Composition for phase difference film and single-layer phase difference material
By using a combination of side chain copolymers and organic solvents, and through photoreaction and heat treatment, a single-layer retardation material with a high NZ coefficient of 0.4 ≤ NZ ≤ 0.6 was successfully produced, solving the problem of prevention in the existing technology. The problem of insufficient external light reflection achieves efficient improvement of optical characteristics.
Patent Information
- Application Number
- CN202380025154.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-10
- Filing Date
- 2023-03-09
- Publication Date
- 2024-10-29
AI Technical Summary
When the existing retardation film is used for a circularly polarizing plate in an organic EL display device, the anti-reflection characteristics of external light in the oblique direction are insufficient, resulting in undesirable coloring problems, and it is difficult to produce it through a simple process with an NZ coefficient of 0.4 ≤ NZ ≤ 0.6 high phase difference materials.
Using a composition containing a specific side chain copolymer, the terminal carboxylic acid side chain of the photoreactive site and the side chain polymer with an aromatic ring structure of more than 2 rings are combined with an organic solvent and subjected to ultraviolet irradiation and heat treatment to form Highly efficient oriented single layer retardation material.
It achieves the production of high phase difference materials with NZ coefficients of 0.4≤NZ≤0.6, improves the optical anisotropy of the film, improves the anti-external light reflection effect in the oblique direction, and solves the problem of anti-external light reflection in the existing technology. Sufficient question.
Smart Images

Figure CN118871828A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a composition for phase difference film and a single-layer phase difference material. Specifically, it relates to a material having optical properties suitable for use in display devices, recording materials, etc., in particular, a liquid crystal polymer suitable for optical compensation films such as polarizing plates and phase difference plates of liquid crystal displays and organic EL (Electro Luminescence) display devices, a composition containing the polymer, and a single-layer phase difference material obtained from the composition. Background Art
[0002] In view of the requirements of improving the display quality and lightening of liquid crystal display devices and organic EL display devices, the requirements for polymer films with controlled internal molecular orientation structures as optical compensation films such as polarizing plates and phase difference plates are increasing. In order to meet this requirement, films using the optical anisotropy of polymerizable liquid crystal compounds have been developed. The polymerizable liquid crystal compounds used here are generally liquid crystal compounds having a polymerizable group and a liquid crystal structural part (a structural part having a spacer part and a liquid crystal unit (mesogen) part), and acrylic groups are widely used as the polymerizable group.
[0003] Such polymerizable liquid crystal compounds are usually polymerized by irradiation with radiation such as ultraviolet rays to form polymers (films). For example, the following methods are known: a specific polymerizable liquid crystal compound having an acrylic group is loaded between supports that have been oriented, and the compound is irradiated with radiation while being kept in a liquid crystal state to obtain a polymer (Patent Document 1); a photopolymerization initiator is added to a mixture of two polymerizable liquid crystal compounds having acrylic groups or a composition in which a chiral liquid crystal is mixed in the mixture, and ultraviolet rays are irradiated to obtain a polymer (Patent Document 2).
[0004] In addition, various single-layer coating type alignment films have been reported, such as alignment films obtained by using polymerizable liquid crystal compounds and polymers (Patent Documents 3 and 4) without requiring a liquid crystal alignment film, and alignment films obtained by using polymers containing photo-crosslinking sites (Patent Documents 5 and 6).
[0005] Organic EL panel has a reflective metal layer, which is prone to the problem of external light reflection. Therefore, it is known to prevent these problems by providing a circular polarizing plate composed of a linear polarizing plate and a phase difference plate (film). However, when the conventional phase difference plate is used for a circular polarizing plate, there is an insufficient anti-external light reflection characteristic in the oblique direction, resulting in an undesirable coloring problem.
[0006] Here, as a parameter representing the characteristics of the phase difference film, there is an NZ coefficient. The refractive index of the slow axis in the plane of the phase difference film is set to nx, the refractive index of the fast axis is set to ny, and the refractive index in the thickness direction of the film is set to nz. The NZ coefficient is given by the formula {NZ = (nx-nz) / (nx-ny)}. The closer the NZ coefficient is to 0.5, the less the viewing angle dependence of the phase difference value of the phase difference film is, and in the circular polarizing plate of the organic EL, the anti-external light reflection effect in the inclined direction is improved. Prior art literature Patent Literature
[0007] Patent Document 1: Japanese Patent Application Laid-Open No. 62-70407 Patent Document 2: Japanese Patent Application Laid-Open No. 9-208957 Patent Document 3: European Patent Application Publication No. 1090325 Patent Document 4: International Publication No. 2008 / 031243 Patent Document 5: Japanese Patent Application Publication No. 2008-164925 Patent Document 6: Japanese Patent Application Laid-Open No. 11-189665 Summary of the invention Technical problem to be solved by the invention
[0008] The present invention has been made in view of the above problems, and its object is to provide a composition for retardation film that can produce a single-layer retardation material with an NZ coefficient of 0.4≤NZ≤0.6 and a high retardation value by a simpler process, and a single-layer retardation material obtained from the composition. Technical solutions for solving technical problems
[0009] The inventors of the present invention have repeatedly conducted in-depth studies to solve the above-mentioned technical problems, and as a result, found that by using a composition containing a specific polymer, a single-layer phase difference material having an NZ coefficient of 0.4≤NZ≤0.6, a thin film, and high refractive index anisotropy (Δn) can be obtained without using a liquid crystal alignment film, thereby completing the present invention.
[0010] Therefore, the present invention provides the following retardation film composition and single-layer retardation material. <1> A composition for a phase difference film, comprising: (A) a side chain type copolymer, the side chain type copolymer comprising a side chain of a terminal carboxylic acid having a photoreactive site, and a side chain of a terminal carboxylic acid having an aromatic ring structure of two or more rings in which the two rings located at the terminal side are not covalently bonded by a single bond, and (B) Organic solvent. <2> The composition for retardation film according to <1>, wherein the (A) side chain type copolymer is a side chain type polymer having a side chain having a photoreactive site represented by the following formula (a) and a side chain having a site represented by the following formula (b). [Chemistry 1] (Where R 1 is an alkylene group having 1 to 30 carbon atoms, and one or more hydrogen atoms of the alkylene group may be substituted by a fluorine atom or an organic group. 1 -CH 2 CH 2 - can be replaced by -CH=CH-, R 1 -CH 2 - may be substituted by a group selected from -O-, -NH-C(=O)-, -C(=O)-NH-, -C(=O)-O-, -OC(=O)-, -NH-, -NH-C(=O)-NH- and -C(=O)-. 2 - is not replaced by these groups at the same time. R 2 It is a divalent aromatic group, a divalent alicyclic group, a divalent heterocyclic group or a divalent condensed ring group. R 3 is a single bond, -CH 2 -, -O-, -C(=O)-O-, -OC(=O)- or -CH=CH-C(=O)-O-. R 4 It is a divalent aromatic group, -Ph-Cy-, -Cy-Ph-, or a divalent condensed ring group (wherein Ph represents a phenylene group and Cy represents a cyclohexanediyl group). R 5 -CH 2 -, -O-, -NH-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -CH=CH-C(=O)-O-, -C(=O)-NH-, -NH-C(=O)- or -NH-C(=O)-NH-. R 6 is an alkylene group having 1 to 10 carbon atoms, and one or more hydrogen atoms of the alkylene group may be replaced by a fluorine atom or an organic group. 6 -CH 2 - may be substituted by a group selected from -O-, -NH- and -C(=O)-. The adjacent -CH 2 - can be replaced by these groups simultaneously. The hydrogen atoms in the ring structure and the CH=CH structure in formula (a) may be replaced by a substituent selected from an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a halogen group, a cyano group and a nitro group. The hydrogen atoms in the ring structure in formula (b) may be replaced by a substituent selected from an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a halogen group, a cyano group and a nitro group. In the presence of two or more R 2 , R 3 , R 4 or R 5 In the case of multiple R 2 , R 3 , R 4 or R 5 They can be the same or different. a is 0, 1 or 2. b is 0 or 1. c is an integer satisfying 0≤c≤2b+4. d is 1 or 2. e is 0 or 1. f is 0 or 1. The dotted line is a bond.) <3> The composition for a retardation film according to <2>, wherein the side chain having a photoreactive site represented by the formula (a) is a side chain represented by the following formula (a1). [Chemistry 2] (Where R 1 , R 2 and a are the same as above. R 3A is a single bond, -O-, -C(=O)-O- or -OC(=O)-. 3A In the case of multiple R 3A They can be the same or different. The hydrogen atoms in the benzene ring and the CH=CH structure in formula (a1) may be replaced by a substituent selected from an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a halogen group, a cyano group and a nitro group. The dotted line is a bond.) <4> The polymer composition and the composition for a retardation film according to <2> or <3>, wherein the number of ring structures in the side chain represented by the formula (b) is 3 or less. <5> The composition for retardation films according to any one of <1> to <4>, wherein the side chain polymer exhibits liquid crystallinity. <6> A method for manufacturing a single-layer phase difference material, comprising the following steps: (I) a step of applying the retardation film composition according to any one of <1> to <5> on a substrate to form a coating film; (II) irradiating the coating film with polarized ultraviolet rays; and (III) A step of heating the coating film irradiated with ultraviolet rays to obtain a phase difference material. <7> A single-layer phase difference material obtained from the composition according to any one of <1> to <5>. Effects of the Invention
[0011] According to the present invention, it is possible to provide a single-layer retardation material having an NZ coefficient of 0.4≤NZ≤0.6 and having a high retardation value even in a thin film, and a polymer that imparts the single-layer retardation material. DETAILED DESCRIPTION
[0012] The present inventors have conducted intensive studies and, as a result, have obtained the following findings and have completed the present invention. The phase difference film composition of the present invention (hereinafter also referred to as a polymer composition) has a photosensitive side chain polymer (hereinafter also referred to as a side chain polymer) that can show liquid crystal properties. The coating obtained using the above polymer composition is a film having a photosensitive side chain polymer that can show liquid crystal properties. The coating is not subjected to a friction treatment, but is oriented by polarized light irradiation. Then, after the polarized light irradiation, the side chain polymer film is heated to form a film endowed with optical anisotropy (hereinafter also referred to as a single-layer phase difference material). At this time, the slight anisotropy exhibited by irradiating polarized light becomes a driving force, and the liquid crystal side chain polymer itself is effectively reoriented by self-organization. As a result, as a single-layer phase difference material, a highly efficient orientation treatment can be achieved, and a single-layer phase difference material endowed with high optical anisotropy can be obtained.
[0013] In addition, in the polymer composition of the present invention, the side chain polymer includes a side chain of a terminal carboxylic acid having a photo-orientation site represented by a side chain shown in the above formula (a), and includes a side chain represented by a side chain shown in the above formula (b) having an aromatic ring structure of more than 2 rings and a terminal carboxylic acid having a structure that is not covalently bonded with a single bond between the 2 rings located at the terminal side, whereby the ring structure of the 2 rings becomes on the same plane, and the interaction between the side chains is enhanced, so that the liquid crystallinity and photo-orientation are improved, and the orientation in the slow axis direction in the plane is promoted, and the confusion of the orientation in the depth direction is reduced. Thus, the phase difference material obtained by the polymer composition of the present invention shows a high phase difference value even if it is a film, and nx is greater than nz, and nz shows a roughly intermediate value of nx and ny due to the effect of the terminal carboxylic acid. It should be noted that these include the insights of the inventors on the mechanism of the present invention and do not limit the present invention.
[0014] Hereinafter, embodiments of the present invention will be described in detail.
[0015] [Polymer composition] The polymer composition of the present invention is characterized by comprising (A) a photosensitivity side chain polymer that exhibits liquid crystallinity within a predetermined temperature range and (B) an organic solvent.
[0016] [(A) Side chain polymer] The component (A) is a photosensitive side chain polymer that exhibits liquid crystallinity within a specified temperature range, and is a side chain copolymer comprising a side chain of a terminal carboxylic acid having a photoreactive site, and a side chain of a terminal carboxylic acid having a ring structure having more than two rings and a structure in which the two rings located at the terminal side are not covalently bonded by a single bond. As the above-mentioned side chain copolymer, a side chain having a photoreactive site represented by the following formula (a) (hereinafter also referred to as side chain a) and a side chain having a site represented by the following formula (b) (hereinafter also referred to as side chain b). [Chemistry 3]
[0017] In formula (a), R 1 is an alkylene group having 1 to 30 carbon atoms, wherein one or more hydrogen atoms of the alkylene group may be replaced by a fluorine atom or an organic group. 1 -CH 2 CH 2 - can be replaced by -CH=CH-, R 1 -CH 2- may be substituted by a group selected from -O-, -NH-C(=O)-, -C(=O)-NH-, -C(=O)-O-, -OC(=O)-, -NH-, -NH-C(=O)-NH- and -C(=O)-. 2 - is not replaced by these groups at the same time. R 2 It is a divalent aromatic group, a divalent alicyclic group, a divalent heterocyclic group or a divalent condensed ring group. R 3 is a single bond, -CH 2 -, -O-, -C(=O)-O-, -OC(=O)- or -CH=CH-C(=O)-O-. The hydrogen atoms in the ring structure and the CH=CH structure in formula (a) may be replaced by a substituent selected from an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a halogen group, a cyano group and a nitro group. In the presence of two or more R 2 or R 3 In the case of multiple R 2 or R 3 They can be the same or different. a is 0, 1 or 2. b is 0 or 1. c is an integer satisfying 0≤c≤2b+4. The dotted lines are bonding bonds.
[0018] In formula (b), R 1 With R in formula (a) 1 For the same definition, R 4 It is a divalent aromatic group, -Ph-Cy-, -Cy-Ph-, or a divalent condensed ring group (wherein Ph represents a phenylene group and Cy represents a cyclohexanediyl group). R 5 -CH 2 -, -O-, -NH-, -C(=O)-, -C(=O)-O-, -OC(=O)-, -CH=CH-C(=O)-O-, -C(=O)-NH-, -NH-C(=O)- or -NH-C(=O)-NH-. R 6 is an alkylene group having 1 to 10 carbon atoms, and one or more hydrogen atoms of the alkylene group may be replaced by a fluorine atom or an organic group. 6 -CH 2 - may be substituted by a group selected from -O-, -NH- and -C(=O)-. The adjacent -CH 2- can be replaced by these groups simultaneously. The hydrogen atoms in the ring structure in formula (b) may be replaced by a substituent selected from an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a halogen group, a cyano group and a nitro group. In the presence of two or more R 4 or R 5 In the case of multiple R 4 or R 5 They can be the same or different. d is 1 or 2. e is 0 or 1. f is 0 or 1. The dotted lines are bonding bonds.
[0019] R 1 The alkylene group having 1 to 30 carbon atoms may be any of linear, branched or cyclic, and specific examples thereof include methylene, ethylene, propane-1,3-diyl, butane-1,4-diyl, pentane-1,5-diyl, hexane-1,6-diyl, heptane-1,7-diyl, octane-1,8-diyl, nonane-1,9-diyl and decane-1,10-diyl.
[0020] As R 2 The divalent aromatic group represented by , for example, includes phenylene and biphenylene. 2 Examples of the divalent alicyclic group shown in : include cyclohexanediyl and the like. 2 Examples of the divalent heterocyclic group shown in FIG. 1 include furandiyl and the like. 2 Examples of the divalent fused ring group include naphthylene and the like.
[0021] As R 4 The divalent aromatic group represented by , for example, includes phenylene and biphenylene. 4 Examples of the divalent fused ring group include naphthylene and the like.
[0022] R 6 The alkylene group having 1 to 10 carbon atoms may be linear, branched or cyclic. Specific examples thereof include the group consisting of the group R 1 The groups listed as specific examples.
[0023] As the side chain a, a side chain represented by the following formula (a1) (hereinafter also referred to as side chain a1) is preferred. [Chemistry 4]
[0024] In formula (a1), R 1, R 2 and a are the same as above. 3A is a single bond, -O-, -C(=O)-O- or -OC(=O)-. 3A In the case of multiple R 3A They may be the same or different. The hydrogen atoms in the benzene ring and the CH=CH structure in formula (a1) may be replaced by a substituent selected from an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a cyano group, and a nitro group. The dotted line is a bond.
[0025] As the side chain a1, for example, a side chain represented by the following formula (a1-1) is preferred. [Chemistry 5]
[0026] In formula (a1-1), L is a linear or branched alkylene group having 1 to 16 carbon atoms. X is a single bond, -O-, -C(=O)-O-, or -OC(=O)-.
[0027] The side chain polymer (A) preferably reacts to light in the wavelength range of 250 to 400 nm and exhibits liquid crystallinity in the temperature range of 100 to 300° C. The side chain polymer (A) preferably has a photosensitive side chain that reacts to light in the wavelength range of 250 to 400 nm.
[0028] (A) The side chain polymer has a photosensitive side chain bonded to the main chain, which can induce a crosslinking reaction or an isomerization reaction in response to light. The structure of the photosensitive side chain polymer that can exhibit liquid crystallinity is not particularly limited as long as it satisfies the above characteristics, and preferably has a rigid liquid crystal unit component in the side chain structure. When the above side chain polymer is made into a single-layer phase difference material, stable optical anisotropy can be obtained.
[0029] As a more specific example of the structure of a photosensitive side chain polymer capable of exhibiting liquid crystallinity, a structure having a main chain and a side chain a is preferred, wherein the main chain is composed of at least one free radical polymerizable group selected from (meth)acrylate, itaconate, fumarate, maleate, α-methylene-γ-butyrolactone, styrene, vinyl, maleimide, norbornene and the like and siloxane.
[0030] The number of ring structures in the side chain represented by the above formula (b) is preferably 3 or less. Here, the ring structure of the condensed ring is counted as 1. That is, the ring structure in phenylene and naphthylene is 1, and the ring structure in biphenylene and cyclohexanediyl is 2.
[0031] As the side chain b, for example, a side chain represented by the following formula (b1) is preferred. [Chemistry 6]
[0032] In formula (b1), R 1 , R 4 ~R 6 , d and f are the same as above. The number of ring structures in formula (b1) is 3 or less. The hydrogen atoms in the benzene ring in formula (b1) may be replaced by a substituent selected from an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a halogen group, a cyano group and a nitro group. The dotted line is a bond.
[0033] In addition, the side chain polymer (A) preferably has a side chain that only exhibits liquid crystallinity (hereinafter also referred to as side chain c) in order to exhibit liquid crystallinity within a temperature range of 100 to 300° C. It should be noted that, herein, “only exhibits liquid crystallinity” means that the polymer having only the side chain c does not exhibit photo-orientation but only exhibits liquid crystallinity in the preparation process of the phase difference material of the present invention (i.e., steps (I) to (III) described later).
[0034] The side chain c is preferably any one or two or more liquid crystalline side chains selected from the following formulae (1) to (12). [Chemistry 7]
[0035] [Chemistry 8]
[0036] In formulas (1) to (12), A 1 , A 2 are each independently a single bond, -O-, -CH 2 -, -C(=O)-O-, -OC(=O)-, -C(=O)-NH- or -NH-C(=O)-. 2 In the case of multiple A 2 They can be the same or different. 11 For-No 2 , -CN, a halogen atom, a phenyl group, a naphthyl group, a biphenyl group, a furyl group, a monovalent nitrogen-containing heterocyclic group, a monovalent alicyclic hydrocarbon group having 5 to 8 carbon atoms, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms. 12 is a group selected from the group consisting of phenyl, naphthyl, biphenyl, furanyl, a monovalent nitrogen-containing heterocyclic group, a monovalent alicyclic hydrocarbon group having 5 to 8 carbon atoms, and a group obtained by combining the above groups, and the hydrogen atom bonded to the above group may be -NO 2, -CN, a halogen atom, an alkyl group having 1 to 5 carbon atoms, or an alkoxy group having 1 to 5 carbon atoms. 13 For hydrogen atoms, -NO 2 , -CN, a halogen atom, a phenyl group, a naphthyl group, a biphenyl group, a furyl group, a monovalent nitrogen-containing heterocyclic group, a monovalent alicyclic hydrocarbon group having 5 to 8 carbon atoms, an alkyl group having 1 to 12 carbon atoms, or an alkoxy group having 1 to 12 carbon atoms. E is -C(=O)-O- or -OC(=O)-. d is an integer from 1 to 12. k1 to k5 are each independently an integer from 0 to 2, but the total of k1 to k5 is 2 or more. k6 and k7 are each independently an integer from 0 to 2, but the total of k6 and k7 is 1 or more. m1, m2 and m3 are each independently an integer from 1 to 3. n is 0 or 1. Z 1 and Z 2 are each independently a single bond, -C(=O)-, -CH 2 O-, or -CF 2 -. The dotted line is a bond.
[0037] Among them, the side chain c is preferably a side chain represented by any one of formulae (1) to (11).
[0038] The side chain polymer of the component (A) can be obtained by polymerizing a monomer having a structure represented by formula (a), a monomer having a structure represented by formula (b), and, if necessary, a monomer having a structure that exhibits only liquid crystallinity.
[0039] Examples of the monomer having a structure represented by formula (a) (hereinafter also referred to as monomer M1) include compounds represented by the following formula (M1). [Chemistry 9] (Where R 1 , R 2 , R 3 , a and m are the same as above. The hydrogen atoms in the ring structure and the CH=CH structure in the formula may be replaced by a substituent selected from an alkyl group having 1 to 6 carbon atoms, a halogenated alkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a halogenated alkoxy group having 1 to 6 carbon atoms, a halogen group, a cyano group and a nitro group.)
[0040] As the monomer M1, a monomer represented by the following formula (M1A) is preferred. [Chemistry 10] (Where R 1 , R 2 , R 3A, R and a are the same as above. The hydrogen atoms in the ring structure and the CH=CH structure in the formula may be replaced by a substituent selected from an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a halogen group, a cyano group and a nitro group.)
[0041] Among the monomers M1A, a monomer represented by the following formula (M1B) is more preferred. [Chemistry 11] (Wherein, L and X are the same as above.)
[0042] In the formulae (M1), (M1A) and (M1B), PL is a polymerizable group represented by any one of the following formulae (PL-1) to (PL-5). [Chemistry 12]
[0043] In formulas (PL-1) to (PL-5), Q 1 , Q 2 and Q 3 Each is independently a hydrogen atom, a linear or branched alkyl group having 1 to 10 carbon atoms, or a linear or branched alkyl group having 1 to 10 carbon atoms substituted with a halogen. 1 or a bond of L. Some of these monomers are commercially available, and some can be produced from known substances by known production methods.
[0044] Preferred examples of the monomer M1 include monomers represented by the following formulae (M1-1) to (M1-5). [Chemistry 13] (In the formula, PL is the same as above. p is an integer from 2 to 9.)
[0045] Examples of the monomer having a structure represented by formula (b) (hereinafter also referred to as monomer M2) include compounds represented by the following formula (M2). [Chemistry 14] (Where PL, R 1 , R 4 ~R 6 , d, e and f are the same as above. The hydrogen atoms in the ring structure in the formula may be replaced by substituents selected from alkyl groups having 1 to 6 carbon atoms, haloalkyl groups having 1 to 6 carbon atoms, alkoxy groups having 1 to 6 carbon atoms, haloalkoxy groups having 1 to 6 carbon atoms, halogen groups, cyano groups and nitro groups.)
[0046] As the monomer M2, a monomer represented by the following formula (M2A) is preferred. [Chemistry 15] (Where PL, R 1 , R 4 ~R 6 , d and f are the same as above. The hydrogen atom in the benzene ring in the formula may be replaced by a substituent selected from an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a halogen group, a cyano group and a nitro group.)
[0047] As the monomer M2, monomers shown below as M2-1 to M2-6 are preferred. [Chemistry 16] (Where PL and p are the same as above.)
[0048] Some of these monomers are commercially available, and some can be produced from known substances by known production methods.
[0049] The method for synthesizing (M2-1) to (M2-6) is not particularly limited. For example, as shown in the following formula, M3-1 can be synthesized according to the synthesis method described in Japanese Patent Publication No. 9-118717, and the acid chloride (M2-1-1) is obtained using thionyl chloride or oxalyl chloride. Then, M2-1-3 can be obtained by condensing the compound (M2-1-2) with the acid chloride (M2-1-1) protected at the carboxylic acid end in the presence of a base such as triethylamine. As the protecting group (PG), tert-butyl, monomethoxymethyl, etc. can be used. M2-1 can be produced by deprotecting the protecting group (PG) of M2-1-3 with an acid. [Chemistry 17]
[0050] The monomer having a structure that exhibits only liquid crystallinity (hereinafter also referred to as monomer M3) is a monomer in which a polymer derived from the monomer exhibits liquid crystallinity and the polymer can form a mesogen group at a side chain site.
[0051] The mesogen group as a side chain may be a group that forms a mesogen structure independently, such as biphenyl or phenyl benzoate, or a group that forms a mesogen structure by hydrogen bonding such as benzoic acid. The following structure is preferred as a mesogen group as a side chain. [Chemistry 18]
[0052] As a more specific example of the monomer M3, a structure having a polymerizable group and a structure containing at least one of the above formulas (1) to (12) is preferred, wherein the polymerizable group is selected from at least one of free radical polymerizable groups such as hydrocarbon, (meth)acrylate, itaconate, fumarate, maleate, α-methylene-γ-butyrolactone, styrene, vinyl, maleimide, norbornene, and siloxane. In particular, the monomer M3 is preferably a monomer having a (meth)acrylate as a polymerizable group, and preferably a monomer having -COOH at the end of the side chain.
[0053] Preferred examples of the monomer M3 include monomers represented by the following formulae (M3-1) to (M3-9). [Chemistry 19]
[0054] [Chemistry 20] (Where PL and p are the same as above.)
[0055] In addition, other monomers can be copolymerized within the range that does not impair the performance of photoreactivity and / or liquid crystal properties. Examples of other monomers include monomers that are industrially available and capable of free radical polymerization. Specific examples of other monomers include unsaturated carboxylic acids, acrylate compounds, methacrylate compounds, maleimide compounds, acrylonitrile, maleic anhydride, styrene compounds, vinyl compounds, and the like.
[0056] Specific examples of the unsaturated carboxylic acid include acrylic acid, methacrylic acid, itaconic acid, maleic acid, and fumaric acid.
[0057] Examples of the acrylate compound include methyl acrylate, ethyl acrylate, isopropyl acrylate, benzyl acrylate, naphthyl acrylate, anthracene acrylate, anthracene methyl acrylate, phenyl acrylate, 2,2,2-trifluoroethyl acrylate, tert-butyl acrylate, cyclohexyl acrylate, isobornyl acrylate, 2-methoxyethyl acrylate, methoxytriethylene glycol acrylate, 2-ethoxyethyl acrylate, tetrahydrofurfuryl acrylate, 3-methoxybutyl acrylate, 2-methyl-2-adamantyl acrylate, 2-propyl-2-adamantyl acrylate, 8-methyl-8-tricyclodecanyl acrylate, and 8-ethyl-8-tricyclodecanyl acrylate.
[0058] Examples of the methacrylate compound include methyl methacrylate, ethyl methacrylate, isopropyl methacrylate, benzyl methacrylate, naphthyl methacrylate, anthracene methacrylate, anthracene methyl methacrylate, phenyl methacrylate, 2,2,2-trifluoroethyl methacrylate, tert-butyl methacrylate, cyclohexyl methacrylate, isobornyl methacrylate, 2-methoxyethyl methacrylate, methoxytriethylene glycol methacrylate, 2-ethoxyethyl methacrylate, tetrahydrofurfuryl methacrylate, 3-methoxybutyl methacrylate, 2-methyl-2-adamantyl methacrylate, 2-propyl-2-adamantyl methacrylate, 8-methyl-8-tricyclodecanyl methacrylate, and 8-ethyl-8-tricyclodecanyl methacrylate.
[0059] Examples of the vinyl compound include vinyl ether, methyl vinyl ether, benzyl vinyl ether, 2-hydroxyethyl vinyl ether, phenyl vinyl ether, propyl vinyl ether, etc. Examples of the styrene compound include styrene, 4-methylstyrene, 4-chlorostyrene, 4-bromostyrene, etc. Examples of the maleimide compound include maleimide, N-methylmaleimide, N-phenylmaleimide, N-cyclohexylmaleimide, etc.
[0060] From the viewpoint of photoreactivity, the content of the side chain a in the side chain type polymer of the present invention is preferably 5 to 90 mol %, more preferably 5 to 80 mol %, and even more preferably 5 to 50 mol %.
[0061] From the viewpoint of the phase difference value, the content of the side chain b in the side chain type polymer of the present invention is preferably 10 to 95 mol %, more preferably 5 to 70 mol %, and even more preferably 10 to 70 mol %.
[0062] From the viewpoint of phase difference, when the total content of the side chains a and b is less than 100 mol %, the content of the side chain c in the side chain type polymer of the present invention is preferably 10 to 100 mol % of the remainder.
[0063] As described above, the side chain type polymer of the present invention may contain other side chains. When the total content of the side chains a to c is less than 100 mol %, the content of the other side chains is the remainder.
[0064] The manufacturing method of the side chain polymer of component (A) is not particularly limited, and a general method for industrial processing can be used. Specifically, it can be manufactured by free radical polymerization, cationic polymerization or anionic polymerization of vinyl groups of the above-mentioned monomer M1, monomer M2, monomer M3 as required and other monomers as required. Among them, free radical polymerization is particularly preferred from the viewpoint of the ease of reaction control, etc.
[0065] As the polymerization initiator for radical polymerization, known compounds such as radical polymerization initiators (radical thermal polymerization initiators, radical photopolymerization initiators) and reversible addition-fragmentation chain transfer (RAFT) polymerization agents can be used.
[0066] The free radical thermal polymerization initiator is a compound that generates free radicals by heating to a temperature higher than the decomposition temperature. Examples of such free radical thermal polymerization initiators include ketone peroxides (methyl ethyl ketone peroxide, cyclohexanone peroxide, etc.), diacyl peroxides (acetyl peroxide, benzoyl peroxide, etc.), hydroperoxides (hydrogen peroxide, tert-butyl hydroperoxide, cumyl hydroperoxide, etc.), dialkyl peroxides (di-tert-butyl peroxide, dicumyl peroxide, dilauroyl peroxide, etc.), peroxyketals (dibutyl peroxycyclohexane, etc.), alkyl peresters (tert-butyl peroxyneodecanoate, tert-butyl peroxypivalate, tert-amyl peroxy-2-ethylcyclohexane, etc.), persulfates (potassium persulfate, sodium persulfate, ammonium persulfate, etc.), and azo compounds (azobisisobutyronitrile, 2,2′-bis(2-hydroxyethyl)azobisisobutyronitrile, etc.). The free radical thermal polymerization initiator may be used alone or in combination of two or more.
[0067] The radical photopolymerization initiator is not particularly limited as long as it is a compound that initiates radical polymerization by light irradiation. Examples of such radical photopolymerization initiators include benzophenone, Michler's ketone, 4,4'-bis(diethylamino)benzophenone, xanthone, thioxanthone, isopropylxanthone, 2,4-diethylthioxanthone, 2-ethylanthraquinone, acetophenone, 2-hydroxy-2-methylpropiophenone, 2-hydroxy-2-methyl-4'-isopropylpropiophenone, 1-hydroxycyclohexylphenyl ketone, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, camphorquinone, benzanthrone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholinyl-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinylphenyl)-butanone-1,4-dimethylamino-1-[4-(methylthio)phenyl]-2-morpholinyl-1-propanone, and 2-benzyl-2-dimethylamino-1-(4-morpholinylphenyl)-butanone-1,4-dimethylamino-1-[4-(methylthio)phenyl]-2-morpholinyl-1-propanone. -Dimethylaminobenzoic acid ethyl ester, 4-dimethylaminobenzoic acid isopentyl ester, 4,4'-di(tert-butylperoxycarbonyl)benzophenone, 3,4,4'-tri(tert-butylperoxycarbonyl)benzophenone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 2-(4'-methoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(3',4'-dimethoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(2',4'-dimethoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(2'-methoxyphenylvinyl)-4,6-bis(trichloromethyl)-s-triazine, 2-(4'-pentyloxyphenylvinyl)-4,6-bis( trichloromethyl)-s-triazine, 4-[p-N,N-bis(ethoxycarbonylmethyl)]-2,6-bis(trichloromethyl)-s-triazine, 1,3-bis(trichloromethyl)-5-(2′-chlorophenyl)-s-triazine, 1,3-bis(trichloromethyl)-5-(4′-methoxyphenyl)-s-triazine, 2-(p-dimethylaminophenyl)benzoxazole, 2-(p-dimethylaminophenyl)benzothiazole, 2-mercaptobenzothiazole, 3,3′-carbonylbis(7-diethylaminocoumarin), 2-(o-chlorophenyl)-4,4′,5,5′-tetraphenyl-1,2′-biimidazole, 2,2′-bis(2-chlorophenyl)-4,4′,5,5′-tetrakis(4-ethoxycarbonylphenyl)-1,2 '-Bis(2,4-dichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2,4-dibromophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 2,2'-bis(2,4,6-trichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 3-(2-methyl-2-dimethylaminopropionyl)carbazole, 3,6-bis(2-methyl-2-morpholinopropionyl)-9-n-dodecylcarbazole, 1-hydroxycyclohexyl phenyl ketone, bis(5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, 3,3',4,4'-tetra(tert-butylperoxycarbonyl)benzophenone, 3,3',4,4'-tetra(tert-hexylperoxycarbonyl)benzophenone, 3,3'-di(methoxycarbonyl)-4,4'-di(tert-butylperoxycarbonyl)benzophenone, 3,4'-di(methoxycarbonyl)-4,3'-di(tert-butylperoxycarbonyl)benzophenone, 4,4'-di(methoxycarbonyl)-3,3'-di(tert-butylperoxycarbonyl)benzophenone, 2-(3-methyl-3H-benzothiazol-2-ylidene)-1-naphth-2-yl-ethanone, 2-(3-methyl-1,3-benzothiazol-2(3H)-ylidene)-1-(2-benzoyl)ethanone, etc. The free radical photopolymerization initiator may be used alone or in combination of two or more.
[0068] The radical polymerization method is not particularly limited, and emulsion polymerization, suspension polymerization, dispersion polymerization, precipitation polymerization, bulk polymerization, solution polymerization, and the like can be used.
[0069] The organic solvent used in the polymerization reaction is not particularly limited as long as it is an organic solvent that dissolves the generated polymer. Specific examples thereof include: N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-methyl-ε-caprolactam, dimethyl sulfoxide, tetramethylurea, pyridine, dimethyl sulfone, hexamethyl sulfoxide, γ-butyrolactone, isopropyl alcohol, methoxymethylpentanol, dipentene, ethyl amyl ketone, methyl nonyl ketone, methyl ethyl ketone, methyl isoamyl ketone, methyl isopropyl ketone, methyl cellosolve, ethyl cellosolve, Methyl Cellosolve Acetate, Ethyl Cellosolve Acetate, Butyl Carbitol, Ethyl Carbitol, Ethyl Glycol, Ethylene Glycol Monoacetate, Ethylene Glycol Monoisopropyl Ether, Ethylene Glycol Monobutyl Ether, Propylene Glycol, Propylene Glycol Monoacetate, Propylene Glycol Monomethyl Ether, Propylene Glycol Tert-Butyl Ether, Diethylene Glycol, Diethylene Glycol Monoacetate, Diethylene Glycol Dimethyl Ether, Dipropylene Glycol Monoacetate Monomethyl Ether, Dipropylene Glycol Monomethyl Ether, Dipropylene Glycol Monoethyl Ether, Dipropylene Glycol Monoacetate Monoethyl Ether, Dipropylene Glycol Monopropyl Ether, Dipropylene Glycol Monoacetate Monopropyl ether, 3-methyl-3-methoxybutyl acetate, tripropylene glycol methyl ether, 3-methyl-3-methoxybutanol, diisopropyl ether, ethyl isobutyl ether, diisobutylene, amyl acetate, butyl butyrate, butyl ether, diisobutyl ketone, methyl cyclohexene, propyl ether, dihexyl ether, 1,4-dioxane, n-hexane, n-pentane, n-octane, diethyl ether, cyclohexanone, ethylene carbonate, propylene carbonate, methyl lactate, ethyl lactate, methyl acetate, ethyl acetate, n-butyl acetate, Propylene glycol monoethyl acetate, methyl pyruvate, ethyl pyruvate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-ethoxypropionic acid, 3-methoxypropionic acid, propyl 3-methoxypropionate, butyl 3-methoxypropionate, diethylene glycol dimethyl ether, 4-hydroxy-4-methyl-2-pentanone, 3-methoxy-N,N-dimethylpropionamide, 3-ethoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, etc.
[0070] Above-mentioned organic solvent can use one kind alone, also can mix and use more than two kinds.In addition, even if it is the solvent of the polymkeric substance that does not dissolve generation, in the scope that the polymkeric substance that generates does not separate out, also can be mixed in above-mentioned organic solvent and use.In addition, in free radical polymerization, the oxygen in the organic solvent becomes the reason that hinders polyreaction, so organic solvent preferably uses the organic solvent of degassing as far as possible.
[0071] The polymerization temperature during free radical polymerization can be selected from any temperature of 30 to 150° C., preferably in the range of 50 to 100° C. In addition, the reaction can be carried out at any concentration. If the concentration is too low, it is difficult to obtain a high molecular weight polymer. If the concentration is too high, the viscosity of the reaction solution becomes too high, and uniform stirring becomes difficult. Therefore, the monomer concentration is preferably 1 to 50% by mass, more preferably 5 to 30% by mass. The reaction can be carried out at a high concentration at the beginning, and then an organic solvent can be added.
[0072] In the above-mentioned free radical polymerization reaction, if the ratio of the free radical polymerization initiator is large relative to the monomer, the molecular weight of the obtained polymer becomes small, and if the ratio of the free radical polymerization initiator is small relative to the monomer, the molecular weight of the obtained polymer becomes large, so the ratio of the free radical initiator is preferably 0.1 to 10 mol% relative to the monomer to be polymerized. In addition, various monomer components, solvents, initiators, etc. can also be added during polymerization.
[0073] When the polymers generated are recovered from the reaction solution obtained by the above reaction, the reaction solution is put into a poor solvent to precipitate the polymers. Examples of the poor solvent used in the precipitation include methanol, acetone, hexane, heptane, butyl cellosolve, heptane, methyl ethyl ketone, methyl isobutyl ketone, ethanol, toluene, benzene, diethyl ether, methyl ethyl ether, water, etc. The polymer precipitated by being put into the poor solvent can be dried at room temperature or under normal pressure or reduced pressure, or by heating after being filtered and recovered. In addition, if the recovered polymer is redissolved in an organic solvent and the operation of reprecipitation and recovery is repeated 2 to 10 times, the impurities in the polymer can be reduced. Examples of the poor solvent at this time include alcohols, ketones, hydrocarbons, etc. If more than three poor solvents selected from them are used, the efficiency of purification is further improved, so it is preferred.
[0074] Taking into account the strength of the obtained coating film, workability during coating film formation and uniformity of the coating film, the weight average molecular weight of the side chain polymer (A) of the present invention as measured by GPC (Gel Permeation Chromatography) is preferably 2,000 to 2,000,000, more preferably 2,000 to 1,000,000, and even more preferably 5,000 to 200,000.
[0075] [(B) Organic solvent] The organic solvent of component (B) is not particularly limited as long as it is an organic solvent that dissolves the polymer component. Specific examples thereof include: N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-methyl-ε-caprolactam, 2-pyrrolidone, N-ethyl-2-pyrrolidone, N-vinyl-2-pyrrolidone, dimethyl sulfoxide, tetramethylurea, pyridine, dimethyl sulfone, hexamethyl sulfoxide, γ-butyrolactone, 3-methoxy-N,N-dimethylpropionamide, 3-ethoxy-N,N-dimethylpropionamide, 3-butoxy-N,N-dimethylpropionamide, 1,3-dimethyl-2-imidazolidinone, ethyl amyl ketone, Methyl nonyl ketone, methyl ethyl ketone, methyl isoamyl ketone, methyl isopropyl ketone, cyclohexanone, ethylene carbonate, propylene carbonate, diethylene glycol dimethyl ether, 4-hydroxy-4-methyl-2-pentanone, propylene glycol monoacetate, propylene glycol monomethyl ether, propylene glycol tert-butyl ether, diethylene glycol, diethylene glycol monoacetate, diethylene glycol dimethyl ether, dipropylene glycol monoacetate monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoacetate monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monoacetate monopropyl ether, 3-methyl-3-methoxybutyl acetate, tripropylene glycol methyl ether, etc. These may be used alone or in combination of two or more.
[0076] [Other ingredients] The polymer composition of the present invention may also include components other than (A) and (B). Examples thereof include solvents and compounds that improve uniformity of film thickness and surface smoothness when the polymer composition is applied, compounds that improve adhesion of the phase difference material to the substrate, etc., but are not limited to these.
[0077] Specific examples of solvents (poor solvents) for improving uniformity of film thickness and surface smoothness include isopropyl alcohol, methoxymethylpentyl alcohol, methyl cellosolve, ethyl cellosolve, butyl cellosolve, methyl cellosolve acetate, ethyl cellosolve acetate, butyl carbitol, ethyl carbitol, ethyl carbitol acetate, ethylene glycol, ethylene glycol monoacetate, ethylene glycol monoisopropyl ether, ethylene glycol monobutyl ether, propylene glycol, propylene glycol monomethyl ether, propylene glycol tert-butyl ether, Diethylene glycol, diethylene glycol monoacetate, diethylene glycol dimethyl ether, dipropylene glycol monoacetate monomethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol monoethyl ether, dipropylene glycol monoacetate monoethyl ether, dipropylene glycol monopropyl ether, dipropylene glycol monoacetate monopropyl ether, 3-methyl-3-methoxybutyl acetate, tripropylene glycol methyl ether, 3-methyl-3-methoxybutanol, diisopropyl ether, ethyl isobutyl ether, diisobutylene, amyl acetate, butyl butyrate, butyl ether, Diisobutyl ketone, methylcyclohexene, propyl ether, dihexyl ether, 1-hexanol, n-hexane, n-pentane, n-octane, diethyl ether, methyl lactate, ethyl lactate, n-propyl lactate, n-butyl lactate, isopentyl lactate, methyl acetate, ethyl acetate, n-butyl acetate, propylene glycol acetate monoethyl ether, methyl pyruvate, ethyl pyruvate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, 3-ethoxypropionic acid, 3-methyl Solvents having low surface tension such as propylene glycol monoacetate, propylene glycol diacetate, propylene glycol-1-monomethyl ether-2-acetate, propylene glycol-1-monoethyl ether-2-acetate, dipropylene glycol, and 2-(2-ethoxypropoxy)propanol are also useful.
[0078] These poor solvents can be used alone or in combination of two or more. When the poor solvent is used, the content of the poor solvent is preferably 5 to 80% by mass, more preferably 20 to 60% by mass, in the solvent in order not to significantly reduce the solubility of the overall solvent contained in the polymer composition.
[0079] As compounds for improving film thickness uniformity and surface smoothness, fluorine-based surfactants, silicone-based surfactants, nonionic surfactants, etc. can be cited. Specific examples thereof include: EFTOP (registered trademark) 301, EF303, EF352 (manufactured by Tohkem Products Co., Ltd.), MEGAFAC (registered trademark) F171, F173, F560, F563, R-30, R-40, R-41 (manufactured by DIC Corporation), Fluorad FC430, FC431 (manufactured by 3M Corporation), AsahiGuard (registered trademark) AG710 (manufactured by AGC Corporation), SURFLON (registered trademark) S-382, SC101, SC102, SC103, SC104, SC105, SC106 (manufactured by AGC Seimi Chemical Co., Ltd.), etc. The content of these surfactants is preferably 0.01 to 2 parts by mass, more preferably 0.01 to 1 part by mass, based on 100 parts by mass of the component (A).
[0080] As specific examples of compounds that improve the adhesion between the phase difference material and the substrate, compounds containing functional silanes can be cited, and as specific examples thereof, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 2-aminopropyltrimethoxysilane, 2-aminopropyltriethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-ureidopropyltrimethoxysilane, 3-ureidopropyltriethoxysilane, N-ethoxycarbonyl-3-aminopropyltrimethoxysilane, N-ethoxycarbonyl-3-aminopropyltrimethoxysilane, 1-Trimethoxysilyl-1,4,7-triazadecane, 10-triethoxysilyl-1,4,7-triazadecane, 9-trimethoxysilyl-3,6-diazanonyl acetate, 9-triethoxysilyl-3,6-diazanonyl acetate, N-benzyl-3-aminopropyl trimethoxysilane, N-benzyl-3-aminopropyl triethoxysilane, N-phenyl-3-aminopropyl trimethoxysilane, N-phenyl-3-aminopropyl triethoxysilane, etc.
[0081] Furthermore, in order to improve the adhesion between the substrate and the phase difference material and prevent the degradation of characteristics due to backlight when constituting a polarizing plate, a phenoplast compound or an epoxy group-containing compound may be added to the polymer composition.
[0082] Specific examples of the phenolic plastic additive are shown below, but the additive is not limited to these. [Chemistry 21]
[0083] Specific examples of the epoxy group-containing compound include ethylene glycol diglycidyl ether, polyethylene glycol diglycidyl ether, propylene glycol diglycidyl ether, tripropylene glycol diglycidyl ether, polypropylene glycol diglycidyl ether, neopentyl glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, glycerol diglycidyl ether, 2,2-dibromoneopentyl glycol diglycidyl ether, 1,3,5,6-tetraglycidyl-2,4-hexanediol, N,N,N′,N′-tetraglycidyl-m-xylenediamine, 1,3-bis(N,N-diglycidylaminomethyl)cyclohexane, and N,N,N′,N′-tetraglycidyl-4,4′-diaminodiphenylmethane.
[0084] When using a compound that improves adhesion to the substrate, the content is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, relative to 100 parts by mass of the polymer component contained in the polymer composition. If the content is less than 0.1 parts by mass, the effect of improving adhesion cannot be expected, and if it is more than 30 parts by mass, there is a situation where the orientation of the liquid crystal deteriorates.
[0085] As an additive, a photosensitizer can also be used. As the photosensitizer, a colorless sensitizer and a triplet sensitizer are preferred.
[0086] Examples of the photosensitizer include aromatic nitro compounds, coumarins (7-diethylamino-4-methylcoumarin, 7-hydroxy-4-methylcoumarin), ketocoumarins, carbonyl dicoumarins, aromatic 2-hydroxyketones, aromatic 2-hydroxyketones (2-hydroxybenzophenone, mono-p-(dimethylamino)-2-hydroxybenzophenone or di-p-(dimethylamino)-2-hydroxybenzophenone, etc.), acetophenones, anthraquinones, xanthone, thioxanthone, benzanthrone, thiazolines (2-benzoylmethylene- 3-methyl-β-naphthothiazoline, 2-(β-naphthoylmethylene)-3-methylbenzothiazoline, 2-(α-naphthoylmethylene)-3-methylbenzothiazoline, 2-(4-biphenylylmethylene)-3-methylbenzothiazoline, 2-(β-naphthoylmethylene)-3-methyl-β-naphthothiazoline, 2-(4-biphenylylmethylene)-3-methyl-β-naphthothiazoline, 2-(p-fluorobenzoylmethylene)-3-methyl-β-naphthothiazoline, etc.), oxadiazine oxazoline (2-benzoylmethylene-3-methyl-β-naphthooxazoline, 2-(β-naphthoylmethylene)-3-methylbenzoxazoline, 2-(α-naphthoylmethylene)-3-methylbenzoxazoline, 2-(4-biphenylmethylene)-3-methylbenzoxazoline, 2-(β-naphthoylmethylene)-3-methyl-β-naphthooxazoline, 2-(4-biphenylmethylene)-3-methyl-β-naphthooxazoline, 2-(p-fluorobenzoylmethylene)-3-methyl
[0043] The present invention also includes benzothiazole, nitroaniline (m-nitroaniline or p-nitroaniline, 2,4,6-trinitroaniline, etc.), nitroacenaphthene (5-nitroacenaphthene, etc.), 2-[(m-hydroxy-p-methoxy)phenyl]benzothiazole, benzoin alkyl ether, N-alkylated phthaloyl ketone, acetophenone ketal (2,2-dimethoxyphenylacetophenone, etc.), naphthalene (2-naphthylmethanol, 2-naphthoic acid, etc.), anthracene (9-anthracenemethanol, 9-anthracenecarboxylic acid, etc.), benzopyran, azoindolizine, furanocoumarin, etc. Among these, aromatic 2-hydroxyketone (benzophenone), coumarin, ketocoumarin, carbonyl dicoumarin, acetophenone, anthraquinone, xanthone, thioxanthone, and acetophenone ketal are preferred.
[0087] In the polymer composition of the present invention, in addition to the above-mentioned substances, dielectrics and conductive substances may be added to change the electrical properties such as the dielectric constant and conductivity of the phase difference material within the range that does not impair the effects of the present invention. In addition, cross-linking compounds may be added to increase the hardness and density of the film when the phase difference material is made.
[0088] [Preparation of polymer composition] The polymer composition of the present invention is preferably prepared as a coating liquid in a manner suitable for the formation of a monolayer phase difference material. That is, the polymer composition used in the present invention is preferably prepared as a solution in which the component (A) and the above-mentioned solvent or compound for improving the uniformity of film thickness and surface smoothness, the compound for improving the adhesion of the liquid crystal alignment film to the substrate, etc. are dissolved in the organic solvent of the component (B). Here, the content of the component (A) is preferably 1 to 30% by mass in the composition of the present invention, and more preferably 5 to 30% by mass.
[0089] The polymer composition of the present invention may contain other polymers in addition to the polymer of component (A) without damaging the liquid crystal performance and photosensitivity. At this time, the content of other polymers in the polymer component is preferably 0.5 to 80% by mass, more preferably 1 to 50% by mass. Other polymers include, for example, polymers that are not photosensitive side chain polymers that can show liquid crystal properties, such as poly (meth) acrylates, polyamic acids, and polyimides.
[0090] [Single-layer phase difference material] The single-layer retardation material of the present invention can be produced by a method including the following steps (I) to (III). (I) a step of applying the composition of the present invention onto a substrate to form a coating film; (II) irradiating the coating film with polarized ultraviolet rays; and (III) A step of heating the coating film irradiated with ultraviolet rays to obtain a phase difference material.
[0091] [Step (I)] Step (I) is a step of applying the composition of the present invention on a substrate to form a coating film. More specifically, the composition of the present invention is applied on a substrate (e.g., a silicon / silicon dioxide coated substrate, a silicon nitride substrate, a metal coated substrate (e.g., aluminum, molybdenum, chromium, etc.), a glass substrate, a quartz substrate, an ITO substrate, etc.), a film (e.g., a resin film such as a triacetylcellulose (TAC) film, a cycloolefin polymer film, a polyethylene terephthalate film, an acrylic film, etc.) by a method such as rod coating, spin coating, flow coating, roller coating, slit coating, slit coating followed by spin coating, inkjet method, printing method, etc. After coating, the solvent can be evaporated at 50 to 200° C., preferably 50 to 150° C. by heating means such as a hot plate, a hot air circulation oven, an IR (infrared) oven, etc. to obtain a coating film.
[0092] [Step (II)] In step (II), the coating obtained in step (I) is irradiated with polarized ultraviolet rays. When the film surface of the coating is irradiated with polarized ultraviolet rays, the substrate is irradiated with polarized ultraviolet rays from a specific direction through a polarizing plate. As the above-mentioned ultraviolet rays, ultraviolet rays with a wavelength range of 100 to 400 nm can be used. It is preferred to select the optimal wavelength through a filter or the like according to the type of coating used. Then, for example, in order to selectively induce a photocrosslinking reaction, ultraviolet rays with a wavelength range of 290 nm to 400 nm can be selected. As ultraviolet rays, for example, light radiated from a high-pressure mercury lamp can be used.
[0093] The irradiation amount of polarized ultraviolet rays depends on the coating film used. The irradiation amount is preferably set to be within the range of 1 to 70% of the amount of polarized ultraviolet rays that achieves the maximum value of ΔA, which is the difference between the ultraviolet absorbance in the direction parallel to the polarization direction of the polarized ultraviolet rays in the coating film and the ultraviolet absorbance in the direction perpendicular to the polarization direction, more preferably within the range of 1 to 50%.
[0094] [Step (III)] In step (III), the coating film irradiated with polarized ultraviolet rays in step (II) is heated. Heating can impart orientation control capability to the coating film.
[0095] The heating can be performed by using a heating means such as a hot plate, a hot air circulation type oven, an IR (infrared) type oven, etc. The heating temperature can be determined in consideration of the temperature at which the coating film to be used exhibits liquid crystallinity.
[0096] The heating temperature is preferably within the temperature range at which the polymer of the component (A) contained in the composition of the present invention exhibits liquid crystallinity (hereinafter referred to as the liquid crystal exhibiting temperature). In the case of a thin film surface such as a coating, it is expected that the liquid crystal exhibiting temperature of the coating surface is lower than the liquid crystal exhibiting temperature when the polymer of the component (A) is observed as a body. Therefore, the heating temperature is more preferably within the temperature range of the liquid crystal exhibiting temperature of the coating surface. That is, the temperature range of the heating temperature after polarized ultraviolet irradiation is preferably a temperature with a lower limit of 10°C lower than the lower limit of the temperature range of the liquid crystal exhibiting temperature of the polymer of the component (A) as the lower limit and a temperature with a lower limit of 10°C lower than the upper limit of the liquid crystal temperature range as the upper limit. If the heating temperature is lower than the above temperature range, there is a tendency that the anisotropic enhancement effect generated by heat in the coating becomes insufficient. In addition, if the heating temperature is too high compared to the above temperature range, there is a tendency that the state of the coating is close to an isotropic liquid state (isotropic phase), in which case it is sometimes difficult to reorient in one direction by self-organization.
[0097] It should be noted that the liquid crystal display temperature refers to a temperature above the liquid crystal transition temperature at which a phase transition occurs from a solid phase to a liquid crystal phase on the surface of a polymer or coating film, and below the isotropic phase transition temperature (Tiso) at which a phase transition occurs from a liquid crystal phase to an isotropic phase. For example, the liquid crystal property is displayed below 130°C, which means that the liquid crystal transition temperature at which a phase transition occurs from a solid phase to a liquid crystal phase is below 130°C.
[0098] The thickness of the coating film formed after heating can be appropriately selected in consideration of the height difference and optical properties of the substrate to be used, and is preferably 0.5 to 10 μm, for example.
[0099] The NZ coefficient of the film obtained from the retardation film composition of the present invention is 0.4≤NZ≤0.6, preferably 0.41≤NZ≤0.58, and even the film can provide a single-layer retardation material with a high retardation value.
[0100] The thus obtained single-layer retardation material of the present invention has optical properties suitable for use in display devices, recording materials, and the like, and is particularly suitable as an optical compensation film for polarizing plates and retardation plates of liquid crystal displays and organic ELs. Example
[0101] Hereinafter, the present invention will be described in more detail with reference to Synthesis Examples, Preparation Examples, Examples and Comparative Examples, but the present invention is not limited to the following Examples.
[0102] The monomers MA1, MB1 to MB6, MC1 to MC3, and MD1 used in the examples are shown below. MA1 was synthesized according to the synthesis method described in International Publication No. 2011 / 084546. MB1 and MC2 were synthesized according to the synthesis method described in International Publication No. 2017 / 135130. MB3 was synthesized according to the synthesis method described in International Publication No. 2014 / 054785. MB6 was synthesized according to the synthesis method described in Japanese Patent Application Laid-Open No. 2016-128403. MC1 was synthesized according to the synthesis method described in Japanese Patent Application Laid-Open No. 9-118717. MC3 was synthesized according to the synthesis method described in Japanese Patent Application Laid-Open No. 2009-19117. MD1 was synthesized according to the synthesis method described in Japanese Patent Application Laid-Open No. 2012-27354. MB2, MB4 and MB5 are novel compounds, and their synthesis methods are shown below. The side chain derived from MA1 corresponds to side chain a, the side chains derived from MB1 to MB6 correspond to side chain b, the side chains derived from MC1 to MC3 correspond to side chain c, and the side chain derived from MD1 does not correspond to any of side chain a, side chain b and side chain c. [Chemistry 22]
[0103] In addition, the abbreviations of the reagents used in this example are shown below. (Organic Solvent) NMP: N-methyl-2-pyrrolidone BCS: Butyl Cellosolve CPN: Cyclopentanone THF: Tetrahydrofuran DMF: N,N-dimethylformamide THF: Tetrahydrofuran MeCN: Acetonitrile PGME: Propylene glycol monomethyl ether PGMEA: Propylene glycol monomethyl ether acetate DMAc: N,N-dimethylacetamide (polymerization initiator) AIBN: 2,2′-azobisisobutyronitrile (Surfactant) R40: MEGAFAC R-40 (manufactured by DIC Corporation) F563: MEGAFAC F-563 (manufactured by DIC Corporation)
[0104] < 1 H-NMR measurement> Apparatus: Fourier transform superconducting nuclear magnetic resonance (FT-NMR) "AVANCE III" (manufactured by BRUKER), 500 MHz. Solvent: deuterated dimethyl sulfoxide (DMSO-d 6 ). Standard substance: tetramethylsilane (TMS).
[0105] [1]Synthesis of monomers <<Synthesis of MB2>> [Chemistry 23]
[0106] <Synthesis of [MB2-1] and [MB2-2]> DMAc (400 g), ethyl 4-hydroxy-3-methoxybenzoate (100 g, 510 mmol), potassium carbonate (98.6 g, 714 mmol) and potassium iodide (8.46 g, 51.0 mmol) were added to a 3000 mL four-necked flask, and 6-chloro-1-hexanol (83.6 g, 612 mmol) was added dropwise under heating conditions of 85° C. for 2 hours. After the addition, the reaction was carried out at the same temperature for 22 hours to eliminate the raw materials. After the reaction was completed, the mixture was diluted with ethyl acetate (1200 g) and the organic phase was washed 3 times with pure water. Then, the organic phase was recovered and concentrated under reduced pressure to obtain [MB2-1] as a crude product. Methanol (MeOH, 300 g), pure water (225 g) and potassium hydroxide (50.5 g) were added to the obtained crude product [MB2-1], and the mixture was reacted at 40° C. for 3 hours. After the reaction was completed, 3.0 mol / L aqueous hydrochloric acid solution was added to the reaction solution to precipitate crystals, which were recovered by filtration. Next, the obtained crystals were slurried and washed with pure water (500 g), and then slurried with MeCN (250 g), and the filtrate was dried under reduced pressure to obtain [MB2-2] 124 g (white crystals) (yield: 91%).
[0107] <Synthesis of [MB2-3], [MB2-4], and [MB2-5]> THF (494 g), [MB2-2] (82.3 g, 307 mmol) and triethylamine (Et 3 N, 80.0 g, 790 mmol), chloromethyl methyl ether (27.6 g, 343 mmol) was added dropwise under nitrogen atmosphere and ice-cooling conditions. After the addition, the mixture was reacted under ice-cooling conditions for 2 hours to synthesize [MB2-3]. 4-Dimethylaminopyridine (0.966 g, 7.90 mmol) was added to the reaction solution, and methacryloyl chloride (33.0 g, 316 mmol) was added dropwise under nitrogen atmosphere and ice-cooling conditions. After the addition, the reaction was allowed to react at room temperature for 20 hours to eliminate the raw materials. After the reaction was completed, the reaction solution was diluted with ethyl acetate (1230 g), and the organic phase was washed 3 times with pure water. Then, the organic phase was dehydrated with sodium sulfate, and 2,6-di-tert-butyl-p-cresol (291 mg, 1.32 mmol) was added to the organic phase, and the mixture was concentrated under reduced pressure to obtain a crude product of [MB2-4]. Ethanol (EtOH, 410 g) and pyridinium p-toluenesulfonate (13.2 g, 52.7 mmol) were added to the obtained crude product [MB2-4], and the mixture was reacted at 70°C for 19 hours. After the reaction, the reaction solution was added to pure water (1500 g) to precipitate crude crystals, which were then recovered by filtration. Next, the crude crystals were recrystallized from ethyl acetate (450 g) and MeCN (200 g), and the crystals were filtered out and dried under reduced pressure to obtain 64.6 g (white crystals) of [MB2-5] (yield: 63%).
[0108] <Synthesis of [MB2-6]> THF (213 g), [MB2-5] (35.5 g, 106 mmol) tert-butyl 4-hydroxybenzoate (22.1 g, 114 mmol) and 4-dimethylaminopyridine (DMAP, 1.29 g, 10.6 mmol) were added to a 1000 mL four-necked flask, and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC·HCl, 24.3 g, 127 mmol) was added under nitrogen atmosphere at room temperature, and the reaction was carried out for 23 hours to eliminate the raw materials. After the reaction was completed, the reaction solution was diluted with ethyl acetate (530 g), and the organic phase was washed 3 times with pure water. After the organic phase was recovered, it was concentrated under reduced pressure to obtain a crude product. The obtained crude product was diluted with 2-propanol (76 g) and hexane (70 g), and cooled to -20°C to precipitate crystals, which were filtered and dried under reduced pressure to obtain 43.9 g (yield: 81%) of [MB2-6].
[0109] <Synthesis of [MB2]> In a 1000mL four-necked flask, formic acid (307g) and [MB2-6] (43.9g, 85.6mmol) were added, and the reaction was carried out at 50°C for 1 hour to eliminate the raw materials. After the reaction, the reaction solution was added to pure water (880g) to precipitate crystals, and the crude product was recovered by filtration. The crude product was dissolved in THF (132g), and the solution weight was reduced to 44g by concentrating under reduced pressure. MeCN (66g) was added for slurry washing, and the filtrate was dried under reduced pressure to obtain [MB2] 22.4g (white crystals) (yield: 57%). 1 The results of H-NMR are shown below. From these results, it was confirmed that the obtained solid was the target MB2. 1 H-NMR (400MHz, [D 6]-DMSO): δ (ppm) = 13.1 (s, 1H), 8.02-8.06 (m, 2H), 7.76-7.79 (m, 1H), 7.59 (d, 1H), 7.39-7.42 (m, 2H), 7.16 (d, 1H), 6.02 ( s,1H),5.67(s,1H),4.07-4.12(m,4H),3.85(s,3H),1.88(s,3H),1.74-1.79(m,2H),1.62-1.69(m,2H),1.38-1.48(m,4H)
[0110] <<Synthesis of MB4>> [Chemistry 24] MC1 (10.0 g, 32.6 mmol), DMF (50 mg) and THF (50 g) were added to a 200 mL four-necked flask, oxalyl chloride (4.56 g, 35.9 mmol) was added dropwise, and the mixture was stirred at room temperature. After the reaction was completed, the reaction solution was concentrated with a rotary evaporator to obtain a chloride (light yellow liquid). THF (50 g) and methoxymethyl 3-(4-hydroxyphenyl) propionate (7.19 g, 34.2 mmol) were added to the obtained chloride, ice-cooled under a nitrogen atmosphere, triethylamine (3.96 g, 39.1 mmol) was added dropwise, and the mixture was stirred at room temperature. After the reaction was completed, the reaction solution was concentrated with a rotary evaporator. Ethyl acetate (100 g) was added and extracted with pure water (200 g). The organic layer was concentrated with a rotary evaporator, and the solvent was distilled off to obtain MB4-1 (light brown liquid). MB4-1, MeCN (150 g) and 1 N hydrochloric acid (50 g) were added to a 500 mL single-necked flask and stirred at room temperature. After the reaction was completed, the reaction solution was injected into pure water (200 g) and the precipitate was filtered out. The crude product was recrystallized with ethanol (50 g) to obtain 11.2 g of MB4 (white solid) (yield 76%). 1 The results of H-NMR are shown below. From these results, it was confirmed that the obtained solid was the target MB4. 1 H-NMR (400MHz, [D 6]-DMSO): δ (ppm) = 12.2 (s, 1H), 8.03-8.07 (d, 2H), 7.28-7.32 (d, 2H), 7.13-7.17 (d, 2H), 7.08-7.12 (d, 2H), 6.02 (s, 1H), 5.66 (s, 1 H),4.06-4.13(m,4H),2.82-2.88(m,2H),2.54-2.59(t,2H),1.88(s,3H),1.72-1.80(m,2H),1.61-1.69(m,2H),1.38-1.50(m,4H).
[0111] <<Synthesis of MB5>> [Chemistry 25] MB1 (15.0 g, 35.2 mmol), methoxymethyl 3-(4-hydroxyphenyl)propionate (7.78 g, 37.0 mmol), THF (75 g), 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (8.09 g, 42.2 mmol) and 4-dimethylaminopyridine (0.43 g, 3.52 mmol) were added to a 200 mL four-necked flask and stirred at room temperature. After the reaction was completed, it was poured into pure water (450 g) and the precipitate was filtered out to obtain MB5-1 (white solid). MB5-1, MeCN (225 g) and 1 equivalent hydrochloric acid (75 g) were added to a 500 mL single-necked flask and stirred at room temperature. After the reaction was completed, the precipitate was filtered out and repulp washing was performed with MeCN (45 g). The obtained crude product was recrystallized from a mixed solvent of THF (150 g) and MeCN (150 g), thereby obtaining 12.7 g (yield 63%) of MB5 (white solid). 1 The results of H-NMR are shown below. From these results, it was confirmed that the obtained solid was the target MB5. 1 H-NMR (400MHz, [D 6]-DMSO): δ (ppm) = 12.2 (s, 1H), 8.20-8.24 (d, 2H), 8.08-8.12 (d, 2H), 7.50 -7.54(d,2H),7.31-7.35(d,2H),7.19-7.23(d,2H),7.11-7.16(d,2H),6.0 2(s,1H),5.67(s,1H),4.08-4.14(m,4H),2.84-2.89(t,2H),2.54-2.60(t, 2H),1.88(s,3H),1.73-1.81(m,2H),1.62-1.69(m,2H),1.38-1.51(m,4H).
[0112] [1] Synthesis of polymers <Synthesis example 1> MA1 (3.99 g, 12.0 mmol), MC1 (4.90 g, 16.0 mmol), MB1 (5.12 g, 12.0 mmol) and AIBN (0.66 g, 4.00 mmol) were dissolved in NMP (20.5 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (13.7 g) at 60° C. for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60° C. for 12 hours to obtain a polymer solution P-1.
[0113] <Synthesis example 2> MA1 (3.69 g, 11.1 mmol), MC1 (1.13 g, 3.70 mmol), MB1 (9.47 g, 22.2 mmol) and AIBN (0.61 g, 3.70 mmol) were dissolved in NMP (24.3 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (10.4 g) at 60° C. for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60° C. for 12 hours to obtain a polymer solution P-2.
[0114] <Synthesis Example 3> MA1 (3.59 g, 10.8 mmol), MB1 (10.8 g, 25.2 mmol) and AIBN (0.59 g, 3.60 mmol) were dissolved in NMP (24.4 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (10.4 g) at 60°C for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60°C for 12 hours to obtain a polymer solution P-3.
[0115] <Synthesis example 4> MA1 (3.59 g, 10.8 mmol), MB1 (9.98 g, 23.4 mmol), MC2 (0.69 g, 1.80 mmol) and AIBN (0.59 g, 3.60 mmol) were dissolved in NMP (24.3 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (10.4 g) at 60° C. for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60° C. for 12 hours to obtain a polymer solution P-4.
[0116] <Synthesis example 5> MA1 (3.69 g, 11.1 mmol), MC1 (2.27 g, 7.40 mmol), MB1 (6.31 g, 14.8 mmol), MC2 (1.42 g, 3.70 mmol) and AIBN (0.61 g, 3.70 mmol) were dissolved in NMP (20.0 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (13.3 g) at 60° C. for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60° C. for 12 hours to obtain a polymer solution P-5.
[0117] <Synthesis Example 6> MA1 (3.89 g, 11.7 mmol), MC1 (2.39 g, 7.80 mmol), MB1 (4.99 g, 11.7 mmol), MC2 (2.98 g, 7.80 mmol) and AIBN (0.64 g, 3.90 mmol) were dissolved in NMP (20.8 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (13.9 g) at 60° C. for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60° C. for 12 hours to obtain a polymer solution P-6.
[0118] <Synthesis Example 7> MA1 (2.09 g, 6.30 mmol), MC1 (8.36 g, 27.3 mmol), MB1 (3.58 g, 8.40 mmol) and AIBN (0.69 g, 4.20 mmol) were dissolved in NMP (20.6 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (13.7 g) at 60° C. for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60° C. for 12 hours to obtain a polymer solution P-7.
[0119] <Synthesis example 8> MA1 (1.94 g, 5.85 mmol), MC1 (5.38 g, 17.6 mmol), MB1 (6.65 g, 15.6 mmol) and AIBN (0.64 g, 3.90 mmol) were dissolved in NMP (20.5 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (13.6 g) at 60° C. for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60° C. for 12 hours to obtain a polymer solution P-8.
[0120] <Synthesis Example 9> MA1 (1.84 g, 5.55 mmol), MC1 (2.83 g, 9.25 mmol), MB1 (9.47 g, 22.2 mmol) and AIBN (0.61 g, 3.70 mmol) were dissolved in NMP (24.1 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (10.3 g) at 60°C for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60°C for 12 hours to obtain a polymer solution P-9.
[0121] <Synthesis Example 10> MA1 (1.94 g, 5.85 mmol), MC1 (5.38 g, 17.6 mmol), MB1 (4.99 g, 11.7 mmol), MB2 (1.78 g, 3.90 mmol) and AIBN (0.64 g, 3.90 mmol) were dissolved in NMP (20.6 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (13.7 g) at 60° C. for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60° C. for 12 hours to obtain a polymer solution P-10.
[0122] <Synthesis Example 11> MA1 (2.09 g, 6.30 mmol), MC1 (8.36 g, 27.3 mmol), MB2 (3.83 g, 8.40 mmol) and AIBN (0.69 g, 4.20 mmol) were dissolved in NMP (21.0 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (14.0 g) at 60° C. for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60° C. for 12 hours to obtain a polymer solution P-11.
[0123] <Synthesis Example 12> MA1 (1.99 g, 6.00 mmol), MC1 (5.51 g, 18.0 mmol), MB1 (5.12 g, 12.0 mmol), MC3 (1.65 g, 4.00 mmol) and AIBN (0.66 g, 4.00 mmol) were dissolved in NMP (20.9 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (13.9 g) at 60° C. for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60° C. for 12 hours to obtain a polymer solution P-12.
[0124] <Synthesis Example 13> MA1 (2.09 g, 6.30 mmol), MC1 (8.36 g, 27.3 mmol), MB3 (3.80 g, 8.40 mmol) and AIBN (0.69 g, 4.20 mmol) were dissolved in NMP (20.9 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (14.0 g) at 60° C. for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60° C. for 12 hours to obtain a polymer solution P-13.
[0125] <Synthesis Example 14> MA1 (1.94 g, 5.85 mmol), MC1 (5.38 g, 17.6 mmol), MB4 (7.09 g, 15.6 mmol) and AIBN (0.64 g, 3.90 mmol) were dissolved in NMP (21.1 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (14.0 g) at 60° C. for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60° C. for 12 hours to obtain a polymer solution P-14.
[0126] <Synthesis Example 15> MA1 (1.99 g, 6.00 mmol), MC1 (7.97 g, 26.0 mmol), MB5 (4.58 g, 8.00 mmol) and AIBN (0.66 g, 4.00 mmol) were dissolved in NMP (21.3 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (14.2 g) at 60° C. for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60° C. for 12 hours to obtain a polymer solution P-15.
[0127] <Synthesis Example 16> MA1 (2.04 g, 6.15 mmol), MC1 (6.91 g, 22.6 mmol), MB6 (5.41 g, 12.3 mmol) and AIBN (0.67 g, 4.10 mmol) were dissolved in NMP (21.1 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (14.0 g) at 60°C for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60°C for 12 hours to obtain a polymer solution P-16.
[0128] <Synthesis Example 17> MA1 (2.24 g, 6.75 mmol), MC1 (11.7 g, 38.3 mmol) and AIBN (0.74 g, 4.50 mmol) were dissolved in NMP (20.6 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (13.7 g) at 60°C for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60°C for 12 hours to obtain a polymer solution P-17.
[0129] <Synthesis Example 18> MA1 (4.39 g, 13.2 mmol), MC1 (8.09 g, 26.4 mmol), MC2 (1.68 g, 4.40 mmol) and AIBN (0.72 g, 4.40 mmol) were dissolved in NMP (20.8 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (13.9 g) at 60° C. for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60° C. for 12 hours to obtain a polymer solution P-18.
[0130] <Synthesis Example 19> MA1 (4.19 g, 12.6 mmol), MC1 (5.15 g, 16.8 mmol), MC3 (5.20 g, 12.6 mmol) and AIBN (0.69 g, 4.20 mmol) were dissolved in NMP (21.3 g) to prepare a monomer mixed solution. The monomer mixed solution was added dropwise to NMP (14.2 g) at 60° C. for 2 hours under a nitrogen atmosphere. After the addition was completed, the mixture was reacted at 60° C. for 12 hours to obtain a polymer solution P-19.
[0131] <Synthesis Example 20> Dissolve MD1 (17.5 g, 39.9 mmol) and AIBN (0.328 g, 2.00 mmol) in THF (50.0 g) to prepare a monomer mixed solution. Add the monomer mixed solution dropwise to THF (21.4 g) at 60°C for 2 hours under a nitrogen atmosphere. After the addition is completed, react at 60°C for 12 hours. After the reaction is completed, add the reaction solution to a mixed solution of methanol (450 g) and pure water (180 g) to reprecipitate the polymer. Then, filter, wash with methanol, and dry to obtain polymer powder P-20.
[0132] The monomer compositions of the polymer solutions P-1 to P-19 and polymer powder P-20 obtained above are shown in Table 1. In Table 1, the numerical values in parentheses of the composition represent the blending amount (parts by mole) of each monomer relative to 100 parts by mole of the total monomers used. [Table 1]
[0133] [2] Preparation of materials for forming phase difference films <Preparation Example 1> NMP (0.4 g), BCS (3.6 g) and R40 (3.0 mg) were added to the polymer solution P-1 (20 g) obtained in Synthesis Example 1 and stirred to obtain a polymer solution T-1. The polymer solution T-1 was used as a material for forming a retardation film.
[0134] <Preparation Examples 2 to 19> Polymer solutions T-2 to T-19 were obtained in the same manner as in Preparation Example 1 except that the polymer solution used was replaced by P-2 to P-19 instead of P-1. The polymer solutions T-2 to T-19 were used as materials for forming a retardation film.
[0135] <Preparation Example 20> CPN (11.3 g), BCS (3.75 g) and R40 (2.0 mg) were added to the polymer powder P-20 (3.75 g) obtained in Synthesis Example 20 and stirred to obtain a polymer solution T-20. The polymer solution T-20 was used as a material for forming a retardation film.
[0136] <Preparation Example 21> The polymer solution P-8 (20 g) obtained in Synthesis Example 8 was injected into a methanol / pure water mixed solvent to precipitate the polymer, and the mixture was filtered and washed with methanol to obtain a polymer powder P-8 (4.5 g). NMP (2.0 g), PGME (3.5 g), BCS (1.0 g), PGMEA (1.7 g) and F563 (9.0 mg) were added to the obtained polymer powder P-8 (1.8 g) and stirred to obtain a polymer solution T-21. The polymer solution T-21 was directly used as a material for forming a phase difference film.
[0137] [3]Manufacturing of single-layer retardation film <Example 1> The polymer solution T-1 was filtered through a filter with a pore size of 5.0 μm and then applied to an alkali-free glass substrate using a spin coater in a film thickness of about 3.0 μm. The substrate was dried on a hot plate at 60°C for 4 minutes and then irradiated with ultraviolet light (900 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 170° C. for 20 minutes to prepare a glass substrate S-1 with a retardation film.
[0138] <Example 2> The polymer solution T-2 was filtered through a filter with a pore size of 5.0 μm, and then coated on an alkali-free glass substrate using a spin coater so that the film thickness was about 3.0 μm. The substrate was dried on a hot plate at 60°C for 4 minutes, and then irradiated with ultraviolet light (600 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 190° C. for 20 minutes to prepare a glass substrate S-2 with a retardation film.
[0139] <Example 3> The polymer solution T-3 was filtered through a filter with a pore size of 5.0 μm, and then coated on an alkali-free glass substrate using a spin coater so that the film thickness was about 3.5 μm. The substrate was dried on a hot plate at 60°C for 4 minutes, and then irradiated with ultraviolet light (400 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 200° C. for 20 minutes to prepare a glass substrate S-3 with a retardation film.
[0140] <Example 4> The polymer solution T-4 was filtered through a filter with a pore size of 5.0 μm and then applied to an alkali-free glass substrate using a spin coater in a film thickness of about 3.5 μm. The substrate was dried on a hot plate at 60°C for 4 minutes and then irradiated with ultraviolet light (800 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 200° C. for 20 minutes to prepare a glass substrate S-4 with a retardation film.
[0141] <Example 5> The polymer solution T-5 was filtered through a filter with a pore size of 5.0 μm and then applied to an alkali-free glass substrate using a spin coater in a film thickness of about 3.0 μm. The substrate was dried on a hot plate at 60°C for 4 minutes and then irradiated with ultraviolet light (400 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 190° C. for 20 minutes to prepare a glass substrate S-5 with a retardation film.
[0142] <Example 6> The polymer solution T-6 was filtered through a filter with a pore size of 5.0 μm, and then coated on an alkali-free glass substrate using a spin coater so that the film thickness was about 3.0 μm. The substrate was dried on a hot plate at 60°C for 4 minutes, and then irradiated with ultraviolet light (600 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 190° C. for 20 minutes to prepare a glass substrate S-6 with a retardation film.
[0143] <Example 7> The polymer solution T-7 was filtered through a filter with a pore size of 5.0 μm, and then coated on an alkali-free glass substrate using a spin coater so that the film thickness was about 3.5 μm. The substrate was dried on a hot plate at 60°C for 4 minutes, and then irradiated with ultraviolet light (800 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 170° C. for 20 minutes to prepare a glass substrate S-7 with a retardation film.
[0144] <Example 8> The polymer solution T-8 was filtered through a filter with a pore size of 5.0 μm, and then coated on an alkali-free glass substrate using a spin coater so that the film thickness was about 2.0 μm. The substrate was dried on a hot plate at 60°C for 4 minutes, and then irradiated with ultraviolet light (1000 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 190° C. for 20 minutes to prepare a glass substrate S-8 with a retardation film.
[0145] <Example 9> The polymer solution T-9 was filtered through a filter with a pore size of 5.0 μm, and then coated on an alkali-free glass substrate using a spin coater so that the film thickness was about 3.5 μm. The substrate was dried on a hot plate at 60°C for 4 minutes, and then irradiated with ultraviolet light (800 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 170° C. for 20 minutes to prepare a glass substrate S-9 with a retardation film.
[0146] <Example 10> The polymer solution T-10 was filtered through a filter with a pore size of 5.0 μm, and then applied to an alkali-free glass substrate using a spin coater so that the film thickness was about 3.0 μm. The substrate was dried on a hot plate at 60°C for 4 minutes, and then irradiated with ultraviolet light (400 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 180° C. for 20 minutes to prepare a glass substrate S-10 with a retardation film.
[0147] <Example 11> The polymer solution T-11 was filtered through a filter with a pore size of 5.0 μm and then applied to an alkali-free glass substrate using a spin coater in a film thickness of about 4.0 μm. The substrate was dried on a hot plate at 60°C for 4 minutes and then irradiated with ultraviolet light (200 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 140° C. for 20 minutes to prepare a glass substrate S-11 with a retardation film.
[0148] <Example 12> The polymer solution T-12 was filtered through a filter with a pore size of 5.0 μm and then applied to an alkali-free glass substrate using a spin coater in a film thickness of about 3.0 μm. The substrate was dried on a hot plate at 60°C for 4 minutes and then irradiated with ultraviolet light (200 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 160° C. for 20 minutes to prepare a glass substrate S-12 with a retardation film.
[0149] <Example 13> The polymer solution T-13 was filtered through a filter with a pore size of 5.0 μm, and then applied to an alkali-free glass substrate using a spin coater so that the film thickness was about 2.5 μm. The substrate was dried on a hot plate at 60°C for 4 minutes, and then irradiated with ultraviolet light (400 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 160° C. for 20 minutes to prepare a glass substrate S-13 with a retardation film.
[0150] <Example 14> The polymer solution T-14 was filtered through a filter with a pore size of 5.0 μm and then applied to an alkali-free glass substrate using a spin coater in a film thickness of about 3.2 μm. The substrate was dried on a hot plate at 60°C for 4 minutes and then irradiated with ultraviolet light (100 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 140° C. for 20 minutes to prepare a glass substrate S-14 with a retardation film.
[0151] <Example 15> The polymer solution T-15 was filtered through a filter with a pore size of 5.0 μm and then applied to an alkali-free glass substrate using a spin coater in a film thickness of about 3.2 μm. The substrate was dried on a hot plate at 60°C for 4 minutes and then irradiated with ultraviolet light (200 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 170° C. for 20 minutes to prepare a glass substrate S-15 with a retardation film.
[0152] <Example 16> The polymer solution T-16 was filtered through a filter with a pore size of 5.0 μm and then applied to an alkali-free glass substrate using a spin coater in a film thickness of about 2.3 μm. The substrate was dried on a hot plate at 60°C for 4 minutes and then irradiated with ultraviolet light (800 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 120° C. for 20 minutes to prepare a glass substrate S-16 with a retardation film.
[0153] <Example 17> The polymer solution T-21 was filtered through a filter with a pore size of 5.0 μm, and then applied to an alkali-free glass substrate using a spin coater in a manner such that the film thickness was about 2.5 μm. The substrate was dried in a heat cycle oven at 80°C for 4.5 minutes, and then irradiated with ultraviolet light (1000 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 190° C. for 20 minutes to prepare a glass substrate S-17 with a retardation film.
[0154] <Comparative Example 1> The polymer solution T-17 was filtered through a filter with a pore size of 5.0 μm and then applied to an alkali-free glass substrate using a spin coater in a film thickness of about 3.0 μm. The substrate was dried on a hot plate at 60°C for 4 minutes and then irradiated with ultraviolet light (800 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 140° C. for 20 minutes to prepare a glass substrate R-1 with a retardation film.
[0155] <Comparative Example 2> The polymer solution T-18 was filtered through a filter with a pore size of 5.0 μm, and then coated on an alkali-free glass substrate using a spin coater so that the film thickness was about 3.0 μm. The substrate was dried on a hot plate at 60°C for 4 minutes, and then irradiated with ultraviolet light (200 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 160° C. for 20 minutes to prepare a glass substrate R-2 with a retardation film.
[0156] <Comparative Example 3> The polymer solution T-19 was filtered through a filter with a pore size of 5.0 μm, and then coated on an alkali-free glass substrate using a spin coater so that the film thickness was about 3.0 μm. The substrate was dried on a hot plate at 60°C for 4 minutes, and then irradiated with ultraviolet light (50 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (365 nm bandpass filter) and a polarizing plate. 2 ). The substrate was heated in an IR oven at 110° C. for 20 minutes to prepare a glass substrate R-3 with a retardation film.
[0157] <Comparative Example 4> The polymer solution T-20 was filtered through a filter with a pore size of 5.0 μm and then applied to an alkali-free glass substrate using a spin coater in a film thickness of about 0.8 μm. The substrate was dried on a hot plate at 60°C for 4 minutes and then irradiated with ultraviolet light (600 mJ / cm2) at a wavelength of 365 nm from a high-pressure mercury lamp through a cutoff filter (325 nm long-wave pass filter) and a polarizing plate. 2 ). The substrate was heated in a heat circulation oven at 130° C. for 20 minutes to prepare a glass substrate R-4 with a retardation film.
[0158] The retardation values and NZ coefficients of the substrates S-1 to S-17 and R-1 to R-4 with retardation films were evaluated by the following methods.
[0159] [Phase difference evaluation] The linear phase difference at a wavelength of 550 nm was evaluated using AxoScan manufactured by Axometrics, and the results are summarized in Table 2.
[0160] [NZ coefficient evaluation] The refractive index in the three-dimensional direction of the retardation film at a wavelength of 550 nm was measured using AxoScan manufactured by Axometrics, and the NZ coefficient was calculated. The NZ coefficient is an index of the magnitude relationship of the three-dimensional refractive index and is represented by the following formula. NZ coefficient = (nx-nz) / (nx-ny) nx: Refractive index in the x-axis direction (slow axis direction) ny: Refractive index in the y-axis direction (direction perpendicular to the slow axis) nz: refractive index in the z-axis direction (thickness direction) For the glass substrates S-1 to S-17 and R-1 to R-3 with retardation film, it was assumed that the average refractive index of the retardation film was 1.55, and for the glass substrate R-4 with retardation film, it was assumed that the average refractive index was 1.60, and the NZ coefficient was calculated. The results are summarized in Table 2.
[0161] [Table 2] Substrate serial number Phase difference [nm] NZ coefficient Example 1 S-1 303 0.53 Example 2 S-2 286 0.50 Example 3 S-3 271 0.44 Example 4 S-4 372 0.53 Example 5 S-5 290 0.52 Example 6 S-6 309 0.53 Example 7 S-7 333 0.49 Example 8 S-8 181 0.50 Example 9 S-9 256 0.58 Example 10 S-10 286 0.49 Embodiment 11 S-11 112 0.45 Example 12 S-12 324 0.53 Embodiment 13 S-13 259 0.52 Embodiment 14 S-14 321 0.54 Embodiment 15 S-15 336 0.51 Example 16 S-16 203 0.41 Embodiment 17 S-17 235 0.51 Comparative Example 1 R-1 210 0.19 Comparative Example 2 R-2 190 -0.02 Comparative Example 3 R-3 194 -0.13 Comparative Example 4 R-4 119 0.97
[0162] The NZ coefficients of the retardation films R-1 to R-4 that do not contain a side chain of a terminal carboxylic acid having a ring structure having two or more rings and in which the two rings located at the terminal side are not covalently bonded by a single bond are values close to 0 or 1. On the other hand, the NZ coefficients of the retardation films S-1 to S-17 prepared with the composition having the above side chains are 0.4 to 0.6.
Claims
1. A composition for a phase difference film, characterized in that: Include: (A) a side chain type copolymer comprising a terminal carboxylic acid side chain having a photoreactive site and a terminal carboxylic acid side chain having an aromatic ring structure of two or more rings in which the two rings located at the terminal side are not covalently bonded by a single bond, and (B) Organic solvent.
2. The composition for phase difference film according to claim 1, wherein The side chain type copolymer (A) is a side chain type polymer having a side chain having a photoreactive site represented by the following formula (a) and a side chain having a site represented by the following formula (b), In the formula, R 1 is an alkylene group having 1 to 30 carbon atoms, wherein one or more hydrogen atoms of the alkylene group may be replaced by a fluorine atom or an organic group; in addition, R 1 The -CH2CH2- in the R 1 The -CH2- in the formula (a) is or is not replaced by a group selected from -O-, -NH-C(=O)-, -C(=O)-NH-, -C(=O)-O-, -OC(=O)-, -NH-, -NH-C(=O)-NH- and -C(=O)-, wherein adjacent -CH2- are not replaced by these groups at the same time, R 2 is a divalent aromatic group, a divalent alicyclic group, a divalent heterocyclic group or a divalent condensed ring group, R 3 is a single bond, -CH2-, -O-, -C(=O)-O-, -OC(=O)- or -CH=CH-C(=O)- O-, R 4 is a divalent aromatic group, -Ph-Cy-, -Cy-Ph- or a divalent condensed ring group, wherein Ph represents a phenylene group, and Cy represents a cyclohexanediyl group, R 5 is -CH2-, -O-, -NH-, -C(=O)-, -C(=O)-O-, -O-C(=O)-, -CH= CH-C(=O)-O-, -C(=O)-NH-, -NH-C(=O)- or -NH-C(=O)-NH-, R 6 is an alkylene group having 1 to 10 carbon atoms, wherein one or more hydrogen atoms of the alkylene group may be replaced by a fluorine atom or an organic group; in addition, R 6 The -CH2- in the -CH2- is or is not replaced by a group selected from -O-, -NH- and -C(=O)-, and when replaced, the adjacent -CH2- is or are not replaced by these groups at the same time, The hydrogen atoms in the ring structure and the CH=CH structure in formula (a) are or are not replaced by a substituent selected from an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a halogen group, a cyano group and a nitro group, The hydrogen atoms in the ring structure in formula (b) are or are not replaced by a substituent selected from an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a halogen group, a cyano group and a nitro group, In the presence of two or more R 2 , R 3 , R 4 or R 5 In the case of multiple R 2 , R 3 , R 4 or R 5 Same or different from each other, a is 0, 1, or 2, b is 0 or 1, c is an integer satisfying 0≤c≤2b+4, d is 1 or 2, e is 0 or 1, f is 0 or 1, The dotted lines are bonding bonds.
3. The composition for phase difference film according to claim 2, wherein The side chain having a photoreactive site represented by the formula (a) is a side chain represented by the following formula (a1), In formula (a1), R 1 , R 2 and a are the same as above, R 3A is a single bond, -O-, -C(=O)-O- or -OC(=O)-; when there are two or more R 3A In the case of multiple R 3A Same or different from each other, The hydrogen atoms in the benzene ring and the CH═CH structure in formula (a1) are or are not replaced by a substituent selected from an alkyl group having 1 to 6 carbon atoms, a haloalkyl group having 1 to 6 carbon atoms, an alkoxy group having 1 to 6 carbon atoms, a haloalkoxy group having 1 to 6 carbon atoms, a halogen group, a cyano group and a nitro group, The dotted lines are bonding bonds.
4. The polymer composition and the composition for phase difference film according to claim 2, wherein: The number of ring structures in the side chain represented by the formula (b) is 3 or less.
5. The composition for phase difference film according to claim 1, wherein Side chain polymers exhibit liquid crystal properties.
6. A method for manufacturing a single-layer phase difference material, characterized in that: The process includes the following steps: (I) a step of applying the phase difference film composition according to any one of claims 1 to 5 onto a substrate to form a coating film; (II) irradiating the coating film with polarized ultraviolet rays; and (III) A step of heating the coating film irradiated with ultraviolet rays to obtain a phase difference material.
7. A single-layer phase difference material, characterized in that: The composition is obtained from any one of claims 1 to 5.
Citation Information
Patent Citations
Production of optical isomer
JP1997208957A
Birefringent film and its production
JP1999189665A
Retardation film and method for producing the same
JP2008164925A
Ink for color filter, color filter, manufacturing method for color filter, image display device, and electronic equipment
JP2009019117A
Photo-aligning agent comprising photosensitive high polymer, liquid crystal aligned layer using photo-aligning agent, and liquid crystal display element using liquid crystal aligned layer