Vacuum thin film modifying agent, thin film modifying composition comprising same, thin film forming method using same, semiconductor substrate produced

By using aromatic compounds containing hydrocarbon and halogen groups as vacuum film modifiers in semiconductor components, combined with organic solvents with low dielectric constants, the problems of film growth rate control and impurity contamination at high temperatures are solved, and high step coverage is achieved. Film formation with uniformity and thickness improves film quality and electrical properties.

CN118872027APending Publication Date: 2024-10-29SOULBRAIN CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027561.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-10-26
Filing Date
2023-10-11
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

In semiconductor components, it is difficult to form a thin film with uniform thickness on a substrate with a complex structure at high temperature using existing technology, and it is difficult to achieve 100% step coverage, and there is also the problem of impurity contamination.

Method used

Aromatic compounds containing hydrocarbon groups and halogen groups are used as vacuum film modifiers. By controlling the growth rate and reaction surface of the film, combined with organic solvents with a dielectric constant of less than 15, vacuum deposition or etching processes are performed to form high step coverage. and thickness uniformity of the film.

Benefits of technology

It significantly improves step coverage and film thickness uniformity, reduces contamination from impurities such as carbon, improves film quality and electrical properties, and reduces the risk of corrosion and degradation of process by-products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118872027A_ABST
    Figure CN118872027A_ABST
Patent Text Reader

Abstract

The present invention relates to a vacuum thin film modifying agent, a thin film modifying composition comprising the same, a thin film forming method using the same, a semiconductor substrate manufactured by the method, and a semiconductor device, by providing a compound having a predetermined structure as a vacuum thin film modifying agent, to appropriately reduce the growth rate of a deposited film in a vacuum thin film process, and to a method for forming a thin film using the same. According to the present invention, even if a thin film is formed on a substrate having a complicated structure, the step cover and the thickness uniformity of the thin film can be greatly improved, the efficiency of etching the film can be improved, and the contamination of impurities such as carbon can be significantly reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a vacuum thin film modifier, a thin film modification composition containing the same, a thin film forming method using the same, and a semiconductor substrate and a semiconductor element manufactured by the method. Specifically, a vacuum thin film modifier, a thin film modification composition containing the same, a thin film forming method using the same, and a semiconductor substrate manufactured by the method are provided. By providing a compound of a specified structure as a vacuum thin film modifier, the growth rate of the deposited film can be appropriately reduced in the vacuum thin film process, so that even if a thin film is formed on a substrate with a complex structure, the step coverage and the thickness uniformity of the thin film can be greatly improved, the efficiency of etching the film can be improved, and the contamination of impurities such as carbon can be significantly reduced. Background Art

[0002] As the integration of memory and non-memory semiconductor elements increases, the fine structure of the substrate becomes increasingly complex.

[0003] As an example, the ratio of the width to the depth of the fine structure (hereinafter also referred to as the "aspect ratio") increases to above 20:1, or even above 100:1. The larger the aspect ratio, the more difficult it is to form a deposition layer of uniform thickness along the surface of the complex fine structure.

[0004] Therefore, the step coverage in the depth direction of the fine structure (step coverage; defined as the ratio of the thickness of the deposited layer formed on the upper and lower parts) remains at around 90%, making it increasingly difficult to show the electrical characteristics of the component, and therefore its importance is gradually increasing. When the above step coverage is 100%, it means that the thickness of the deposited layer formed on the upper and lower parts of the fine structure is the same, so it is necessary to develop a technology that makes the step coverage as close to 100% as possible.

[0005] The above-mentioned semiconductor thin films include nitride films, oxide films, metal films, etc. The above-mentioned nitride films include silicon nitride (SiN), titanium nitride (TiN), tantalum nitride (TaN), etc. The above-mentioned oxide films include silicon oxide (SiO2), hafnium oxide (HfO2), zirconium oxide (ZrO2), etc. The above-mentioned metal films include molybdenum (Mo), tungsten (W), etc.

[0006] The above-mentioned thin film is generally used as a diffusion barrier between a doped semiconductor silicon layer and aluminum (Al), copper (Cu), etc. used as an interlayer wiring material. However, when a tungsten (W) thin film is deposited on a substrate, it is used as an adhesion layer.

[0007] As mentioned above, in order to obtain excellent and uniform physical properties of the thin film deposited on the substrate, high step coverage of the thin film is essential. Therefore, the atomic layer deposition (ALD) process using surface reaction is used instead of the chemical vapor deposition (CVD) process mainly using gas phase reaction. However, it is still difficult to achieve 100% step coverage.

[0008] When the deposition temperature is increased for the purpose of achieving 100% step coverage, there are still difficulties in step coverage. First, in the deposition process consisting of two components, the precursor and the reactant, the increase in deposition temperature will not only cause a sharp increase in the film growth rate (GPC), but even if the ALD process is used and implemented at 300°C to alleviate the increase in GPC caused by the increase in deposition temperature, it will also cause an increase in deposition temperature during the process. Therefore, it cannot be regarded as a good solution.

[0009] In addition, in order to achieve excellent metal thin films in semiconductor devices, high-temperature processes are required. It has been reported that increasing the atomic layer deposition temperature to 400°C reduces the concentration of residual carbon and hydrogen in the film (see the paper J. Vac. Sci. Technol. A, 35 (2017) 01B130).

[0010] However, the higher the deposition temperature, the more difficult it is to ensure step coverage. First, in a deposition process consisting of two components, the precursor and the reactant, an increase in deposition temperature can lead to a sharp increase in GPC (film growth rate). In addition, it can be confirmed that even if a conventional shielding agent is used to alleviate the increase in GPC caused by the increase in deposition temperature, GPC will increase by about 10% at 300°C. In other words, when deposition is performed at a temperature above 360°C, it is difficult to expect the GPC reduction effect provided by the shielding agent in the prior art.

[0011] Therefore, it is necessary to develop a method for forming a thin film that can effectively form a thin film with a complex structure even at high temperatures, has low residual impurities, and can significantly improve step coverage and thickness uniformity of the thin film, as well as a semiconductor substrate manufactured by the method. Summary of the invention

[0012] Problem that the invention aims to solve

[0013] In order to solve the problems in the prior art as described above, the object of the present invention is to provide a vacuum thin film modifier, a thin film forming method using the same, and a semiconductor substrate manufactured by the method, which provides a compound of a specified structure as a vacuum thin film modifier to appropriately reduce the thin film growth rate in the vacuum thin film process, so that even if a thin film is formed on a substrate with a complex structure, the step coverage and the thickness uniformity of the thin film can be greatly improved, and impurity contamination can be significantly reduced.

[0014] The object of the present invention is to improve the crystallinity and oxidation fraction of a thin film, thereby improving the density and dielectric properties of the thin film.

[0015] The above-mentioned object and other multiple objects of the present invention can be fully achieved by the present invention described below.

[0016] Means used to solve problems

[0017] In order to achieve the above-mentioned object, the present invention provides a vacuum film modifier, which includes an aromatic compound containing a hydrocarbon group and a halogen group, and is used to control the growth or film quality of a vacuum film formed from a precursor compound.

[0018] The above-mentioned vacuum thin film may be a vacuum deposited film or a vacuum etched film.

[0019] The aromatic compound including a hydrocarbon group and a halogen group may include a compound represented by Chemical Formula 1.

[0020] [Chemical formula 1]

[0021]

[0022] In the above chemical formula 1, the above R', R" and X are independently selected from hydrogen, an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms and a halogen group, and contain at least one halogen group.

[0023] In the chemical formula 1, R', R", and X may be hydrogen, an alkyl group having 1 to 5 carbon atoms, and a halogen group, respectively.

[0024] The refractive index of the aromatic compound containing a hydrocarbon group and a halogen group may be 1.50 to 1.60, 1.50 to 1.58, or 1.51 to 1.57.

[0025] When the thin film is a deposited film, the vacuum thin film modifier may include a compound represented by Chemical Formula 1-1 and a compound represented by Chemical Formula 1-2.

[0026] [Chemical formula 1-1 to Chemical formula 1-2]

[0027]

[0028] When the thin film is an etching film, the vacuum thin film modifier may include a compound represented by Chemical Formula 1-3.

[0029] [Chemical formula 1-3]

[0030]

[0031] The vacuum film modifier can control the reaction surface of the film formed from the silane-based precursor compound.

[0032] In addition, the present invention provides a vacuum film modification composition, which comprises the above-mentioned vacuum film modifier and an organic solvent having a dielectric constant of 15 or less.

[0033] The organic solvent having a dielectric constant of 15 or less may be a hydrocarbon solvent or a solvent containing a heterocyclic ring.

[0034] The organic solvent having a dielectric constant of 15 or less may be octane, dimethylethylamine or tetrahydrofuran.

[0035] In addition, the present invention provides a thin film forming method, which comprises the following steps:

[0036] Using the vacuum film modifying agent or the vacuum film modifying composition to treat the surface of a substrate loaded in a chamber; and

[0037] Precursor compounds and reaction gases are sequentially injected into the chamber, and a vacuum deposited film is formed on the substrate at 20° C. to 800° C. and a vacuum state lower than 760 torr.

[0038] Wherein, the reaction gas is an oxidant or a reducing agent.

[0039] The chamber may be an atomic layer deposition (ALD) chamber, a chemical vapor deposition (CVD) chamber, a plasma enhanced atomic layer deposition (PEALD) chamber or a plasma enhanced chemical vapor deposition (PECVD) chamber.

[0040] The vacuum film modifier, vacuum film modifier composition and precursor compound may be delivered into the chamber by vapor flow control (VFC), direct liquid injection (DLI) or liquid delivery system (LDS).

[0041] At this time, the heating temperature of the above-mentioned deposition delivery pipeline (hereinafter referred to as "injection pipeline") for the substrate can be in the range of 25°C to 200°C.

[0042] The above-mentioned thin film may be an oxide film or a nitride film.

[0043] The reaction gas may include O2, O3, N2O, NO2, H2O or O2 plasma.

[0044] The above-mentioned thin film can be a thin film formed by stacking one or more layers of one or more metals selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd.

[0045] The above-mentioned thin film can be used as an anti-diffusion film, an etching stopper film, an electrode film, a dielectric film, a gate insulating film, a block film, or a charge trap.

[0046] In addition, the present invention provides a thin film forming method, which comprises the following steps:

[0047] Using the vacuum film modifying agent or the vacuum film modifying composition to treat the surface of a substrate loaded in a chamber; and

[0048] An etching material is injected into the chamber to form a vacuum etching film on the substrate, wherein the etching material is one or more selected from Cl2, CCl4, CF2Cl2, CF3Cl, CF4, CHF3, C2F6, SF6, BCl3, Br2 and CF3Br.

[0049] The above chamber may be an ALD chamber, a CVD chamber, a PEALD chamber or a PECVD chamber.

[0050] The vacuum film modifying agent, vacuum film modifying composition and precursor compound may be delivered into the chamber by VFC method, DLI method or LDS method.

[0051] The above etching substances can be used in a mixture with Ar, H2 or O2.

[0052] The above-mentioned film modification method comprises the following steps:

[0053] Step (i), vaporizing the vacuum film modifying agent or vacuum film modifying composition and forming a modified area on the surface of the substrate loaded in the chamber; and

[0054] Step (ii) is to perform a first purge on the interior of the chamber using a purge gas.

[0055] The above-mentioned thin film forming method comprises the following steps:

[0056] Step (i), vaporizing the vacuum film modifying agent or vacuum film modifying composition and forming a modified area on the surface of a substrate loaded in a chamber;

[0057] Step (ii), using a purge gas to purge the interior of the chamber for the first time;

[0058] Step (iii), vaporizing the precursor compound and adsorbing it in a region separated from the modified region;

[0059] Step (iv), purging the interior of the chamber a second time using a purge gas;

[0060] Step (v), supplying a reaction gas into the interior of the chamber; and

[0061] Step (vi), using a purge gas to purge the interior of the chamber for a third time.

[0062] The vacuum thin film modifying agent or vacuum thin film modifying composition may be provided in a manner of being applied to a substrate loaded in a chamber at 20° C. to 800° C.

[0063] The above-mentioned precursor compound, as a molecule formed by one or more selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd, can be a precursor with a vapor pressure greater than 0.01mTorr and less than or equal to 100Torr at 25°C.

[0064] The present invention may include the following steps: after vaporizing and injecting the above-mentioned vacuum film modifying agent, vacuum film modifying composition or precursor compound, a plasma post-treatment is performed.

[0065] The amount of the purge gas injected into the interior of the chamber in the above step (ii) and the above step (iv) may be 10 to 100,000 times the volume of the injected film modifier, film modifier composition or precursor compound.

[0066] The reaction gas is an oxidant or a reducing agent. The reaction gas, vacuum film modifying agent, vacuum film modifying composition and precursor compound may be transported into the chamber by VFC, DLI or LDS.

[0067] The substrate loaded in the chamber is heated to 100° C. to 800° C., and the ratio of the amount (mg / cycle) of the vacuum film modifier or vacuum film modifier composition to the amount of the precursor compound injected into the chamber may be 1:1 to 1:20.

[0068] In addition, the present invention provides a semiconductor substrate including a thin film manufactured by the above-mentioned thin film forming method.

[0069] The above-mentioned film can be a multi-layer structure of two layers or three layers or more.

[0070] In addition, the present invention provides a semiconductor element, which includes the semiconductor substrate described above.

[0071] The semiconductor substrate may be low resistive metal gate interconnects, high aspect ratio 3D metal-insulator-metal (MIM) capacitors, DRAM trench capacitors, 3D gate-all-around (GAA) or 3D NAND flash memory.

[0072] Effects of the Invention

[0073] According to the present invention, a vacuum thin film modifier or a vacuum thin film modifier composition can be provided, which can appropriately reduce the growth rate of the thin film in the vacuum thin film process, so that even if the thin film is formed on a substrate with a complex structure, the step coverage and the thickness uniformity of the thin film can be greatly improved, and the contamination of impurities such as carbon can be significantly reduced.

[0074] In addition, when forming a thin film, process byproducts are more effectively reduced to prevent corrosion and degradation, and the film quality is improved to improve the crystallinity of the thin film, thereby improving the electrical properties of the thin film.

[0075] In addition, when forming a thin film, process byproducts are reduced, reaction speed is reduced, and the film growth rate is appropriately reduced, so that even if a thin film is formed on a substrate with a complex structure, step coverage and film density can be improved. Furthermore, the present invention also provides a thin film forming method using the same and a semiconductor substrate manufactured by the method. BRIEF DESCRIPTION OF THE DRAWINGS

[0076] Figure 1 This is a diagram showing the XPS depth analysis of a 10 nm thick SiN thin film produced using the thin film modification composition of the present invention to confirm whether carbon remains in the thin film.

[0077] Figures 2 to 5 It is measured 1 H NMR to confirm the reactivity of the film-modifying composition during synthesis and deposition, Figure 2 , Figure 3 , Figure 4 , Figure 5 These respectively represent the situations when octane, dimethylethylamine, tetrahydrofuran, ethanol and (1-chloroethyl)benzene are mixed. DETAILED DESCRIPTION

[0078] Hereinafter, the vacuum thin film modifier of the present invention, the thin film modifier composition containing the same, the thin film forming method using the same, and the semiconductor substrate produced by the method will be described in detail.

[0079] In the present invention, unless otherwise defined, the term "thin film modification" means controlling the surface of a substrate used as a surface chemical reaction surface in a deposition process.

[0080] In the present invention, unless otherwise defined, the term "shielding" means not only reducing, preventing or blocking the adsorption of precursor compounds for forming a thin film onto a substrate, but also reducing, preventing or blocking the adsorption of process byproducts onto a substrate.

[0081] The inventors of the present invention have confirmed that when a compound of a prescribed structure is used as a thin film modifier for modifying the surface of a substrate in a vacuum deposition process or an etching process and improving the deposition process or the etching process, the growth rate of the deposited film can be appropriately reduced, so that even if a thin film is formed on a substrate with a complex structure, the step coverage and the thickness uniformity of the thin film can be greatly improved, and the efficiency of the etching film can be improved, in particular, it can be deposited with a thinner thickness and improve the amount of O, Si, metal, metal oxides remaining as process byproducts and the amount of residual carbon that is difficult to reduce in the prior art. Based on this, vacuum thin film modifiers were studied, thereby completing the present invention.

[0082] The vacuum film modifier of the present invention can be applied to vacuum deposited films or vacuum etched films.

[0083] As an example, the above-mentioned deposited film or etched film can be formed by one or more precursors selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd, and can provide an oxide film, a nitride film, a metal film or a modified area for their selective thin films. At this time, the effect to be achieved by the present invention can be fully obtained.

[0084] As a specific example, the thin film may have a film composition of a silicon oxide film or a silicon nitride film.

[0085] The above-mentioned thin film can be used not only as a generally used diffusion prevention film in a semiconductor element, but also as an etching stopper film, an electrode film, a dielectric film, a gate insulating film, a barrier film or a charge trap.

[0086] In one example of the present invention, the compound represented by Chemical Formula 2 may be used as the precursor compound for forming the thin film.

[0087] [Chemical formula 2]

[0088]

[0089] In the above chemical formula 2, M is one or more selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd, and L 1 , L 2 , L 3 and L 4 is -H, -X, -R, -OR, -NR2 or Cp (cyclopentadiene) and may be the same or different from each other, wherein -X is F, Cl, Br or I, -R is a C1-C10 alkyl, C1-C10 alkenyl or C1-C10 alkynyl and may be linear or cyclic, and the above L 1 , L 2 , L 3 and L 4 The number of the ions may be 2 to 6 depending on the oxidation valence of the central metal.

[0090] For example, when the central metal is divalent, L 1 and L 2 It can act as a ligand to bind to the central metal. When the central metal is hexavalent, L 1 , L 2 , L 3 , L 4 , L 5 , L 6 Can be combined with the central metal, corresponding to L 1 To L 6 The ligands may be the same as or different from each other.

[0091] The above-mentioned M can be a type corresponding to a trivalent metal, a tetravalent metal, a pentavalent metal or a hexavalent metal, preferably hafnium (Hf), zirconium (Zr), aluminum (Al), niobium (Nb) or tantalum (Ta). At this time, the process by-products are significantly reduced, the step coverage is excellent, and it has the advantages of improving the film density, and the electrical properties, insulation and dielectric properties of the film are better.

[0092] The above L 1 , L 2 , L 3 and L 4 is -R, -X or Cp and may be the same as or different from each other, wherein -R is a C1-C10 alkyl, a C1-C10 alkenyl or a C1-C10 alkynyl and may have a linear or cyclic structure.

[0093] In addition, the above L 1 , L 2 , L 3 and L 4 It is -NR2 or Cp and may be the same as or different from each other, wherein -R may be H, C1-C10 alkyl, C1-C10 alkenyl, C1-C10 alkynyl, iPr (isopropyl) or tBu (tert-butyl).

[0094] In addition, in the above chemical formula 2, L 1 , L 2 , L 3 and L 4 is -H or -X and may be the same as or different from each other, wherein -X may be F, Cl, Br or I.

[0095] Specifically, the aluminum precursor compound may be, for example, Al(CH 3 ) 3 , AlCl 4 , or the like.

[0096] Examples of the hafnium precursor compound include cyclopentadienyltris(dimethylamino)hafnium (CpHf(NMe2)3) and (methyl-3-cyclopentadienylpropylamino)bis(dimethylamino)hafnium (Cp(CH2)3NM3Hf(NMe2)2).

[0097] Examples of silicon precursor compounds include hexachlorodisilane (HCDS), dichlorosilane (DCS), tris(dimethylamino)silane (3DMAS), bis(diethylamino)silane (BDEAS), and octamethylcyclotetrasiloxane (OMCTS).

[0098] The vacuum film modifier of the present invention can pre-control the substrate surface on which the precursor compound is to be adsorbed, thereby reducing the speed of adsorbing the precursor compound on the substrate to control the growth of the vacuum film or control the film quality.

[0099] The above-mentioned vacuum film modifier may include an aromatic compound containing a hydrocarbon group and a halogen group. In this case, when forming a deposited film or an etched film, side reactions can be suppressed and the film growth rate can be adjusted to reduce process by-products in the film, thereby reducing corrosion and degradation, and improving the crystallinity of the film. Moreover, even if a thin film is formed on a substrate with a complex structure, the step coverage and the thickness uniformity of the film can be greatly improved, and it has the effect of minimizing the contamination of impurities.

[0100] As a specific example, the refractive index of the above-mentioned aromatic compound containing hydrocarbon groups and halogen groups can be in the range of 1.50-1.60, 1.50-1.58 or 1.51-1.57. At this time, the effect of reducing process by-products is significant, the step coverage is excellent, and the film density is improved and the electrical properties of the film are better.

[0101] The vacuum film modifier includes the compound represented by Chemical Formula 1, so that the process by-product reduction effect is significant, the step coverage is excellent, and the film density improvement effect and the electrical characteristics of the film are more outstanding.

[0102] [Chemical formula 1]

[0103]

[0104] In the above chemical formula 1, the above R', R" and X are independently selected from hydrogen, an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms and a halogen group, and contain at least one halogen group.

[0105] As a specific example, the above R', R" and X can be hydrogen, an alkyl group with 1 to 5 carbon atoms and a halogen group, respectively. In this case, the process by-product reduction effect is significant, the step coverage is excellent, and the film density is improved and the electrical properties of the film are more outstanding.

[0106] Preferably, when the thin film is a deposited film, the above-mentioned vacuum film modifier can be one or more selected from the compounds represented by Chemical Formula 1-1 and the compounds represented by Chemical Formula 1-2. In this case, when forming a deposited film, it is possible to suppress side reactions while forming a relatively sparse thin film, and adjust the film growth rate to reduce process by-products in the thin film, thereby reducing corrosion and degradation, and improving the crystallinity of the thin film. Even if a thin film is formed on a substrate with a complex structure, the step coverage and the thickness uniformity of the thin film can be greatly improved. Not only that, it can also minimize impurity contamination.

[0107] [Chemical formula 1-1 to Chemical formula 1-2]

[0108]

[0109] Preferably, when the thin film is an etching film, the vacuum film modifier may be a compound represented by Chemical Formula 1-3. In this case, contamination by impurities can be minimized and the etching process can be effectively performed.

[0110] [Chemical formula 1-3]

[0111]

[0112] The above-mentioned vacuum film modifier can be used alone, but in consideration of the harsh vacuum atmosphere, it is preferred to use it together with a specific organic solvent because the process can be carried out efficiently.

[0113] As an example, at this time, using an organic solvent with a dielectric constant of 15 or less not only does not affect the reaction mechanism of the vacuum film modifier under vacuum, but also can improve the process.

[0114] The organic solvent having a dielectric constant of 15 or less may be, for example, a hydrocarbon solvent or a solvent containing a heterocyclic ring.

[0115] The hydrocarbon solvent may be a linear hydrocarbon compound containing an alkyl group having 1 to 10 carbon atoms, and as an example, octane (d: 1.9 at 25° C.) may be used.

[0116] The above-mentioned heterocyclic ring-containing solvent may contain nitrogen or oxygen.

[0117] As an example, the nitrogen-containing solvent may be dimethylethylamine (d: 3.7 at 25° C.) or the like.

[0118] As an example, the oxygen-containing solvent may be tetrahydrofuran (d: 7.6 at 25° C.) or the like.

[0119] As a specific example, the vacuum film modification composition may include: one or more compounds selected from the compounds represented by the chemical formula 1-1 to the compounds represented by the chemical formula 1-3; and the organic solvent having a dielectric constant of 15 or less. At this time, the effect of adjusting the growth rate of the deposited film is significant, the effect of removing process byproducts is also significant, and the step coverage and film quality improvement effects are excellent. Not only that, even if applied to a substrate with a complex structure, the uniformity of the film can be ensured, thereby greatly improving the step coverage. In particular, it can be deposited with a thinner thickness, and the amount of residual O, Si, metal, metal oxides and residual carbon that are difficult to reduce in the prior art that remain as process byproducts can be improved. In addition, when manufacturing an etching film, it can also provide a film quality improvement effect.

[0120] The reaction gas may include O2, NH3 or H2.

[0121] The above-mentioned thin film can be a thin film formed by stacking one or more layers of one or more metals selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd.

[0122] The vacuum thin film modifier described above can form a modified region for a thin film.

[0123] The vacuum film modifier does not remain on the film.

[0124] At this time, unless otherwise specifically defined, no residue means that when the components are analyzed by XPS, the C element is 0.1 atomic % (atom%), the Si element is less than 0.1 atomic % (atom%), the N element is less than 0.1 atomic % (atom%), and the halogen element is less than 0.1 atomic % (atom%). More preferably, in a secondary ion mass spectrometry (SIMS) measurement method or an X-ray photoelectron spectroscopy (XPS) measurement method that measures by digging into the substrate in the depth direction, when considering the increase and decrease rates of C, N, Si, and halogen impurities before and after using a vacuum film modifier under the same deposition conditions, the signal intensity (intensity) increase and decrease rate of each element type is preferably 5% or less.

[0125] As an example, the content of the halogen compound in the thin film may be 100 ppm or less.

[0126] The above-mentioned thin film may be used as an anti-diffusion film, an etching stopper film, an electrode film, a dielectric film, a gate insulating film, a blocking film, or a charge trap, but is not limited thereto.

[0127] Preferably, the above-mentioned vacuum film modifier, organic solvent and precursor compound can be a compound with a purity of 99.9% or more, a compound with a purity of 99.95% or more, or a compound with a purity of 99.99% or more. For reference, when a compound with a purity of less than 99% is used, impurities may remain in the film or cause side reactions with the precursor or reactant. Therefore, substances with a purity of 99% or more should be used as much as possible.

[0128] Preferably, the vacuum film modifier is used in an atomic layer deposition (ALD) process, in which case it has the following advantages: while not hindering the adsorption of precursor compounds, it effectively protects the surface of the substrate as a vacuum film modifier and effectively removes process byproducts.

[0129] Preferably, the vacuum film modifier is liquid at room temperature (22°C) and has a density of 0.8 to 2.5 g / cm 3 or 0.8~1.5g / cm 3 The vapor pressure (20°C) can be 0.1 to 300 mmHg or 1 to 300 mmHg. Within this range, a modified region can be effectively formed, and has excellent effects of improving step coverage, film thickness uniformity, and film quality.

[0130] More preferably, the density of the vacuum film modifier may be 0.75 to 2.0 g / cm 3 or 0.8~1.3g / cm 3 The vapor pressure (20°C) can be 1 to 260 mmHg. Within this range, the modified region can be effectively formed, and has excellent effects of improving step coverage, film thickness uniformity and film quality.

[0131] The vacuum thin film modifier is preferably used in an atomic layer deposition (ALE) process. At this time, since chemical etching is used, it has the effect of being able to achieve selective etching of the etching film to be provided and isotropic etching characteristics.

[0132] The thin film forming method of the present invention comprises the following steps:

[0133] Using the vacuum film modifying agent or the vacuum film modifying composition to treat the surface of a substrate loaded in a chamber; and

[0134] Precursor compounds and reaction gases are sequentially injected into the chamber, and a vacuum deposited film is formed on the substrate at 20° C. to 800° C. and under a vacuum state of less than 760 torr.

[0135] Among them, the above-mentioned reaction gas is an oxidant or a reducing agent. At this time, the deposition rate of the thin film can be reduced, and the growth rate of the thin film can be appropriately reduced. Therefore, even if a thin film is formed on a substrate with a complex structure, the step coverage and the thickness uniformity of the thin film can be greatly improved, and it has the effect of minimizing impurity contamination.

[0136] In the above-mentioned step of treating with a vacuum film modifier or a vacuum film modifier composition, the feeding time (Feeding Time, sec) of the vacuum film modifier or the vacuum film modifier composition to the surface of the substrate per cycle is preferably 0.01 to 10 seconds, more preferably 0.02 to 8 seconds, even more preferably 0.04 to 6 seconds, and further preferably 0.05 to 5 seconds. Within this range, not only is the film growth rate low, but the step coverage and economy are excellent, and it also has the advantage of minimizing impurity contamination.

[0137] In the present invention, the feeding time of the precursor compound is based on a flow rate of 0.1 to 500 mg / cycle when the volume of the chamber is 15 to 20 L, and more specifically, based on a flow rate of 0.8 to 200 mg / cycle when the volume of the chamber is 18 L.

[0138] The film modification method of the present invention may include the following steps:

[0139] Step (i), vaporizing the vacuum film modifying agent or vacuum film modifying composition and forming a modified area on the surface of the substrate loaded in the chamber; and

[0140] Step (ii) is to perform a first purge on the interior of the chamber using a purge gas.

[0141] As a preferred embodiment, the above-mentioned film modification method, in particular, the film forming method may include the following steps:

[0142] Step (i), vaporizing the vacuum film modifying agent or the vacuum film modifying composition to treat the surface of the substrate loaded in the chamber;

[0143] Step (ii), using a purge gas to purge the interior of the chamber for the first time;

[0144] Step (iii), vaporizing the precursor compound and allowing it to adsorb onto the surface of a substrate loaded in the chamber;

[0145] Step (iv), purging the interior of the chamber a second time using a purge gas;

[0146] Step (v), supplying a reaction gas into the interior of the chamber; and

[0147] Step (vi), using a purge gas to purge the interior of the chamber for a third time.

[0148] At this time, the above steps (i) to (vi) can be taken as a unit cycle and the above cycles can be repeatedly implemented until a film of desired thickness is obtained. When the vacuum film modifier or vacuum film modification composition of the present invention is injected before the precursor compound in one cycle and adsorbed on the substrate in this way, even if deposition is performed at a high temperature, the film growth rate can be appropriately reduced, and the generated process by-products can be effectively removed to reduce the resistivity of the film, and it has the advantage of greatly improving step coverage.

[0149] As another preferred embodiment, the substrate may be manufactured by coating the vacuum thin film modifying agent or the vacuum thin film modifying composition onto a substrate loaded in a chamber at 20° C. to 800° C.

[0150] As a preferred example, the thin film forming method of the present invention can inject the vacuum thin film modifier or vacuum thin film modification composition of the present invention before the precursor compound to modify the surface of the substrate within one cycle, and then inject the precursor compound and adsorb it on the substrate. At this time, even if the thin film is deposited at a high temperature, the film growth rate can be appropriately reduced, thereby greatly reducing process by-products, and greatly improving step coverage. The crystallinity of the thin film can be increased to reduce the resistivity of the thin film, and even if it is applied to semiconductor elements with a large aspect ratio, the thickness uniformity of the thin film can be greatly improved to ensure the reliability of the semiconductor elements.

[0151] As an example, in the above-mentioned thin film forming method, when the above-mentioned precursor compound is deposited before or after the deposition of the precursor compound, the number of repetitions of the unit cycle implemented can be 1 to 99999 times, preferably 10 to 10000 times, more preferably 50 to 5000 times, and even more preferably 100 to 2000 times, as needed. Within this range, the desired film thickness can be obtained and the effect to be achieved by the present invention can be fully obtained.

[0152] The above-mentioned precursor compound is a molecule with one or more selected from Al, Si, Ti, V, Co, Ni, Cu, Zn, Ga, Ge, Se, Zr, Nb, Mo, Ru, Rh, In, Sn, Sb, Te, Hf, Ta, W, Re, Os, Ir, La, Ce and Nd as the central metal atom (M) and one or more ligands including C, N, O, H, X (halogen), Cp (cyclopentadiene), and can be a precursor with a vapor pressure of 1mTorr to 100Torr at 25°C. At this time, even if it is naturally oxidized, the effect of forming a modified area based on the above-mentioned vacuum film modifier or vacuum film modification composition can be maximized.

[0153] In one example of the present invention, the chamber may be an ALD chamber, a CVD chamber, a PEALD chamber or a PECVD chamber.

[0154] The above-mentioned thin film can be a silicon oxide film, a silicon nitride film, a titanium oxide film, a titanium nitride film, a hafnium oxide film, a hafnium nitride film, a zirconium oxide film, a zirconium nitride film, a tungsten oxide film, a tungsten nitride film, an aluminum oxide film, an aluminum nitride film, a niobium oxide film, a niobium nitride film, a tantalum oxide film, a tantalum nitride film, a tellurium oxide film or a tellurium nitride film.

[0155] In the present invention, the following step may be included: after the above-mentioned precursor compound or film modifier is gasified and injected, a plasma post-treatment is performed, at which time, the growth rate of the film can be improved and process by-products can be reduced.

[0156] When the vacuum film modifier or vacuum film modifier composition is first adsorbed on the substrate, the precursor compound is then adsorbed, and then the reaction gas is adsorbed, the amount of the purge gas injected into the chamber in the step of purging the unadsorbed vacuum film modifier or vacuum film modifier composition is sufficient to remove the unadsorbed vacuum film modifier or vacuum film modifier composition. As an example, it can be 10 to 100,000 times, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times. Within this range, the unadsorbed vacuum film modifier or vacuum film modifier composition can be fully removed, thereby forming a uniform film and preventing the deterioration of the film quality. Among them, the injection amount of the purge gas, vacuum film modifier, and vacuum film modifier composition is based on one cycle, and the volume of the vacuum film modifier and vacuum film modifier composition represents the volume of the vaporized vacuum film modifier or vacuum film modifier composition vapor.

[0157] As a specific example, when the injection amount of the above-mentioned vacuum film modifier or vacuum film modifier composition is set to 200 sccm, and the flow rate of the purge gas in the step of purging the unadsorbed vacuum film modifier or vacuum film modifier composition is set to 5000 sccm, the injection amount of the purge gas is 25 times the injection amount of the vacuum film modifier or the vacuum film modifier composition.

[0158] In addition, in the step of purging the unadsorbed precursor compound, the amount of the purge gas injected into the chamber can be sufficient to remove the unadsorbed precursor compound. For example, it can be 10 to 100,000 times, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times the volume of the precursor compound injected into the chamber. Within this range, the unadsorbed precursor compound can be sufficiently removed to form a uniform thin film and prevent the degradation of the film quality. The injection amounts of the purge gas and the precursor compound are based on one cycle, respectively, and the volume of the precursor compound represents the volume of the vaporized precursor compound vapor.

[0159] In addition, in the purge step performed immediately after the reaction gas supply step, as an example, the amount of the purge gas injected into the chamber may be 10 to 100,000 times, preferably 50 to 50,000 times, and more preferably 100 to 10,000 times the volume of the reaction gas injected into the chamber. Within this range, the desired effect can be fully obtained. The injection amounts of the purge gas and the reaction gas are based on one cycle, respectively.

[0160] Preferably, the vacuum film modifying agent, vacuum film modifying composition and precursor compound can be delivered into the chamber by VFC, DLI or LDS, and more preferably, can be delivered into the chamber by LDS.

[0161] As an example, the substrate loaded in the chamber can be heated to 100°C to 650°C, and as a specific example, it can be heated to 150°C to 550°C. The vacuum film modifier, vacuum film modification composition or precursor compound can be injected into the substrate in an unheated or heated state. According to the deposition efficiency, it is also possible to heat it during the deposition process after injecting it in an unheated state. As an example, it can be injected into the substrate at 100°C to 650°C for 1 to 20 seconds.

[0162] Preferably, the ratio of the amount (mg / cycle) of the above-mentioned precursor compound to the vacuum film modifier or vacuum film modification composition injected into the chamber can be 1:1.5 to 1:20, more preferably 1:2 to 1:15, more preferably 1:2 to 1:12, and further preferably 1:2.5 to 1:10. Within this range, the effect of improving step coverage and reducing process by-products is significant.

[0163] As an example, in the above-mentioned thin film forming method, when the above-mentioned vacuum film modifier or vacuum film modifying composition and the above-mentioned precursor compound are used, the deposition rate reduction rate represented by Mathematical Formula 1 can be 15% or more, as a specific example, it can be 18% or more, preferably 21% or more. At this time, the use of the vacuum film modifier or vacuum film modifying composition having the above-mentioned structure can greatly reduce the growth rate of the formed thin film while forming a relatively sparse thin film. Therefore, even when applied to a substrate with a complex structure at high temperature, the uniformity of the thin film can be ensured, thereby greatly improving the step coverage. In particular, it can be deposited with a thinner thickness and provide an effect of improving the amount of O, Si, metals, metal oxides remaining as process by-products and the amount of residual carbon that is difficult to reduce in the prior art.

[0164] [Mathematical formula 1]

[0165] Deposition rate (DR) reduction rate = [{(DR i )-(DR f )} / (DR i )]×100

[0166] In this formula, DR (Deposition rate, / cycle) is the rate of film deposition. For thin film deposition formed by precursors and reactants, DR i Initial deposition rate is the deposition rate of a thin film formed without injecting a vacuum film modifier or a vacuum film modifier composition. f The final deposition rate is the deposition rate of the film formed by injecting the vacuum film modifier or the vacuum film modifier composition during the above process. The deposition rate (DR) is the value measured by an ellipsometer at room temperature and pressure for a film with a thickness of 3 to 30 nm, and the unit used is / cycle.

[0167] In the above mathematical formula 1, when a vacuum film modifier or a vacuum film modifier composition is used or not, the film growth rate per cycle represents the film deposition thickness per cycle (), that is, the deposition rate. As an example, the above deposition rate can be the average deposition rate obtained by measuring the final thickness of a film with a thickness of 3 to 30 nm using an ellipsometer (Ellipsometery) under normal temperature and pressure conditions and dividing it by the total number of cycles.

[0168] In the above mathematical formula 1, "when a vacuum film modifier or a vacuum film modifier composition is not used" means a case where a thin film is manufactured by adsorbing only a precursor compound on a substrate in a thin film deposition process. As a specific example, it means a case where a thin film is formed by omitting the step of adsorbing a vacuum film modifier or a vacuum film modifier composition and the step of purging the non-adsorbed vacuum film modifier or vacuum film modifier composition in the above-mentioned thin film formation method.

[0169] In the above-mentioned thin film forming method, based on the film thickness of 100, the residual halogen intensity (c / s) in the thin film measured by SIMS is preferably less than 100,000, more preferably less than 70,000, more preferably less than 50,000, and further preferably less than 10,000. As a preferred embodiment, it can be less than 5,000, more preferably 1,000 to 4,000, and more preferably 1,000 to 3,800. Within this range, the effect of preventing corrosion and degradation is excellent.

[0170] In the present invention, the purge is preferably 1000-50000sccm (Standard Cubic Centimeter per Minute), more preferably 2000-30000sccm, and even more preferably 2,500-15000sccm. Within this range, the film growth rate per cycle is properly controlled, and deposition is achieved in an atomic mono-layer or a manner close thereto, which is advantageous in terms of film quality.

[0171] The above-mentioned ALD (atomic layer deposition process) is very beneficial for manufacturing integrated circuits (ICs) requiring high aspect ratios. In particular, it has advantages such as excellent step conformality, uniform coverage, and precise thickness control based on a self-limiting thin film growth mechanism.

[0172] As an example, the above-mentioned thin film forming method can be implemented at a deposition temperature in the range of 50°C to 800°C, preferably, in the range of 300°C to 700°C, more preferably, in the range of 400°C to 650°C, even more preferably, in the range of 400°C to 600°C, and further preferably, in the range of 450°C to 600°C. Within this range, it has the effect of being able to achieve ALD process characteristics while growing a thin film with excellent film quality.

[0173] As an example, the above-mentioned thin film forming method can be implemented at a deposition pressure in the range of 0.01 to 20 Torr, preferably, at a deposition pressure in the range of 0.1 to 20 Torr, more preferably, at a deposition pressure in the range of 0.1 to 10 Torr, and most preferably, at a deposition pressure in the range of 0.3 to 7 Torr. Within this range, the effect of obtaining a thin film with uniform thickness can be achieved.

[0174] In the present invention, the deposition temperature and the deposition pressure may be measured by the temperature and pressure formed in the deposition chamber or by the temperature and pressure applied to the substrate in the deposition chamber.

[0175] Preferably, the above-mentioned thin film forming method may include the following steps: before injecting the above-mentioned precursor compound into the chamber, raising the temperature in the chamber to the deposition temperature; and / or before injecting the above-mentioned precursor compound into the chamber, injecting an inert gas into the chamber for purging.

[0176] In addition, in the present invention, a thin film manufacturing apparatus capable of implementing the above-mentioned thin film manufacturing method may include an ALD chamber, a first vaporizer for vaporizing a precursor compound, a first delivery unit for delivering the vaporized precursor compound into the ALD chamber, a second vaporizer for vaporizing a thin film precursor, and a second delivery unit for delivering the vaporized thin film precursor into the ALD chamber. The vaporizer and the delivery unit may be any vaporizer and the delivery unit conventionally used in the art.

[0177] At this time, the heating temperature of the substrate by the above-mentioned deposition delivery unit (hereinafter referred to as "injection pipeline") can be in the range of 25°C to 200°C, and the above-mentioned reaction gas can include O2, O3, N2O, NO2, H2O or O2 plasma.

[0178] According to another embodiment of the present invention, a thin film forming method can be provided, which comprises the following steps: treating the surface of a substrate loaded in a chamber with the above-mentioned vacuum thin film modifier or the above-mentioned vacuum thin film modifying composition; and injecting an etching substance into the chamber to form a vacuum etching film on the substrate. The above-mentioned etching substance is one or more selected from Cl2, CCl4, CF2Cl2, CF3Cl, CF4, CHF3, C2F6, SF6, BCl3, Br2 and CF3Br.

[0179] The above-mentioned etching materials can be used in a mixture with Ar, H2 or O2. Except for this, the specific description of matters overlapping with the formation of the above-mentioned deposited film will be omitted.

[0180] The present invention also provides a semiconductor substrate produced by the thin film forming method of the present invention, in which the step coverage and thickness uniformity of the thin film are excellent, and the density and electrical characteristics of the thin film are excellent.

[0181] As an example, the thickness of the thin film may be 0.1 to 20 nm, preferably 0.5 to 20 nm, more preferably 1.5 to 15 nm, and even more preferably 2 to 10 nm. Within this range, the film has excellent properties.

[0182] The carbon impurity content of the above-mentioned film is preferably less than 5000 counts / sec or 1 to 3000 counts / sec, more preferably 10 to 1000 counts / sec, and even more preferably 50 to 500 counts / sec. Within this range, the film has excellent film properties and a reduced film growth rate.

[0183] As an example, the step coverage of the above-mentioned film can be above 90%, preferably above 92%, and more preferably above 95%. Within this range, even a thin film with a complex structure can be easily deposited on the substrate. Therefore, it has the advantage of being applicable to the new generation of semiconductor elements.

[0184] Preferably, the thickness of the above-mentioned film is less than 20nm, based on the film thickness of 10nm, the dielectric constants are 5 to 29, the content of carbon, nitrogen and halogen is less than 5000 counts / second, and the step coverage is more than 90%. Within this range, it has excellent performance when used as a dielectric film or a barrier film, but is not limited to this.

[0185] As an example, the film may be a multilayer structure of two or more layers, preferably a multilayer structure of two or three layers, as required. As a specific example, the multilayer film of the two-layer structure may be a structure of a lower film-middle film, and as a specific example, the multilayer film of the three-layer structure may be a structure of a lower film-middle film-upper film.

[0186] As an example, the above-mentioned lower layer film may include one or more selected from Si, SiO2, MgO, Al2O3, CaO, ZrSiO4, ZrO2, HfSiO4, Y2O3, HfO2, LaLuO2, Si3N4, SrO, La2O3, Ta2O5, BaO, and TiO2.

[0187] As an example, the intermediate layer film may include Ti x N y , preferably, may contain TN.

[0188] As an example, the upper layer film may include one or more selected from W and Mo.

[0189] The semiconductor substrate may be low resistive metal gate interconnects, high aspect ratio 3D metal-insulator-metal (MIM) capacitors, DRAM trench capacitors, 3D gate-all-around (GAA) or 3D NAND flash memory.

[0190] Below, preferred embodiments and drawings are proposed to help understand the present invention. The following embodiments and drawings are only used to illustrate the present invention. Those skilled in the art can make various changes and modifications within the scope of the scope of the present invention and technical ideas, and these deformations and modifications fall within the scope of the attached invention application patent.

[0191] [Example]

[0192] Example 1 to Example 2, Comparative Example 1

[0193] An ALD deposition process was performed using the various components and process conditions shown in Tables 1 and 2.

[0194] Specifically, a hexachlorodisilane (HCDS) precursor is used, the canister heating temperature is 35°C, an N2 carrier is injected at a flow rate of 40 sccm for 3 seconds, NH3 is injected at a flow rate of 1000 sccm for 30 seconds, and an N2 purge is injected at a flow rate of 1000 sccm for 12 seconds. These conditions are repeated for 100 to 150 cycles to perform SiN deposition of Comparative Example 1 in Table 1.

[0195] The substance represented by Chemical Formula 1-1 having a purity of 99.6% was used to perform SiN deposition of Example 1 in Table 1.

[0196] [Chemical formula 1-1]

[0197]

[0198] At this time, N2 carrier was injected at a flow rate of 100 sccm for 3 seconds while maintaining the canister heating temperature at 50° C. In addition, the process of injecting the substance represented by Chemical Formula 1-1 for 3 seconds was repeated for 100 to 150 cycles.

[0199] The SiN experiment of Example 2 in Table 1 was performed in the same manner as the SiN experiment of Example 1, except that the substance represented by Chemical Formula 1-1 and the organic solvent represented by Chemical Formula 3-1 were mixed in a mole ratio of 1:1, and a liquid delivery system (LDS) was used to maintain injection at 0.1 g / min for 3 seconds.

[0200] [Chemical formula 3-1]

[0201]

[0202] For the thin films obtained in Comparative Example 1 and Examples 1 and 2, the thickness of the SiN thin film of 10 nm was analyzed by ellipsometry optical analysis method, and the deposition rate was measured.

[0203] XPS depth analysis: Using an X-ray photoelectron spectroscopy (ESCALAB 200R, VG Scientific) equipped with an Al Kα X-ray source, various elements were analyzed in depth by argon sputtering to confirm whether C remained in the SiN film obtained in Example 2. The results are shown in Figure 1 middle.

[0204] Deposition rate measurement: The thickness of the SiN film formed with a thickness of 10 nm measured by ellipsometry optical analysis fitting was divided by the total ALD cycle to measure the thickness per cycle, i.e., the deposition rate. The reduction rate was determined by calculation using Mathematical Formula 1, and the results are shown in Table 1.

[0205] [Mathematical formula 1]

[0206] Deposition rate (DR) reduction rate = [{(DR i )-(DR f )} / (DR i )]×100

[0207] [Table 1]

[0208]

[0209] As shown in Table 1, it can be confirmed that Example 1 using the vacuum film modifier of the present invention has a deposition rate reduction rate of -22% compared to Comparative Example 1 not using the vacuum film modifier. As shown in Table 1, it can be confirmed that Example 2 using the vacuum film modifier composition of the present invention has a deposition rate reduction rate of even -30% compared to Comparative Example 1 not using the vacuum film modifier.

[0210] In addition, if Figure 2 As shown, in Example 2 using the vacuum film modification composition of the present invention, as the sputtering time increases, the element information at different depths from the surface to the inside is confirmed based on the composition of the film, and the degree of contamination caused by carbon is less than the detection limit of 0.1%.

[0211] Examples 2 to 4, Comparative Example 2

[0212] The same process as in Example 2 was repeated, except that the compound represented by Chemical Formula 3-1 used in Example 2 was replaced by the compound represented by Chemical Formula 3-2, the compound represented by Chemical Formula 3-3, and the compound represented by Chemical Formula 3-4, respectively, to manufacture a 10 nm SiN thin film. For reference, Chemical Formula 3-2 corresponds to Example 3, Chemical Formula 3-3 corresponds to Example 4, and Chemical Formula 3-4 corresponds to Comparative Example 2.

[0213] [Chemical formula 3-2]

[0214]

[0215] [Chemical formula 3-3]

[0216]

[0217] [Chemical formula 3-4]

[0218]

[0219] Specifically, for this experiment, the compound represented by the chemical formula 3-1 (d: 1.9 at 25°C), the compound represented by the chemical formula 3-2 (d: 3.7 at 25°C), the compound represented by the chemical formula 3-3 (d: 7.6 at 25°C), the compound represented by the chemical formula 3-4 (d: 24.5 at 25°C) and the compound represented by the chemical formula 1-1 were mixed at a mole ratio of 1:1 in a solvent having a dielectric constant value of less than 15, and the mixture was stirred for 1 h. 1 H-NMR was used to confirm the reactivity based on the presence or absence of new impurity peaks, and the results are summarized in Tables 2 and Figures 2 to 5 When a new impurity peak is observed, it is reactive and is marked as O. When no new impurity peak is observed, it is non-reactive and is marked as X.

[0220] [Table 2]

[0221] Solvents for film modifying compositions Is it reactive? Compound represented by Chemical Formula 3-1 (Example 2) X Compound represented by Chemical Formula 3-2 (Example 3) X Compound represented by Chemical Formula 3-3 (Example 4) X Compound represented by Chemical Formula 3-4 (Comparative Example 2) O

[0222] As shown in Table 2 and Figures 2 to 5 As shown, it was confirmed that in Examples 2 to 4 in which a compound represented by Chemical Formula 3-1, a compound represented by Chemical Formula 3-2, and a compound represented by Chemical Formula 3-3 having a dielectric constant of less than 15 were mixed, there was no reactivity to the vacuum film modifier to be used, and therefore, it was judged to be effective in improving the deposition process.

[0223] On the other hand, in Comparative Example 2 in which the compound represented by Chemical Formula 3-4 having a dielectric constant greater than 15 was mixed, it was confirmed that the compound was reactive with the vacuum film modifier to be used, and therefore was judged to be unsuitable for improving the deposition process.

Claims

1. A vacuum film modifier, characterized in that: The invention comprises an aromatic compound containing a hydrocarbon group and a halogen group, and is used for controlling the growth or film quality of a vacuum film formed from a precursor compound.

2. The vacuum film modifier according to claim 1, characterized in that: The vacuum film is a vacuum deposited film or a vacuum etched film.

3. The vacuum film modifier according to claim 1, characterized in that: The aromatic compound containing a hydrocarbon group and a halogen group includes a compound represented by Chemical Formula 1, [Chemical formula 1] In the above Chemical Formula 1, R', R" and X are independently selected from hydrogen, an alkyl group having 1 to 5 carbon atoms, an alkenyl group having 1 to 5 carbon atoms, an alkoxy group having 1 to 5 carbon atoms and a halogen group, and contain at least one halogen group.

4. The vacuum film modifier according to claim 3, characterized in that: In the above chemical formula 1, R', R" and X are hydrogen, an alkyl group having 1 to 5 carbon atoms and a halogen group, respectively.

5. The vacuum film modifier according to claim 1, characterized in that: The refractive index of the aromatic compound containing a hydrocarbon group and a halogen group is 1.50 to 1.

60.

6. The vacuum film modifier according to claim 1, characterized in that: When the thin film is a deposited film, the vacuum thin film modifier includes a compound represented by Chemical Formula 1-1 and a compound represented by Chemical Formula 1-2; when the thin film is an etched film, the vacuum thin film modifier includes a compound represented by Chemical Formula 1-3. [Chemical formula 1-1 to Chemical formula 1-3] 7. A vacuum film modification composition, characterized in that: Include: The vacuum film modifier according to any one of claims 1 to 6; and An organic solvent with a dielectric constant of 15 or less.

8. The vacuum film modification composition according to claim 7, characterized in that: The organic solvent having a dielectric constant of 15 or less is a hydrocarbon solvent or a solvent containing a heterocyclic ring.

9. The vacuum film modification composition according to claim 7, characterized in that: The organic solvent having a dielectric constant of 15 or less is octane, dimethylethylamine or tetrahydrofuran.

10. A method for forming a thin film, characterized in that: The following steps are involved: Treating the surface of a substrate loaded in a chamber using the vacuum thin film modifier according to claim 1 or the vacuum thin film modifier composition according to claim 7; and Precursor compounds and reaction gases are sequentially injected into the chamber, and a vacuum deposited film is formed on the substrate at 20° C. to 800° C. and a vacuum state lower than 760 torr. Wherein, the reaction gas is an oxidant or a reducing agent.

11. A method for forming a thin film, characterized in that: The following steps are involved: Treating the surface of a substrate loaded in a chamber using the vacuum thin film modifier according to claim 1 or the vacuum thin film modifier composition according to claim 7; and Injecting etching material into the chamber to form a vacuum etching film on the substrate, The above-mentioned etching material is one or more selected from Cl2, CCl4, CF2Cl2, CF3Cl, CF4, CHF3, C2F6, SF6, BCl3, Br2 and CF3Br.

12. The thin film forming method according to claim 10 or 11, characterized in that: The chamber is an atomic layer deposition chamber, a chemical vapor deposition chamber, a plasma enhanced atomic layer deposition chamber or a plasma enhanced chemical vapor deposition chamber.

13. The thin film forming method according to claim 10, characterized in that: The vacuum film modifier, the vacuum film modification composition and the precursor compound are transported into the chamber by gas phase flow control, direct liquid injection or liquid transfer system, and the heating temperature of the injection pipeline for the substrate is 25°C to 200°C.

14. The thin film forming method according to claim 11, characterized in that: The above etching substances are used in mixture with Ar, H2 or O2.

15. A semiconductor substrate, characterized in that: Includes a thin film produced by the thin film forming method according to claim 10 or 11.

16. The semiconductor substrate according to claim 15, characterized in that The film is a multi-layer structure of two or more layers.

17. A semiconductor device, characterized in that: Comprising the semiconductor substrate according to claim 15.