Electrode binder, electrode, lithium ion secondary battery, and method for manufacturing electrode

By using an electrode binder of ultra-high molecular weight olefin-based polymer particles, combined with a dry method, the problems of solvent volatilization and environmental load in the manufacture of lithium-ion secondary battery electrodes have been solved, and the electrode material has achieved excellent charge and discharge capacity and conductivity. sex.

CN118872097APending Publication Date: 2024-10-29MITSUI CHEMICALS INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380027238.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-09-29
Filing Date
2023-03-14
Publication Date
2024-10-29

AI Technical Summary

Technical Problem

Among the existing lithium-ion secondary battery electrode manufacturing methods, the wet method has problems such as complex solvent volatilization, safety and environmental load, and it is difficult to easily produce electrode materials.

Method used

Ultra-high molecular weight olefin polymer particles are used as electrode binders, and active materials and current collectors are mixed through a dry method to prepare electrodes with excellent charge and discharge capacity that meet the requirements of intrinsic viscosity, particle size and screen pass rate. .

Benefits of technology

It realizes the simple and safe production of electrodes by dry method, improves the charge and discharge capacity and conductivity of lithium-ion secondary batteries, reduces environmental load, and improves the adhesion and dispersion of electrode materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005040237160000201
    Figure BDA0005040237160000201
  • Figure BDA0005040237160000241
    Figure BDA0005040237160000241
  • Figure BDA0005040237160000261
    Figure BDA0005040237160000261
Patent Text Reader

Abstract

One embodiment of the present invention relates to an electrode binder, an electrode, a lithium ion secondary battery, or a method for manufacturing an electrode, the electrode binder comprising ultra-high molecular weight olefin polymer microparticles (A) satisfying the following requirements (i) to iii: (i) the intrinsic viscosity [eta] measured in a decalin solvent at 135 DEG C is in the range of 5-50 dl / g; (ii) the average particle diameter (d50) in the mass-based particle size distribution by the Coulter counter method is in the range of 1-50 [mu] m; (iii) 50% by mass or more of the ultra-high molecular weight olefin polymer microparticles (A) pass through a screen having a 45 [mu] m mesh.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] One embodiment of the present invention relates to an electrode binder, an electrode, a lithium ion secondary battery, or a method for producing an electrode. Background Art

[0002] Lithium-ion secondary batteries are used in the fields of mobile phones, notebook personal computers, etc. because they are small and light, have high energy density, and can be repeatedly charged and discharged. In recent years, as the demand and use of lithium-ion secondary batteries have expanded, there are demands for improved performance such as stability, low resistance, and high capacity, environmental considerations during the manufacture of lithium-ion secondary batteries, and cost improvements.

[0003] As a method for manufacturing an electrode for a lithium ion secondary battery, a method widely known is to dissolve or disperse a resin serving as a binder in a solvent, disperse an active material and a conductive aid therein to form a slurry, apply the slurry to the surface of a collector, and then volatilize the solvent (wet method).

[0004] In addition, in order to produce a rolled sheet such as an electrode sheet from a powder containing an active material, a method for producing an electrode by a dry process is also known, in which a powder rolling device is used to compression-mold the powder.

[0005] As a method for manufacturing an electrode by a dry process, for example, Patent Document 1 discloses a method for manufacturing an anode in which lithium metal plating and gas generation can be controlled by pre-doping lithium ions in the anode.

[0006] For example, Patent Document 2 discloses a method for improving the charge and discharge capacity as a battery performance by optimizing the powder characteristics of a positive electrode active material and the mixing process during the production of a positive electrode material.

[0007] Prior art literature

[0008] Patent Literature

[0009] Patent Document 1: Japanese Patent Application No. 2019-508896

[0010] Patent Document 2: Japanese Patent Application Publication No. 2020-202159 Summary of the invention

[0011] In the wet method, when a solvent is used as a dispersion medium of an adhesive, since it is necessary to volatilize the unwanted solvent in the battery, not only the process becomes complicated, but also problems of safety and environmental load are generated. In addition, since the coating amount of the slurry is affected by the viscosity, film thickness, etc. of the solvent, complex parameter management is required, and it is sometimes difficult to simply make electrode materials with a desired composition. Therefore, it is desirable to be able to safely and simply make a method for an electrode.

[0012] One embodiment of the present invention provides an electrode binder, which is an electrode binder that can be used to make an electrode by a dry method, and can obtain a battery with excellent charge and discharge capacity. Another embodiment of the present invention provides an electrode that can obtain a battery with excellent charge and discharge capacity and a method for manufacturing the electrode. Another embodiment of the present invention provides a lithium ion secondary battery with excellent charge and discharge capacity.

[0013] Means for solving problems

[0014] The method for solving the above-mentioned problems includes the following schemes.

[0015] <1> An electrode binder comprising ultrahigh molecular weight olefin polymer microparticles (A) satisfying the following requirements (i) to (iii):

[0016] (i) an intrinsic viscosity [η] measured in a decalin solvent at 135° C. in the range of 5 to 50 dl / g;

[0017] (ii) the average particle size d50 in the mass-based particle size distribution based on the Coulter counter method is in the range of 1 to 50 μm;

[0018] (iii) 50 mass % or more of the ultrahigh molecular weight olefin polymer fine particles (A) pass through a sieve having an opening of 45 μm.

[0019] <2> The electrode binder according to <1>, wherein the average particle size d50 of the ultrahigh molecular weight olefin polymer fine particles (A) is in the range of 3 to 15 μm.

[0020] <3> The electrode binder according to <1> or <2>, wherein the ultrahigh molecular weight olefin-based polymer fine particles (A) are ethylene-based polymer fine particles.

[0021] <4> An electrode comprising the electrode binder according to any one of <1> to <3> and an active material.

[0022] <5> The electrode according to <4>, which is obtained by a dry method.

[0023] <6> A lithium ion secondary battery comprising the electrode according to <4> or <5> and an electrolyte.

[0024] <7> A method for manufacturing an electrode, comprising:

[0025] A step of dry-mixing the electrode binder and the active material according to any one of <1> to <3> to obtain an electrode composite material; and

[0026] A process for producing an electrode comprising the electrode composite material and a current collector.

[0027] Effects of the Invention

[0028] According to one embodiment of the present invention, an electrode binder is provided, which is an electrode binder that can be used to make electrodes by a dry method, and a battery with excellent charge and discharge capacity can be obtained. According to another embodiment of the present invention, an electrode that can be used to make a battery with excellent charge and discharge capacity and a method for manufacturing the electrode can be provided. According to another embodiment of the present invention, a lithium-ion secondary battery with excellent charge and discharge capacity can be provided. DETAILED DESCRIPTION

[0029] Hereinafter, the contents of the present invention will be described in detail. The contents of the constituent elements described below may be described based on representative embodiments of the present invention, but the present invention is not limited to such embodiments.

[0030] In this specification, the term "polymer" is a concept including homopolymers and copolymers.

[0031] In the present specification, "to" indicating a numerical range is used to mean that the numerical values ​​described before and after it are included as the lower limit and the upper limit.

[0032] In the present specification, unless otherwise specified, "to" indicating a numerical range means that the units described before and after it represent the same unit.

[0033] In this specification, a combination of two or more preferred aspects is a more preferred aspect.

[0034] Electrode Binders

[0035] An electrode binder according to one embodiment of the present invention (hereinafter also referred to as “the present binder”) comprises ultrahigh molecular weight olefin polymer microparticles (A) (hereinafter also referred to as “particles (A)”) satisfying the following requirements (i) to (iii).

[0036] (i) an intrinsic viscosity [η] measured in a decalin solvent at 135° C. in the range of 5 to 50 dl / g;

[0037] (ii) the average particle size d50 in the mass-based particle size distribution based on the Coulter counter method is in the range of 1 to 50 μm;

[0038] (iii) 50 mass % or more of the ultrahigh molecular weight olefin polymer fine particles (A) pass through a sieve having an opening of 45 μm.

[0039] The binder contains particles (A) satisfying the above requirements, so that an electrode can be produced by a dry process, and a battery having excellent charge and discharge capacity can be obtained. Although the reason is not clear, it can be inferred as follows.

[0040] When the electrode is made by a dry method, the electrode forming material (electrode composite material) is sometimes made by pressing. The intrinsic viscosity [η] of the particles (A) contained in this adhesive is in the aforementioned range, so when pressed, even if it becomes a molten state, the particles (A) are not easy to flow out from the electrode, and the particle shape can be maintained. Therefore, it is possible to improve the adhesion with active materials, etc., and inhibit them from falling off the electrode.

[0041] The average particle size d50 of the particles (A) contained in the present adhesive is within the above range, and the amount of coarse particles is small, so that the dispersibility of the active material and the like can be improved while suppressing the generation of electrical defects. Furthermore, it is possible to ensure a space in the electrode that can stably store and release lithium ions. As a result, the conductivity of the (lithium ion secondary) battery can be ensured.

[0042] Since the particles (A) contained in the present binder are olefin-based polymers, the binder has excellent solvent resistance to electrolyte solutions and electrical properties.

[0043] <Ultra-high molecular weight olefin polymer microparticles (A)>

[0044] The particles (A) satisfy the following requirements (i) to (iii).

[0045] In addition, regarding the following physical properties of the particles (A) (including average particle diameter d50, etc.), the particles (A) used as a raw material of the present adhesive have only to have the following physical properties.

[0046] The particles (A) used in the present adhesive may be one type or two or more types.

[0047] Requirement (i): The intrinsic viscosity [η] measured in a decalin solvent at 135°C is within the range of 5 to 50 dl / g.

[0048] If the intrinsic viscosity is in the aforementioned range, it is not easy to flow out from the electrode even if it becomes a molten state, and the particle shape can be maintained. Therefore, the adhesion with active materials etc. can be improved, a battery with excellent charge and discharge capacity can be easily obtained, and electrodes can be made by a dry method, so it is preferred.

[0049] From the above viewpoints, the intrinsic viscosity [η] of the particles (A) is preferably 5 to 40 dl / g, more preferably 5 to 30 dl / g, further preferably 5 to 27 dl / g, particularly preferably 10 to 27 dl / g.

[0050] Requirement (ii): The average particle diameter d50 in the mass-based particle size distribution based on the Coulter counter method is in the range of 1 to 50 μm.

[0051] If average particle diameter d50 is in the aforementioned range, it is possible to improve the dispersibility with active materials etc. so as to suppress falling off from the electrode, and then it is possible to ensure that the space for the absorption and release of lithium ions can be stably carried out in the electrode. As a result, it is possible to easily obtain a battery with excellent charge and discharge capacity, and it is possible to make an electrode by a dry method, so it is preferred.

[0052] From the above viewpoints, the average particle diameter d50 is preferably 35 μm or less, more preferably 20 μm or less, further preferably 15 μm or less, particularly preferably 13 μm or less, and preferably 3 μm or more.

[0053] Furthermore, the upper limit of the average particle size d50 is preferably 15 μm, more preferably 12 μm, further preferably 10 μm, and particularly preferably 8 μm. The lower limit of the average particle size d50 is preferably 1 μm, more preferably 3 μm. The range of the average particle size d50 is preferably 1 to 12 μm, more preferably 1 to 10 μm, further preferably 1 to 8 μm, and particularly preferably 3 to 8 μm.

[0054] If the average particle diameter d50 is in the aforementioned range, more binders can enter between particles of active materials, and even if the amount of binder is a small amount, the cohesiveness with the active materials increases, so even if the amount of binder used is reduced, the desired effect can be exerted. Therefore, the amount of active materials in the electrode can be increased, and as a result, a battery with excellent battery performance can be easily obtained.

[0055] In addition, if the average particle size d50 of the particles (A) is the same as the particle size of the positive electrode active material and the negative electrode active material described later, there is a tendency that the positive electrode active material and the negative electrode active material are not easy to fall off. The average particle size d50 of the above particles (A) refers to the average primary particle size.

[0056] The average particle size d50 is a value obtained by measuring the mass-based particle size distribution using the Coulter counter method, where the cumulative value of the particle size distribution becomes 50% by mass. Specifically, it can be determined by the measurement method described in the Examples.

[0057] Requirement (iii): 50 mass % or more of the particles (A) pass through a sieve having an opening of 45 μm.

[0058] The particles (A) are particles of which 50% or more by mass pass through a sieve (JIS Z 8801) with a mesh size of 45 μm using a vibrating sieve or an ultrasonic vibrating sieve. If the amount of the mesh with a mesh size of 45 μm passes through 50% by mass or more relative to the total mass of the particles (A), a battery with excellent charge and discharge capacity can be easily obtained, and electrodes can be made by a dry method, so it is preferred.

[0059] The aforementioned throughput of 50% by mass or more means that the amount of coarse particles is small. When there are few coarse particles, it is believed that the amount of active materials retained by particles (A) is increased, so it is preferred. In addition, when there are few coarse particles, there is a tendency that electrical defects are not easily generated, and the reduction of the obtained battery capacity can be suppressed. As a result, it is believed that a battery with excellent charge and discharge capacity can be easily obtained, so it is preferred.

[0060] From the above viewpoints, the throughput of the particles (A) is preferably 90% by mass or more, more preferably 95% by mass or more, and even more preferably 99% by mass or more.

[0061] As particles (A), for example, there can be mentioned: homopolymer particles of polyethylene, polypropylene, poly-1-butene, poly-4-methyl-1-pentene, etc.; copolymer particles using at least two α-olefins selected from ethylene, propylene, 1-butene, 1-hexene, 1-octene, 4-methyl-1-pentene, etc. as raw materials.

[0062] The particles (A) are preferably ethylene-based polymer microparticles (eg, ethylene homopolymer microparticles, ethylene and one or more α-olefin copolymer microparticles), and are particularly preferably ethylene homopolymer microparticles.

[0063] The fusing point of ethylene polymer is lower than for example polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVDF) etc., therefore when making electrode, even if not set to high temperature, also can keep the binding force with active material etc. In addition, the surface free energy of ethylene polymer is higher than PTFE and PVDF etc., therefore with the affinity of active material etc. high, also uprises with the binding force of active material etc. From the above viewpoint, be preferably ethylene polymer microparticle.

[0064] The content of the constituent units derived from ethylene in the copolymer microparticles of ethylene and one or more α-olefins is preferably 50 mol% or more, more preferably 80 mol% or more, and even more preferably 90 mol% or more, based on 100 mol% of the total of all constituent units constituting the copolymer.

[0065] The melt flow rate (MFR) of the particles (A) is preferably less than 1.0 g / 10 min, more preferably 0.5 g / 10 min or less, and more preferably 0.01 g / 10 min or more.

[0066] The MFR is measured under the conditions of 190° C. and a test load of 21.6 kg in accordance with JIS K 7210-1 (2014).

[0067] The method for producing the particles (A) is not particularly limited as long as the particles (A) satisfy the above requirements (i) to (iii), and the particles (A) can be produced, for example, by the methods disclosed in the following documents.

[0068] (1) International Publication No. 2006 / 054696

[0069] (2) International Publication No. 2008 / 013144

[0070] (3) International Publication No. 2009 / 011231

[0071] (4) International Publication No. 2010 / 074073

[0072] (5) Japanese Patent Application Publication No. 2012-131959

[0073] As the raw material of the particles (A) (for example, monomers such as ethylene and α-olefin), only raw materials derived from biomass, only raw materials derived from fossil fuels, or both raw materials derived from biomass and raw materials derived from fossil fuels may be used.

[0074] Biomass-derived raw materials refer to raw materials derived from plants including fungi, yeast, algae, and bacteria, or from animals, etc., and are made from all (renewable) natural raw materials and their residues. For example, 1×10 -12 The ratio of about 14 A raw material whose C isotope is carbon and whose biomass carbon concentration (unit: pMC) measured according to ASTM D6866 is about 100 pMC. A raw material derived from biomass (for example, monomers such as ethylene and α-olefin) can be obtained by, for example, a conventionally known method.

[0075] From the viewpoint of reducing environmental load (mainly from the perspective of reducing greenhouse gases), the particles (A) preferably include structural units derived from a biomass-derived raw material.

[0076] Regarding the particles (A), if the production conditions of the particles (A) such as the polymerization catalyst, polymerization process, and polymerization temperature are the same, even if the (co)polymer is made of a biomass-derived raw material, except for the 1×10 -12 ~10 -14 The ratio of about 14 Except for the C isotope, the molecular structure is the same as that of the (co)polymer containing the raw material derived from fossil fuels. Therefore, it is believed that there is no difference in performance between the (co)polymer containing the raw material derived from biomass and the (co)polymer containing the raw material derived from fossil fuels.

[0077] From the viewpoint of being able to easily obtain a battery with excellent charge and discharge capacity and being easy to make electrodes by a dry method, the content of the particles (A) in the present binder is preferably 80% by mass or more, more preferably 90% by mass or more, further preferably 95% by mass or more, and particularly preferably 97% by mass or more. The upper limit of the content is preferably 100% by mass.

[0078] <Other ingredients>

[0079] The present adhesive may further contain other components in addition to the particles (A).

[0080] The other components are not particularly limited and may be conventionally known components, for example, olefin polymer particles other than the particles (A), polyvinyl acetate, polymethyl methacrylate, carboxymethyl cellulose (CMC), nitrocellulose, fluororesin, and rubber particles.

[0081] Examples of the fluororesin include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), and vinylidene fluoride-hexafluoropropylene copolymer.

[0082] Examples of the rubber particles include styrene-butadiene rubber (SBR) particles and acrylonitrile rubber particles.

[0083] The above-mentioned other components may be used alone or in combination of two or more.

[0084] The content of the other components in the present adhesive is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less.

[0085] The content of the olefin polymer particles other than the particles (A) in the present adhesive is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 1% by mass or less.

[0086] It is particularly preferred that the present adhesive contain no other components (it is particularly preferred that the content of the other components in the present adhesive is 0% by mass).

[0087] As the raw materials of the above-mentioned other components, only raw materials derived from biomass may be used, only raw materials derived from fossil fuels may be used, or both raw materials derived from biomass and raw materials derived from fossil fuels may be used.

[0088] From the viewpoint of reducing environmental load (mainly from the perspective of reducing greenhouse gases), the other components preferably include a structural unit derived from a biomass-derived raw material.

[0089] "electrode"

[0090] The electrode according to one embodiment of the present invention preferably includes the present binder and an active material.

[0091] Since the electrode contains the present binder, it can be produced by a dry method, and a battery excellent in charge and discharge capacity can be easily obtained.

[0092] The electrode is preferably obtained by a dry method. It should be noted that the method for producing the electrode will be described later.

[0093] The aforementioned electrode may be a positive electrode or a negative electrode.

[0094] <Positive electrode>

[0095] The positive electrode is preferably an electrode capable of absorbing and releasing lithium ions, and the positive electrode preferably comprises the present binder, a conductive aid, and a positive electrode active material, and more preferably comprises a positive electrode mixture layer containing the present binder, a conductive aid, and a positive electrode active material, and a positive electrode collector. In this case, the positive electrode mixture layer is provided on at least a portion of the surface of the positive electrode collector.

[0096] From the viewpoint of achieving both physical properties of the positive electrode mixture layer (e.g., electrolyte permeability, peel strength) and battery performance, the content of the binder in the positive electrode mixture layer is preferably 0.1 to 10 mass %, more preferably 0.1 to 4 mass %, relative to the total mass of the positive electrode mixture layer.

[0097] If the content of this adhesive is 0.1% by mass or more, the adhesion of the positive electrode mixture layer to the positive electrode current collector and the bonding of the positive electrode active material to each other are further improved. If the content of this adhesive is below the aforementioned upper limit, the amount of the positive electrode active material in the positive electrode mixture layer can be made more, so by using this positive electrode mixture layer, a battery with a large capacity can be easily obtained.

[0098] The thickness of the positive electrode mixture layer is not particularly limited and may be the same as that of a conventionally known positive electrode mixture layer, but is preferably 30 to 500 μm, more preferably 30 to 300 μm, and even more preferably 30 to 150 μm.

[0099] [Positive electrode active material]

[0100] The positive electrode active material is preferably a material capable of absorbing and releasing lithium ions, and examples thereof include positive electrode active materials generally used in lithium ion secondary batteries.

[0101] The positive electrode active material may be used alone or in combination of two or more.

[0102] Examples of the positive electrode active material include:

[0103] Oxides with lithium (Li) and nickel (Ni) as constituent metal elements;

[0104] An oxide containing at least one of Li, Ni, and metal elements other than Li and Ni (eg, transition metal elements, typical metal elements) as a constituent metal element.

[0105] When the metal element other than Li and Ni is contained, the metal element is preferably contained in a ratio equal to or less than Ni in terms of the number of atoms.

[0106] The aforementioned metal elements other than Li and Ni may include, for example, at least one selected from the group consisting of Co, Mn, Al, Cr, Fe, V, Mg, Ca, Na, Ti, Zr, Nb, Mo, W, Cu, Zn, Ga, In, Sn, La and Ce.

[0107] The positive electrode active material preferably includes a lithium-containing composite oxide (hereinafter also referred to as "NCM") represented by the following formula (C1). When NCM is used as the positive electrode active material, an electrode having high energy density per unit volume and excellent thermal stability can be easily produced.

[0108] LiNi a Co b Mn c O2···Formula (C1)

[0109] [In formula (C1), a, b and c are each independently greater than 0 and less than 1, and the total of a, b and c is 0.99 to 1.00.]

[0110] As a specific example of NCM, LiNi 0.33 Co 0.33 Mn 0.33 O2、LiNi 0.5 Co 0.3 Mn 0.2 O2、LiNi 0.5 Co 0.2 Mn 0.3 O2、LiNi 0.6 Co 0.2 Mn 0.2 O2、LiNi 0.8 Co 0.1 Mn 0.1 O2.

[0111] The positive electrode active material may include a lithium-containing composite oxide (hereinafter also referred to as “NCA”) represented by the following formula (C2).

[0112] Li t Ni (1-x-y) Co x Aly O2···Formula (C2)

[0113] [In formula (C2), t is 0.95 to 1.15, x is 0 to 0.3, y is 0.01 to 0.2, and the sum of x and y is less than 0.5.]

[0114] As a specific example of NCA, LiNi 0.8 Co 0.15 Al 0.05 O2.

[0115] The content of the positive electrode active material in the positive electrode mixture layer is, for example, 10 to 99.9 mass %, preferably 30 to 99.0 mass %, more preferably 50 to 99.0 mass %, particularly preferably 70 to 99.0 mass % based on the total mass of the positive electrode mixture layer.

[0116] 〔Conductive additive〕

[0117] The conductive auxiliary agent is not particularly limited as long as it is a material other than the above-mentioned active material, and a known conductive auxiliary agent can be used.

[0118] As the known conductive additive, a carbon material having conductivity is preferred, and examples thereof include graphite, carbon black, conductive carbon fibers (eg, carbon nanotubes, carbon nanofibers, carbon fibers), and fullerene.

[0119] The conductive auxiliary agent may be used alone or in combination of two or more.

[0120] As the carbon black, a commercially available product can be used.

[0121] Examples of commercially available carbon black include TOKA BLACK #4300, #4400, #4500, and #5500 (manufactured by Tokai Carbon Co., Ltd., furnace black), Printex L (manufactured by Degussa, furnace black), Raven 7000, 5750, 5250, 5000 ULTRA III, 5000 ULTRA, Conductex SC ULTRA, Conductex 975 ULTRA, Puer BLACK 100, 115, and 205 (manufactured by Columbian Co., Ltd., furnace black), #2350, #2400B, #2600B, #30050B, #3030B, #3230B, #3350B, #3400B, and #5400B (manufactured by Mitsubishi Chemical Co., Ltd., furnace black), MONARCH 1400, 1300, 900, Vulcan XC-72R, Black Pearls 2000, LITX-50, LITX-200 (manufactured by Cabot Corporation, furnace black), Ensaco250G, Ensaco260G, Ensaco350G, Super-P (manufactured by TIMCAL), KETJEN BLACK EC-300J, EC-600JD (manufactured by Akzo Nobel), DENKA BLACK, DENKA BLACK HS-100, FX-35 (manufactured by DENKA Co., Ltd., acetylene black).

[0122] Examples of graphite include artificial graphite and natural graphite (eg, flake graphite, block graphite, and earthy graphite).

[0123] In order to further exert the effect of the conductive additive, the content of the conductive additive in the positive electrode mixture layer is, for example, 1 to 10 mass %, preferably 1 to 5 mass %, based on the total mass of the positive electrode mixture layer.

[0124] 〔Positive electrode collector〕

[0125] The positive electrode current collector is not particularly limited, and a known positive electrode current collector can be used.

[0126] Examples of the material of the positive electrode current collector include metal materials such as aluminum, aluminum alloys, stainless steel, nickel, titanium, and tantalum; and carbon materials such as carbon cloth and carbon paper.

[0127] As the material of the positive electrode current collector, aluminum is preferred among the above materials in terms of the balance between high conductivity and cost, etc. Here, "aluminum" means pure aluminum or an aluminum alloy.

[0128] The positive electrode current collector is preferably an aluminum foil. The material of the aluminum foil is not particularly limited, and examples thereof include A1085 material and A3003 material.

[0129] 〔additive〕

[0130] The positive electrode (or the positive electrode mixture layer when the positive electrode current collector and the positive electrode mixture layer are included) may further contain additives other than the present binder, the conductive auxiliary agent, and the positive electrode active material.

[0131] Examples of the additive include a thickener, a surfactant, a dispersant, a wetting agent, a defoaming agent, and a friction reducing agent.

[0132] The above-mentioned additives may be used alone or in combination of two or more.

[0133] <Negative electrode>

[0134] The negative electrode is preferably an electrode capable of absorbing and releasing lithium ions, and the negative electrode preferably comprises the present binder and a negative electrode active material, and more preferably comprises a negative electrode current collector and a negative electrode mixture layer comprising the present binder and the negative electrode active material. In this case, the negative electrode mixture layer is provided on at least a portion of the surface of the negative electrode current collector.

[0135] From the viewpoint of achieving both physical properties of the negative electrode mixture layer (e.g., electrolyte permeability, peel strength) and battery performance, the content of the present binder in the negative electrode mixture layer is preferably 0.1 to 10 mass %, more preferably 0.1 to 4 mass %, relative to the total mass of the negative electrode mixture layer.

[0136] If the content of this adhesive is 0.1% by mass or more, the adhesiveness of the negative electrode mixture layer to the negative electrode current collector and the bonding properties of the negative electrode active materials are further improved. If the content of this adhesive is below the above upper limit, the amount of the negative electrode active material in the negative electrode mixture layer can be made more, so by using this negative electrode mixture layer, a battery with a large capacity can be easily obtained.

[0137] The thickness of the negative electrode mixture layer is not particularly limited and may be the same as the thickness of a conventionally known negative electrode mixture layer, and is preferably 30 to 500 μm, more preferably 30 to 300 μm, and even more preferably 30 to 150 μm.

[0138] [Negative electrode active material]

[0139] As the negative electrode active material, it is preferably a substance that can absorb and release lithium ions. For example, at least one selected from the group consisting of the following substances can be cited: metallic lithium, lithium-containing alloys, metals or alloys that can be alloyed with lithium, oxides that can be doped and dedoped with lithium ions, transition metal nitrides that can be doped and dedoped with lithium ions, and carbon materials that can be doped and dedoped with lithium ions.

[0140] Among them, carbon materials that can be doped and dedoped with lithium ions are preferred.

[0141] The negative electrode active material may be used alone or in combination of two or more.

[0142] Examples of the carbon material include carbon black, activated carbon, graphite materials (eg, artificial graphite, natural graphite), and amorphous carbon materials.

[0143] The carbon material may be in any shape such as fiber, spherical, potato, or chip.

[0144] The size of the carbon material is not particularly limited, but is preferably 5 to 50 μm, more preferably 20 to 30 μm.

[0145] Examples of the amorphous carbon material include hard carbon, coke, mesocarbon microbeads (MCMB) sintered at 1500° C. or lower, and mesophase pitch carbon fibers (MCF).

[0146] Examples of the graphite material include natural graphite and artificial graphite, and examples of the artificial graphite include graphitized MCMB and graphitized MCF.

[0147] In addition, the graphite material may contain boron. In addition, the graphite material may be a material coated with a metal such as gold, platinum, silver, copper, tin, or amorphous carbon, or may be a mixture of amorphous carbon and graphite.

[0148] 〔Conductive additive〕

[0149] The negative electrode (negative electrode mixture layer when including a negative electrode current collector and a negative electrode mixture layer) may further contain a conductive auxiliary agent in addition to the present binder and the negative electrode active material.

[0150] The conductive aid is not particularly limited as long as it is a material other than the above-mentioned active material, and a known conductive aid can be used. Specific examples of the conductive aid are the same as those of the conductive aid contained in the above-mentioned positive electrode, and preferred examples are also the same.

[0151] In order to better exert the effect of the conductive additive, the content of the conductive additive in the negative electrode mixture layer is, for example, 0 to 10 mass %, more preferably 0 to 5 mass %, and even more preferably 0 to 3 mass % based on the total mass of the negative electrode mixture layer.

[0152] 〔Negative electrode collector〕

[0153] The negative electrode current collector is not particularly limited, and a known negative electrode current collector can be used.

[0154] Examples of the material of the negative electrode current collector include metal materials such as copper, nickel, stainless steel, and nickel-plated steel.

[0155] As the material of the negative electrode current collector, copper is preferred among the above materials in terms of processability and the like, and as the negative electrode current collector, copper foil is preferred.

[0156] 〔additive〕

[0157] The negative electrode (negative electrode mixture layer when including a negative electrode current collector and a negative electrode mixture layer) may further contain additives other than the present binder, the conductive aid, and the negative electrode active material.

[0158] Examples of the additive include a thickener, a surfactant, a dispersant, a wetting agent, a defoaming agent, and a friction reducing agent.

[0159] The above-mentioned additives may be used alone or in combination of two or more.

[0160] 《Electrode manufacturing method》

[0161] From the viewpoint of improving the charge and discharge capacity of the obtained battery, at least one of the positive electrode and the negative electrode is preferably an electrode obtained by a dry process, preferably an electrode produced by a method for producing an electrode including the following steps 1 and 2.

[0162] As the electrode obtained by the dry method, specifically, an electrode obtained by a method for producing an electrode including the following steps 1 and 2 is preferable.

[0163] Step 1: dry-mixing the present binder and the aforementioned active material to obtain an electrode composite material,

[0164] Step 2: Producing an electrode including the electrode composite material and a current collector.

[0165] <Process 1>

[0166] Step 1 is a step of dry-mixing the present binder and the above-mentioned active material without using a solvent.

[0167] In step 1, the above-mentioned conductive auxiliary agent and / or additive may be further used.

[0168] In step 1, the raw material components are preferably dry-mixed in such an amount that the content of each component in the obtained electrode composite material is in the same range as the content of each component in the electrode mixture layer.

[0169] It should be noted that when the aforementioned conductive aid and / or additive is used, there is no particular restriction on the order of mixing the present adhesive, the aforementioned active material, and the aforementioned conductive aid and / or additive. The present adhesive and the active material may be mixed and then the conductive aid and / or additive may be further mixed. Alternatively, the present adhesive, the aforementioned active material, and the aforementioned conductive aid and / or additive may be added and mixed at the same time.

[0170] The method for the dry mixing is not particularly limited, and various known methods can be cited, for example, a method of mixing using a defoaming kneader, a dry ball mill, a dry bead mill, a blade planetary motion mixer, a container rotation planetary motion mixer, a crusher, a mortar, a homogenizer, a low-frequency resonance sound mixer, a jet mill, a tumble mixer, a grinder, a Henschel mixer, etc.

[0171] In addition, during dry mixing, heat treatment may be performed, for example, to soften the binder. The heat treatment is preferably performed at a temperature below which the active material and the like do not decompose.

[0172] <Process 2>

[0173] Process 2 is a process for manufacturing an electrode comprising the aforementioned electrode composite material and a current collector. As specific examples, there can be cited: a process for manufacturing an electrode by applying pressure to the aforementioned electrode composite material to form it, and bonding the obtained aforementioned electrode composite material to the current collector; or a process for manufacturing an electrode by applying pressure to the aforementioned electrode composite material and the current collector at the same time to form them, and bonding the aforementioned electrode composite material to the current collector.

[0174] A preferred example of a method for molding the electrode composite material by applying pressure is press molding.

[0175] As the aforementioned bonding method, a method of pressing the electrode composite material onto the current collector is preferred.

[0176] After the electrode composite material is formed or pressed onto a current collector, it may be further heated and dried.

[0177] As the pressing method for pressing the electrode composite material onto the current collector in the above-mentioned press molding, various known pressing methods such as a roll pressing method and a flat plate pressing method can be appropriately adopted.

[0178] The pressure during the pressing is preferably 0.1 to 100 tons, more preferably 1 to 50 tons. The pressing time is not particularly limited, but is, for example, 0.5 seconds to 1 hour.

[0179] The pressed density of the electrode when the electrode composite material is compressed at a pressure within the above range is preferably 1.0 to 4.0 g / cm 3 .

[0180] The pressing density of the positive electrode is more preferably 2.5 to 4.0 g / cm 3 .

[0181] The compaction density of the negative electrode is more preferably 1.0 to 2.0 g / cm 3 , more preferably 1.3 to 1.8 g / cm 3 .

[0182] The temperature during the pressing is preferably 20 to 300°C, more preferably 80 to 200°C, and even more preferably 100 to 200°C.

[0183] By molding the electrode composite material and bonding the electrode composite material and the current collector within this temperature range, the binder is appropriately softened, and bonding between the binder and the active material and bonding between the electrode composite material and the current collector can be effectively performed.

[0184] Examples of the heating drying method include drying with warm air, hot air, or low-humidity air; vacuum drying; and drying with infrared (eg, far-infrared) irradiation.

[0185] The drying time and drying temperature are not particularly limited, and the drying time is, for example, 1 minute to 24 hours, and the drying temperature is, for example, 80° C. to 180° C. The heating drying can be performed as needed, but is preferably omitted from the perspectives of simplification of electrode production, economy, safety, and environmental load.

[0186] In order to improve the adhesion with the electrode composite material, the current collector used may be subjected to surface processing such as roughening treatment or formation of a conductive adhesive layer in advance.

[0187] The method for producing an electrode may further include other steps in addition to the above-mentioned step 1 and step 2. As the other step, for example, there is a step of preparing the present binder.

[0188] 《Lithium-ion secondary battery》

[0189] The lithium ion secondary battery according to one embodiment of the present invention preferably includes the aforementioned electrode and an electrolyte. The lithium ion secondary battery may include a separator between the negative electrode and the positive electrode, or may include a case that accommodates the aforementioned electrode and the electrolyte.

[0190] Since the lithium ion secondary battery includes an electrode having the present binder, the battery has excellent charge and discharge capacity.

[0191] <Electrode>

[0192] From the perspective of being able to easily obtain a battery with excellent battery characteristics, at least one of the positive and negative electrodes of the lithium ion secondary battery is preferably an electrode obtained by a dry method, particularly an electrode manufactured by the method described in the manufacturing method column of the aforementioned electrode. One of the positive and negative electrodes of the aforementioned lithium ion secondary battery can be an electrode manufactured by a wet method, etc.

[0193] <Electrolytes>

[0194] The lithium ion secondary battery preferably includes an electrolyte. The electrolyte is not particularly limited as long as it can be a conductor of alkali metal cations such as lithium ions. In addition, the properties of the electrolyte are not particularly limited, for example, it can be a liquid dissolved in a non-aqueous solvent described later, it can also be a gel, and it can also be a solid.

[0195] The electrolyte may be used alone or in combination of two or more.

[0196] The electrolyte preferably contains at least one lithium salt containing fluorine (hereinafter also referred to as “fluorine-containing lithium salt”).

[0197] As fluorine-containing lithium salts, for example, there can be mentioned: inorganic acid anion salts such as lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), and lithium hexafluorotantalate (LiTaF6); organic acid anion salts such as lithium trifluoromethanesulfonate (LiCF3SO3), lithium bis(trifluoromethanesulfonyl)imide (Li(CF3SO2)2N), and lithium bis(pentafluoroethanesulfonyl)imide (Li(C2F5SO2)2N). Among them, as a fluorine-containing lithium salt, LiPF6 is particularly preferred.

[0198] Lithium ion secondary batteries may contain an electrolyte that is a fluorine-free lithium salt. Examples of fluorine-free lithium salts include lithium perchlorate (LiClO4), lithium tetrachloroaluminate (LiAlCl4), lithium decachlorodecaborate (Li2B 10 Cl 10 )wait.

[0199] 〔Electrolyte〕

[0200] The lithium ion secondary battery may include an electrolyte solution in which one or more of the above-mentioned electrolytes are dissolved in one or more solvents.

[0201] As the electrolytic solution, a non-aqueous electrolytic solution containing one or more of the above-mentioned electrolytes and one or more of the non-aqueous solvents is more preferable.

[0202] Furthermore, the electrolytic solution may contain conventionally known additives other than the electrolyte and the electrolytic solution for improving battery performance or the like.

[0203] The proportion of the fluorine-containing lithium salt is preferably 50 to 100 mass %, more preferably 60 to 100 mass %, and even more preferably 80 to 100 mass % relative to 100 mass % of the electrolyte in the electrolytic solution.

[0204] In addition, the ratio of LiPF6 to 100 mass % of the electrolyte in the electrolytic solution is preferably 50 to 100 mass %, more preferably 60 to 100 mass %, and further preferably 80 to 100 mass %.

[0205] The concentration of the electrolyte in the electrolytic solution is preferably 0.1 to 3 mol / L, more preferably 0.5 to 2 mol / L.

[0206] In addition, the concentration of LiPF6 in the electrolyte is preferably 0.1 to 3 mol / L, more preferably 0.5 to 2 mol / L.

[0207] The electrolyte preferably contains at least one non-aqueous solvent.

[0208] Examples of the nonaqueous solvent include cyclic carbonates, fluorinated cyclic carbonates, chain carbonates, fluorinated chain carbonates, aliphatic carboxylates, fluorinated aliphatic carboxylates, γ-lactones, fluorinated γ-lactones, cyclic ethers, fluorinated cyclic ethers, chain ethers, fluorinated chain ethers, nitriles, amides, lactams, nitromethane, nitroethane, sulfolane, trimethyl phosphate, dimethyl sulfoxide, and dimethyl sulfoxide phosphoric acid.

[0209] Examples of the cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC).

[0210] Examples of the fluorine-containing cyclic carbonates include fluoroethylene carbonate (FEC).

[0211] Examples of the chain carbonates include dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), and dipropyl carbonate (DPC).

[0212] Examples of the fluorine-containing chain carbonates include 2,2,2-trifluoroethyl methyl carbonate.

[0213] Examples of the aliphatic carboxylic acid esters include methyl formate, methyl acetate, methyl propionate, methyl butyrate, methyl isobutyrate, methyl trimethylbutyrate, ethyl formate, ethyl acetate, ethyl propionate, ethyl butyrate, ethyl isobutyrate, and ethyl trimethylbutyrate.

[0214] Examples of the γ-lactones include γ-butyrolactone and γ-valerolactone.

[0215] Examples of the cyclic ethers include tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, 1,3-dihydrofuran, Alkane, 1,4-di alkyl.

[0216] Examples of the chain ethers include 1,2-ethoxyethane (DEE), ethoxymethoxyethane (EME), diethyl ether, 1,2-dimethoxyethane, and 1,2-dibutoxyethane.

[0217] Examples of the nitriles include acetonitrile, glutaronitrile, adiponitrile, methoxyacetonitrile, and 3-methoxypropionitrile.

[0218] As the amides, for example, N,N-dimethylformamide can be mentioned.

[0219] Examples of lactams include N-methylpyrrolidone, N-methyl Oxazolidinone, N,N'-dimethylimidazolidinone.

[0220] The nonaqueous solvent preferably contains at least one selected from the group consisting of cyclic carbonates, fluorine-containing cyclic carbonates, chain carbonates, and fluorine-containing chain carbonates.

[0221] In this case, the total proportion of cyclic carbonates, fluorinated cyclic carbonates, chain carbonates and fluorinated chain carbonates in the nonaqueous solvent is preferably 50 to 100% by mass, more preferably 60 to 100% by mass, and further preferably 80 to 100% by mass.

[0222] In addition, the nonaqueous solvent preferably contains at least one selected from the group consisting of cyclic carbonates and chain carbonates.

[0223] In this case, the total proportion of the cyclic carbonates and the chain carbonates in the non-aqueous solvent is preferably 50 to 100% by mass, more preferably 60 to 100% by mass, and even more preferably 80 to 100% by mass.

[0224] The proportion of the nonaqueous solvent in the nonaqueous electrolyte is preferably 60% by mass or more, more preferably 70% by mass or more.

[0225] The upper limit of the proportion of the nonaqueous solvent in the nonaqueous electrolyte solution also depends on the contents of other components, and is, for example, 99% by mass, preferably 97% by mass, and more preferably 90% by mass.

[0226] From the viewpoint of further improving the dissociation property of the electrolyte and the mobility of ions, the intrinsic viscosity of the nonaqueous solvent is preferably 10.0 mPa·s or less at 25°C.

[0227] <Diaphragm>

[0228] The separator is not particularly limited as long as it can electrically insulate the positive electrode from the negative electrode and allow lithium ions to pass therethrough.

[0229] Examples of the material of the separator include resins such as polyethylene (PE), polypropylene (PP), polyester, cellulose, and polyamide. Examples of the separator include porous flat plates containing the resins and nonwoven fabrics containing the resins.

[0230] Among them, the separator is preferably a porous resin film having a single-layer or multi-layer structure mainly composed of one or more polyolefin resins.

[0231] The thickness of the separator is, for example, 5 to 30 μm.

[0232] <Housing>

[0233] The case is not particularly limited, and a known case for lithium ion secondary batteries may be mentioned. Specific examples thereof include a case including a laminate film and a case including a battery can and a battery can lid.

[0234] <Method for producing lithium-ion secondary battery>

[0235] As a method for manufacturing a lithium-ion secondary battery, a well-known method for manufacturing a lithium-ion secondary battery can be cited. For example, a manufacturing method comprising the following steps: a precursor manufacturing step of housing a positive electrode, a negative electrode, an electrolyte (or an electrolyte solution) and, if necessary, a separator in a shell to manufacture a lithium-ion secondary battery precursor; and an aging step of aging the lithium-ion secondary battery precursor to obtain a lithium-ion secondary battery.

[0236] The case, positive electrode, negative electrode, electrolyte, separator and electrolytic solution in the method for producing a lithium ion secondary battery have the same meanings as those in the lithium ion secondary battery described above, and preferred embodiments are also the same.

[0237] The precursor preparation step preferably includes: accommodating the positive electrode and the negative electrode (via a separator as needed) in a case; and injecting an electrolyte (or electrolytic solution) into the case accommodating the positive electrode and the negative electrode (via a separator as needed).

[0238] The aging step is preferably performed by subjecting the lithium ion secondary battery precursor to a combination of charge and discharge at least once in an environment of 25 to 70°C.

[0239] By including such an aging step, there is a tendency for the internal resistance (particularly the positive electrode resistance) of the lithium ion secondary battery to be reduced.

[0240] Example

[0241] Hereinafter, one embodiment of the present invention will be described in more detail based on examples, but the present invention is not limited to these examples.

[0242] The measuring methods of various physical properties are as follows.

[0243] <Intrinsic viscosity [η]>

[0244] The intrinsic viscosity [η] of the particles is measured at 135°C by dissolving the particles in decalin.

[0245] <Average particle size d50>

[0246] The average particle size d50 is obtained by measuring the mass-based particle size distribution using the Coulter counter method using a precision particle size distribution analyzer (manufactured by Beckman Coulter, product name: Multisizer 3). The particle size at which the mass accumulation in the mass-based particle size distribution reaches 50% is taken as the average particle size d50.

[0247] <Passage rate of sieve with mesh size of 45μm>

[0248] The pass rate of a sieve with a mesh size of 45 μm (the ratio of particles passing through a sieve with a mesh size of 45 μm) is obtained by measuring the mass of particles passing through a sieve with a mesh size of 45 μm (JIS Z8801-1 (2019)).

[0249] <Electrode Binder 1 (used in Examples 1, 4, and 6)>

[0250] As an electrode binder, ultra-high molecular weight ethylene polymer microparticles (manufactured by Mitsui Chemicals, Inc., MIPELON (registered trademark) PM-200, intrinsic viscosity [η] = 13.0 dl / g, MFR (190°C, 21.6 kg load) = 0.020 g / 10 min, average particle size d50 = 10.5 μm, pass rate through a sieve with a mesh size of 45 μm = 100 mass %) were used.

[0251] <Electrode Binder 2 (used in Examples 2 and 5)>

[0252] As an electrode binder, ultra-high molecular weight ethylene polymer microparticles (manufactured by Mitsui Chemicals, Inc., MIPELON (registered trademark) XM-220, intrinsic viscosity [η] = 14.5 dl / g, MFR (190°C, 21.6 kg load) = 0.015 g / 10 min, average particle size d50 = 32 μm, pass rate through a sieve with a mesh size of 45 μm = 90 mass %) were used.

[0253] <Electrode Binder 3 (used in Example 3)>

[0254] As the electrode binder used in Example 3, ultrahigh molecular weight ethylene polymer microparticles were prepared by the following method.

[0255] (i) Preparation of magnesium-containing carrier component (α-1)

[0256] Decane was added to 95.2 g (1.0 mol) of anhydrous magnesium chloride and 390.6 g (3.0 mol) of 2-ethylhexanol to make the total volume 1000 mL, and the mixture was reacted at 130° C. for 2 hours to obtain a uniform solution.

[0257] Next, in a flask with a volume of 1000 mL fully substituted with nitrogen, 100 mL of the above-mentioned uniform solution (100 mmol in terms of the number of magnesium atoms), 50 mL of refined decane and 560 mL of chlorobenzene were placed, and ClearMix CLM-0.8S manufactured by M Technique (Strain) was used. Under stirring at a speed of 15,000 rpm, while the liquid temperature was maintained at 0°C, 110 mmol of triethylaluminum diluted with refined decane was added dropwise over 30 minutes. Then, the liquid temperature was raised to 80°C over 4 hours and reacted for 1 hour. Then, while maintaining 80°C, 202 mmol of triethylaluminum diluted with refined decane was added dropwise again over 30 minutes, and then the reaction was further heated for 1 hour. After the reaction was completed, the solid portion was collected by filtration, fully washed with toluene, and 100 mL of toluene was added to prepare a toluene slurry containing the magnesium carrier component (α-1).

[0258] (ii) Preparation of solid catalyst component (β-1)

[0259] In a 1000-mL flask that has been fully purged with nitrogen, a toluene slurry of the aforementioned magnesium-containing carrier component (α-1) (20 mmol in terms of the number of magnesium atoms) and 600 mL of purified toluene are placed. While stirring and maintaining at room temperature, 38.9 mL of a toluene solution (0.0001 mmol / mL) of a transition metal compound represented by the following formula (I) is added dropwise over 20 minutes.

[0260] After stirring for 1 hour, the solid portion was collected by filtration, and washed thoroughly with toluene. Purified decane was added to prepare 200 mL of decane slurry of the solid catalyst component (β-1).

[0261] [Chemistry 1]

[0262]

[0263] (iii) Preparation of ultra-high molecular weight ethylene polymer microparticles

[0264] In a 1L SUS autoclave fully purged with nitrogen, 500mL of purified heptane was placed, and ethylene was allowed to flow at 100L / hr for 15 minutes at room temperature to saturate the liquid phase and gas phase. Next, after the temperature was raised to 65°C, 1.25mL of a decane solution of triethylaluminum (1.0mmol / mL in terms of aluminum atom) and 200mL of a decane slurry of the solid catalyst component (β-1) in terms of 0.00008mmol in terms of zirconium atom were added while ethylene was flowing at 12L / hr. The mixture was stirred for 3 minutes while maintaining the temperature. 40mg of EMULGEN 108 (manufactured by Kao Corporation) was added and the ethylene pressure was immediately increased. The ethylene pressure was raised to 0.8MPa·G over 10 minutes, and polymerization was carried out at 70°C for 2 hours while ethylene was supplied to maintain the pressure. Then, the autoclave was cooled and the ethylene pressure was released. The obtained polymer slurry was filtered, washed with hexane, and dried under reduced pressure at 80° C. for 10 hours to obtain 40.9 g of ultrahigh molecular weight ethylene-based polymer microparticles.

[0265] The obtained ultrahigh molecular weight ethylene polymer microparticles had an intrinsic viscosity [η] of 23.0 dl / g, an average particle size d50 of 10.7 μm, and a pass rate through a sieve with a mesh size of 45 μm of 99% by mass.

[0266] <Electrode Binder 4 (used in Comparative Example 1)>

[0267] A high-density polyethylene (HDPE) having an intrinsic viscosity [η] of 1.3 dl / g, an average particle size d50 of 25 μm, and a passing rate through a sieve with a mesh size of 45 μm of 92% by mass was used.

[0268] <Electrode Binder 5 (used in Comparative Example 2)>

[0269] Ultra-high molecular weight polyethylene (PE) having an intrinsic viscosity [η] of 14.0 dl / g and an average particle size d50 of 110 μm was used.

[0270] <Electrode production by dry mixing>

[0271] - Positive Electrode Preparation (Examples 1 to 3 and Comparative Examples 1 to 2) -

[0272] NCM523 (manufactured by Umicore, with a composition formula of LiNi) as the positive electrode active material was kneaded using a debubbling kneader (Non-bubbling Kneader NBK-1, manufactured by Nippon Seiki Seisakusho Co., Ltd.) 0.5 Co 0.2 Mn 0.3O2) 920 g, Super-P as a conductive additive (manufactured by TIMCAL, conductive carbon black, BET specific surface area: 62 m 2 / g) 20 g and KS-6 (produced by TIMREX, flaky graphite) 20 g, and 12 g of any one of the electrode binders 1 to 3 or the electrode binders 4 to 5 were dry-mixed at a rotation speed of 95 rpm to prepare a positive electrode composite material (electrode composite material).

[0273] The positive electrode composite material obtained above was evenly spread on both sides of the main surface of the aluminum foil (thickness 20 μm, width 80 mm) as the collector, and the gap between the upper and lower rollers was adjusted. A 1-ton roller press was used to obtain a single-sided pressing density of the positive electrode of 3.1 ± 0.1 g / cm 3 Then, the mixture was dried and baked in a vacuum drying oven at 150° C. for 1 hour.

[0274] The dried double-sided coated aluminum foil obtained above was cut into electrodes so as to obtain a coated portion (front side: 56 mm×334 mm, back side: 56 mm×408 mm) and a tab welding margin to obtain a positive electrode.

[0275] - Negative Electrode Preparation (Examples 4 and 5) -

[0276] Using a debubbling kneader (Non-bubbling Kneader NBK-1 manufactured by Nippon Seiki Manufacturing Co., Ltd.), 960 g of natural graphite as a negative electrode active material, 10 g of Super-P (conductive carbon black) as a conductive aid, and 22.5 g of either electrode binder 1 or 2 were dry mixed at a rotation speed of 95 rpm to produce a negative electrode composite material.

[0277] The negative electrode composite material obtained above was evenly spread on both sides of the main surface of the copper foil as the collector, and the gap between the upper and lower rollers was adjusted. A 1-ton roller press was used to obtain a single-sided pressing density of the negative electrode of 1.45±0.05 g / cm 3 Then, the mixture was dried and baked in a vacuum drying oven at 150° C. for 1 hour.

[0278] The dried double-sided coated copper foil obtained above was cut into electrodes so as to obtain a coated portion (front side: 56 mm×334 mm, back side: 56 mm×408 mm) and a tab welding margin to obtain a negative electrode.

[0279] <Electrode production by wet mixing>

[0280] - Positive Electrode Preparation (Examples 4 and 5) -

[0281] 1. Slurry Preparation

[0282] NCM523 (manufactured by Umicore, with a composition of LiNi) as the positive electrode active material was prepared using a 5L planetary disperser. 0.5 Co 0.2 Mn 0.3 After mixing 920 g of 1,000 g of N-methylpyrrolidone (NMP) and 920 g of 1,000 g of 2-nitropropene (SiO2), 20 g of Super-P (conductive carbon black) as a conductive aid, and 20 g of KS-6 (flaky graphite) for 10 minutes, 100 g of N-methylpyrrolidone (NMP) was added and mixed for further 20 minutes.

[0283] Next, 150 g of 8% by mass polyvinylidene fluoride (PVDF) solution ((Strain) Kureha Manufacturing, a solution in which PVDF W#7200 is dissolved in NMP, hereinafter also referred to as "8%-PVDF solution.") was added, and after kneading for 30 minutes, 150 g of 8%-PVDF solution was further added and mixed for 30 minutes. Then, 200 g of 8%-PVDF solution was added and mixed for 30 minutes. Next, 80 g of 8%-PVDF solution was added and mixed for 30 minutes. Then, NMP27 g was added to adjust the viscosity and mixed for 30 minutes, followed by 30 minutes of vacuum defoaming to prepare a slurry having a solid content concentration of 60% by mass.

[0284] 2. Coating and drying

[0285] The coating mass after drying is 19.0 mg / cm 2 The slurry was applied to one side of the main surface of an aluminum foil (thickness 20 μm, width 200 mm) using a die coater and dried. Next, the opposite side of the main surface of the aluminum foil (uncoated side) was coated with the slurry in the same manner with a coating mass of 19.0 mg / cm 2 The slurry is applied by a die coater and dried.

[0286] The obtained double-sided coated aluminum foil (coating amount on both sides totaled 38.0 mg / cm 2 ) was dried in a vacuum drying oven at 130°C for 12 hours.

[0287] 3. Suppression

[0288] Using a 1-ton roller press, the gap between the upper and lower rollers was adjusted to press the double-sided coated aluminum foil obtained above to a density of 2.9±0.05 g / cm on one side. 3 way to suppress it.

[0289] 4. Cutting

[0290] The electrodes were cut into pieces after the pressing process by coating both sides with aluminum foil to obtain coated portions (front side: 56 mm×334 mm, back side: 56 mm×408 mm) and tabs with welded edges to obtain positive electrodes.

[0291] - Negative Electrode Preparation (Examples 1 to 3 and Comparative Examples 1 to 2) -

[0292] 1. Slurry Preparation

[0293] Using a 5L planetary disperser, 960g of natural graphite as a negative electrode active material and 10g of Super-P (conductive carbon black) as a conductive aid were mixed for 5 minutes, and then 450g of 1% carboxymethyl cellulose (CMC) (a solution prepared by dissolving CMC in pure water, hereinafter also referred to as "1%-CMC aqueous solution") was added and further mixed for 30 minutes. Next, 300g of 1%-CMC aqueous solution was added and kneaded for 30 minutes, and then 250g of 1%-CMC was further added and kneaded for 30 minutes. Then, 25g of styrene-butadiene rubber (SBR) (40% by mass emulsifying solvent) as a binder was added and mixed for 30 minutes, and vacuum defoaming was performed for 30 minutes to prepare a slurry with a solid content concentration of 45% by mass.

[0294] 2. Coating and drying

[0295] The coating mass after drying is 11.0 mg / cm 2 The slurry was applied to one side of the main surface of a copper foil (thickness 10 μm) as a current collector using a die coater and dried. Next, the opposite side (uncoated side) of the main surface of the copper foil was coated with the slurry in the same manner with a coating mass of 11.0 mg / cm 2 The slurry is applied by a die coater and dried.

[0296] The obtained double-sided coated copper foil (coating amount on both sides is 22.0 mg / cm 2 ) was dried in a vacuum drying oven at 120°C for 12 hours.

[0297] 3. Suppression

[0298] Using a 1-ton roller press, the gap between the upper and lower rollers was adjusted to press the double-sided coated copper foil obtained above to a density of 1.45±0.05 g / cm on one side. 3 way to suppress it.

[0299] 4. Cutting

[0300] The electrodes were slit in such a way that the copper foils on both sides of the pressed electrodes were coated to obtain the coated portion (front side: 58 mm×372 mm, back side: 58 mm×431 mm) and the tabs were welded to obtain the negative electrodes.

[0301] <Battery production>

[0302] Batteries were fabricated using the electrodes prepared above in the following order.

[0303] First, an aluminum tab is bonded to a tab weld margin of the positive electrode using an ultrasonic bonding machine, and a nickel tab is bonded to a tab weld margin of the negative electrode using an ultrasonic bonding machine.

[0304] As the separator, a polyethylene porous film (183 mm×100 mm) having a porosity of 45% and a thickness of 25 μm was used.

[0305] 1. Layering

[0306] The negative electrode, separator, positive electrode, separator and negative electrode were alternately stacked in the order of 5 positive electrode layers and 6 negative electrode layers in total. It should be noted that at this time, the positive electrode and the negative electrode were stacked so that the tabs were on the same side.

[0307] Next, the obtained stacked body is sandwiched between laminate sheets, and the three sides of the laminate sheets are heat-sealed to prepare a case containing electrodes. It should be noted that at this time, the three sides other than the tab side are heat-sealed so that the tabs of the positive and negative electrodes protrude from the laminate sheets.

[0308] 2. Electrolyte injection

[0309] Before the electrolyte injection, the shell containing the electrodes was dried under reduced pressure at 70°C for 12 hours using a vacuum dryer. Then, 19.6±0.3g of electrolyte (1mol / L-LiPF6, solvent: ethylene carbonate (EC) / diethyl carbonate (DEC) = 3 / 7 (volume ratio), containing vinyl carbonate (VC) as an additive in a manner of 1.0 mass % relative to the final electrolyte) was injected into the dried shell containing the electrodes, and then the remaining side of the shell containing the electrodes was evacuated and heat-sealed in a manner that the positive and negative pole tabs protruded from the laminate.

[0310] 3. Activation (aging) treatment

[0311] The shell containing electrodes after sealing the four sides was subjected to multiple cycles of charging at 2.5 to 4.2 V, maintaining for 0.5 to 12 hours, charging to 4.2 V, and discharging to 2.8 V at room temperature. The battery was stored at 25°C for 5 days in the fully charged state of 4.2 V (SOC 100%), thereby producing a battery (laminated type battery [designed capacity 5 Ah]).

[0312] <Measurement of charge capacity and discharge capacity>

[0313] The prepared battery (after activation treatment) was charged to a constant voltage of 4.2 V at room temperature, and the charge capacity was measured. Then, it was discharged to 2.8 V at a constant current of 0.1 C at room temperature, and the discharge capacity was measured. The results are shown in Table 1.

[0314] [Table 1]

[0315]

[0316] In Table 1, the intrinsic viscosity [η] and the average particle size refer to the intrinsic viscosity [η] and the average particle size d50 of the electrode binder used in the dry method. In Table 1, "-" means that there is no measured value for the corresponding item.

[0317] It is found that the use of the present binder enables the production of electrodes by a dry process, and that the (lithium ion secondary) batteries of Examples 1 to 5 have improved charge and discharge capacities compared to the (lithium ion secondary) batteries of Comparative Examples 1 and 2.

[0318] <Electrode Binder 6 (used in Examples 7 to 9)>

[0319] As the electrode binder used in Examples 7 to 9, ultrahigh molecular weight ethylene polymer microparticles were prepared by the following method.

[0320] (i) Preparation of magnesium-containing carrier component (α-2)

[0321] In a 2L glass container equipped with a stirrer and fully purged with nitrogen, 95.2g (1.0mol) of anhydrous magnesium chloride, 442mL of dehydrated decane, 260.4g (2.0mol) of 2-ethylhexanol and 298.5g (1.0mol) of 2-octyldodecanol were placed and reacted at 155°C for 4 hours to obtain a uniform transparent solution.

[0322] Next, in another 1L glass container with a stirrer fully replaced with nitrogen, the above-mentioned uniform transparent solution of 100mmol in terms of magnesium atom conversion and 610mL of dehydrated decane were loaded, and a homogenizer (ClearMix CLM-1.5S manufactured by M Technique (Strain)) was used. Under strong stirring at a speed of 18000rpm, the liquid temperature was maintained at 0°C while 109mmol of triethylaluminum was slowly added dropwise. Then, the liquid temperature was raised to 80°C over 4 hours, and while maintaining 80°C, 188mmol of triethylaluminum was slowly added dropwise again, and the reaction was further carried out for 1 hour. After the reaction was completed, the solid portion was collected by filtration, fully washed with dehydrated xylene, and 200mL of dehydrated xylene was added to prepare a xylene slurry containing a magnesium carrier component (α-2). The magnesium concentration of the prepared magnesium-containing carrier component (α-2) was 0.21mmol / mL, and the aluminum concentration was 0.022mmol / mL.

[0323] (ii) Preparation of solid catalyst component (β-2)

[0324] In a 200mL glass reactor fully purged with nitrogen, 56.1mL of xylene was added, and under stirring, 28.9mL of xylene slurry (5.95mmol in terms of magnesium atom conversion) of the magnesium-containing carrier component (α-2) prepared above was loaded. Then, 28.3mg of the transition metal compound represented by the following formula (II) (0.0329mmol in terms of zirconium atom conversion) was loaded and reacted at room temperature for 1 hour. Then, the reactant was filtered, and the filter cake was washed once with 50mL of xylene and twice with 50mL of decane. Then, after filtering, 105mL of decane was added to the filter cake to prepare a decane slurry of a solid catalyst component (β-2).

[0325] A portion of the obtained decane slurry of the solid catalyst component (β-2) was collected and its concentration was checked. As a result, the zirconium concentration was 0.000373 mmol / mL and the magnesium concentration was 0.0699 mmol / mL.

[0326] [Chemistry 2]

[0327]

[0328] (iii) Preparation of ultra-high molecular weight ethylene polymer microparticles

[0329] In a 1L SUS autoclave fully purged with nitrogen, 500mL of decane was charged, and ethylene was flowed at 0.4NL / min for 15 minutes at room temperature to saturate the liquid phase and the gas phase. Next, after the temperature was raised to 65°C, 1.25mL of a decane solution of triisobutylaluminum (1.0mmol / mL in terms of aluminum atom) and 11.4mL of a decane slurry of the solid catalyst component (β-2) (0.80mmol in terms of magnesium atom) were added while ethylene was flowed at 0.4NL / min, and the mixture was stirred for 5 minutes while maintaining the temperature. Then, 6mL of a decane solution of EMULGEN 108 (manufactured by Kao Corporation) (15mg / mL) was charged, the flow of ethylene was temporarily stopped, 1mL of hydrogen was charged, and the temperature was raised to 70°C. Then, ethylene was added at 1.0 NL / min until the pressure reached 0.35 MPaG. After reaching 0.35 MPaG, polymerization was carried out while maintaining the temperature and pressure until the supply of ethylene reached 56 NL. Then, the autoclave was cooled and the ethylene pressure was released. The obtained slurry containing white solid was filtered, and the filter cake was washed with heptane and dried under reduced pressure at 80°C for 10 hours to obtain 68.6 g of ultrahigh molecular weight ethylene polymer microparticles.

[0330] The obtained ultrahigh molecular weight ethylene polymer microparticles had an intrinsic viscosity [η] of 11.9 dl / g, an average particle size d50 of 6.2 μm, and a passing rate through a sieve with a mesh size of 45 μm of 100 mass %.

[0331] <Electrode Binder 7 (used in Example 10)>

[0332] As the electrode binder used in Example 10, ultrahigh molecular weight ethylene polymer microparticles were prepared by the following method.

[0333] The magnesium-containing support component (α-2) and the solid catalyst component (β-2) were prepared in the same manner as in the electrode binder 6.

[0334] In the preparation process of ultrahigh molecular weight ethylene polymer microparticles of electrode binder 6, 69.8 g of ultrahigh molecular weight ethylene polymer microparticles were obtained by the same method as electrode binder 6, except that after the decane solution of EMULGEN 108 was charged, the flow of ethylene was not stopped and 1 mL of hydrogen was not charged.

[0335] The obtained ultrahigh molecular weight ethylene polymer microparticles had an intrinsic viscosity [η] of 24.6 dl / g, an average particle size d50 of 6.4 μm, and a passing rate through a sieve with a mesh size of 45 μm of 100 mass %.

[0336] [Example 6]

[0337] A negative electrode composite material was prepared by dry mixing 48 g of natural graphite as a negative electrode active material and an electrode binder in a ratio of 1:2.0 g at a rotation speed of 20,000 rpm using a Labo Miler (IFM-800LM-PLUS manufactured by Iwatani Industry Co., Ltd.).

[0338] The negative electrode composite material obtained above was placed in the gap between two rolls of a calender roll forming machine set at 200°C, and the gap between the rolls was adjusted to 1.45±0.05 g / cm 3 , a negative electrode mixture layer with a thickness of 135 μm was obtained.

[0339] <Tensile strength of negative electrode mixture layer>

[0340] The obtained negative electrode mixture layer was cut in such a way that the width of the roller in the rolling direction became 5 mm to prepare a test piece. Using the prepared test piece, the tensile (breaking) strength of the test piece in the rolling direction was measured using a tensile testing machine (manufactured by Instron, universal testing machine 5982) at a temperature of 23°C, a clamp spacing of 10 mm, and a tensile speed of 1 mm / min.

[0341] <Permeability of electrolyte>

[0342] The obtained negative electrode mixture layer was punched into a diameter of 17 mm, and attached to a parallel smooth glass surface in a manner to prevent the negative electrode mixture layer from moving. 0.2 mL of the same electrolyte as that used in the preparation of the button-type battery described later was dripped onto the surface of the negative electrode mixture layer, and covered with a glass petri dish to prevent the electrolyte from drying, and the time for the electrolyte to penetrate into the negative electrode mixture layer was visually measured.

[0343] <Production of button-type batteries>

[0344] An electrolyte solution (1 mol / L-LiPF6, solvent: ethylene carbonate (EC) / diethyl carbonate (DEC) = 3 / 7 (volume ratio), containing vinylene carbonate (VC) as an additive in such a manner as to be 1.0 mass % relative to the finally obtained electrolyte solution) was prepared.

[0345] The aforementioned negative electrode mixture layer and a copper foil with a thickness of 10 mm were overlapped and punched into a disc shape with a diameter of 14 mm. Furthermore, the lithium foil as the positive electrode was punched into a disc shape with a diameter of 13 mm to obtain a button-shaped negative electrode (a laminate of the negative electrode mixture layer and the copper foil) and a button-shaped positive electrode.

[0346] Separately, a microporous polyethylene film having a thickness of 20 μm was punched out into a disk shape having a diameter of 17 mm to obtain a button-shaped separator.

[0347] The obtained button-shaped negative electrode, separator and positive electrode were stacked in order in a stainless steel battery can (2032 size), and then 20 μL of the above-obtained electrolyte was injected into the battery can to impregnate the separator, positive electrode and negative electrode with the electrolyte.

[0348] Next, an aluminum plate (1.2 mm thick, 16 mm in diameter) and a spring were placed on the positive electrode, and the battery can lid was tightened via a polypropylene gasket to seal the battery.

[0349] Through the above operation, a button-type battery (ie, a button-type lithium secondary battery) having a diameter of 20 mm and a height of 3.2 mm was obtained.

[0350] The obtained button-type battery was activated (aged) by charging at 2.5 to 4.2 V, maintaining for 0.5 to 12 hours, charging to 4.2 V, and discharging to 2.8 V at room temperature for multiple times. It was then stored at 25°C for 5 days in a fully charged state of 4.2 V (SOC 100%).

[0351] <Measurement of charge capacity and discharge capacity>

[0352] The activated button-type battery was charged to a constant voltage of 4.2 V at room temperature, and the charge capacity was measured (1st cycle). Then, it was discharged to 2.8 V at a constant current of 0.1 C at room temperature, and the discharge capacity was measured (1st cycle). The results are shown in Table 2.

[0353] <Measurement of charging efficiency and discharging efficiency>

[0354] The same operation as in the above-mentioned measurement of the charge capacity and the discharge capacity was further repeated to measure the charge capacity (second cycle) and the discharge capacity (second cycle).

[0355] The ratio of the charging capacity (second cycle) obtained above to the charging capacity (first cycle) was calculated as the charging efficiency.

[0356] The ratio of the discharge capacity (second cycle) obtained above to the discharge capacity (first cycle) was calculated as the discharge efficiency.

[0357] [Example 7]

[0358] A battery was produced and evaluated in the same manner as in Example 6 except that the type of electrode binder used was changed from electrode binder 1 to electrode binder 6.

[0359] [Example 8]

[0360] A battery was prepared and evaluated in the same manner as in Example 6 except that the type of binder used was changed from electrode binder 1 to electrode binder 6 and the amount of binder used was changed from 2.0 g to 1.5 g.

[0361] [Example 9]

[0362] A battery was prepared and evaluated in the same manner as in Example 6 except that the type of binder used was changed from electrode binder 1 to electrode binder 6 and the amount of binder used was changed from 2.0 g to 1.0 g.

[0363] [Example 10]

[0364] A battery was produced and evaluated in the same manner as in Example 6 except that the type of binder used was changed from electrode binder 1 to electrode binder 7.

[0365] [Table 2]

[0366]

[0367] In Table 2, the intrinsic viscosity [η] and the average particle size refer to the intrinsic viscosity [η] and the average particle size d50 of the electrode binder used in the dry method.

[0368] It is found that the use of the present binder enables the production of electrodes by a dry process, and that the lithium ion secondary batteries of Examples 6 to 10 are excellent in charge and discharge capacity and charge and discharge efficiency.

Claims

1. An electrode binder comprising ultrahigh molecular weight olefin polymer microparticles (A) satisfying the following requirements (i) to (iii): (i) an intrinsic viscosity η measured in a decalin solvent at 135°C is in the range of 5 to 50 dl / g; (ii) the average particle size d50 in the mass-based particle size distribution based on the Coulter counter method is in the range of 1 to 50 μm; (iii) 50 mass % or more of the ultrahigh molecular weight olefin polymer fine particles (A) pass through a sieve having an opening of 45 μm. 2 . The electrode binder according to claim 1 , wherein the average particle size d50 of the ultrahigh molecular weight olefin polymer fine particles (A) is in the range of 3 to 15 μm. 3 . The electrode binder according to claim 1 , wherein the ultrahigh molecular weight olefin-based polymer fine particles (A) are ethylene-based polymer fine particles. 4 . An electrode comprising the electrode binder according to claim 1 and an active material. The electrode according to claim 4 , which is an electrode obtained by a dry method. 6 . A lithium ion secondary battery comprising the electrode according to claim 4 or 5 and an electrolyte.

7. A method for manufacturing an electrode, comprising: A step of dry-mixing the electrode binder and the active material according to any one of claims 1 to 3 to obtain an electrode composite material; as well as A process for producing an electrode comprising the electrode composite material and a current collector.