Binder composition and electrode plate prepared from same

CN118872095APending Publication Date: 2024-10-29CONTEMPORARY AMPEREX TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280090021.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2022-09-09
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Existing lithium-ion battery binders are prone to excessive brittleness during the long life cycle of the electrode, leading to cracking and demoulding of the pole piece. Especially when the energy density is high and the active material load increases, the adhesive force is insufficient and cannot adapt to the expansion of the electrode. .

Method used

A combination of starch and polyvinyl alcohol is used as a binder. By adjusting the ratio and molecular weight of amylose and amylopectin, and combining it with a cross-linking agent, a binder with high adhesion and self-healing properties is formed to ensure extreme The sheets are not easy to crack during the drying process.

Benefits of technology

Significantly improves the adhesion and flexibility of the electrode pole pieces, prevents cracking and demoulding, adapts to the stability of the electrode under high stress conditions, and extends the life cycle of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118872095A_ABST
    Figure CN118872095A_ABST
Patent Text Reader

Abstract

According to the binder composition, the binder composition contains starch and polyvinyl alcohol, and the starch contains amylose and amylopectin. The invention also relates to a battery pole piece composition containing the binder composition, a battery pole piece prepared from the battery pole piece composition, a secondary battery containing the battery pole piece, a battery pack containing the secondary battery and an electric device.
Need to check novelty before this filing date? Find Prior Art

Description

A binder composition and an electrode sheet prepared therefrom Technical Field

[0001] The present application relates to a binder composition comprising starch and polyvinyl alcohol, wherein the starch comprises amylose and amylopectin. The present application also relates to a battery electrode composition comprising the binder composition, a battery electrode prepared from the composition, a secondary battery comprising the battery electrode, a battery pack comprising the secondary battery, and an electrical device. Background Art

[0002] Secondary batteries have become the most popular energy storage system due to their low cost, long life and good safety. They are now widely used in pure electric vehicles, hybrid electric vehicles and smart grids. Secondary batteries are mainly composed of positive electrode sheets, negative electrode sheets, separators and electrolytes. The preparation of battery sheets (positive and negative electrodes) requires the use of binder materials to firmly bond the active substances of the sheets with conductive agents and other additives. So far, most lithium-ion battery binders are mainly artificial synthetic polymer materials such as PVDF, SBR, and CMC. However, the bonding ability of these materials still needs to be improved, especially when the electrodes expand significantly under multiple cycles during the long life cycle of the battery or under high energy density and high active material loading, which can easily lead to brittle sheets and even cracking and demolding.

[0003] Therefore, there is still a need to provide a new adhesive that can have sufficient bonding strength at a lower dosage and can inhibit the tendency of the pole piece to crack and demold under electrode expansion.

[0004] Summary of the Invention

[0005] The present application is made in view of the above-mentioned problems, and its purpose is to provide a binder to solve the technical problem that the electrode plates of the secondary battery prepared by the binder are too brittle and easy to crack and demould.

[0006] In order to achieve the above-mentioned object, the present application provides a first aspect of a binder composition, wherein the composition contains starch and polyvinyl alcohol, and the starch contains amylose and amylopectin.

[0007] The adhesive composition of the present application, by comprising a mixture of starch and polyvinyl alcohol, can significantly improve the brittleness of the electrode. The large number of hydroxyl groups on the starch and polyvinyl alcohol ensures that when the active material loading and thickness of the electrode are increased, the water loss rate in the thickness direction does not produce a large gradient, which may cause the electrode to crack. At the same time, because the selected starch contains a large amount of amylopectin, it releases stress during the heat drying process, which can effectively improve the bonding strength of the electrode and prevent cracking and demolding.

[0008] In any embodiment, the number average molecular weight of the amylose is 500-160000 g / mol, optionally 2000-50000 g / mol, further optionally 5000-20000 g / mol; and / or the number average molecular weight of the amylopectin is 100000-1000000 g / mol, optionally 150000-800000 g / mol, further optionally 300000-600000 g / mol. In any embodiment, the weight ratio of amylose to amylopectin in the starch is 1:1 to 1:10, optionally 1:3 to 1:8, further optionally 1:4 to 1:6. In any embodiment, the content of the starch is 10-95% by weight, optionally 80-92% by weight, based on the dry weight of the binder composition. Amylose has a linear structure, which increases the overall strength of the composition; amylopectin has a branched structure, which improves the flexibility of the composition. By adjusting the ratio of amylose to amylopectin in the starch and selecting the appropriate molecular weight range for each, further improved bonding strength and processing properties can be achieved.

[0009] In any embodiment, the weight ratio of starch and polyvinyl alcohol in the composition is 1.5: 1 to 20: 1, optionally 2: 1 to 20: 1, and further optionally 5: 1 to 10: 1. In any embodiment, the weight average molecular weight of the polyvinyl alcohol is 15000-250000 g / mol, optionally 25000-120000 g / mol, and further optionally 30000-80000 g / mol. In any embodiment, the content of the polyvinyl alcohol is 1-35% by weight, optionally 7-20% by weight, based on the gross weight of the binder composition. The hydroxyl group contained in the polyvinyl alcohol can form hydrogen bonds with the electrode active material, while improving the bonding force, also making this connection have a certain degree of "self-healing". By adjusting the molecular weight and content of polyvinyl alcohol, compositions with different bonding strengths can be obtained.

[0010] In any embodiment, the binder composition further comprises at least one cross-linking agent, the cross-linking agent being selected from one or more of oxalic acid, polyvinyl pyrrolidone, phosphorus oxychloride, sodium trimetaphosphate, adipic acid, and hexametaphosphate, optionally oxalic acid. In any embodiment, the content of the cross-linking agent is 0.01-5% by weight, optionally 0.2-1% by weight, based on the dry weight of the binder composition. The cross-linking agent can connect different parts of the starch or polyvinyl alcohol molecular chain by, for example, reacting with hydroxyl groups, thereby playing an "interlocking" role. By setting its content within a specific range, the bonding strength of the starch and polyvinyl alcohol mixture can be further adjusted.

[0011] In any embodiment, the binder composition is an aqueous dispersion containing water as a solvent. In any embodiment, the binder composition has a solid content of 15-60% by weight, optionally 20-40% by weight. By adjusting the solid content of the binder composition by adding water, a binder suitable for different battery systems can be prepared.

[0012] The present application also relates to a method for preparing a binder composition selected from the first aspect of the present application, comprising the following steps:

[0013] 1) adding starch to deionized water and adding polyvinyl alcohol, wherein the weight ratio of starch to polyvinyl alcohol is 1.5:1 to 20:1, the starch contains amylose and amylopectin in a weight ratio of 1:1 to 1:10, wherein the number average molecular weight of the amylose is 500-160,000 g / mol, and the number average molecular weight of the amylopectin is 100,000-1,000,000 g / mol;

[0014] 2) stirring the mixture obtained in 1) at 50-99° C. for 0.5-24 hours;

[0015] 3) Optionally, at least one cross-linking agent is added to the above mixture, and stirring is continued at 10-99° C. for 0.5-24 hours.

[0016] In any embodiment, the temperature in step 2) is 70-95° C., and / or the stirring time is 8-15 hours. In any embodiment, the temperature in step 3) is 70-95° C., and / or the stirring time is 8-15 hours.

[0017] The second aspect of the present application provides a composition for preparing a battery electrode sheet, which comprises a positive or negative electrode active material, a conductive agent, and the binder composition according to the first aspect of the present application, and optionally water and a dispersant.

[0018] A third aspect of the present application provides an electrode plate, which is prepared by using the binder composition selected from the first aspect of the present application.

[0019] The fourth aspect of the present application provides a secondary battery, comprising an electrode plate selected from the third aspect of the present application. The electrode plate may be a positive electrode plate and / or a negative electrode plate.

[0020] A fifth aspect of the present application provides a battery pack comprising a secondary battery selected from the fourth aspect of the present application.

[0021] A sixth aspect of the present application provides an electrical device comprising a secondary battery selected from the fourth aspect of the present application or a battery pack according to the fifth aspect of the present application. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] To more clearly illustrate the technical solution of this application, the following briefly introduces the drawings required for use in the embodiments of this application. Obviously, the drawings described below are only some embodiments of this application. For those skilled in the art, other drawings can be obtained based on the drawings without inventive effort.

[0023] FIG1 is a schematic diagram of a lithium-ion secondary battery in one embodiment of the present application.

[0024] FIG. 2 is an exploded view of the lithium-ion secondary battery in one embodiment of the present application shown in FIG. 1 .

[0025] FIG3 is a schematic diagram of a battery pack in one embodiment of the present application.

[0026] FIG. 4 is an exploded view of the battery pack shown in FIG. 3 according to one embodiment of the present application.

[0027] FIG5 is a schematic diagram of a device using a battery pack as a power source in one embodiment of the present application.

[0028] FIG6 is a schematic diagram of the bonding between starch molecules and cross-linker molecules and active materials.

[0029] Description of Reference Numerals

[0030] 1 battery pack

[0031] 2 upper box

[0032] 3 lower cabinets

[0033] 4 battery modules

[0034] 5Lithium-ion secondary batteries

[0035] 51 shell

[0036] 52 electrode assembly

[0037] 53 cover DETAILED DESCRIPTION

[0038] For the sake of clarity, this application specifically discloses certain numerical ranges. However, any lower limit may be combined with any upper limit to form an unspecified range; and any lower limit may be combined with other lower limits to form an unspecified range, and similarly, any upper limit may be combined with any other upper limit to form an unspecified range. In addition, each individually disclosed point or single value may itself serve as a lower limit or upper limit and be combined with any other point or single value, or with other lower limits or upper limits, to form an unspecified range.

[0039] With the rapid adoption of electric vehicles, including electric vehicles, the market demand for high-energy-density lithium-ion batteries is becoming increasingly urgent. Reducing the content of auxiliary materials, such as adhesives, or adding silicon to anode materials are currently key approaches to increasing energy density. Reducing binder usage requires increasing its binding strength per unit mass. Current methods include grafting, copolymerization, and blending existing adhesive polymers. To improve the binding capacity of high-expansion silicon materials, additives with hydroxyl or carboxyl groups are often added to the silicon surface to coat the material. Another approach to increasing energy density is to increase the active material loading per unit area of ​​the electrode. However, during the electrode coating process, increased loading means increased electrode thickness. This increases the electrode's brittleness and cracking during the drying process, affecting its appearance and performance. Adding a softener to the electrode can lead to residual additive residue and increase the weight of the battery cell.

[0040] The selection of a binder requires careful consideration of the connections between active particles, between active particles and conductive agents, and between active particles and current collectors. Furthermore, the binder's suitability for the coating and drying process during electrode processing must be considered to ensure proper solvent removal and maintain electrode integrity. Because existing battery electrodes, especially anodes, undergo significant volume changes during lithium insertion and extraction, the binder must be able to maintain its adhesion and resist failure despite this constant volume change.

[0041] Existing commonly used anode binders, such as a combination of SBR and CMC, can maintain effective bonding in the initial stage, but cannot adapt to the long-term volume expansion of the anode, especially the increasing number of silicon-containing anodes, which will cause greater expansion than graphite anodes. Since SBR and CMC are both rigid polymer chains, they cannot heal after breaking. Generally, in the late stage of the battery life cycle, the thickness of the adhesive electrode increases significantly, and the expansion force soars, seriously affecting the safety of the battery cell. On the other hand, in order to increase the energy density of the battery cell, the active material loading of the electrode is also greatly increased. During the coating and drying process, the difference in drying speed caused by the increase in thickness can easily cause the electrode to crack, making it difficult to manufacture.

[0042] Therefore, there is a need in the art to provide a new binder composition that can be used to prepare electrode plates with improved brittleness and adhesion, so that secondary batteries are not easily cracked and demolded after multiple cycles over a long life cycle, even when the electrodes undergo significant expansion.

[0043] Specifically, the first aspect of the present application provides an adhesive composition, wherein the composition contains starch and polyvinyl alcohol, and the starch contains amylose and amylopectin.

[0044] The inventors have discovered that the adhesive composition of the present application, by comprising a mixture of starch and polyvinyl alcohol, can significantly improve the brittleness of the electrode. Without being bound by any theory, the inventors believe that the large number of hydroxyl groups on the starch and polyvinyl alcohol can ensure that when the active material loading and the electrode thickness are increased significantly, the water loss rate in the thickness direction of the electrode does not produce a large gradient, which may lead to cracking of the electrode. At the same time, because the selected starch contains a large amount of amylopectin, stress is released during the heat drying process, which can effectively improve the adhesion of the electrode and prevent cracking and demolding. In addition, starch and polyvinyl alcohol are connected to each other through a large number of hydrogen bonds, which can tightly bind to the active material, especially silicon or silicon oxide materials. Even under conditions of large stress changes, hydrogen bonds have a stronger binding force on the active material than other van der Waals bonding forces. Compared with the rigid chains connected by chemical bonds, hydrogen bonds can automatically repair after the hydrogen bonds are broken, and have a certain "self-healing" ability. The molecular chain consists of both rigid chains composed of starch straight chains and flexible chains composed of branches. The branches connected by polyvinyl alcohol at different positions are interconnected, enhancing the overall adhesion.

[0045] Starch is a cheap, abundant and biodegradable natural polymer, which is a mixture of amylose and amylopectin. Amylose is composed of linear straight-chain polysaccharides, and amylopectin is a highly branched polysaccharide. At present, amylose and amylopectin can be separated from starch mixtures by technical means, and the main means include compounding agent separation method, salt separation method, polymer controlled crystallization method, cellulose adsorption method and chromatographic separation method. In some embodiments of the present application, the starch consists of amylose and amylopectin. There are a large number of hydroxyl groups in starch molecules, which can slow down the rapid evaporation of water molecules during processing, ensure that the electrode has a certain flexibility, and promote bonding with the hydroxyl groups on the surface of silicon nanoparticles during use of the electrode. Intermolecular hydrogen bonds can be formed between starch molecules and silicon nanoparticles, and their strength is better than the poor van der Waals force connection between silicon and conventional adhesives such as PVDF and SBR.

[0046] In some embodiments, the number average molecular weight of the amylose is 500-160000 g / mol, optionally 2000-50000 g / mol, optionally 5000-20000 g / mol; and / or the number average molecular weight of the amylopectin is 100000-1000000 g / mol, optionally 150000-800000 g / mol, optionally 300000-600000 g / mol. The number average molecular weight is measured according to GB / T 36214-2018 standard. The inventors have found that by selecting the number average molecular weight of amylose and amylose within a specific range, pole pieces with higher bonding force and cohesion can be obtained. In addition, the starch may also contain amylose and / or amylopectin having a number average molecular weight outside the above range, and its content does not exceed 10% by weight, optionally does not exceed 5% by weight, or does not exceed 1% by weight, or is 0% by weight, based on the total weight of the starch.

[0047] In some embodiments, in any embodiment, the weight ratio of amylose to amylopectin in the starch is 1:1 to 1:10, optionally 1:3 to 1:8, optionally 1:4 to 1:6. The ratio of amylose to amylopectin in starch can be used to adjust the strength and toughness of the binder composition. In some embodiments, the starch content is 10-95% by weight, optionally 80-92% by weight, based on the dry weight of the binder composition. The inventors have found that by selecting amylose and amylopectin within a specific weight ratio range, pole pieces with fewer surface cracks and higher cohesion can be obtained. When the starch in the composition contains only amylose, or only contains amylose, the pole pieces made therefrom do not even meet the requirements for pole pieces in the art, such as a large amount of obvious cracking and powder loss.

[0048] In some embodiments, the weight ratio of starch to polyvinyl alcohol in the composition is 1.5:1-20:1, alternatively 2:1 to 20:1, alternatively 5:1 to 10:1. In some embodiments, the weight average molecular weight of the polyvinyl alcohol is 15,000-250,000 g / mol, alternatively 25,000-120,000 g / mol. Further alternatively 30,000-80,000 g / mol. In some embodiments, the content of the polyvinyl alcohol is 1-35 weight %, alternatively 7-20 weight %, based on the dry weight of the binder composition.

[0049] In some embodiments, the binder composition further comprises at least one cross-linking agent selected from one or more of oxalic acid, polyvinyl pyrrolidone, phosphorus oxychloride, sodium trimetaphosphate, adipic acid, and hexametaphosphate, optionally oxalic acid. Adding a portion of the cross-linking agent to the mixture of starch and polyvinyl alcohol can further enhance the "interlocking" effect of the binder. As shown in Figure 6, the cross-linking agent, specifically oxalic acid, can form ester bonds with two hydroxyl groups at different positions in amylose and / or amylopectin, "locking" these different positions together, thereby increasing the bonding ability of the binder molecular chain. The polyvinyl alcohol molecules are not shown in Figure 6. In fact, the polyvinyl alcohol molecular chain also contains hydroxyl groups, which can also react with the cross-linking agent, further enhancing the "interlocking" effect of the binder. In some embodiments, the content of the cross-linking agent is 0.01-5% by weight, optionally 0.2-1% by weight, based on the dry weight of the binder composition. Of course, the addition of a cross-linking agent is not required. In some embodiments, the binder composition does not include any cross-linking agent.

[0050] In some embodiments, the binder composition may further comprise other additives. The additives may be, for example, film-forming aids, rheology modifiers, tackifiers, flame retardants, or defoamers. The other additives may be present in an amount of 0-10% by weight, and optionally 1-5% by weight, based on the dry weight of the binder composition.

[0051] In some embodiments, the binder composition is an aqueous dispersion comprising water as a solvent. A starch mixture comprising a specific proportion of amylose and amylopectin can be dispersed in deionized water by stirring at an elevated temperature, then adding a specific proportion of polyvinyl alcohol, heating and stirring simultaneously, thereby forming an aqueous dispersion of the binder composition. In addition, the binder composition can also include a small amount of other solvents, such as conventional organic solvents, such as ethanol, toluene, dimethyl sulfoxide, N,N-dimethylformamide, etc. In some embodiments, the solid content of the binder composition is 15-60% by weight, alternatively 20-40% by weight. The content of organic solvent in the binder composition is less than 5% by weight, alternatively less than 1% by weight, further alternatively 0% by weight. Of course, the solid content of the binder composition can be adjusted as needed by changing the addition of water, and is not limited to the above range.

[0052] The present application also relates to a method for preparing a binder composition selected from the first aspect of the present application, comprising the following steps:

[0053] 1) adding starch to deionized water and adding polyvinyl alcohol, wherein the weight ratio of starch to polyvinyl alcohol is 1.5:1 to 20:1, the starch contains amylose and amylopectin in a weight ratio of 1:1 to 1:10, wherein the number average molecular weight of the amylose is 500-160,000 g / mol, and the number average molecular weight of the amylopectin is 100,000-1,000,000 g / mol;

[0054] 2) stirring the mixture obtained in 1) at 50-99° C. for 0.5-24 hours;

[0055] 3) optionally adding at least one cross-linking agent to the above mixture and continuing stirring at 10-99° C. for 0.5-24 hours;

[0056] 4) Optionally cool the mixture.

[0057] The starch may be pre-processed to remove impurities and then dried in an oven. The drying temperature may be, for example, 60-100°C for 2-24 hours. The components may be mixed by stirring in a container, for example, using a stirrer at 2000 rpm, until no sediment is visible at the bottom of the container.

[0058] In some embodiments, the temperature in step 2) is 70-95°C, and / or the stirring time is 8-15 hours. In some embodiments, the temperature in step 3) is 70-95°C, and / or the stirring time is 8-15 hours. The temperature and stirring time in steps 2) and 3) can be adjusted accordingly according to actual conditions and are not limited to the above ranges. The obtained mixture is allowed to stand and cool, for example, to room temperature, and then the solid content of the mixture can be measured. The solid content of the mixture can be adjusted by changing the amount of deionized water added to meet the requirements of different battery systems. In some embodiments, the solid content of the mixture is 15-60% by weight, optionally 20-40% by weight. In some embodiments, the mixture can be heated so that the mixture is in the form of a paste.

[0059] The second aspect of the present application provides a composition for preparing a battery electrode sheet, comprising an electrode active material, a conductive agent, and the binder composition according to the first aspect of the present application, and optionally water and a dispersant. The battery electrode sheet is specifically a positive electrode sheet and / or a negative electrode sheet. The electrode active material can be a positive electrode active material or a negative electrode active material. The electrode active material and the conductive agent can be conventionally selected as needed, which will be described in detail below.

[0060] A third aspect of the present application provides an electrode plate, which is prepared by using the binder composition selected from the first aspect of the present application.

[0061] The fourth aspect of the present application provides a secondary battery, comprising an electrode plate selected from the third aspect of the present application. The electrode plate may be a positive electrode plate and / or a negative electrode plate.

[0062] A fifth aspect of the present application provides a battery pack comprising a secondary battery selected from the fourth aspect of the present application.

[0063] A sixth aspect of the present application provides an electrical device comprising a secondary battery selected from the fourth aspect of the present application or a battery pack according to the fifth aspect of the present application.

[0064] The materials of the various components of the battery mentioned in this application can be selected from a wide range. In some embodiments, the battery is particularly a lithium-ion secondary battery. The battery cells of the lithium-ion secondary battery are described in detail below.

[0065] Typically, a lithium-ion secondary battery consists of a positive electrode, a negative electrode, a separator, and an electrolyte. During the battery's charge and discharge processes, active ions are inserted and removed between the positive and negative electrodes. The separator is placed between the positive and negative electrodes to provide isolation. The electrolyte conducts ions between the positive and negative electrodes.

[0066] [Electrolyte]

[0067] The electrolyte conducts ions between the positive and negative electrodes and consists of electrolyte salts and solvents.

[0068] In the present application, the electrolyte salt may be a commonly used electrolyte salt in lithium-ion secondary batteries, such as a lithium salt, including the lithium salts described above as high thermal stability salts, lithium salts as low impedance additives, or lithium salts that inhibit corrosion of aluminum foil. As an example, the electrolyte salt may be selected from one or more of lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium trifluoromethanesulfonate (LiTFS), lithium difluorooxalatoborate (LiDFOB), lithium difluorophosphate (LiPO2F2), lithium difluorobis(oxalatophosphate) (LiDFOP), lithium fluorosulfonate (LiSO3F), difluorobis(oxalato) (NDFOP), Li2F(SO2N)2SO2F, KFSI, CsFSI, Ba(FSI)2, and LiFSO2NSO2CH2CH2CF3.

[0069] The type of solvent is not particularly limited and can be selected according to actual needs. In some embodiments, the solvent is a non-aqueous solvent. Alternatively, the solvent may include one or more of linear carbonate, cyclic carbonate, and carboxylate. In some embodiments, the solvent may be selected from ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), tetrahydrofuran, sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS) and diethyl sulfone (ESE).

[0070] In some embodiments, the electrolyte may optionally include other additives. For example, the additives may include negative electrode film-forming additives, positive electrode film-forming additives, and additives that can improve certain battery properties, such as additives that improve battery overcharge performance, additives that improve battery high temperature performance, and additives that improve battery low temperature performance. As an example, the additive is selected from at least one of a cyclic carbonate compound containing an unsaturated bond, a halogen-substituted cyclic carbonate compound, a sulfate compound, a sulfite compound, a sultone compound, a disulfonic acid compound, a nitrile compound, an aromatic compound, an isocyanate compound, a phosphazene compound, a cyclic acid anhydride compound, a phosphite compound, a phosphate compound, a borate compound, and a carboxylate compound.

[0071] [Positive electrode]

[0072] The positive electrode sheet includes a positive electrode current collector and a positive electrode active material layer disposed on at least one surface of the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material and a conductive agent.

[0073] As an example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode active material layer is provided on either or both of the two facing surfaces of the positive electrode current collector.

[0074] In the lithium-ion secondary battery of the present application, the positive electrode current collector may be a metal foil or a composite current collector. For example, aluminum foil may be used as the metal foil. The composite current collector may include a polymer material base and a metal layer formed on at least one surface of the polymer material base. The composite current collector may be formed by forming a metal material (e.g., aluminum, aluminum alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer material substrate (e.g., a substrate of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0075] The positive electrode active material layer disposed on the surface of the positive electrode current collector includes a positive electrode active material. The positive electrode active material used in this application may be any conventional positive electrode active material used in secondary batteries. In some embodiments, the positive electrode active material may include one or more selected from lithium transition metal oxides, olivine-structured lithium-containing phosphates, and their respective modified compounds. Examples of lithium transition metal oxides may include, but are not limited to, one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel cobalt oxide, lithium manganese cobalt oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and their modified compounds. Examples of olivine-structured lithium-containing phosphates may include, but are not limited to, one or more of lithium iron phosphate, a composite material of lithium iron phosphate and carbon, lithium manganese phosphate, a composite material of lithium manganese phosphate and carbon, lithium manganese iron phosphate, a composite material of lithium manganese iron phosphate and carbon, and their modified compounds. All of these materials can be obtained commercially. The surface of the positive electrode active material may be coated with carbon.

[0076] The positive electrode active material layer may optionally include a conductive agent. However, the type of conductive agent is not particularly limited, and those skilled in the art may select one based on actual needs. For example, the conductive agent used in the positive electrode material may be selected from one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0077] The positive electrode active material layer also includes a binder. The binder is the binder composition described above. In addition to the binder composition described above, the binder may also include other binders. As an example, the other binders may be one or more of styrene-butadiene rubber (SBR), water-based acrylic resin, polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyacrylic acid (PAA), carboxymethyl cellulose (CMC), polyvinyl alcohol (PVA) and polyvinyl butyral (PVB).

[0078] In this application, the positive electrode sheet can be prepared according to methods known in the art. For example, a carbon-coated positive electrode active material, a conductive agent, and an aqueous binder can be dispersed in a solvent (e.g., water) to form a uniform positive electrode slurry; the positive electrode slurry is coated on a positive electrode current collector, and after drying, cold pressing, and other processes, a positive electrode sheet is obtained.

[0079] [Negative electrode]

[0080] The negative electrode sheet includes a negative electrode current collector and a negative electrode material layer disposed on at least one surface of the negative electrode current collector, wherein the negative electrode material layer includes a negative electrode active material.

[0081] As an example, the negative electrode current collector has two surfaces facing each other in its thickness direction, and the negative electrode material layer is disposed on either or both of the two facing surfaces of the negative electrode current collector.

[0082] In the lithium-ion secondary battery of the present application, the negative electrode current collector may be a metal foil or a composite current collector. For example, copper foil may be used as the metal foil. The composite current collector may include a polymer material base layer and a metal layer formed on at least one surface of the polymer material base material. The composite current collector may be formed by forming a metal material (e.g., copper, copper alloy, nickel, nickel alloy, titanium, titanium alloy, silver, and silver alloy, etc.) on a polymer material base material (e.g., a base material of polypropylene (PP), polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polystyrene (PS), polyethylene (PE), etc.).

[0083] In the lithium-ion secondary battery of the present application, the negative electrode material layer generally comprises a negative electrode active material and an optional binder, an optional conductive agent, and other optional additives, and is generally formed by coating and drying a negative electrode slurry. The negative electrode slurry coating is generally formed by dispersing the negative electrode active material and the optional conductive agent and binder in a solvent and stirring the mixture uniformly. The solvent may be N-methylpyrrolidone (NMP) or deionized water.

[0084] The specific type of negative electrode active material is not limited. Active materials known in the art for use in lithium-ion secondary battery negative electrodes can be used, and those skilled in the art can select the active material based on actual needs. By way of example, the negative electrode active material can be selected from one or more of graphite, soft carbon, hard carbon, mesocarbon microbeads, carbon fibers, carbon nanotubes, elemental silicon, silicon oxides, silicon-carbon composites, and lithium titanate.

[0085] As an example, the conductive agent may be selected from one or more of superconducting carbon, acetylene black, carbon black, Ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0086] The negative electrode active material layer also includes a binder. The binder is the binder composition described above. In addition to the binder composition described above, the binder may also include other binders. As an example, the other binder can be selected from one or more of styrene-butadiene rubber (SBR), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyacrylamide (PAM), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), and carboxymethyl chitosan (CMCS).

[0087] Other optional auxiliary agents include, for example, thickeners (such as sodium carboxymethyl cellulose (CMC-Na)).

[0088] [Isolation film]

[0089] The lithium-ion secondary battery using an electrolyte also includes an isolation membrane. The isolation membrane is arranged between the positive electrode plate and the negative electrode plate to play an isolation role. The present application has no particular restrictions on the type of isolation membrane, and any well-known porous structure isolation membrane with good chemical stability and mechanical stability can be selected. In some embodiments, the material of the isolation membrane can be selected from one or more of glass fiber, non-woven fabric, polyethylene, polypropylene and polyvinylidene fluoride. The isolation membrane can be a single-layer film or a multi-layer composite film, without special restrictions. When the isolation membrane is a multi-layer composite film, the materials of each layer can be the same or different, without special restrictions.

[0090] In some embodiments, the positive electrode sheet, the negative electrode sheet, and the separator can be formed into an electrode assembly through a winding process or a lamination process.

[0091] In some embodiments, the secondary battery may include an outer packaging that can be used to encapsulate the electrode assembly and the electrolyte.

[0092] In some embodiments, the outer packaging of the secondary battery can be a hard shell, such as a hard plastic shell, an aluminum shell, a steel shell, etc. The outer packaging of the secondary battery can also be a soft package, such as a pouch-type soft package. The soft package can be made of plastic, such as polypropylene (PP), polybutylene terephthalate (PBT), and polybutylene succinate (PBS).

[0093] The present application has no particular limitation on the shape of the secondary battery, which may be cylindrical, square, or any other shape. For example, FIG1 shows a lithium-ion secondary battery 5 having a square structure as an example.

[0094] In some embodiments, referring to Figure 2, the outer packaging may include a shell 51 and a cover plate 53. The shell 51 may include a bottom plate and a side plate connected to the bottom plate, and the bottom plate and the side plate enclose a receiving cavity. The shell 51 has an opening connected to the receiving cavity, and the cover plate 53 can be covered on the opening to close the receiving cavity. The positive electrode sheet, the negative electrode sheet and the isolation membrane can be formed into an electrode assembly 52 through a winding process or a lamination process. The electrode assembly 52 is encapsulated in the receiving cavity. The electrolyte is infiltrated in the electrode assembly 52. ​​The number of electrode assemblies 52 contained in the lithium-ion secondary battery 5 can be one or more, and those skilled in the art can select according to specific actual needs.

[0095] In some embodiments, lithium-ion secondary batteries can be assembled into a battery module 4. The number of lithium-ion secondary batteries contained in the battery module 4 can be one or more. The specific number can be selected by those skilled in the art according to the application and capacity of the battery module 4. In the battery module 4, multiple lithium-ion secondary batteries 5 can be arranged in sequence along the length direction of the battery module. Of course, they can also be arranged in any other manner. The multiple lithium-ion secondary batteries 5 can further be fixed by fasteners. Optionally, the battery module 4 can also include a shell having a storage space, and the multiple lithium-ion secondary batteries 5 are accommodated in the storage space.

[0096] In some embodiments, the lithium-ion secondary batteries 5 or battery modules 4 can be assembled into a battery pack 1 , and the number of lithium-ion secondary batteries 5 or battery modules 4 contained in the battery pack 1 can be selected by those skilled in the art based on the application and capacity of the battery pack 1 .

[0097] Figures 3 and 4 illustrate an example battery pack 1. Referring to Figures 3 and 4 , the battery pack 1 may include a battery box and a plurality of battery cells disposed within the box. The battery box comprises an upper case 2 and a lower case 3. The upper case 2 can be placed over the lower case 3 to form an enclosed space for accommodating the battery cells.

[0098] In addition, the present application also provides a device, which includes a battery pack provided in the present application. The battery pack can be used as a power source for the device, and can also be used as an energy storage unit for the device. The device can be, but is not limited to, a mobile device (such as a mobile phone, a laptop computer, etc.), an electric vehicle (such as a pure electric vehicle, a hybrid electric vehicle, a plug-in hybrid electric vehicle, an electric bicycle, an electric scooter, an electric golf cart, an electric truck, etc.), an electric train, a ship and a satellite, an energy storage system, etc. As the device, a battery pack can be selected according to its usage requirements.

[0099] Figure 5 shows an example device. This device is a pure electric vehicle, hybrid electric vehicle, or plug-in hybrid electric vehicle. To meet the device's requirements for high power and high energy density of lithium-ion secondary batteries, a battery pack or battery module can be used.

[0100] Example

[0101] Below, the examples of the present application are described. The examples described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific techniques or conditions are specified in the examples, the techniques or conditions described in the literature in this field or the product instructions are used. The reagents or instruments used that do not specify the manufacturer are conventional products that can be obtained commercially. Unless otherwise specified, all content ratios are weight ratios, and all experiments are carried out at room temperature (25°C) and normal pressure.

[0102] The following ingredients were used:

[0103] Amylose A1: number average molecular weight 15000 g / mol, density 1.5 g / cm 3 , purchased from Sigma-Aldrich;

[0104] Amylose A2: number average molecular weight 5000 g / mol, density 1.5 g / cm 3 , purchased from Sigma-Aldrich;

[0105] Amylose A3: number average molecular weight 2000 g / mol, density 1.5 g / cm 3 , purchased from Sigma-Aldrich;

[0106] Amylose A4: number average molecular weight 150,000 g / mol, density 1.5 g / cm 3 , purchased from Sigma-Aldrich;

[0107] Amylopectin B1: number average molecular weight 350,000 g / mol, density 1.6 g / cm 3 , purchased from Sigma-Aldrich;

[0108] Amylopectin B2: number average molecular weight 600,000 g / mol, density 1.6 g / cm 3 , purchased from Sigma-Aldrich;

[0109] Amylopectin B3: number average molecular weight 150,000 g / mol, density 1.6 g / cm 3 , purchased from Sigma-Aldrich;

[0110] Amylopectin B4: number average molecular weight 800,000 g / mol, density 1.6 g / cm 3 , purchased from Sigma-Aldrich;

[0111] Polyvinyl alcohol V1: weight average molecular weight 47000 g / mol, purchased from Aladdin Reagent (Shanghai) Co., Ltd.

[0112] Polyvinyl alcohol V2: weight average molecular weight 31000 g / mol, purchased from Aladdin Reagent (Shanghai) Co., Ltd.

[0113] Polyvinyl alcohol V3: weight average molecular weight 107000 g / mol, purchased from Aladdin Reagent (Shanghai) Co., Ltd.

[0114] Polyvinyl alcohol V4: weight average molecular weight is 205000 g / mol, purchased from Aladdin Reagent (Shanghai) Co., Ltd.

[0115] Example 1:

[0116] Take a certain amount of amylose A1 and amylopectin B1 and dry them separately in an oven at 80°C for 12 hours. Take 2 parts of amylose A1 and 8 parts of amylopectin B1 and add all 10 parts of starch to 30 parts of deionized water. Stir at room temperature for 30 minutes. Add 2 parts of polyvinyl alcohol V1 to this mixture and stir at 80°C for 12 hours. Then add 0.05 parts of oxalic acid, raise the temperature to 90°C, and continue stirring for 2 hours. After cooling to room temperature, test the solids content and set aside.

[0117] Preparation of negative electrode sheet: Take 94 parts of artificial graphite, 1 part of carbon black, and 5 parts of the binder prepared above (5 parts refers to the actual solid amount), dissolve them in deionized water, mix them evenly and prepare negative electrode slurry. The negative electrode slurry is evenly coated on the negative electrode current collector copper foil in multiple times, and the negative electrode sheet is obtained after drying, cold pressing and cutting. The load and compaction density of the negative electrode sheet: the coating weight is 10mg / mm 2 , compacted density is 1.6g / cm 3 .

[0118] Preparation of lithium-ion batteries:

[0119] The positive electrode active material LiNi 0.8 Co 0.1 Mn 0.1O2 (NCM811), conductive agent acetylene black, and binder polyvinylidene fluoride (PVDF) are dissolved in solvent N-methylpyrrolidone (NMP) in a weight ratio of 90:5:5, and the mixture is stirred thoroughly to obtain a positive electrode slurry; the positive electrode slurry is then evenly coated on the positive electrode current collector, and then dried, cold pressed, and cut to obtain a single-sided positive electrode sheet with a film weight of 350mg / 1540.25mm 2 Positive electrode.

[0120] In an argon atmosphere glove box (H2O<0.1ppm, O2<0.1ppm), the organic solvent EC / EMC was mixed evenly in a volume ratio of 3 / 7, 12.5% ​​LiPF6 lithium salt was added and dissolved in the organic solvent, and stirred evenly to obtain the corresponding electrolyte.

[0121] An 8μm PE porous film is used as the substrate, and a 2μm ceramic coating is coated on both sides to serve as the isolation membrane.

[0122] The positive electrode sheet, separator, and negative electrode sheet prepared as described above were stacked in order, with the separator positioned between the positive and negative electrode sheets to provide isolation. The cells were then wound to obtain a bare cell. The tabs were welded to the bare cell and placed in an aluminum casing. The cells were then baked at 80°C to remove moisture. The electrolyte was then injected and sealed to obtain an uncharged battery. The uncharged battery then underwent a series of steps, including resting, hot and cold pressing, formation, shaping, and capacity testing, to obtain the lithium-ion secondary battery product of Example 1.

[0123] Example 2-5:

[0124] Example 1 was repeated, except that the weight ratio of starch and polyvinyl alcohol was as shown in Table 1 below (by adjusting the amount of polyvinyl alcohol added). In each example, the corresponding negative electrode sheet and the corresponding lithium ion secondary battery product were prepared as described above.

[0125] The negative electrode sheets and lithium-ion secondary batteries of Examples 1-5 were tested, and the results are shown in Table 1 below.

[0126] Table 1

[0127] Starch and polyvinyl alcohol weight ratio Coating appearance Adhesion Cohesion Expansion after 1000 cycles Example 1 5: 1 No crack 21 N / m 1.14 MPa 27% Example 2 10: 1 No crack 23 N / m 1.28 MPa 27% Example 3 1.5: 1 Intermittent small crack 5 N / m 0.52 MPa 35% Example 4 2: 1 Intermittent small crack 8 N / m 0.56 MPa 35% Example 5 20: 1 Intermittent small crack 13 N / m 0.77 MPa 34%

[0128] Coating appearance inspection methods and standards:

[0129] Observe the electrode appearance at the electrode reel at the tail end of the coating oven. If the electrode has fewer than three cracks less than 3 mm in length within any continuous 100-meter inner surface, it is defined as crack-free. If there are fewer than five cracks less than 5 mm in length, and none of them are considered crack-free, it is defined as intermittent minor cracks. If the length and number of cracks exceed the above standards, it is defined as continuous major cracks.

[0130] Pole piece adhesion test method:

[0131] Step 1: Select a flat steel plate. Wipe the surface with dust-free paper and alcohol. Apply special double-sided tape to the steel plate. The tape should be 20mm wide and 90-150mm long. The tape should be parallel to the edge of the steel plate and the distance between the tape and the two edges of the steel plate should be equal. (Note: Do not touch the adhesive surface of the double-sided tape with your hands.)

[0132] Step 2: Take the electrode to be tested, use a blade to cut a sample with a width of 30mm and a length of 100-160mm, and stick the cut electrode sample on the double-sided tape. Align the edge of the electrode with the edge of the steel plate to ensure that the electrode and the double-sided tape are flat.

[0133] Step 3: When the length of the steel plate is greater than the length of the pole piece, use paper tape to insert it above or below the pole and fix it with wrinkle glue, with the test surface facing up, and use a 2kg roller to roll back and forth 3-4 times.

[0134] Step 4: Fold the paper tape upwards and fix the end of the steel plate without the electrode with the lower clamp, and clamp the paper tape with the upper clamp parallel to the steel plate.

[0135] Step 5: Operate the tensile testing machine, set and read the bonding strength value.

[0136] Pole cohesion test method:

[0137] Step 1: Stick the special double-sided tape on the steel plate, with the tape width 20mm and length 90-150mm.

[0138] Step 2: Stick the electrode sample cut in step 1 on the double-sided tape with the test side facing up.

[0139] Step 3: Stick a low-viscosity green tape with a width of 20mm and a length 80-200mm longer than the sample length evenly on the test surface, and roll it three times in the same direction with a roller.

[0140] Step 4: Turn on the power of the high-speed rail tensile testing machine, the indicator light will light up, and adjust the limit block to the appropriate position.

[0141] Step 5: Fix the end of the steel plate without the electrode with the lower clamp. Fold the green glue with the hard paper upwards and fix it with the upper clamp.

[0142] Step 6: Set the parameters of the tensile testing machine, where the tensile speed is 10mm / min and the length is greater than 15mm.

[0143] Step 7: Read the cohesion value, repeat three times, and take the average value

[0144] Expansion measurement method after 1000 cycles:

[0145] Take the battery cell after 1000 cycles of 0.33C charge and discharge test, use the screw micrometer to measure the electrode thickness h1, and compare it with the initial state of the battery cell electrode thickness h0.

[0146] The performance data of the subsequent examples are all the same as the above test methods.

[0147] Examples 6-12 and Comparative Examples 1-2:

[0148] Example 1 was repeated, except that the weight ratio of amylose to amylopectin in the starch was as shown in Table 2 below (the total weight of starch remained unchanged). Each example was prepared as described above to obtain the corresponding negative electrode sheet and the corresponding lithium-ion secondary battery product.

[0149] The negative electrode sheets and lithium-ion secondary batteries of Examples 6-12 and Comparative Examples 1-2 were tested, and the results were summarized with the results of Example 1, as shown in Table 2 below.

[0150] Table 2

[0151]

[0152] *: The electrode shows obvious cracking and powder loss.

[0153] Examples 13-15:

[0154] Example 1 was repeated, except that the type of amylose in the starch was as shown in Table 3. Each example was prepared as described above to obtain the corresponding negative electrode sheet and the corresponding lithium-ion secondary battery product.

[0155] The negative electrode sheets and lithium-ion secondary batteries of Examples 13-15 were tested, and the results were summarized with the results of Example 1, as shown in Table 3 below.

[0156] Table 3

[0157] Amylose Type Coating Appearance Adhesion Cohesion Expansion after 1000 cycles Example 1A1 No crack 21 N / m 1.14 MPa 27% Example 13A2 No crack 15 N / m 0.88 MPa 29% Example 14A3 Intermittent minor cracks 7 N / m 0.55 MPa 31% Example 15A4 Intermittent minor cracks 6 N / m 0.31 MPa 32%

[0158] Examples 16-18:

[0159] Example 1 was repeated, except that the type of amylopectin in the starch was as shown in Table 4. Each example was prepared as described above to obtain the corresponding negative electrode sheet and the corresponding lithium-ion secondary battery product.

[0160] The negative electrode sheets and lithium-ion secondary batteries of Examples 16-18 were tested, and the results were summarized with the results of Example 1, as shown in Table 4 below.

[0161] Table 4

[0162] Pullulan Type Coating Appearance Adhesion Cohesion Expansion after 1000 cycles Example 1B1 No crack 21 N / m 1.14 MPa 27% Example 16B2 No crack 15 N / m 0.77 MPa 30% Example 17B3 Continuous and numerous cracks 8 N / m 0.55 MPa 38% Example 18B4 Intermittent and minor cracks 5 N / m 0.37 MPa 37%

[0163] Examples 19-21:

[0164] Example 1 was repeated, except that the type of polyvinyl alcohol was as shown in Table 5. Each example was prepared as described above to obtain the corresponding negative electrode sheet and the corresponding lithium-ion secondary battery product.

[0165] The negative electrode sheets and lithium-ion secondary batteries of Examples 19-21 were tested, and the results were summarized with the results of Example 1, as shown in Table 5 below.

[0166] Table 5

[0167] Polyvinyl alcohol type Coating appearance Adhesion Cohesion Expansion after 1000 cycles Example 1 V1 No crack 21 N / m 1.14 MPa 27% Example 19 V2 No crack 17 N / m 0.77 MPa 30% Example 20 V3 Intermittent small cracks 8 N / m 0.55 MPa 33% Example 21 V4 Continuous large cracks 3 N / m 0.12 MPa 40%

[0168] Examples 22-23:

[0169] Example 1 was repeated, except that the type of cross-linking agent was used as shown in Table 6. Each example was prepared as described above to obtain the corresponding negative electrode sheet and the corresponding lithium-ion secondary battery product.

[0170] The negative electrode sheets and lithium-ion secondary batteries of Examples 22-23 were tested, and the results were summarized with the results of Example 1, as shown in Table 6 below.

[0171] Table 6

[0172] Crosslinking agent type Coating appearance Adhesion Cohesion Expansion after 1000 cycles Example 1 Oxalic acid No crack 21 N / m 1.14 MPa 27% Example 22 Adipic acid No crack 10 N / m 0.87 MPa 31% Example 23 Polyvinyl pyrrolidone No crack 8 N / m 0.67 MPa 31%

[0173] Although the present application has been described with reference to the embodiments, various modifications may be made thereto and components may be substituted with equivalents without departing from the scope of the present application. In particular, the various technical features described in the various embodiments may be combined in any manner as long as there are no structural conflicts. The present application is not limited to the specific embodiments disclosed herein, but encompasses all technical solutions within the scope of the claims.

Claims

1. A binder composition, wherein the composition comprises starch and polyvinyl alcohol, and the starch comprises amylose and amylopectin.

2. The binder composition according to claim 1, wherein the number average molecular weight of the amylose is 500-160,000 g / mol, optionally 2,000-50,000 g / mol, optionally 5,000-20,000 g / mol; and / or the number average molecular weight of the amylopectin is 100,000-1,000,000 g / mol, optionally 150,000-800,000 g / mol, optionally 300,000-600,000 g / mol.

3. The binder composition according to any one of claims 1 to 2, wherein the weight ratio of starch to polyvinyl alcohol in the composition is 1.5:1-20:1, optionally 2:1 to 20:1, optionally 5:1 to 10:

1. 4 . The binder composition according to claim 1 , wherein the weight ratio of amylose to amylopectin in the starch is 1:1 to 1:10, optionally 1:3 to 1:8, optionally 1:4 to 1:

6.

5. The binder composition according to any one of claims 1 to 4, wherein the starch content is 10-95 wt%, optionally 80-92 wt%, based on the dry weight of the binder composition.

6. The adhesive composition according to any one of claims 1 to 5, wherein the weight average molecular weight of the polyvinyl alcohol is 15,000-250,000 g / mol, optionally 25,000-120,000 g / mol, further optionally 30,000-80,000 g / mol.

7. The binder composition according to any one of claims 1 to 6, wherein the content of the polyvinyl alcohol is 1-35 wt%, optionally 7-20 wt%, based on the dry weight of the binder composition.

8. The binder composition according to any one of claims 1 to 7, further comprising at least one cross-linking agent, wherein the cross-linking agent is selected from one or more of oxalic acid, polyvinylpyrrolidone, phosphorus oxychloride, sodium trimetaphosphate, adipic acid, and hexametaphosphate, and is optionally oxalic acid. 9 . The adhesive composition according to claim 8 , wherein the content of the crosslinking agent is 0.01-5 wt %, optionally 0.2-1 wt %, based on the dry weight of the adhesive composition. 10 . The binder composition according to claim 1 , which is an aqueous dispersion comprising water as a solvent.

11. A method for preparing the binder composition according to any one of claims 1 to 10, comprising the following steps: 1) adding starch to deionized water and adding polyvinyl alcohol, wherein the weight ratio of starch to polyvinyl alcohol is 1.5:1 to 20:1, the starch contains amylose and amylopectin in a weight ratio of 1:1 to 1:10, wherein the number average molecular weight of the amylose is 500-160,000 g / mol, and the number average molecular weight of the amylopectin is 100,000-1,000,000 g / mol; 2) stirring the mixture obtained in 1) at 50-99° C. for 0.5-24 hours; 3) Optionally, at least one cross-linking agent is added to the above mixture, and stirring is continued at 10-99° C. for 0.5-24 hours.

12. The method according to claim 11, wherein the temperature in step 2) is 70-95°C, and / or the stirring time is 8-15 hours.

13. The method according to claim 11 or 12, wherein the temperature in step 3) is 70-95°C, and / or the stirring time is 8-15 hours. 14 . A composition for preparing a battery pole sheet, comprising an electrode active material, a conductive agent, and the binder composition according to claim 1 , and optionally water and a dispersant. 15 . A battery pole sheet, prepared by using the binder composition according to claim 1 or the composition according to claim 14 . The battery electrode according to claim 15 , which is a positive electrode and / or a negative electrode. 17 . A secondary battery comprising the battery electrode according to claim 15 or 16 . 18 . A battery pack comprising the secondary battery according to claim 17 . 19 . An electric device comprising the secondary battery according to claim 17 or the battery pack according to claim 18 .