Brazing method, brazed joint and brazing filler metal

By using the reaction between the active solder and the AgC contacts and the Cu carrier to form metal carbides and directly soldering the AgC contacts to the Cu carrier, the problems of increased cost and complexity in the existing technology are solved and high quality is achieved. joint combination.

CN118872015APending Publication Date: 2024-10-29ABB (SCHWEIZ) AG
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380026915.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-26
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

When bonding silver graphite-based contacts (AgC contacts) to a Cu carrier, the existing technology requires an Ag layer to be formed on the back of the contact to ensure wetting, but this increases cost and manufacturing complexity, and pure silver and copper cannot Wets graphite, resulting in low strength and high resistance in the bonded area.

Method used

The AgC contacts are soldered directly to the Cu carrier using active solder, and active elements such as Ti, Hf, Zr, Cr, Si and V react with graphite to form metal carbides to achieve wetting and bonding, avoiding additional processing steps. and material addition.

Benefits of technology

The manufacturing process is simplified, cost is reduced, the environmental footprint is reduced, and a high-quality joint is produced, ensuring good bonding of the AgC contacts to the Cu carrier.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118872015A_ABST
    Figure CN118872015A_ABST
Patent Text Reader

Abstract

A brazing method for providing a brazed joint is provided. The method includes brazing the AgC contact directly to the Cu support using an active solder.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a brazing method, a brazing joint and a brazing material. Background Art

[0002] Currently, when a silver graphite-based contact (hereinafter referred to as an AgC contact) is bonded to a Cu carrier, this requires the formation of an Ag layer on the back side of the contact to ensure wetting by the solder. This layer is formed by adding Ag.

[0003] More specifically, conventional brazing alloys, typically of the Cu-Ag-P family, wet only the metal portion of the contact, but do not form any bond with the carbon / graphite contained. Neither pure silver nor copper (and their binary alloys) wet graphite, since there is no chemical reaction. This reduces the bonding area, leaving a low-strength and high-resistance joint. In practice, this problem is solved by joining an Ag layer (also referred to as a backing layer) to the contact, for example by rolling or electroplating.

[0004] This increases costs due to additional processing steps during contact manufacturing and / or by adding expensive materials.

[0005] It is an object of the present invention to provide a method and a solder which allow the bonding of AgC contacts to a Cu carrier while alleviating at least some of the above-mentioned disadvantages. Summary of the invention

[0006] This object is achieved by the present invention. The present invention provides a brazing method, a brazing joint and a brazing filler metal according to the independent claims. Preferred embodiments are listed in the dependent claims.

[0007] The present invention provides a brazing method for obtaining a brazed joint. The method comprises brazing an AgC contact directly to a Cu carrier using an active brazing filler metal.

[0008] The advantage of this method is that no additional processing steps are required, such as adding a backing layer. Therefore, manufacturing is simplified and costs are reduced. The method also allows for a reduced environmental footprint.

[0009] According to the present disclosure, the AgC contact is brazed directly onto the Cu carrier, for example, without creating a wetting backing layer.The present disclosure uses an active brazing filler metal, which in this particular case allows wetting and bonding to the graphite portion of the contact material.

[0010] According to the present disclosure, directly brazing the AgC contact to the Cu carrier may mean that, except for the brazing material, there is no added material layer between the AgC contact and the Cu carrier. In particular, this excludes the backing layer. In addition, the method according to the present disclosure may require that the AgC contact material is not decarburized before brazing.

[0011] In the present disclosure, the AgC contact may be made of any AgC-based contact material, in particular AgC with and without additives. For example, the AgC contact may include at least Ag and C, and may optionally include one or more additives.

[0012] An active element may be an element that has a high affinity for carbon, forms carbides or dissolves carbon and thus promotes wetting. Further details on active elements are provided below.

[0013] Brazed Contacts of the Disclosure The disclosure may be used as contacts of a switching device, such as a contactor or a circuit breaker.

[0014] The active brazing filler metal according to the present disclosure may be an alloy including one or more active elements, particularly active elements that react with the exposed carbon of the AgC contact, particularly, to form metal carbides and / or dissolve carbon.

[0015] Metal carbide layers can grow on and into graphite. Therefore, they adhere well and are also wetted by the metal brazing filler metal. This allows metal brazing, especially active brazing fillers based on Cu-Ag, to be bonded to large areas of contact material.

[0016] According to the present disclosure, the one or more active elements include at least one of Ti, Hf, Zr, Cr, Si, and V.

[0017] Alternatively or additionally, in accordance with the present disclosure, the one or more active elements may include an element having a high affinity for carbon / graphite.

[0018] High affinity can refer to a negative heat of formation of the corresponding metal carbide. A more negative heat of formation indicates a higher affinity and ability to form the corresponding metal carbide. In particular, elements that form metal carbides have a heat of formation more negative than -40 kcal / mol, showing the highest affinity, however, elements with a heat of formation as high as -5 kcal / mol may have sufficient affinity.

[0019] Alternatively or additionally, according to the present disclosure, the one or more active elements may include elements that promote wetting of the active braze to the contact and / or bonding of the active braze to the contact, particularly including elements that allow the braze to wet the graphite in the AgC contact.

[0020] The one or more active elements may include elements that form carbides or dissolve carbon to form a metal-carbon solid solution, particularly at brazing temperatures. This allows wetting of the brazing material because the brazing alloy is now not in direct contact with the graphite / carbon, but rather with the reaction products of the active element and the carbon / graphite.

[0021] Alternatively or additionally, according to the present disclosure, each of the one or more active elements may be added in an amount equal to or less than 5 wt %. In particular, the active brazing material may include exactly one active element, and the amount of the active element added may be equal to or less than 5 wt %.

[0022] According to the present disclosure, the active solder may include at least one of Ag and Cu. These solder elements are compatible with AgC and Cu. This does not exclude the addition of other compatible solder elements, such as Ni.

[0023] According to the present disclosure, the solidus of the active solder may be equal to or less than the melting point of Ag. For example, the solidus may be equal to or less than 962°C.

[0024] The method of the present disclosure may include applying an active solder to the AgC contact and / or Cu carrier in the form of a powder and / or paste and / or foil. In particular, the method of the present disclosure may include placing an active solder, such as a paste, powder or foil, on the AgC contact or the Cu carrier, and then sandwiching the solder between the AgC contact and the Cu carrier. It should be understood that the applying step is performed before applying heat for brazing.

[0025] The method of the present disclosure may include, in a processing step separate from brazing, in particular prior to brazing, producing a coated AgC contact coated with an active brazing material, such that the coated AgC contact is suitable for storage and suitable for brazing at a later point in time by applying heat. The coated AgC contact may be used as the AgC contact described throughout the present disclosure.

[0026] Alternatively or additionally, the method of the present disclosure may include producing a coated Cu carrier coated with an active brazing filler metal in a processing step separate from brazing, in particular prior to brazing, such that the coated Cu carrier is suitable for storage and suitable for brazing at a later point in time by applying heat. The coated Cu carrier may be used as the Cu carrier described throughout the present disclosure.

[0027] The use of coated Cu supports or AgC contacts can simplify subsequent processing steps and material handling.

[0028] According to the present disclosure, directly brazing the AgC contact to the Cu carrier may include performing heating, wherein the active brazing material is interposed between the Cu carrier and the AgC contact and contacts each of the Cu carrier and the AgC contact, in particular, wherein the heating includes induction heating and / or resistance heating and / or furnace heating.

[0029] According to the present disclosure, brazing may be performed in an oxidizing atmosphere, such as air, or in a protective gas atmosphere, or in a vacuum.

[0030] For example, brazing can be performed in a protective gas or vacuum to minimize the risk of oxidation by resistive heating, or can be performed by induction heating in air. The operating speed of induction or resistive heating allows a reaction to occur between the brazing material and the contact before significant oxidation occurs. Therefore, a protective atmosphere is not required.

[0031] According to the present disclosure, brazing may be performed within a heating time of 20 seconds or less, in particular 15 seconds or less, in particular 10 seconds or less, in particular 5 seconds or less, in particular 3 seconds.

[0032] According to the present disclosure, brazing may be performed at a temperature equal to or less than 1000° C. and equal to or greater than 500° C., particularly equal to or less than 1000° C. and equal to or greater than 600° C., particularly equal to or less than 1000° C. and equal to or greater than 700° C., particularly equal to or less than 1000° C. and equal to or greater than 800° C. As an example, brazing may be performed at a temperature equal to or less than 962° C. and equal to or greater than 640° C.

[0033] An example of the method of the present disclosure includes induction brazing in air or argon using AgCuTi active brazing filler metal in foil form, for example by heating at a temperature between 818° C. and 962° C. for 12 seconds.

[0034] Another example of the method of the present disclosure includes resistance brazing in air using AgCuTi active brazing filler metal in paste form, for example by heating at a temperature between 818° C. and 962° C. for 3 seconds.

[0035] Another example of the method of the present disclosure includes brazing in air using an AgCuCr active brazing filler metal, for example by heating at a temperature between 818° C. and 962° C. for 3 seconds.

[0036] Another example of the method of the present disclosure includes brazing with a AgCuCr active brazing filler metal at a maximum temperature of less than 962° C. for 12 seconds.

[0037] Another example of the method of the present disclosure includes brazing with AgCuCr active brazing filler metal in a vacuum furnace at 800° C. to 960° C. for 5 to 15 minutes.

[0038] The present invention also provides an active brazing filler metal configured to allow direct brazing of AgC contacts to a Cu carrier. In particular, the active brazing filler metal of the present invention may be configured to be used in a method according to the present disclosure, in particular as described above.

[0039] The active brazing filler metal according to the present disclosure may be an alloy including one or more active elements, in particular to react with the exposed carbon of the AgC contact, in particular, to form metal carbides and / or dissolve carbon.

[0040] The one or more active elements may include at least one of Ti, Hf, Zr, Cr, Si and V. Alternatively or additionally, the one or more active elements may include an element with a high affinity for carbon / graphite. Alternatively or additionally, the one or more active elements include an element that promotes wetting of the contacts by an active brazing filler metal and / or promotes bonding of the contacts by an active brazing filler metal, particularly an element that allows brazing wetting of graphite in an AgC contact.

[0041] The addition amount of each of the one or more active elements may be equal to or less than 5 wt.%. In particular, the active brazing material may include exactly one active element, and the addition amount of the active element may be equal to or less than 5 wt.%.

[0042] The solidus of the active solder of the present disclosure may be equal to or less than the melting point of Ag, in particular, equal to or less than 962° C. Alternatively or additionally, the active solder may include at least one of Ag and Cu in addition to the one or more active elements.

[0043] The invention also provides a brazed joint 1 having an AgC contact brazed directly to a Cu carrier by means of an active brazing filler metal, in particular an active brazing filler metal according to the present disclosure, for example, as described or claimed. The brazed joint may be a brazed joint obtained by implementing a method according to the present disclosure, in particular as described or claimed.

[0044] The features and advantages of the above-described methods are also applicable to the active brazing filler metals and brazed joints described herein.

[0045] Further features, examples and advantages will become apparent from the detailed description taken with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0046] In the accompanying drawings,

[0047] Figure 1 schematically illustrates a brazed joint according to the present disclosure;

[0048] Figure 2 The diagram shows Ag5C brazed directly to a Cu support with Ag-35.25Cu-1.75Ti;

[0049] Figure 3 Elemental mapping of induction brazed joints of Ag5C to Cu using Ag-35.25Cu-1.75Ti is illustrated; and

[0050] Figure 4 The connection of the AgC contact to the Cu carrier via a backing layer provided by the prior art is schematically illustrated. DETAILED DESCRIPTION

[0051] Figure 1 A brazed joint 1 is schematically illustrated comprising an AgC contact 2 brazed directly to a Cu carrier 3 using an active brazing filler metal 4 according to the present disclosure.

[0052] The active solder may include Ag and / or Cu and an active element selected from Ti, Hf, Zr, Cr, Si and V. For example, the active solder may include an AgCu alloy including one or more of the elements, such as an AgCuTi or AcCuCr alloy. It will be appreciated that additional elements, in particular additional active elements, may be included in the alloy.

[0053] The brazing method according to the present disclosure includes brazing the AgC contact 2 directly to the Cu carrier 3 using an active brazing material, such as the above-mentioned active brazing material, such as an AgCu alloy including active elements (such as Ti and / or Cr). Therefore, a brazing joint 1 according to the present disclosure can be obtained. Brazing can include performing heating, such as conductive heating, resistance heating or furnace heating, in the case where the active brazing material is between the Cu carrier and the AgC contact and in contact with each of the Cu carrier and the AgC contact. Heating can be performed in air or a protective gas atmosphere. The method may include, before brazing, placing an active brazing material in the form of a foil or paste between the Cu carrier and the AgC brazing material, or applying the active brazing material to the Cu carrier or the AgC contact by coating the Cu carrier or the AgC contact with the active brazing material.

[0054] Figure 2 The brazing of Ag5C directly to a Cu carrier with Ag-35.25Cu-1.75Ti in argon and air is illustrated. Both atmospheres give good joints and wet the graphite in Ag5C. In this specific example, Ag5C contacts (5.5×7 mm) were induction brazed to Cu using Ag-35.25Cu-1.75Ti (wt.%) brazing foil in air. The power level was 8.5 kW and the brazing was performed in 10 seconds.

[0055] If brazing was performed under Ar or in air, the resulting joint showed no pores along the interface and showed good bonding to the Ag5C. Thus, the technique is suitable for rapid active brazing even in an oxidizing environment. This is significantly different from the typical use of active brazing filler metals, such as brazing ceramics in a high vacuum furnace.

[0056] Figure 3Elemental mapping of an induction brazed joint of Ag5C to Cu using Ag-35.25Cu-1.75Ti in air, performed by energy dispersive X-ray spectroscopy in an electron microscope, is shown. The mapping demonstrates the extent of the Ag5C extending into the brazed joint and the enrichment of Ti in the interface region. The remaining Ti in the braze forms Cu-Ti intermetallics throughout the joint. No extensive oxidation was observed within the brazed joint.

[0057] This demonstrates that direct brazing of AgC contacts to a Cu carrier using an active brazing filler metal in accordance with the present disclosure does produce a high quality joint.

[0058] Other examples of brazing methods of the present disclosure are provided below.

[0059] Example 1: AgC was induction brazed in air with Ag-35.25Cu-1.75Ti foil (commercially available) at temperatures between 818°C and 962°C in 12 seconds.

[0060] Example 2: Induction brazing of AgC with Ag-35.25Cu-1.75Ti foil (commercially available) in argon at temperatures between 818°C and 962°C in 12 seconds.

[0061] Example 3: Resistance brazing of AgC in air with Ag-35.25Cu-1.75Ti paste (commercially available) at temperatures between 818°C and 962°C in 3 seconds.

[0062] Example 4: Induction brazing of AgC with Ag-(20 to 80)Cu-<5Cr in 12 seconds at a maximum temperature below 962°C.

[0063] Example 5: AgC was brazed with Cu-(20-80)Ag-<2Cr filler metal in a vacuum furnace at 800°C to 960°C within 5 to 15 minutes.

[0064] As can be seen from the above, the present disclosure provides a new bonding concept, which uses active solder to braze AgC contacts, such as for circuit breakers, directly to Cu carriers. The active solder can contain Ti, Hf, Zr, Cr, Si and / or V, which react with the non-wetting graphite (C) usually in the AgC contact material, thereby ensuring wettability and good bonding without the need for an Ag backing layer. This allows for a reduced environmental footprint and cost.

[0065] For example, AgC contacts are soldered directly to a Cu support without a backing layer to create wetting by deoxidation or plating on the contacts.

[0066] The solder according to the present disclosure may contain one or more of Ti, Hf, Zr, Cr, Si and / or V as active elements, wherein the remainder of the solder may be one or more of Ag, Cu and Ni. The solder may be applied in the form of a powder, paste or foil. The solder may be placed on a contact or carrier in a previous step, or may be applied immediately before brazing. Brazing may be performed by resistance or induction heating or by providing heat in a furnace in a protective gas, vacuum or air.

[0067] The present disclosure uses active brazing filler metal to achieve wetting and bonding of the graphite portion of the contact material. The active brazing filler metal can be achieved by adding an active element or a mixture of several elements to the alloy.

[0068] As an example, an element can be added to the brazing alloy, usually in an amount of <5wt.%, showing a high affinity for carbon / graphite. Suitable elements include Ti, Zr, Hf, Cr, Si and V, which all form stable metal carbides. If these elements are added to the brazing alloy, they will react with the carbon exposed in the contact material, thereby locally forming metal carbides. These layers grow on graphite and enter the graphite. Therefore, they adhere well, but are also wetted by the metal brazing filler metal. This allows the metal brazing filler metal, typically based on Cu-Ag, to be bonded to the contact material of large area.

[0069] The method disclosed herein is compatible with different brazing methods. The solder can be applied in the form of foil, powder or paste. The solder can be placed between the contact and the carrier immediately before brazing, or added to the contact or carrier in a previous operation. The latter simplifies later / subsequent processing steps and material handling. Brazing can be performed in a protective gas or vacuum to minimize the risk of oxidation by resistance or induction heating, or can be performed in air by resistance or induction heating. The operating speed of induction heating allows a reaction to occur between the solder and the contact before significant oxidation occurs.

[0070] Figure 4 It is schematically illustrated that the AgC contact 2 is bonded to the Cu carrier 3 via a backing layer 6 and a solder 5 provided in the prior art.

[0071] Although the present invention has been described in detail in the drawings and the foregoing description, such description and illustration are to be considered as illustrative rather than restrictive. The present invention is not limited to the disclosed embodiments. In view of the foregoing description and the drawings, it will be apparent to those skilled in the art that various modifications may be made within the scope of the present invention as defined by the claims.

Claims

1. A brazing method for obtaining a brazed joint (1), the method comprising brazing an AgC contact (2) directly to a Cu carrier (3) using an active brazing filler metal (4).

2. The method according to claim 1, wherein the active brazing filler metal (4) is an alloy comprising one or more active elements, in particular active elements that react with the exposed carbon of the AgC contact, in particular, so as to form metal carbides and / or dissolve the carbon.

3. The method of claim 2, wherein the one or more active elements include at least one of Ti, Hf, Zr, Cr, Si and V.

4. A method according to claim 2 or 3, wherein the one or more active elements include an element having a high affinity for carbon / graphite.

5. The method according to any one of claims 2 to 4, wherein the one or more active elements include elements that promote wetting of the contact by the active brazing filler metal and / or promote bonding of the contact by the active brazing filler metal, in particular including elements that allow the brazing filler metal to wet the graphite in the AgC contact.

6. The method according to any one of claims 2 to 5, wherein the amount of each of the one or more active elements added is equal to or less than 5 wt.%, in particular, wherein the active solder comprises exactly one active element and the amount of the active element added is equal to or less than 5 wt.%.

7. The method according to any one of claims 2 to 6, wherein the active solder (4) comprises at least one of Ag and Cu.

8. The method according to any one of the preceding claims, wherein the solidus of the active solder (4) is equal to or less than the melting point of Ag.

9. The method according to any of the preceding claims, comprising applying the active brazing material (4) to the AgC contact (2) and / or the Cu carrier (3) in the form of a powder and / or a paste and / or a foil.

10. The method according to any one of claims 1 to 8, further comprising: producing, in a processing step separate from said brazing, a coated AgC contact coated with said active brazing material (4), such that said coated AgC contact is suitable for storage and for brazing at a later point in time by applying heat, and in particular for use as said AgC contact (2), and / or In a processing step separate from the brazing, a coated Cu carrier coated with the active brazing material (4) is produced, so that the coated Cu carrier is suitable for storage and for brazing by applying heat at a later point in time, and in particular, the coated Cu carrier is used as the Cu carrier (3).

11. The method according to any one of the preceding claims, wherein directly brazing the AgC contact (2) to the Cu carrier (3) comprises performing heating, wherein the active brazing material (4) is interposed between the Cu carrier (3) and the AgC contact (2) and is in contact with each of the Cu carrier (3) and the AgC contact (2), in particular, wherein the heating comprises induction heating and / or resistance heating and / or furnace heating.

12. The method according to any one of the preceding claims, wherein the brazing is performed in an oxidizing atmosphere, such as air, or in a protective gas atmosphere, or in a vacuum, and / or wherein the brazing is performed in a time equal to or less than 20 seconds, in particular equal to or less than 15 seconds, in particular equal to or less than 10 seconds, in particular equal to or less than 5 seconds, in particular 3 seconds, and / or Wherein the brazing is performed at a temperature equal to or less than 1000°C and equal to or greater than 500°C, particularly equal to or less than 1000°C and equal to or greater than 600°C, particularly equal to or less than 1000°C and equal to or greater than 700°C, particularly equal to or less than 1000°C and equal to or greater than 800°C.

13. An active solder (4) configured to allow direct soldering of an AgC contact (2) to a Cu carrier (3), in particular configured to be used in a method according to any one of the preceding claims.

14. The solder according to claim 13, wherein the active brazing filler metal is an alloy comprising one or more active elements, in particular reacting with exposed carbon of the AgC contact, in particular thereby forming metal carbides and / or dissolved carbon, and / or wherein the one or more active elements include at least one of Ti, Hf, Zr, Cr, Si and V, and / or wherein the one or more active elements include an element having a high affinity for carbon / graphite, and / or wherein the one or more active elements include elements that promote wetting of the contact by the active brazing filler metal and / or promote bonding of the contact by the active brazing filler metal, in particular including elements that allow the brazing filler metal to wet the graphite in the AgC contact, and / or wherein the amount of each of the one or more active elements added is equal to or less than 5 wt.%, in particular, wherein the active solder comprises exactly one active element and the amount of the active element added is equal to or less than 5 wt.%, and / or The solidus of the active solder is equal to or less than the melting point of Ag, in particular equal to or less than 962°C, and / or In addition to the one or more active elements, the active solder includes at least one of Ag and Cu.

15. A solder joint (1) having an AgC contact (2) soldered directly to a Cu carrier (3) by means of an active solder (4), in particular an active solder (4) according to claim 13 or 14, in particular a solder joint (1) obtained by implementing a method according to any one of claims 1 to 12.