Polyurethane urea and preparation method thereof
Through the reaction of modified PolyTHF with diisocyanate and chain extender, polyurethane urea fiber with low modulus, high elongation and good heat resistance is prepared, which solves the problems in modulus and elongation of polyurethane urea fiber in the existing technology. It meets the high performance needs of textiles and non-textiles by eliminating deficiencies in efficiency and heat resistance.
Patent Information
- Application Number
- CN202380026358.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-10
- Filing Date
- 2023-03-02
- Publication Date
- 2024-10-29
AI Technical Summary
Existing polyurethaneurea fibers suffer from deficiencies in low modulus, high elongation and heat resistance, resulting in compromised functionality and aesthetics in textile and non-textile applications.
By using modified PolyTHF to react with diisocyanate and chain extender, combined with a chain terminator, a polyurethane urea fiber or film with low modulus, high elongation and good heat resistance is prepared. The specific steps include making m-PolyTHF React with diisocyanate to form a prepolymer, add a chain extender and a chain terminator to the prepolymer, and then spin or cast to prepare fibers or membranes.
It achieves low modulus, high elongation and high elastic recovery rate of polyurethaneurea fiber, and maintains good heat resistance under high temperature conditions, making it suitable for diversified downstream applications.
Smart Images

Figure BDA0005033729690000091 
Figure BDA0005033729690000101 
Figure BDA0005033729690000111
Abstract
Description
Technical Field
[0001] The present invention relates to a polyurethaneurea and a method for preparing the same. The present invention further relates to a polyurethaneurea fiber or film having low modulus, high elongation and good heat resistance produced from modified PolyTHF, isocyanate, chain extender and, if appropriate, chain terminator. Background Art
[0002] Commercial polyurethaneurea fibers, i.e., spandex fibers, are produced by a process comprising the steps of: a) reacting a polymeric diol or polyol with an isocyanate to form a polyurethane prepolymer; and b) then reacting the polyurethane prepolymer with a chain extender, (if appropriate) a chain terminator, and further additives to form a polyurethaneurea.
[0003] Polyurethane urea fibers with excellent elasticity are widely used in the field of textiles, such as sportswear, general clothing and stockings, and non-textiles, such as sanitary products. Diversified downstream applications have put forward higher requirements on both the comfort and appearance of elastic fabrics. On the one hand, lower modulus, higher elongation and higher elastic recovery are required to make elastic fabrics easier to stretch and reduce restrictions on the human body. On the other hand, since polyurethane urea fibers need to be interwoven, dyed and shaped with polyester, nylon, cotton, etc., where the dyeing temperature of polyester is about 130°C and the dry setting temperature is higher than 160°C, excellent heat resistance is also required. If the heat resistance of polyurethane urea fibers is not high enough, the function and appearance of the fabrics prepared from polyurethane urea fibers will be affected.
[0004] US 5000899A discloses a low modulus polyurethaneurea fiber using a copolymer diol of tetrahydrofuran and 3-methyltetrahydrofuran as the soft segment of the material, which improves the heat setting properties of the fiber. However, the heat resistance of the fiber is sacrificed.
[0005] US20070117951A discloses a low modulus spandex prepared from a copolymer of tetrahydrofuran and ethylene oxide having a high molecular weight, however, the spandex exhibits a high residual deformation.
[0006] US20090182113A discloses polyurethane urea produced by the following steps: a) reacting a polymeric diol with a substance that can react therewith to form an OH-terminated prepolymer; b) reacting the OH-terminated prepolymer with a diisocyanate to form an isocyanate-terminated prepolymer; c) reacting the isocyanate-terminated prepolymer with a chain extender, and optionally a chain terminator and an additive to form a polyurethane urea; and d) spinning the polyurethane urea to form a fiber. However, the heat resistance of the fiber is not disclosed.
[0007] CN 101555634A discloses a method for improving the heat resistance of polyurethane urea fibers by increasing the proportion of hard segment components 4,4'-methylene diphenyl diisocyanate (4,4'-MDI) or 1,2-ethylenediamine. CN 1310991C discloses a method for improving the heat resistance of polyurethane urea fibers by introducing polyols with aromatic functional groups. However, these documents do not disclose low modulus fibers. Generally speaking, increasing the proportion of hard segments leads to reduced elongation and increased modulus. In addition, increasing the proportion of hard segments also reduces the solubility of polyurethane urea fibers in dimethylacetamide or dimethylformamide solvents.
[0008] Therefore, there is a need to provide polyurethaneureas with low modulus, high elongation, and good elastic recovery and heat resistance. Summary of the invention
[0009] The object of the present invention is to provide a polyurethane urea having low modulus, high elongation and good elastic recovery and heat resistance.
[0010] Another object of the present invention is to provide a method for producing the polyurethane urea of the present invention from modified PolyTHF, diisocyanate, chain extender and chain terminator.
[0011] It has been unexpectedly found that the above objects can be achieved by the following embodiments: DETAILED DESCRIPTION
[0012] Unless defined otherwise, all technical and scientific terms used herein have the meaning commonly understood by one of ordinary skill in the art to which the invention belongs. As used herein, the following terms have the meanings ascribed to them below unless otherwise indicated.
[0013] The undefined articles "a," "an," and "the" refer to one or more of the species specified by the term following the article.
[0014] m-PolyTHF, which stands for modified PolyTHF, refers to polyester alcohol derived from copolymerization of PolyTHF with dicarboxylic acid and / or its anhydride and / or its ester.
[0015] Mn, represents the number average molecular weight, in g / mol, which is tested according to ASTM E1899-2016.
[0016] Elongation at break (De) represents the stretching ratio when the specimen breaks.
[0017] Modulus, expressed as the stress of a specimen at 300% elongation, is measured in MPa.
[0018] The strength retention rate represents the stress retained by the specimen after heat treatment at 300% tension, compared to the stress value before heat treatment at 300% tension.
[0019] Elastic recovery rate (RER%): The recovery rate of the sample after repeated stretching.
[0020] Energy loss factor (b5), energy loss of the specimen after repeated stretching to 300% elongation.
[0021] In the context of the present disclosure, any specific values mentioned for features (including specific values mentioned as endpoints in ranges) can be recombined to form new ranges.
[0022] Further embodiments of the invention can be seen from the claims, the description and the examples.It will be understood that the features of the subject matter of the invention which remain to be elucidated hereinafter can be used not only in the combination indicated but also in other combinations without departing from the scope of the invention.
[0023] One aspect of the present invention relates to a polyurethane urea, wherein its De is higher than 500%, its modulus is less than 10 MPa, its strength retention is higher than 80%, its RER% is higher than 85%, and its b5 is less than 15.
[0024] In a preferred embodiment, the De of the polyurethaneurea of the present invention is higher than 650%, preferably higher than 700%, more preferably higher than 750%.
[0025] In a preferred embodiment, the modulus of the polyurethaneurea of the present invention is less than 9 MPa, preferably less than 8 MPa, more preferably less than 7.5 MPa.
[0026] In a preferred embodiment, the strength retention rate of the polyurethane urea of the present invention is higher than 85%, preferably higher than 90%.
[0027] In a preferred embodiment, the RER% of the polyurethaneurea of the present invention is higher than 90%.
[0028] In a preferred embodiment, the b5 of the polyurethane urea of the present invention is less than 13, preferably less than 12.
[0029] One embodiment of the present invention relates to a method for producing the polyurethane urea of the present invention, the method comprising:
[0030] a) m-PolyTHF is reacted with a diisocyanate to obtain a prepolymer.
[0031] b) adding a chain extender and optionally a chain terminator to the prepolymer to obtain a polyurethaneurea solution.
[0032] c) spinning or casting the solution obtained in step b) to obtain polyurethane urea.
[0033] In one embodiment, the m-PolyTHF used in the present invention can be prepared according to the method disclosed in US 2012 / 0059142A1. More specifically, the m-PolyTHF is prepared based on polytetrahydrofuran and dicarboxylic acid and / or its anhydride and / or its ester.
[0034] In a preferred embodiment, m-PolyTHF is prepared based on polytetrahydrofuran and an aromatic dicarboxylic acid and / or its anhydride and / or its ester. Preferably, the aromatic dicarboxylic acid is selected from isophthalic acid, phthalic acid, terephthalic acid and mixtures thereof; more preferably, the aromatic dicarboxylic acid is isophthalic acid.
[0035] The Mn of the m-PolyTHF used in the present invention is preferably in the range of 2000 to 4000 g / mol, preferably 2000 to 3500 g / mol.
[0036] The Mn of the polytetrahydrofuran used for preparing m-PolyTHF in the present invention is preferably in the range of 200 to 2000 g / mol, more preferably 200 to 1800 g / mol, most preferably 200 to 1500 g / mol.
[0037] The diisocyanate used in the above step a) can be any desired organic diisocyanate. Preferred diisocyanates include linear aliphatic isocyanates, such as 1,2-ethylene diisocyanate, 1,3-propylene diisocyanate, 1,4-butylene diisocyanate, 1,6-hexamethylene diisocyanate, 1,8-octamethylene diisocyanate, 1,5-diisocyanato-2,2,4-trimethylpentane, 3-oxo-1,5-pentane diisocyanate and mixtures thereof; alicyclic diisocyanates, such as isophorone diisocyanate, cyclopentane ... Hexane diisocyanate or mixtures thereof, preferably 1,4-cyclohexane diisocyanate, 4,4'-diisocyanato-dicyclohexylmethane (HMDI); and aromatic diisocyanates, such as 2,2'-, 2,4'- and 4,4'-diphenylmethane diisocyanate, mixtures of various monomeric diphenylmethane diisocyanates, 2,4- or 2,6-toluene diisocyanate (TDI) or mixtures thereof, naphthalene diisocyanate (NDI) or mixtures thereof. Particularly preferred diisocyanates are 4,4'-MDI, and 2,4- or 2,6-toluene diisocyanate, preferably 4,4'-MDI.
[0038] In another embodiment, the diisocyanate used in step a) is in excess. Preferably, the molar ratio of m-PolyTHF to diisocyanate is in the range of 1:1.2 to 1:3, more preferably 1:1.3 to 1:2. The reaction is initiated by mixing m-PolyTHF with diisocyanate at a temperature of 20°C to 120°C, preferably 50°C to 100°C, more preferably 70°C to 90°C. The reaction is preferably carried out in the absence of a solvent. When a solvent is used, preferably, the solvent is a polar aprotic solvent such as N,N-dimethylacetamide or N,N-dimethylformamide. The reaction is preferably carried out in the absence of a catalyst. When a catalyst is used, for example, phosphoric acid can be used at a concentration preferably of 50 to 200ppm based on the reaction mixture.
[0039] Useful chain extenders include compounds having two isocyanate-reactive hydrogen atoms and a molecular weight of less than 500 g / mol. For example, ethylenediamine, 1,2-propylenediamine, 1,3-propylenediamine, 1,4-butylenediamine, 1,5-diaminopentane, hydrazine, m-phenylenediamine, p-phenylenediamine, 1,4-cyclohexanediamine, 1,3-cyclohexanediamine, 1,3-diamine-4-methylcyclohexane, 1-amino-3-aminoethyl-3,5,5-trimethylcyclohexane (isophoronediamine), 1,1'-methylenebis(4,4'-diamino-hexane), toluenediamine, piperazine, ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butylenediol, 1,5-pentanediol, 1,6-hexanediol, or mixtures thereof can be used. Particularly preferred are diamines such as ethylenediamine, 1,2-propylenediamine, 1,3-propylenediamine, 1,4-butylenediamine, 1,5-diaminopentane, hydrazine, m-xylylenediamine, p-xylylenediamine, 1,4-cyclohexanediamine, 1,3-cyclohexanediamine, 1,3-diamine-4-methylcyclohexane, 1-amino-3-aminoethyl-3,5,5-trimethylcyclohexane (isophoronediamine), 1,1′-methylenebis(4,4′-diaminohexane) and mixtures thereof, particularly preferred are ethylenediamine, 1,2-propylenediamine and mixtures thereof.
[0040] In a preferred embodiment, the chain extender of the present invention further comprises an aromatic diamine as a co-chain extender, wherein the aromatic diamine has two hydrogen atoms that can react with isocyanate groups; preferably, the aromatic diamine is selected from toluenediamine, 1,3-m-phenylenediamine, 1,4-p-phenylenediamine, 4,4'-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 4,4'-diaminophenylsulfone, 1,4-naphthalenediamine, 1,5-naphthalenediamine, 1,6-naphthalenediamine or a mixture thereof. The molar ratio of the aromatic diamine to the aliphatic diamine is 2:98 to 50:50, preferably 2:98 to 40:60, more preferably 5:95 to 30:70, and most preferably 10:90 to 25:75.
[0041] In other embodiments, useful chain terminators include, for example, secondary amines, such as dimethylamine, dibutylamine, dicyclohexylamine; or primary amines, such as ethanolamine, or primary alcohols, such as n-butanol, alone or in the form of a mixture. Preferably, the chain terminator is a monofunctional amine.
[0042] In an embodiment, specific amines, such as diethylenetriamine or diethanolamine, are optionally used as long as the smooth production is not affected.
[0043] When a chain terminator and / or a specific amine are used together with a chain extender, the fraction of the chain extender(s) is preferably 85% by weight or more, and more preferably 90% by weight or more, based on the total weight of the chain extender, chain terminator and specific amine.
[0044] These chain terminators and specific amines can each be used alone, or together with a chain extender. By alone is meant that the components can be added simultaneously in various streams, or at different times.
[0045] The ratio of isocyanate groups to amine groups is preferably in the range of 1:1 to 1:1.15, more preferably 1:1 to 1:1.05.
[0046] The conversion of the prepolymer into the polyurethane urea of the invention preferably takes place in solution. Polar aprotic solvents can be used. Polar aprotic solvents are solvents which dissolve the prepolymer but are substantially unreactive with isocyanate groups. Examples of such solvents are N,N-dimethylacetamide, N,N-dimethylformamide, dimethyl sulfoxide, N-methylpyrrolidone and the like. Preference is given to using N,N-dimethylacetamide or N,N-dimethylformamide, particular preference is given to using N,N-dimethylacetamide. Preferably, the prepolymer, the chain extender, (if appropriate) the chain terminator and (if appropriate) the specific amine are dissolved in a solvent in each case and the resulting solutions are subsequently mixed with one another. Preferably, the corresponding solutions are added separately to the prepolymer solution. This can take place simultaneously or at different times. Alternatively, the solutions of the chain extender, the chain terminator and the specific amine can be mixed before being added to the prepolymer. The temperature at which the reaction takes place is preferably in the range of 0° C. to 80° C., more preferably 8° C. to 50° C., most preferably 10° C. to 35° C. Typically, all isocyanate-reactive materials are used in amounts such that the isocyanate-reactive groups (usually amino groups) are in small excess.
[0047] Subsequently, the fully reacted solution is spun to form fibers. Any spinning method in which the fibers according to the invention can be produced can be used. Such spinning methods are described, for example, in "Kunststoffhandbuch [Plastics Handbook], 7, Polyurethane [Polyurethane]", Carl Hanser Verlag, 3rd edition, 1993, Chapter 13.2. These spinning methods include dry spinning or wet spinning methods, preferably dry spinning methods. In the spinning method, a spinning solution containing the polyurethane urea of the invention is spun through a spinneret die to form a thread. For example, the polyurethane urea fiber of the invention is obtained by removing the spinning solution by drying or in a coagulation bath.
[0048] The polyurethane urea of the present invention may further comprise additives. Any additive known for segmented polyurethane urea fibers may be used herein. For example, matting agents, fillers, antioxidants, dyes, pigments, dye enhancers (e.g., Methacrol 2462B), and stabilizers that resist heat, light, UV radiation, chlorinated water, and smoke and air pollution such as NO or NO2 may be included. Examples of antioxidants, stabilizers that resist heat, light or UV radiation are stabilizers from the group of: sterically hindered phenols (e.g., Cyanox 1790), hindered amine light stabilizers, triazines, benzophenones and benzotriazoles. Examples of pigments and matting agents are titanium dioxide, magnesium stearate, silicone oils, zinc oxide and barium sulfate. Examples of dyes are acid dyes, disperse dyes and pigments and optical brighteners. Examples of stabilizers that resist fiber degradation caused by chlorine or chlorinated water are zinc oxide, magnesium oxide, or coated or uncoated aluminum hydroxycarbonate magnesium (e.g., hydrotalcite or calcite).
[0049] The polyurethaneurea according to the invention has advantageous properties in terms of De, modulus, strength retention, elastic recovery and energy loss. These advantageous properties are characterized using solution cast polyurethaneurea films. These films are obtainable by casting the polyurethaneurea solution on a planer plane and removing the solvent by drying.
[0050] The polyurethane ureas of the present invention can be used to produce spandex fibers for elastic textiles such as wovens, knitwear, and other textiles.
[0051] Preferably, the polyurethane urea spinning fluid of the present invention has a viscosity of 120,000 to 500,000 mPa·s, and a viscosity increase rate of less than 5,000 mPa·s / h.
[0052] The following examples further illustrate the present invention.
[0053] In the present invention, the testing methods of various characteristics are as follows:
[0054] For reasons of handling and reproducibility, the mechanical properties of the polyurethaneureas were measured on films. To this end, the prepared polyurethaneurea solutions were converted into films by casting the solutions onto precisely horizontally aligned glass plates and allowing them to dry at 50° C. in a slow N2 flow. The amount and concentration of the solution and the plate area were matched to one another in order to produce films with a thickness of about 0.20 to 0.26 mm.
[0055] The trends observed in the films are generally consistent with those in the fibers, and the effects of polymer chain orientation seen in the fibers and imparted by the spinning process are not reflected in the films. These differences do not detract from the spirit of the present invention.
[0056] De: The change in length of a polyurethane urea film sample of standard shape and size taken according to ISO37:2005 when the sample is broken after being stretched, expressed as % of the original length.
[0057] Modulus: Take a film sample of polyurethane urea of standard shape and size according to ISO37:2005, and test the stress of the sample at 300% elongation according to ISO37:2005, the unit is MPa.
[0058] Strength retention rate: Take a standard film sample of polyurethane urea according to ISO37:2005, place it in an oven at 175°C for 10 minutes, and test the 300% elongation stress according to ISO37:2005. Strength retention rate (%) = (300% elongation stress after heat treatment / 300% elongation stress before heat treatment) * 100.
[0059] RER%: Take a film sample of polyurethane urea of standard shape and size according to ISO37:2005, stretch the sample to 300% elongation 5 times according to DIN53835-2:1981, and then measure the length of the sample thereafter. RER%=(1-(fifth recovery length at 300% elongation-initial length) / (300% elongation length-initial length))*100.
[0060] b5: Take a polyurethaneurea film sample of standard shape and size according to ISO37:2005, and stretch the sample to 300% elongation 5 times according to DIN53835-2:1981. b5=(first 300% elongation stress-fifth 300% elongation stress) / first 300% elongation stress*100.
[0061] Examples
[0062] Materials used in the examples
[0063] M: MDI from BASF
[0064] DDM: 4,4'-diaminodiphenylmethane from BASF
[0065] DMAC: Dimethylacetamide from Sinopharm Group (SINOPHARM)
[0066] EDA: 1,2-ethylenediamine from BASF
[0067] DEA: Diethylamine from BASF
[0068] PPD: 1,4-p-phenylenediamine from Sigma-Aldrich
[0069] 245: CAS 36443-68-2 from BASF
[0070] 622: CAS 70198-29-7 from BASF
[0071] m-PolyTHF: modified based on the following procedure
[0072] m-PolyTHF-1 is m-PolyTHF prepared according to the procedure in Example 1 of US2012 / 0059143. 650 parts by weight of 20 ppm of tetrabutyl orthotitanate were catalyzed by gradually increasing the temperature to 220°C and reducing the pressure to 20 mbar to make 857 parts of 650 was reacted with 166 parts of isophthalic acid. When the acid value reached 1 mg KOH / g or less, the temperature was cooled to 200°C, 20 ppm by weight of 85% phosphoric acid was charged, and then further cooled, and the OH value of the obtained m-PolyTHF-1 was 36 mg KOH / g. m-PolyTHF-2 and m-PolyTHF-3 were prepared according to the same procedure as described above for m-PolyTHF-1, starting with The number average molecular weight Mn of and the corresponding Mn of m-PolyTHF are summarized in Table 1, both of which are tested according to ASTM E1899-2016.
[0073] Table 1m-PolyTHF material information
[0074]
[0075] Example 1
[0076] 200.00 parts by weight of m-PolyTHF-1 and 27.42 parts by weight of M was charged into a reactor purged with N2 and reacted at 80°C for 120 minutes to produce a prepolymer having an NCO% content of 1.66% by weight; the temperature was lowered to below 50°C, and the produced prepolymer was dissolved with 277.95 parts by weight of DMAC (referred to as DMAC-1 in Table 2). A solution of 2.27 parts by weight of EDA, 0.45 parts by weight of PPD, 0.72 parts by weight of DEA and 156.49 parts by weight of DMAC (referred to as DMAC-2 in Table 2) was charged into the diluted prepolymer solution by high-speed mixing to obtain a uniform polyurethaneurea solution.
[0077] Add 0.2% (by weight of polyurethane urea, the same below) heat stabilizer 245 and 0.1% UV stabilizer 622 was added to the doping part of the polyurethaneurea solution to obtain the polyurethaneurea spinning solution. The relevant properties of the obtained spinning solution were tested using a cast film, wherein the film thickness was controlled within 200±30 um, the same below.
[0078] Examples 2-6 and Comparative Example 1
[0079] A polyurethaneurea film was prepared in a similar manner to Example 1, except that the corresponding raw materials and the amounts thereof shown in Table 2 were used. The properties of the polyurethaneurea film thus obtained were tested according to the methods as described above, and the measurement results are summarized in Table 3.
[0080] Table 2: Raw material feed of Examples 1-6 and Comparative Example 1
[0081]
[0082] Remark:
[0083] Co-CE stands for co-chain extender
[0084] m-PolyTHF type: 1 represents m-PolyTHF-1, 2 represents m-PolyTHF-2, and 3 represents m-PolyTHF-3, as shown in Table 1.
[0085] Table 3: Film performance test results of Examples 1-6 and Comparative Example 1
[0086]
Claims
1. A polyurethane urea, wherein Its elongation at break (De) is higher than 500%, its modulus is less than 10MPa, its strength retention rate is higher than 80%, its elastic recovery rate RER% is higher than 85%, and its energy loss factor (b5) is less than 15, wherein the De, modulus and strength retention rate of the polyurethane urea are tested according to ISO37:2005.
2. The polyurethane urea according to claim 1, wherein De of the polyurethane urea of the present invention is higher than 650%, preferably higher than 700%, more preferably higher than 750%.
3. The polyurethane urea according to claim 1 or 2, having a modulus of less than 9 MPa, preferably less than 8 MPa, more preferably less than 7.5 MPa.
4. The polyurethane urea according to any one of claims 1 to 3, wherein The strength retention rate of the polyurethaneurea is higher than 85%, preferably higher than 90%.
5. The polyurethane urea according to any one of claims 1 to 4, wherein The RER% of the polyurethaneurea is higher than 90%.
6. The polyurethane urea according to any one of claims 1 to 5, wherein The energy loss factor (b5) of the polyurethaneurea is less than 13, preferably less than 12.
7. A method for producing a polyurethane urea according to any one of claims 1 to 6, comprising: a) reacting m-PolyTHF with a diisocyanate to obtain a prepolymer, b) adding a chain extender and optionally a chain terminator to the prepolymer to obtain a polyurethane urea spinning solution, c) spinning or casting the solution obtained in step b) to obtain the polyurethane urea.
8. The method according to claim 7, wherein: The m-PolyTHF used in step a) is obtained by condensation of polytetrahydrofuran with a dicarboxylic acid and / or its anhydride and / or its ester; preferably, the dicarboxylic acid is an aromatic dicarboxylic acid; more preferably, the dicarboxylic acid is isophthalic acid, phthalic acid, terephthalic acid or a mixture thereof; most preferably, the dicarboxylic acid is isophthalic acid.
9. The method according to claim 7 or 8, wherein: The Mn (number average molecular weight) of the polytetrahydrofuran is 200 to 2000 g / mol, preferably 200 to 1800 g / mol, most preferably 200 to 1500 g / mol.
10. The method according to any one of claims 7 to 9, wherein: The Mn of m-PolyTHF is 2000 to 4000 g / mol, preferably 2000 to 3500 g / mol.
11. The method according to any one of claims 7 to 10, wherein: The diisocyanate used in step a) comprises 4,4'-diisocyanate, preferably comprises more than 60% of 4,4'-diisocyanate, more preferably more than 80% of 4,4'-diisocyanate, most preferably more than 95% of 4,4'-diisocyanate.
12. The method according to any one of claims 7 to 11, wherein: The molar ratio of m-PolyTHF to diisocyanate is 1:1 to 1:3, preferably 1:1.2 to 1:3, more preferably 1:1.3 to 1:
2.
13. The method according to any one of claims 7 to 12, wherein: The chain extender comprises an aliphatic diamine having two hydrogen atoms that can react with isocyanate groups; preferably, the aliphatic diamine is selected from 1,2-ethylenediamine, 1,2-propylenediamine, 1,3-propylenediamine, 1,4-butylenediamine, 1,5-pentanediamine, 1,4-cyclohexanediamine and mixtures thereof; more preferably, the aliphatic diamine is 1,2-ethylenediamine.
14. The method according to any one of claims 7 to 13, wherein: The chain extender further comprises an aromatic diamine, wherein the aromatic diamine has two hydrogen atoms that can react with isocyanate groups; preferably, the aromatic diamine is selected from 1,4-phenylenediamine, toluenediamine, 1,3-m-phenylenediamine, 1,4-p-phenylenediamine, 4,4'-diphenylmethanediamine, 2,2-bis(4-aminophenyl)propane, 4,4'-diaminophenylsulfone, 1,4-naphthalenediamine, 1,5-naphthalenediamine, 1,6-naphthalenediamine or a mixture thereof.
15. The method according to any one of claims 7 to 14, wherein: The molar ratio of the aromatic diamine to the aliphatic diamine is 2:98 to 50:50; preferably 2:98 to 40:60, more preferably 5:95 to 30:70, most preferably 10:90 to 25:
75.
16. The method according to any one of claims 7 to 15, wherein: The chain terminator is an alkyl alcohol and / or diallylamine; preferably, the chain terminator is selected from n-butanol, cyclohexanol, ethanolamine, diethanolamine, N,N-diethylamine, N,N-dibutylamine or a mixture thereof.
Citation Information
Patent Citations
High temperature resistant chromophil polyurethane elastic fiber and preparation method thereof
CN101555634A
Improved spandex compositions
CN1310991C
Spandex from high molecular weight poly (tetramethylene-co-ethyleneether) glycols
US20070117951A1
Segmented polyurethane elastomers with high elongation at tear
US20090182113A1
Preparing polyester alcohols
US20120059142A1