / Al2O3 aged sample, which indicates that the average Pt crystallite size is the largest among the three aged samples.
[0223] Although the embodiments disclosed herein have been described with reference to specific embodiments, it should be understood that these embodiments are merely illustrative of the principles and applications of the invention currently claimed. It will be apparent to those skilled in the art that various modifications and variations may be made to the methods and apparatus of the invention currently claimed without departing from the spirit and scope of the invention currently claimed. Therefore, the invention currently claimed is intended to include modifications and variations within the scope of the appended claims and their equivalents, and the embodiments described above are presented for purposes of illustration and not limitation.
Claims
1. A catalyst composition, comprising: a) platinum; and b) at least one composite material, wherein platinum is loaded on the composite material, The composite material comprises: i. Based on the total weight of the composite material, 5.0 wt % to 50 wt % of cerium dioxide (as CeO 2 calculate); ii. Aluminum oxide (in terms of Al2O3) in an amount of 10% to 80% by weight based on the total weight of the composite material. 2 O 3 calculation); and iii. magnesium oxide (calculated as MgO) in an amount of 10 wt% to 80 wt%, based on the total weight of the composite material.
2. The catalyst composition according to claim 1, wherein the cerium dioxide is in the form of nanoparticles having an average particle size ranging from 5.0 nm to 100 nm.
3. The catalyst composition according to any one of claims 1 to 2, wherein the magnesium oxide (calculated as MgO) and the aluminum oxide (calculated as Al 2 O 3 The weight ratio (calculated) is 1:4 to 4:
1.
4. The catalyst composition according to any one of claims 1 to 3, wherein the magnesium oxide (calculated as MgO) and the aluminum oxide (calculated as Al 2 O 3 The weight ratio of the two groups is 7:
3.
5. The catalyst composition according to any one of claims 1 to 4, wherein the total amount of platinum supported on the composite material is in the range of 0.1 wt% to 10 wt% relative to the total weight of the composite material.
6. The catalyst composition according to any one of claims 1 to 5, wherein the composite material comprises a dopant selected from lanthanum oxide, titanium oxide, hafnium oxide, calcium oxide, strontium oxide, barium oxide, zirconium oxide or oxides of yttrium, praseodymium, neodymium, iron or any combination thereof.
7. The catalyst composition according to any one of claims 1 to 6, wherein the cerium dioxide (as CeO 2 % to 40% by weight).
8. The catalyst composition according to any one of claims 1 to 7, wherein the aluminum oxide (as Al 2 O 3 % to 32% by weight).
9. The catalyst composition according to any one of claims 1 to 8, wherein the magnesium oxide (calculated as MgO) in the composite material is present in an amount of 35 wt% to 65 wt%, based on the total weight of the composite material.
10. The catalyst composition according to any one of claims 1 to 9, wherein the cerium dioxide (as CeO 2 Calculated) and alumina (calculated as Al 2 O 3 The weight ratio (calculated) is in the range of 0.6 to 3.
3.
11. The catalyst composition according to any one of claims 1 to 10, wherein the amount of the composite material is 80 wt% to 100 wt% of the total weight of the catalyst composition.
12. A method for preparing a catalyst composition according to any one of claims 1 to 11, wherein the method comprises mixing magnesium oxide and aluminum oxide to obtain a first composite material comprising magnesium oxide and aluminum oxide; impregnating ceria on the first composite material to obtain a second composite material; and impregnating platinum on the second composite material, followed by calcination to obtain the catalyst composition.
13. The method of claim 12, wherein the ceria is colloidal ceria having an average particle size in the range of 10 nm to 80 nm.
14. A method for preparing a catalyst composition according to any one of claims 1 to 11, said method include: - mixing magnesium oxide and aluminum oxide to obtain a composite material comprising magnesium oxide and aluminum oxide; as well as - Co-impregnation of ceria and platinum on the composite material followed by calcination to obtain the catalyst composition.
15. A catalytic article wherein the catalyst composition according to any one of claims 1 to 11 is deposited on a substrate.
16. The catalytic article according to claim 15, wherein the catalytic article is a monolayer catalytic article, wherein the catalyst composition according to any one of claims 1 to 11 is deposited as a monolayer on the substrate.
17. The catalytic article of claim 15, wherein the catalytic article is a two-layer article, the two-layer article include: a) First layer; b) Second layer; and c) substrate, wherein the first layer is deposited on at least a portion of the substrate, and the second layer is deposited on at least a portion of the first layer, at least a portion of the substrate, or both, wherein the first layer comprises the catalyst composition according to any one of claims 1 to 10 and optionally palladium, Wherein the second layer comprises rhodium.
18. The catalytic article of claim 15, wherein the catalytic article is a two-layer article, the two-layer article include: a) First layer; b) second layer; and c) substrate, wherein the first layer is deposited on at least a portion of the substrate, and the second layer is deposited on at least a portion of the first layer, at least a portion of the substrate, or both, wherein the first layer comprises rhodium, Wherein the second layer comprises the catalyst composition according to any one of claims 1 to 10 and optionally palladium.
19. The catalytic article of claim 15, wherein the catalytic article is a two-layer article, the two-layer article include: a) First layer; b) second layer; and c) substrate, wherein the first layer is deposited on at least a portion of the substrate, and the second layer is deposited on at least a portion of the first layer, at least a portion of the substrate, or both, wherein the first layer comprises the catalyst composition according to any one of claims 1 to 11 and palladium, Wherein the second layer comprises rhodium and the catalyst composition according to any one of claims 1 to 11.
20. The catalytic article of any one of claims 15 to 16, wherein the catalytic article has a partitioned structure, wherein the partitioned structure includes a first zone and a second zone, wherein the first zone, the second zone, or both contain the catalyst composition of any one of claims 1 to 11.
21. The catalytic article according to any one of claims 17 to 19, wherein the catalytic article is a two-layer article comprising a first layer and a second layer, wherein the first layer, the second layer or both have a partitioned structure, wherein the partitioned structure comprises a first zone and a second zone, wherein the first zone, the second zone or both contain the catalyst composition according to any one of claims 1 to 11.
22. The catalytic article of any one of claims 15 to 21, wherein the substrate is selected from a ceramic substrate, a metal substrate, a ceramic foam substrate, or a woven fiber substrate.
23. A method for preparing a catalytic article according to any one of claims 15 to 16, wherein the method include: - preparing a first slurry comprising a catalyst composition according to any one of claims 1 to 11; as well as - depositing the first slurry on the substrate followed by calcination at a temperature ranging from 400°C to 700°C.
24. A method for preparing the catalytic article of claim 17, wherein the method include: - Preparing a first slurry comprising the catalyst composition according to any one of claims 1 to 11 and optionally palladium. - preparing a second slurry comprising rhodium; - depositing the first slurry on the substrate to obtain a first layer, followed by calcination at a temperature ranging from 400° C. to 700° C.; as well as - depositing the second slurry on the first layer to obtain a second layer, followed by calcination at a temperature ranging from 400°C to 700°C.
25. A method for preparing the catalytic article of claim 18, wherein the method include: - preparing a first slurry comprising a catalyst composition according to any one of claims 1 to 11 and optionally palladium; - preparing a second slurry comprising rhodium; - depositing the second slurry on the substrate to obtain a first layer, followed by calcination at a temperature ranging from 400° C. to 700° C.; as well as - depositing the first slurry on the first layer to obtain a second layer, followed by calcination at a temperature ranging from 400°C to 700°C.
26. A method for preparing the catalytic article of claim 19, wherein the method include: - preparing a first slurry comprising a catalyst composition according to any one of claims 1 to 11 and palladium; - preparing a second slurry comprising rhodium and a catalyst composition according to any one of claims 1 to 11; - depositing the first slurry on the substrate to obtain a first layer, followed by calcination at a temperature ranging from 400° C. to 700° C.; as well as - depositing the second slurry on the first layer to obtain a second layer, followed by calcination at a temperature ranging from 400°C to 700°C.
27. An exhaust gas treatment system for an internal combustion engine, the system comprising the catalytic article according to any one of claims 15 to 22.
28. A method of treating a gaseous exhaust stream comprising hydrocarbons, carbon monoxide, nitrogen oxides and particulates, the method comprising contacting the exhaust stream with a catalytic article according to any one of claims 15 to 22 or an exhaust treatment system according to claim 27.
29. A method of reducing the levels of hydrocarbons, carbon monoxide and nitrogen oxides in a gaseous exhaust stream, the method comprising contacting the gaseous exhaust stream with a catalytic article according to any one of claims 15 to 22 or an exhaust treatment system according to claim 27 to reduce the levels of hydrocarbons, carbon monoxide and nitrogen oxides in the exhaust gas.
30. Use of a catalytic article according to any one of claims 15 to 22 or an exhaust gas treatment system according to claim 27 for purifying a gaseous exhaust stream comprising hydrocarbons, carbon monoxide and nitrogen oxides.
Citation Information
Patent Citations
Catalyst materials for NO oxidation
CN105188919A
Coke oven gas ammonia decomposition catalyst and preparation method thereof
CN108031474A
Lean-burn NOx trapping catalyst of diesel engine exhaust purifying system and preparation method of lean-burn NOx trapping catalyst
CN109603823A
Catalyst for reducing nitrogen oxide content in wast gas of impoverished burning engine