Temporary fixing substrate, method for manufacturing temporary fixing substrate, and temporary fixing method
By forming chamfered areas and polishing on the main and back surfaces of the temporarily fixed substrate, the problem of poor resin peeling and edge chipping at the outer periphery of the temporarily fixed substrate is solved, and the yield and durability of the semiconductor package are improved.
Patent Information
- Application Number
- CN202380025404.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-31
- Filing Date
- 2023-03-02
- Publication Date
- 2024-10-29
AI Technical Summary
Existing temporarily fixed substrates are prone to poor resin peeling and edge chipping at the periphery, resulting in reduced yield.
A chamfered area is formed on the outer peripheral ends of the main surface and the back surface of the temporarily fixed substrate. The arithmetic mean roughness of the chamfered area is 0.1 μm to 10 μm. The chamfering and polishing processes are used to form chamfered areas with different inclination angles relative to the main surface. The arithmetic mean roughness of the first chamfered portion and the second chamfered portion, and the side end portion is smaller than the roughness of the chamfered area.
It effectively suppresses peeling defects and edge chipping between the temporarily fixed substrate and the resin, improves the yield of semiconductor packages, and ensures high flatness and durability.
Smart Images

Figure CN118872045A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a temporary fixing substrate used in a manufacturing process of a semiconductor package. Background Art
[0002] As a manufacturing technology for semiconductor packages, FOWLP (Fan-out Wafer Level Package) technology is known. FOWLP technology generally obtains a semiconductor package that is thinner than before through the following four steps, namely, a step of resin molding on a temporary fixing substrate to which a semiconductor chip is temporarily fixed by an adhesive, a step of grinding the resin molded part to expose the electrode terminal of the semiconductor chip, a step of forming a thin film rewiring layer (multilayer wiring) and solder balls on the surface where the electrode terminal is exposed, and a step of singulating each package and peeling it from the temporary fixing substrate.
[0003] As a temporary fixing substrate for chips in the FOWLP technology, a method of using a translucent ceramic substrate is known (for example, see Patent Documents 1 and 2). The translucent ceramic substrate has all the requirements required for a temporary fixing substrate, that is, high flatness required to expose the electrode terminal, high rigidity and anti-warping shape required to suppress warping when forming multi-layer wiring, light transmittance to allow laser light for curing the adhesive to pass through, and chemical resistance for cleaning and reuse after use.
[0004] However, the conventional temporary fixing substrate has a problem that a peeling failure occurs in which the resin partially peels off at the outer periphery, thereby reducing the yield.
[0005] In addition, conventional temporary fixing substrates have a problem in that tipping (chipping) occurs at the outer periphery, which results in a reduction in yield. Prior art literature Patent Literature
[0006] Patent Document 1: Japanese Patent No. 6430081 Patent Document 2: Japanese Patent No. 6420023 Summary of the invention
[0007] The present invention has been made in view of the above-mentioned problems, and an object of the present invention is to provide a temporary fixing substrate capable of suppressing peeling failure and obtaining a semiconductor package at a higher yield than before.
[0008] Furthermore, a second object of the present invention is to suppress chipping in the outer peripheral portion of a temporarily fixed substrate.
[0009] In order to solve the above-mentioned problem, the first scheme of the present invention is a temporary fixing substrate, which temporarily fixes a specified fixing object on one main surface, and is characterized in that a chamfered area is provided at the end of the entire outer periphery of each of the one main surface and the other main surface, and the arithmetic mean roughness of the chamfered area on at least the one main surface side is 0.1μm to 10μm, and is greater than the arithmetic mean roughness of the one main surface.
[0010] A second aspect of the present invention is the temporary fixing substrate according to the first aspect, wherein the chamfered region includes a first chamfered portion and a second chamfered portion having different inclination angles with respect to the one main surface.
[0011] A third aspect of the present invention is the temporary fixing substrate according to the first or second aspect, wherein the arithmetic mean roughness of the one main surface and the other main surface is 100 nm or less.
[0012] A fourth aspect of the present invention is the temporary fixing substrate according to any one of the first to third aspects, wherein the arithmetic mean roughness of the side end portion is smaller than the arithmetic mean roughness of the chamfered area.
[0013] A fifth aspect of the present invention is the temporary fixing substrate according to the fourth aspect, wherein the arithmetic mean roughness of the side end portion is larger than the arithmetic mean roughness of the one main surface and is 5 μm or less.
[0014] A sixth aspect of the present invention is the temporary fixing substrate according to the fifth aspect, wherein the arithmetic mean roughness of the side end portion is 2 μm or less.
[0015] A seventh aspect of the present invention is the temporary fixing substrate according to any one of the first to sixth aspects, wherein the predetermined fixing objects are a plurality of electronic components or semiconductor substrates.
[0016] The eighth scheme of the present invention is a method for manufacturing a temporary fixed substrate for temporarily fixing a specified fixed object on a main surface, characterized in that it comprises: a forming step for producing a circular plate-shaped formed body with translucent ceramic as a main component; a firing step for firing the formed body to obtain a sintered body; a chamfering step for forming a chamfered area at the end of the entire outer circumference of each of one main surface and another peripheral surface of the sintered body; and a grinding step for grinding the sintered body with the chamfered area formed thereon to obtain a temporary fixed substrate, the arithmetic mean roughness of the chamfered area on at least one main surface side of the temporary fixed substrate obtained by the grinding step is 0.1μm to 10μm, and is a value larger than the arithmetic mean roughness of one main surface of the temporary fixed substrate.
[0017] The ninth scheme of the present invention is based on the manufacturing method of the temporary fixed substrate involved in the eighth scheme, characterized in that in the chamfering process, the chamfered area is formed into two sections, a first chamfered portion and a second chamfered portion, which have different inclination angles relative to the one main surface of the temporary fixed substrate.
[0018] A tenth aspect of the present invention is the method for manufacturing a temporary fixing substrate according to the eighth or ninth aspect, wherein the arithmetic mean roughness of the one main surface and the other main surface of the temporary fixing substrate obtained by the polishing step is 100 nm or less.
[0019] The eleventh embodiment of the present invention is a method for manufacturing a temporary fixed substrate according to any one of the eighth to tenth embodiments, characterized in that the arithmetic mean roughness of the side end portion of the temporary fixed substrate obtained by the grinding step is smaller than the arithmetic mean roughness of the chamfered area.
[0020] A twelfth aspect of the present invention is a method for manufacturing a temporary fixing substrate according to the eleventh aspect, wherein the arithmetic mean roughness of the side end portion is greater than the arithmetic mean roughness of the one main surface of the temporary fixing substrate and is 5 μm or less.
[0021] A thirteenth aspect of the present invention is the method for manufacturing a temporary fixing substrate according to any one of the eighth to twelfth aspects, wherein the predetermined fixing objects are a plurality of electronic components or semiconductor substrates.
[0022] The fourteenth scheme of the present invention is a method for temporarily fixing a specified fixed object to a temporarily fixed substrate, characterized in that it comprises a process of preparing a temporarily fixed substrate having a chamfered area at the end of the entire outer periphery of a main surface, a process of forming an adhesive layer on the temporarily fixed substrate, a process of arranging a specified fixed object on the adhesive layer, and a process of making an adhesive layer by curing the adhesive layer, thereby bonding the specified fixed object to the temporarily fixed substrate, wherein the arithmetic mean roughness of the chamfered area is 0.1μm to 10μm and is greater than the arithmetic mean roughness of the one main surface.
[0023] A fifteenth aspect of the present invention is the temporary fixing method according to the fourteenth aspect, wherein the chamfered region includes a first chamfered portion and a second chamfered portion having different inclination angles with respect to the one main surface.
[0024] The sixteenth embodiment of the present invention is a temporary fixing method according to the fourteenth or fifteenth embodiment, characterized in that the specified fixing object is a plurality of electronic components, and the temporary fixing method also includes a step of forming a resin molded part on the adhesive layer and the plurality of electronic components bonded to the temporary fixing substrate by the adhesive layer.
[0025] A seventeenth aspect of the present invention is the temporary fixing method according to the fourteenth or fifteenth aspect, wherein the predetermined fixing object is a semiconductor substrate.
[0026] According to the first to seventeenth aspects of the present invention, during the process of temporarily fixing an object such as an electronic component to a temporary fixing substrate, it is possible to appropriately suppress separation between the temporary fixing substrate and the object, the adhesive layer or other resins such as the bonding layer.
[0027] In particular, according to the fifth, sixth and twelfth aspects, it is possible to appropriately suppress the occurrence of chipping at the side end portion of the temporary fixing substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 It is a plan view of one principal surface (front surface) 1 a of the temporary fixing substrate 1 according to the first embodiment. Figure 2 It is an enlarged cross-sectional view of the vicinity of the side end portion 1 e of the temporary fixing substrate 1 , showing the condition of the chamfered region 2 . Figure 3 It is a schematic cross-sectional view showing in stages the state of a semiconductor package manufacturing process using the temporary fixing substrate 1 based on the FOWLP technique. Figure 4 1 is a flow chart schematically showing a manufacturing process of the temporary fixed substrate 1 . Figure 5 1 is a diagram schematically showing a state in which a temporarily fixed substrate 1 is chamfered using the chamfering device 100 . Figure 6 Indicates the status of chamfering. Figure 5 An enlarged schematic diagram of part A. Figure 7 1 is a schematic cross-sectional view showing a main part of a lapping apparatus 200 for lapping a temporarily fixed substrate 1 . Figure 8 It is a perspective view of the main parts of the buffing and grinding device 200 with the upper platform 202 omitted. Fig. 9 1 is a diagram schematically showing a state in which the buffing and polishing apparatus 200 polishes the side end portion 1 e of the temporary fixed substrate 1 on which the chamfered region 2 is not formed. DETAILED DESCRIPTION
[0029] <First Embodiment> <Temporary fixing substrate> Figure 1 The figure is a plan view of a main surface (front) 1a of a temporary fixing substrate 1 according to the first embodiment of the present invention. The temporary fixing substrate 1 is a substrate for temporarily fixing semiconductor chips when a semiconductor package is manufactured by FOWLP (Fan-out Wafer Level Package) technology.
[0030] The temporary fixed substrate 1 is a light-transmitting ceramic substrate having a diameter of several hundred mm (for example, 300 mm), a thickness of several hundred μm to several mm (for example, 1 mm), a thickness difference within a surface of several μm (for example, within 3 μm), and a warpage of several hundred μm or less (for example, 200 μm). It should be noted that in the present embodiment, the light-transmitting ceramic refers to a ceramic having a total front light transmittance of 20% or more in the full wavelength region of 200 nm to 1500 nm. Examples of such light-transmitting ceramics include aluminum oxide, silicon nitride, aluminum nitride, silicon oxide, and the like. For example, a substrate having aluminum oxide as a main component and a total front light transmittance of 70% or more at a wavelength of 1500 nm is a preferred example of the temporary fixed substrate 1. In the case of aluminum oxide as the main component, it is preferred to use a high-purity aluminum oxide powder of 99.9% or more (more preferably 99.95% or more) as a raw material, and it is preferred to add magnesium oxide and zirconium oxide (ZrO 2 ) and yttrium oxide (Y 2 O 3 ).
[0031] The surface 1a as the configuration surface of the semiconductor chip is pre-ground together with the other main surface (back side) 1b, thereby forming a flat ground surface with a small surface roughness. In more detail, in the surface 1a and the back side 1b, the thickness difference within the surface within the above-mentioned several μm and the arithmetic average roughness Ra below 100nm (preferably below 20nm) are achieved. More specifically, the surface 1a and the back side 1b are both surfaces that have been polished. It should be noted that the lower limit of the arithmetic average roughness Ra of the surface 1a and the back side 1b is not particularly limited, as long as it is 1nm, it is sufficient in practical use.
[0032] However, the temporary fixed substrate 1 involved in this embodiment has a chamfered area 2 at the end of the entire periphery of the surface 1a. In addition, although not shown in the figure, the chamfered area 2 is also provided in the back surface 1b. Therefore, strictly speaking, the arithmetic mean roughness Ra of the surface 1a and the back surface 1b of less than 100 nm described above is achieved in the area other than the chamfered area 2. It should be noted that, hereinafter, the surface 1a and the back surface 1b other than the chamfered area 2 are also referred to as the flat surface 1a and the flat back surface 1b, respectively.
[0033] Figure 2 It is an enlarged cross-sectional view of the vicinity of the side end portion 1 e of the temporary fixing substrate 1 , showing the condition of the chamfered region 2 .
[0034] exist Figure 2 In the case shown, the chamfered area 2 has a two-stage structure in which the first chamfered portion 2a is inclined at an inclination angle θ1 relative to the flat surface 1a and the second chamfered portion 2b is inclined at an inclination angle θ2 (>θ1) relative to the flat surface 1a. The second chamfered portion 2b is provided in a range of a predetermined width b (<a) from the side end portion 1e. The chamfered area 2 having a two-stage structure of the first chamfered portion 2a and the second chamfered portion 2b is also provided on the flat back surface 1b side. It should be noted that the second chamfered portion 2b may be omitted, and the chamfered area 2 may be a one-stage structure consisting only of the first chamfered portion 2a.
[0035] The inclination angle θ1 is preferably 5° to 55° (eg, 30°). Furthermore, the inclination angle θ2 when the chamfered area 2 has a two-stage structure is preferably 35° to 85° (eg, 60°). θ1<θ2.
[0036] In the temporary fixing substrate 1, by having the chamfered area 2 that satisfies the above-mentioned range of the inclination angle, the generation of chipping can be appropriately suppressed. That is, in the case of the temporary fixing substrate 1 without the chamfered area 2, chipping of the edge due to the defect of the vertical corner between the surface 1a and the back surface 1b and the side end 1e is easy to occur, but in the case of the temporary fixing substrate 1 involved in the present embodiment, since it has the chamfered area 2, there is no such vertical corner, and the angle formed by the chamfered area 2 and the surface 1a and the back surface 1b, and the angle formed by the chamfered area 2 and the side end 1e are all obtuse angles, so it is extremely difficult to generate chipping.
[0037] That is, the chamfered area 2 has the following effects: it suppresses defects caused by chipping and improves the manufacturing yield of the temporary fixed substrate 1. In particular, the chamfered area 2 is a two-stage structure of the first chamfered portion 2a and the second chamfered portion 2b, which is more effective in suppressing the chipping because the obtuse angle is set in two stages.
[0038] <Semiconductor package manufacturing process and the effect of chamfer roughening> In the above-mentioned manner, at least the chamfered area 2 provided on the surface (one main surface) 1a side of the temporarily fixed substrate 1 is a rough surface having a surface roughness greater than that of the flat surface 1a. Specifically, the arithmetic mean roughness Ra of the chamfered area 2 is 0.1 μm to 10 μm. This is intended to ensure the manufacturing yield of the semiconductor package. This point is explained below.
[0039] Figure 3 1 is a schematic cross-sectional view showing the state of the semiconductor package manufacturing process using the temporary fixing substrate 1 in stages based on the FOWLP technology. Figure 3 In order to simplify the illustration, only the chamfered region 2 on the surface 1a side is indicated by oblique lines.
[0040] In the manufacturing process of semiconductor package, first, Figure 3 As shown in (a), a layer (adhesive layer) 3α composed of an adhesive is formed on the temporary fixing substrate 1. As the adhesive, double-sided tape and hot melt adhesive can be exemplified, and the adhesive can be formed by various known methods such as roller coating, spray coating, screen printing, spin coating, etc.
[0041] Then, if Figure 3 As shown in (b), a plurality (a large number) of semiconductor chips 4 are arranged on the adhesive layer 3α. The semiconductor chip 4 is arranged in an area closer to the inside than the chamfered area 2. Next, the adhesive layer 3α is cured to form the adhesive layer 3. The curing method is selected from heating, ultraviolet irradiation, etc. according to the material of the adhesive used in the adhesive layer 3α. Thus, the semiconductor chip 4 is bonded and fixed to the temporary fixing substrate 1.
[0042] When the semiconductor chip 4 is fixed to the temporary fixing substrate 1 in this manner, the mold resin flows over the entire upper surface of the temporary fixing substrate 1, that is, the gap 5 between the semiconductor chips 4 and the entire upper surface of the semiconductor chip 4. By curing the mold resin, Figure 3 As shown in (c), a resin mold 6 is formed. Examples of the mold resin include epoxy resins, polyimide resins, polyurethane resins, and urethane resins.
[0043] After that, the resin mold 6 is ground until the electrode terminals of the semiconductor chip 4 are exposed, and then a rewiring layer and solder balls are formed on the ground surface. Finally, individual packages are singulated and the temporary fixed substrate 1 is separated by laser lift-off.
[0044] The chamfered area 2 provided on the periphery of the temporary fixed substrate 1 plays an effect (peeling inhibition effect) of suppressing the occurrence of defective peeling (defective peeling) of the resin (adhesive layer 3 and resin molded part 6) from the temporary fixed substrate 1 during the period before singulation and laser peeling in the manufacturing process of the semiconductor package as described above.
[0045] In the case of a conventional temporary fixing substrate, in the middle of the manufacturing process of the semiconductor package, air enters from the outside between the temporary fixing substrate and the resin near the periphery of the temporary fixing substrate, forming bubbles, which may cause the temporary fixing substrate and the resin to peel off.
[0046] However, when the temporary fixing substrate 1 involved in the present embodiment is used, the adhesive and the molded resin enter the rough surface provided on the periphery of the surface 1a, i.e., the chamfered area 2, which has a surface roughness sufficiently larger than that of the surface 1a, thereby generating an anchoring effect with the resin in the chamfered area 2. This anchoring effect suppresses the formation of bubbles at the periphery of the temporary fixing substrate 1 and the peeling of the resin. It should be noted that the presence or absence of bubbles can be confirmed by visually observing the temporary fixing substrate 1 from the back side 1b or using a stereo microscope. In the present embodiment, not only is it considered that the resin is peeled off when the temporary fixing substrate 1 is visually observed from the side end 1e side and a portion where the resin is separated from the temporary fixing substrate 1 is confirmed, but also it is considered that the resin is peeled off when the bubbles having a size of 3 mm or more in the long side or short side direction are confirmed as a result of visually observing or using a stereo microscope from the back side 1b.
[0047] When the temporary fixed substrate 1 is provided with the chamfered area 2 satisfying the arithmetic mean roughness Ra of 0.1 μm to 10 μm, the occurrence rate of peeling failure counted per substrate unit (peeling failure rate) is suppressed to 3% or less. The arithmetic mean roughness Ra of the chamfered area 2 is preferably 0.5 μm to 2 μm.
[0048] It should be noted that from the perspective of the peeling suppression, the width a of the chamfered area 2 is only 1% of the radius r of the temporary fixed substrate 1, and the chamfered area 2 may not be set further inside than the width. For example, in the case of a temporary fixed substrate 1 with a diameter of 300 mm (r = 150 mm), it is preferably about 0.2 mm to 0.5 mm. The width b of the second chamfered portion 2b is preferably about 0.01 mm to 0.11 mm. It should be noted that the presence of the chamfered area 2 does not hinder laser peeling.
[0049] <Manufacturing process of temporary fixed substrate> Next, a process for manufacturing the temporary fixed substrate 1 having the chamfered region 2 will be described. Figure 41 is a flow chart schematically showing the manufacturing process of the temporary fixing substrate 1. The temporary fixing substrate 1 is manufactured roughly through a compact manufacturing step (step S1), a sintering step (step S2), a chamfering step (step S3), and a grinding step (step S4).
[0050] When manufacturing the temporary fixed substrate 1, first, a molded body with translucent ceramic powder as the main component is made (step S1). For example, the above-mentioned aluminum oxide and other translucent ceramic raw material powders, magnesium, sintering aids and other ceramic powders, adhesives, solvents and other organic materials are mixed with a ball mill to produce a grinding liquid, and the grinding liquid is formed into a belt. Multiple rectangular sheets of a specified size obtained by shearing (cutting) the obtained belt are stacked and pressed, and the pressed stacked body is cut into a circle. Thus, a circular plate-shaped molded body is obtained. Alternatively, the molded body can be obtained by a scraper method, an extrusion method, a gel casting method, etc.
[0051] Next, the formed compact is fired (step S2 ), whereby the organic components are removed, and a ceramic sintered body (temporary fixed substrate 1 before chamfering and polishing) is obtained.
[0052] The sintering is preferably performed by calcining in an atmospheric furnace and then final sintering in a hydrogen furnace. From the viewpoint of densification of the sintered body, the sintering temperature during the final sintering is preferably 1700°C to 1900°C, more preferably 1750°C to 1850°C.
[0053] It should be noted that after the formal sintering, the obtained sintered body can be further annealed in a hydrogen furnace in order to adjust (correct) the warpage. From the viewpoint of preventing deformation and abnormal grain growth and promoting the discharge of sintering aids, the annealing treatment is preferably carried out at a temperature within ±100°C of the highest temperature during the formal sintering, and more preferably below 1900°C. In addition, the annealing time is preferably 1 to 6 hours.
[0054] If a sintered body (temporary fixed substrate 1 before chamfering and before grinding) is obtained, then the outer periphery of the front and back sides (two main surfaces) of the sintered body is chamfered as a whole (step S3). It should be noted that in the following description, for convenience, the temporary fixed substrate 1 before chamfering and the temporary fixed substrate 1 before grinding are also referred to as temporary fixed substrate 1.
[0055] Figure 5 1 is a diagram schematically showing a state in which a temporarily fixed substrate 1 is chamfered using a chamfering device (chamfering machine) 100. The chamfering device 100 includes a table 101, a table rotating mechanism 102, a grindstone holding and moving mechanism 103, and a grindstone 104. Figure 6 Indicates the status of chamfering. Figure 5 An enlarged schematic diagram of part A.
[0056] The table 101 can horizontally place the temporarily fixed substrate 1 to be chamfered on its upper surface, and can rotate together with the temporarily fixed substrate 1 placed thereon in a horizontal plane by the operation of the table rotating mechanism 102 .
[0057] The grindstone holding and moving mechanism 103 can hold a disk-shaped grindstone 104 in a horizontal posture at its lower end, and can perform a rotational movement and an advance and retreat movement in a horizontal plane while holding the grindstone 104 .
[0058] The grinding stone 104 is in the shape of a disk and Figure 6 The grit number of the grindstone 104 (blade 104a) is selected so that the arithmetic mean roughness Ra of the chamfered area 2 finally formed is within the above-mentioned range of 0.1 μm to 10 μm.
[0059] When chamfering, first, the temporary fixed substrate 1 is placed on the upper surface of the table 101. On the other hand, the grindstone 104 is mounted on the grindstone holding and moving mechanism 103. At this time, the temporary fixed substrate 1 and the grindstone 104 are aligned so that the center heights in the thickness direction (vertical position) of each are the same.
[0060] Then, while the workbench 101 carrying the temporarily fixed substrate 1 is horizontally rotated as indicated by arrow AR1 (AR1a, AR1b) under the action of the workbench rotating mechanism 102, the grindstone holding and moving mechanism 103 causes the grindstone 104 to rotate horizontally in the opposite direction relative to the workbench 101 as indicated by arrow AR2 (AR2a, AR2b), and to move translationally toward the side end 1e of the temporarily fixed substrate 1 as indicated by arrow AR3 (AR3a, AR3b).
[0061] With the rotation and translation, the blade 104a of the grindstone 104 approaches the side end 1e of the temporary fixing substrate 1, and finally abuts against the upper and lower edge portions 1ea and 1eb of the side end 1e of the temporary fixing substrate 1. By continuing the rotation and translation of the grindstone 104 even after the abutment, the side end 1e of the temporary fixing substrate 1 is gradually cut from the edge portions 1ea and 1eb, and finally the chamfered area 2 is formed.
[0062] When the chamfered area 2 is configured in two stages, two types of grindstones 104 having blades 104a with different angles are used sequentially. Alternatively, one grindstone 104 may be provided with a plurality of blades 104a with different angles, and the chamfered area 2 may be configured in two stages by using them sequentially.
[0063] It should be noted that the semiconductor chip 4 is not usually mounted on the back side 1b of the temporary fixed substrate 1 based on the above process, so the chamfered area 2 formed on the back side 1b is not necessarily roughened from the point of view of suppressing the peeling of the resin, but there is no particular disadvantage in that the chamfered area 2 on the back side 1b is roughened together with the front side 1a during chamfering by the chamfering device 100. On the contrary, from the viewpoint of the symmetry of the shape of the side end 1e, it can also be said that it is preferable that the front side 1a side and the back side 1b side are chamfered in the same manner by the blade 104a of the same grain size number.
[0064] Finally, the front and back surfaces (both main surfaces) of the chamfered temporary fixing substrate 1 are polished (step S4).
[0065] Figure 7 1 is a schematic cross-sectional view showing a main part of a buffing and polishing apparatus 200 for performing buffing and polishing of a temporarily fixed substrate 1. The buffing and polishing apparatus 200 includes a lower stage 201, an upper stage 202, and a plurality of carriers 203. Figure 8 It is a perspective view of the main parts of the buffing and grinding device 200 with the upper platform 202 omitted.
[0066] The lower platform 201 and the upper platform 202 can be coaxially rotated in opposite directions in a horizontal plane as shown by arrows AR4 and AR5. As the material of the lower platform 201 and the upper platform 202, copper, resin copper, tin, etc. can be exemplified. Alternatively, a grinding pad can be pasted on a metal platform for use. In this case, a hard polyurethane pad, a non-woven pad, and a suede pad can be exemplified as the grinding pad.
[0067] Each carrier 203 has a circular through hole 203 h into which the temporarily fixed substrate 1 to be polished is inserted, and can rotate or revolve between the annular guide 204 and the central axis 205 as the lower surface plate 201 and the upper surface plate 202 rotate.
[0068] In the polishing and grinding device 200, a plurality of carriers 203 embedded with temporary fixed substrates 1 as grinding objects are sandwiched between the lower platform 201 and the upper platform 202, while the grinding liquid SL is dripped between the lower platform 201 and the upper platform 202, and the lower platform 201 and the upper platform 202 are rotated in opposite directions as shown by arrows AR4 and AR5. Thus, the two main surfaces of the temporary fixed substrate 1 can be ground at the same time to obtain a flat surface 1a and a flat back surface 1b with an arithmetic mean roughness Ra of less than 100nm (preferably less than 20nm). As the grinding liquid SL, an aqueous or oily diamond grinding liquid can be exemplified.
[0069] It should be noted that, while the chamfered region 2 is also ground to some extent during the buffing, the surface roughness of the chamfered region 2 that has been roughened in advance is almost unchanged from that before the grinding.
[0070] Through the above steps, the temporary fixing substrate 1 of the present embodiment having the chamfered region 2 is obtained.
[0071] As described above, according to the present embodiment, by providing chamfered areas on the entire peripheries of the two main surfaces of the temporary fixing substrate used for temporary fixing of the semiconductor chip in the manufacturing process of manufacturing the semiconductor package based on the FOWLP technology, it is possible to appropriately suppress the occurrence of chipping at the corners of the temporary fixing substrate. In addition, by making the chamfered areas provided on the periphery of the main surface for temporarily fixing the semiconductor chip a rough surface with a larger surface roughness than the main surface, it is possible to appropriately suppress the peeling of the temporary fixing substrate and the resin in the middle of the above process.
[0072] <Second Embodiment> In the first embodiment, after the chamfered area 2 is roughened in the chamfering device 100 , both main surfaces of the temporary fixing substrate 1 are polished by the polishing device 200 , thereby forming a flat surface 1 a for temporarily fixing the semiconductor chip 4 .
[0073] In the process of polishing and grinding by the polishing and grinding device 200, the side end 1e is also polished to some extent due to the nature of the method. That is, the surface roughness of the side end 1e decreases with the polishing and grinding. Therefore, in addition to the flat surface 1a and the flat back surface 1b, the surface roughness (arithmetic mean roughness Ra) of the side end 1e also becomes smaller than the surface roughness (arithmetic mean roughness Ra) of the chamfered area 2. By implementing the polishing and grinding in this way to reduce the surface roughness of the side end 1e, it has the effect of suppressing the occurrence of edge collapse in the surface of the side end 1e. Moreover, this effect can be obtained even if it is not in the temporary fixed substrate 1 formed with the chamfered area 2, in other words, in the temporary fixed substrate 1 in which the chamfering process is omitted.
[0074] Fig. 9 1 is a diagram schematically showing a state in which the buffing and polishing apparatus 200 polishes the side end portion 1 e of the temporary fixed substrate 1 on which the chamfered region 2 is not formed.
[0075] As described above, in the polishing and grinding apparatus, the polishing liquid SL is dripped between the lower platform 201 and the upper platform 202 that sandwich the carrier 203 and the temporary fixed substrate 1, but the polishing liquid SL Fig. 9 As shown, the polishing liquid SL also enters between the side end 1e of the temporary fixing substrate 1 and the carrier 203. The side end 1e of the temporary fixing substrate 1 is polished by the polishing liquid SL that has entered. This is also the same when the temporary fixing substrate 1 is provided with the chamfered area 2.
[0076] When the arithmetic mean roughness Ra of the side end 1e is 5 μm or less, the occurrence rate of chipping (chipping defect rate) counted per substrate unit is suppressed to less than 3.0%. When the arithmetic mean roughness Ra of the side end 1e is 2 μm or less, the chipping defect rate is suppressed to less than 1.0%.
[0077] Furthermore, in the case of the temporary fixing substrate 1 having the chamfered region 2 as in the first embodiment, if the arithmetic mean roughness Ra of the side end portion 1 e is 2 μm or less, the chipping defect rate is suppressed to 0.5% or less.
[0078] The lower limit of the arithmetic mean roughness Ra of the side end 1e is not particularly limited, and it is sufficient for practical use as long as it is 0.01 μm or more. Among them, the polishing grinding is only mainly for the main surface of the temporary fixed substrate 1, so the grinding of the side end 1e is gentler than that of the main surface. Therefore, the arithmetic mean roughness Ra of the side end 1e is usually a value greater than the arithmetic mean roughness Ra of the flat surface 1a and the flat back surface 1b.
[0079] As described above, according to this embodiment, by setting the arithmetic mean roughness Ra of the side edge of the temporary fixing substrate used for temporary fixing of the semiconductor chip in the manufacturing process of manufacturing a semiconductor package based on the FOWLP technology to 5 μm or less, it is possible to appropriately suppress the occurrence of chipping at the side edge.
[0080] (Variation Example) In the above-mentioned embodiment, the temporary fixing substrate having the chamfered area is used as a substrate for temporarily fixing a plurality of semiconductor chips when manufacturing a semiconductor package by the FOWLP technology, but the use of the temporary fixing substrate is not limited to this, and it can also be used for temporarily fixing electronic components other than semiconductor chips. That is, in order to suppress the peeling of the resin and the temporary fixing substrate when a resin molded part is formed after a plurality of electronic components are bonded to the temporary fixing substrate by an adhesive, the temporary fixing substrate involved in the above-mentioned embodiment can also be used.
[0081] Alternatively, various semiconductor substrates may be temporarily fixed to a temporary fixing substrate having a chamfered area using an adhesive, and after the temporarily fixed semiconductor substrate is subjected to a desired treatment, the temporary fixing substrate may be peeled off in the same manner as in the above embodiment. As semiconductor substrates, various substrates such as silicon substrates, compound semiconductor substrates, epitaxial substrates and other composite substrates, multi-layer substrates, and multi-layer substrates using these as base substrates may be exemplified. In this case, the same effects as in the above embodiment can be obtained. Example
[0082] (Confirm the effect of roughening the chamfered area) Five types of temporary fixing substrates 1 (conditions 1 to 5) with different combinations of arithmetic mean roughness Ra of the flat surface 1a and the chamfered area 2 were prepared, 200 pieces each. The chamfered area 2 had a two-stage structure, and the inclination angles θ1 and θ2 were 30° and 60°, respectively. For each temporary fixing substrate 1, Figure 3 The illustrated process is performed until the semiconductor chip 4 is temporarily fixed by the resin mold 6 .
[0083] Furthermore, a temporary fixed substrate was produced in the same manner as Conditions 1, 4, and 5 except that the chamfered region 2 was not formed (Condition 6).
[0084] For all the obtained samples (the laminate of the temporary fixing substrate 1, the semiconductor chip 4, and the resin), it was visually confirmed whether the temporary fixing substrate 1 and the resin were peeled off, and the peeling failure rate in each example was calculated. Specifically, the temporary fixing substrate 1 was visually observed from the side end 1e side and the back side 1b side. When the separation of the resin mold 6 and the temporary fixing substrate 1 was confirmed at the side end 1e, or when bubbles with a minimum size of 3 mm or more were present in at least one of the radial or circumferential directions of the temporary fixing substrate 1 when observed from the back side 1b, it was determined that peeling had occurred.
[0085] Table 1 lists the evaluation results of the values of the arithmetic mean roughness Ra of the flat surface 1 a and the chamfered region 2 and the peeling failure rate in each of the Examples and Comparative Examples.
[0086] [Table 1]
[0087] It should be noted that regarding the evaluation of the peeling failure rate, the temporary fixing substrate 1 produced under the condition that the peeling failure rate is 3% or less is judged to have well suppressed the peeling of the resin. Specifically, conditions 1 to 5 meet this judgment. In Table 1, "0" (circled) is marked in the "peeling failure rate" column of these conditions 1 to 5.
[0088] On the other hand, for the temporary fixing substrate 1 produced under the condition where the value of the peeling failure rate exceeds 3%, it is judged that the suppression of resin peeling is insufficient. Specifically, only condition 6 meets this judgment. Specifically, the peeling failure rate in the case of condition 6 is 4.5%. In Table 1, "×" (circled) is marked in the "peeling failure rate" column of condition 6.
[0089] The above results show that the chamfered region 2 having a rough surface having an arithmetic mean roughness Ra in the range of 0.1 μm to 10 μm and being sufficiently larger than the surface 1 a is effective in suppressing the separation between the temporary fixing substrate 1 and the resin.
[0090] (Confirm the effect of grinding the side end) The chamfered area 2 was formed in the same manner as in condition 3 and the arithmetic mean roughness Ra of the side end 1e was different for five types of temporary fixed substrates 1 (conditions 3-1 to 3-5), and 200 pieces were each produced. It should be noted that the arithmetic mean roughness Ra was measured using a laser microscope. In addition, the chamfered area 2 was formed in the same manner as in condition 4 and the arithmetic mean roughness Ra of the side end 1e was different for three types of temporary fixed substrates 1 (conditions 4-1 to 4-3), and 200 pieces were each produced. Furthermore, in the same manner as in condition 6, the chamfered area 2 was not formed and the arithmetic mean roughness Ra of the side end 1e was different for two types of temporary fixed substrates 1 (conditions 6-1 to 6-2), and 200 pieces were each produced.
[0091] The side end 1e of each temporary fixing substrate 1 was observed with a stereo microscope to check whether there was edge chipping. When a defect with a size of 5 mm or more in the circumferential direction of the temporary fixing substrate 1 and a size of 1 mm or more in the radial direction was confirmed, it was determined that edge chipping had occurred.
[0092] Table 2 lists the evaluation results of the values of the arithmetic mean roughness Ra and the chipping defect rate of the chamfered region 2 and the side end portion 1 e of each example.
[0093] [Table 2]
[0094] It should be noted that, regarding the evaluation of the edge chipping rate, when the edge chipping rate is 0.5% or less, it is judged that the occurrence of edge chipping is extremely well suppressed. Specifically, conditions 3-1, 3-3, 4-2, and 4-3 meet this judgment. In Table 2, the "edge chipping rate" column for these conditions is marked as (Make a double circle).
[0095] In addition, when the chipping defect rate is more than 0.5% and less than 1.0%, it is judged that the chipping is generally well suppressed. Specifically, condition 6-2 meets this judgment. In Table 2, "0" (circled) is marked in the "chipping defect rate" column of this condition.
[0096] Furthermore, when the value of the edge chipping defect rate exceeds 1.0% and is less than 3.0%, it is judged that the generation of edge chipping is suppressed to a certain extent. Specifically, condition 3-2, condition 3-4, and condition 4-1 meet this judgment. In Table 2, "△" (with a triangle) is marked in the "edge chipping defect rate" column of these conditions.
[0097] On the other hand, when the value of the edge collapse defect rate obtained exceeds 3%, it is judged that the edge collapse is not sufficiently suppressed. Specifically, conditions 3-5 and condition 6-1 meet this judgment. In Table 1, "×" (circled) is marked in the "edge collapse defect rate" column of these conditions. For example, the edge collapse defect rate under condition 6-1 is 4.0%.
[0098] The above results show that the side end 1e having an arithmetic mean roughness Ra of 5 μm or less has a certain degree of effect in suppressing edge chipping at the side end 1e, and specifically, the edge chipping rate is suppressed to less than 3%. In addition, it shows that when the arithmetic mean roughness Ra of the side end 1e is 2 μm or less, the edge chipping rate is suppressed to less than 1%, and when the temporary fixed substrate 1 further has a chamfered area 2, the edge chipping rate is suppressed to less than 0.5.
Claims
1. A temporary fixed substrate, It is characterized in that A fixed object is temporarily fixed on one main surface. The one main surface and the other main surface each have a chamfered area at an end portion of the entire outer circumference, The arithmetic mean roughness of the chamfered region on at least the one main surface side is 0.1 μm to 10 μm and is larger than the arithmetic mean roughness of the one main surface.
2. The temporary fixing substrate according to claim 1, It is characterized in that The chamfered region includes a first chamfered portion and a second chamfered portion having different inclination angles with respect to the one main surface.
3. The temporary fixing substrate according to claim 1 or 2, It is characterized in that The arithmetic mean roughness of the one main surface and the other main surface is 100 nm or less.
4. The temporary fixing substrate according to any one of claims 1 to 3, It is characterized in that The arithmetic mean roughness of the side end portion is smaller than the arithmetic mean roughness of the chamfered area.
5. The temporary fixing substrate according to claim 4, It is characterized in that The arithmetic mean roughness of the side end portion is greater than the arithmetic mean roughness of the one main surface and is 5 μm or less.
6. The temporary fixing substrate according to claim 5, It is characterized in that The arithmetic mean roughness of the side end portion is 2 μm or less.
7. The temporary fixing substrate according to any one of claims 1 to 6, It is characterized in that The predetermined fixing objects are a plurality of electronic components or semiconductor substrates.
8. A method for manufacturing a temporary fixing substrate, for manufacturing a temporary fixing substrate for temporarily fixing a predetermined fixing object on one main surface, It is characterized in that have: A forming step for producing a disk-shaped formed body mainly composed of translucent ceramics; A sintering step of sintering the molded body to obtain a sintered body; a chamfering step of forming a chamfered area at an end portion of the entire outer circumference of each of one main surface and the other peripheral surface of the sintered body; as well as a grinding step of grinding the sintered body having the chamfered area formed therein to obtain a temporary fixed substrate, The arithmetic mean roughness of the chamfered region on at least one main surface side of the temporary fixing substrate obtained by the polishing step is 0.1 μm to 10 μm and is greater than the arithmetic mean roughness of one main surface of the temporary fixing substrate.
9. The method for manufacturing a temporary fixed substrate according to claim 8, It is characterized in that In the chamfering step, the chamfered region is formed into two stages, a first chamfered portion and a second chamfered portion having different inclination angles with respect to the one main surface of the temporary fixing substrate.
10. The method for manufacturing a temporary fixed substrate according to claim 8 or 9, It is characterized in that The arithmetic mean roughness of the one main surface and the other main surface of the temporary fixing substrate obtained by the polishing step is 100 nm or less.
11. The method for manufacturing a temporary fixing substrate according to any one of claims 8 to 10, It is characterized in that The arithmetic mean roughness of the side end portion of the temporary fixing substrate obtained by the polishing step is smaller than the arithmetic mean roughness of the chamfered region.
12. The method for manufacturing a temporary fixed substrate according to claim 11, It is characterized in that The arithmetic mean roughness of the side end portion is greater than the arithmetic mean roughness of the one main surface of the temporary fixing substrate and is a value of 5 μm or less.
13. The method for manufacturing a temporary fixing substrate according to any one of claims 8 to 12, It is characterized in that The predetermined fixing objects are a plurality of electronic components or semiconductor substrates.
14. A temporary fixing method for temporarily fixing a predetermined fixing object to a temporary fixing substrate, It is characterized in that have: A step of preparing a temporary fixing substrate having a chamfered area at an end portion of the entire outer circumference of one main surface; forming an adhesive layer on the temporary fixed substrate; a step of placing a predetermined fixing object on the adhesive layer; and a step of bonding the predetermined fixing object to the temporary fixing substrate by curing the adhesive layer to form an adhesive layer, The arithmetic mean roughness of the chamfered area is 0.1 μm to 10 μm, and is greater than the arithmetic mean roughness of the one main surface.
15. The temporary fixing method according to claim 14, It is characterized in that The chamfered region includes a first chamfered portion and a second chamfered portion having different inclination angles with respect to the one main surface.
16. The temporary fixing method according to claim 14 or 15, It is characterized in that The predetermined fixed objects are a plurality of electronic components, The temporary fixing method further includes a step of forming a resin mold on the adhesive layer and the plurality of electronic components bonded to the temporary fixing substrate via the adhesive layer.
17. The temporary fixing method according to claim 14 or 15, It is characterized in that The predetermined fixing object is a semiconductor substrate.