Cooker and manufacturing method thereof

By spraying the magnetic permeability layer of nickel-based alloy on the outer surface of the bottom wall of the pot, the temperature of its Curie temperature characteristics can be automatically controlled, which solves the problems of high-temperature aging of the magnetic permeability layer and food burning during the use of the induction cooker, and extends the use of the pot Lifespan and improve safety.

CN118872991APending Publication Date: 2024-11-01WUHAN SUPOR COOKWARE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411082163.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

Existing pots and cookers need to manually adjust their power when using induction cookers, resulting in the magnetic permeability being in a high temperature state for a long time, shortening their service life, and possibly leading to food burning and safety hazards.

Method used

Using a nickel-based alloy magneto-permeable layer, its Curie temperature is in the range of 230℃-300℃, and is formed in the pot. The outer surface of the bottom wall realizes automatic temperature control and protection.

Benefits of technology

It extends the service life of the magnetic permeability layer, avoids food burning and safety hazards, and ensures the stability and safety of cooking temperature.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118872991A_ABST
    Figure CN118872991A_ABST
Patent Text Reader

Abstract

The invention provides a cooker and a manufacturing method thereof. The cooker comprises a cooker body and a nickel-based alloy magnetic conductive layer, the cooker body is made of silicate mineral inorganic nonmetal, the nickel-based alloy magnetic conductive layer is at least formed on the bottom wall of the cooker body through a nickel-based alloy material, the Curie temperature of the nickel-based alloy material ranges from 230 DEG C to 300 DEG C, and the Curie temperature of the nickel-based alloy material ranges from 230 DEG C to 300 DEG C. The nickel-based alloy material comprises nickel, iron and auxiliary elements, and the auxiliary elements comprise at least two of cobalt, chromium, silicon, manganese, molybdenum, vanadium and copper. According to the cooker, the magnetic conduction service life is long.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of cookers, and in particular to a cooker and a manufacturing method thereof. Background Art

[0002] Some commonly used materials for making cookware (for example, ceramics, glass, stone, etc.) are not magnetic. In order to meet the general conditions of induction cookers, realizing the magnetic heating function becomes a problem that must be faced.

[0003] At present, a layer of magnetic conductive material (such as iron layer, etc.) is usually added to the bottom of the cookware, so that the bottom of the cookware, which is originally non-magnetic, can sense the magnetic field generated by the induction cooker, thereby achieving heating. However, cookware with the function of a general induction cooker usually has many problems during use. For example, it is usually necessary to manually adjust the power of the induction cooker to adjust the operating temperature of the cookware. If the user forgets or fails to adjust it in time, the magnetic conductive layer will continue to be in a high temperature state, thereby accelerating aging or damage, and affecting the magnetic conductive service life of the cookware. Summary of the invention

[0004] Therefore, the purpose of the present application is to provide a cooker and a manufacturing method thereof, so as to solve the many problems that occur when the cooker with the function of a general induction cooker is used in the prior art.

[0005] The purpose of the present application is to provide a cooker, wherein the cooker comprises a cooker body and a nickel-based alloy magnetic conductive layer, wherein the cooker body is made of inorganic non-metallic silicate minerals; the nickel-based alloy magnetic conductive layer is formed at least on the bottom wall of the cooker body by a nickel-based alloy material, wherein the Curie temperature of the nickel-based alloy material is in the range of 230°C-300°C, and the nickel-based alloy material comprises nickel, iron and auxiliary elements, wherein the auxiliary elements comprise at least two of cobalt, chromium, silicon, manganese, molybdenum, vanadium and copper.

[0006] According to the present application, the temperature of the cooker during use is controllable, so that the cooker can be prevented from being in a high-temperature working state for a long time, which may accelerate aging or damage the magnetic conductive layer, thereby increasing the magnetic conductive service life of the magnetic conductive cooker. In addition, the temperature of the cooker during use is continuously at a suitable temperature, which can also ensure that the nickel-based alloy magnetic conductive layer is not easily burned. Therefore, the cooker provided according to the present application has a longer magnetic conductive life.

[0007] In some embodiments, based on the total weight of the nickel-based alloy material being 100%, the weight of the nickel accounts for 30%-50% of the total weight of the nickel-based alloy material, the weight of the auxiliary elements accounts for 5%-30% of the total weight of the nickel-based alloy material, the weight of the iron accounts for 20%-45% of the total weight of the nickel-based alloy material, and the sum of the weights of the nickel, iron and auxiliary elements is 100%. In this way, the formed nickel-based alloy magnetic conductive layer of the cooker has a Curie temperature in the range of 230°C-300°C. During the cooking process, the nickel-based alloy magnetic conductive layer can control the temperature of the outer wall of the cooker from being too high. In this case, a small part of the bottom wall is lost. Under the heat conduction effect of the bottom wall, the temperature of the inner wall of the cooker can be maintained in the range of 150°C-230°C. In this way, the temperature of the cooker during cooking can be continuously in a stable temperature range, ensuring that the food is not easily burnt, and ensuring a good cooking experience.

[0008] In some embodiments, the auxiliary elements include silicon and cobalt, the weight of the silicon accounts for 0.2%-0.4% of the total weight of the nickel-based alloy material, and the weight of the cobalt accounts for 7%-20% of the total weight of the nickel-based alloy material.

[0009] In these embodiments, the auxiliary elements are silicon and cobalt, and silicon mainly plays a role in improving corrosion resistance and oxidation resistance in nickel-based alloy materials. Although its content is relatively low, the addition of silicon can significantly improve the stability of nickel-based alloy materials in high temperature environments. In addition, silicon also helps to refine the grain structure of nickel-based alloy materials and improve the mechanical properties of nickel-based alloy materials. The addition of cobalt can significantly improve the high temperature resistance, corrosion resistance and hardness of nickel-based alloy materials. Cobalt can also enhance the magnetic properties of nickel-based alloy materials and ensure the ability to maintain the magnetic properties at high temperatures. In this way, the nickel-based alloy material can have good magnetic conductivity, high temperature resistance, corrosion resistance and mechanical strength while meeting the Curie temperature point of the present application.

[0010] In some embodiments, the nickel-based alloy material includes nickel, iron, manganese, silicon, cobalt and chromium. Taking the total weight of the nickel-based alloy material as 100%, the weight of the nickel accounts for 41.5%-42.5% of the total weight of the nickel-based alloy material, the weight of the manganese accounts for 0.1%-0.4% of the total weight of the nickel-based alloy material, the weight of the silicon accounts for 0.1%-0.3% of the total weight of the nickel-based alloy material, the weight of the cobalt accounts for 5%-9.5% of the total weight of the nickel-based alloy material, the weight of the chromium accounts for 5.5%-6.3% of the total weight of the nickel-based alloy material, and the balance is iron.

[0011] In these embodiments, the nickel-based alloy material includes nickel, iron, manganese, silicon and chromium, and manganese, silicon and chromium are auxiliary elements, and the content of manganese accounts for 0.1%-0.4% of the total weight of the nickel-based alloy material. Manganese plays a major role in deoxidation and desulfurization in the nickel-based alloy material, which helps to reduce the content of impurity elements in the nickel-based alloy material and improve the purity and performance of the nickel-based alloy material. At the same time, manganese can also enhance the strength and toughness of the nickel-based alloy material and improve its processing performance. The content of manganese within this ratio range can avoid adverse effects on the magnetic conductivity of the nickel-based alloy material, while playing its positive role. Silicon plays a major role in improving corrosion resistance and oxidation resistance in the nickel-based alloy material. Although its content is relatively low, the addition of silicon can significantly improve the stability of the nickel-based alloy material in a high temperature environment. In addition, silicon also helps to refine the grain structure of the nickel-based alloy material and improve the mechanical properties of the nickel-based alloy material. The addition of cobalt can significantly improve the high temperature resistance, corrosion resistance and hardness of the nickel-based alloy material. Cobalt can also enhance the magnetic properties of the nickel-based alloy material and ensure the ability to maintain the magnetic properties at high temperatures. Chromium can form a dense oxide film with oxygen, covering the surface of the nickel-based alloy material, thereby protecting the nickel-based alloy material from corrosion by corrosive media and significantly improving the corrosion resistance of the nickel-based alloy material. In this way, the nickel-based alloy material can have good magnetic conductivity, high temperature resistance, corrosion resistance and mechanical strength while meeting the Curie temperature point of this application.

[0012] In some embodiments, the thickness of the nickel-based alloy magnetic conductive layer is 40 microns to 90 microns. Within this range, various aspects such as magnetic conductive heating efficiency, cost, and stress can be balanced, and a higher magnetic conductive service life can be achieved. If the thickness of the nickel-based alloy magnetic conductive layer is too thin, the magnetic conductive heating efficiency is affected. If the thickness of the nickel-based alloy magnetic conductive layer is too thick, the cost is too high, stress is increased, and adhesion is reduced.

[0013] In some embodiments, the particle size of the nickel-based alloy material is 15 microns to 75 microns, so as to ensure the compactness of the nickel-based alloy magnetic conductive layer formed by spraying.

[0014] In some embodiments, the cooker further comprises a ceramic protective layer disposed outside the nickel-based alloy magnetic conductive layer, wherein the ceramic protective layer is formed of a ceramic coating. In this way, the risk of the nickel-based alloy magnetic conductive layer being directly exposed to the outside and being damaged can be reduced, thereby further improving the magnetic conductive life of the cooker.

[0015] In some embodiments, the ceramic coating is a ceramic coating with a temperature tolerance range of 250° C. to 650° C. In this way, a ceramic protective layer with good temperature resistance can be formed, and the ceramic protective layer itself can withstand high temperatures to better protect the nickel-based alloy magnetic conductive layer.

[0016] In some embodiments, the auxiliary element also includes carbon. In the nickel-based alloy material, the weight proportion of the carbon is 0.01%-0.05%. In this way, the hardness and wear resistance of the nickel-based alloy magnetic conductive layer formed by the nickel-based alloy material can be ensured.

[0017] According to a second aspect of the present application, a method for manufacturing cookware is provided, wherein the method comprises: providing a cookware substrate, wherein the cookware substrate is made of inorganic non-metallic silicate minerals; spraying a nickel-based alloy material at least on a bottom wall of the cookware substrate to form a nickel-based alloy magnetic conductive layer, thereby manufacturing the cookware, wherein the Curie temperature of the nickel-based alloy material is in the range of 230°C-300°C, and the nickel-based alloy material comprises nickel, iron and auxiliary elements, wherein the auxiliary elements comprise at least two of cobalt, chromium, silicon, manganese, molybdenum, vanadium and copper.

[0018] In some embodiments, the nickel-based alloy material is formed by melting and smelting a mixture of raw material nickel, raw material iron and raw material auxiliary elements, or by melting and smelting a mixture of nickel iron ore and raw material auxiliary elements. The nickel-based alloy material formed by melting and smelting a mixture has excellent properties, such as high temperature strength, corrosion resistance and good processing performance.

[0019] In some embodiments, before forming the nickel-based alloy magnetic conductive layer, plasma surface treatment is performed on the cookware substrate to form a rough structure on the surface of the cookware substrate to enhance the bonding force between the cookware substrate and the nickel-based alloy magnetic conductive layer.

[0020] In some embodiments, after forming the nickel-based alloy magnetic conductive layer, the method further comprises forming a ceramic protective layer on the outer surface of the nickel-based alloy magnetic conductive layer by air spraying a ceramic coating. In this way, the risk of the nickel-based alloy magnetic conductive layer being directly exposed to the outside and being damaged can be reduced, further improving the magnetic conductive life of the cooker. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] The above and other objects and features of the present application will become more apparent through the following description of the embodiments in conjunction with the accompanying drawings, in which:

[0022] Figure 1 is a schematic cross-sectional structural diagram of a cooker provided according to an embodiment of the present application;

[0023] Figure 2 yes Figure 1 Enlarged schematic diagram of point I in the middle.

[0024] Explanation of symbols

[0025] 10. Cooker body;

[0026] 11. side wall; 12. bottom wall;

[0027] 20. Nickel-based alloy magnetic conductive layer; 30. Ceramic protective layer. DETAILED DESCRIPTION

[0028] The inventive concept will be described more fully below in conjunction with exemplary embodiments, however, the inventive concept can be implemented in many different forms and should not be interpreted as being limited to the embodiments set forth herein. On the contrary, these embodiments are provided so that this disclosure will be thorough and complete, and will fully convey the scope of the inventive concept to those skilled in the art.

[0029] Cookware with induction cooker heating function can be heated mainly by the magnetic conductive layer or its own magnetic conductivity, which can effectively interact with the magnetic field generated by the induction cooker to generate eddy currents and achieve heating. Cookware without induction cooker heating function, such as ceramic pots without magnetic conductive layer or ceramic pots with insufficient magnetic conductive layer thickness, cannot generate enough eddy currents and are therefore not suitable for induction cooker heating. It is understandable that even if used on an induction cooker, the induction cooker's electromagnetic heating function will not be activated.

[0030] Cookware made of ceramics, glass, stone, etc. has many advantages, such as slow fire heating and uniform heat conduction. Therefore, this cookware can be loved by more users. However, if there is no magnetic conductive layer or the thickness of the magnetic conductive layer is not enough, the cookware made of ceramics, glass, stone, etc. itself cannot be magnetic. If it is necessary to meet the general conditions of induction cookers, realizing the magnetic conductive heating function becomes a problem that must be faced.

[0031] At present, by adding a magnetic conductive layer (such as an iron layer, etc.) to the bottom of the cookware, the bottom of the cookware that is originally non-magnetic can sense the magnetic field generated by the electromagnetic cooker, thereby achieving heating. However, cookers with the function of a general electromagnetic cooker usually have many problems during use. For example, it is usually necessary to manually adjust the power of the electromagnetic cooker to adjust the operating temperature of the cooker. If the user forgets or fails to adjust it in time, the magnetic conductive layer will continue to be in a high temperature state, thereby accelerating aging or damage, affecting the magnetic conductive service life of the cooker. In addition, when the temperature of the cooker is at a high temperature for a long time and the user forgets or fails to adjust it in time, the food may burn due to the excessive temperature of the cookware, which poses certain safety hazards. In addition, there will be problems such as excessively high local temperature, which affects the taste of the cooked food, and it is easy to generate a large amount of oil smoke, which affects health.

[0032] To this end, the present application provides a cooker made by spraying a nickel-based alloy magnetic conductive layer with a Curie temperature point in the range of 230°C-300°C on at least the outer surface of the bottom wall of the cooker base. The Curie temperature of the nickel-based alloy magnetic conductive layer of the cooker is in the range of 230°C-300°C, so that the temperature of the cooker can be controlled when in use, thereby preventing the cooker from being in a high-temperature working state for a long time and accelerating aging or damaging the magnetic conductive layer, thereby increasing the magnetic conductive service life of the magnetic conductive cooker. In addition, the temperature of the cooker during use is continuously at a suitable and stable heating temperature, which can also ensure that the nickel-based alloy magnetic conductive layer is not easily burned or deformed. Therefore, the cooker provided according to the present application has a longer magnetic conductive life.

[0033] In addition, the temperature of the cooker can be controlled during use, which can prevent the temperature from continuing to rise during the cooking process. In this case, even if the user fails to control the induction cooker to reduce the power in time or forgets to do so, the food will not be burnt, thus avoiding fire and other dangers and reducing safety hazards. Moreover, the cooking temperature of the cooker can be controlled at 150℃-230℃ during the cooking process, which can better cook food and reduce the generation of oil smoke.

[0034] According to a first aspect of the present application, a method for manufacturing a cooker is provided, wherein the cooker can be used at least in combination with an induction cooker, and the method for manufacturing the cooker comprises:

[0035] Step S101, providing a cookware base, wherein the cookware base is made of inorganic non-metallic silicate minerals.

[0036] Step S102, spraying a nickel-based alloy material on at least the bottom wall of the cookware base to form a nickel-based alloy magnetic conductive layer with a Curie temperature in the temperature range of 230°C-300°C, thereby manufacturing the cookware, wherein the nickel-based alloy material has a Curie temperature in the range of 230°C-300°C and includes nickel, iron and auxiliary elements, wherein the auxiliary elements include at least two of cobalt, chromium, silicon, manganese, molybdenum, vanadium and copper.

[0037] In the embodiment of the present application, the Curie temperature point (Tc) can be called the magnetic transition point, which refers to the temperature when the spontaneous magnetization intensity in the nickel-based alloy magnetic conductive layer drops to zero. It is the critical point for ferromagnetic or ferrimagnetic materials to transform into paramagnetic materials.

[0038] According to the manufacturing method of the cooker provided in the embodiment of the present application, a nickel-based alloy material is sprayed at least on the outer surface of the bottom wall of the cooker base to form a nickel-based alloy magnetic conductive layer with a Curie temperature in the temperature range of 230°C-300°C, which serves as an overheating protection component of the cooker. When the temperature at the bottom of the cooker is too high, the nickel-based alloy magnetic conductive layer will automatically lose its ferromagnetism and stop the electromagnetic heating function, so that the temperature of the cooker can be controlled when in use. According to the present application, the Curie temperature of the nickel-based alloy magnetic conductive layer is in the range of 230°C-300°C. In the embodiment, the Curie temperature can be in the range of 230°C-300°C, 240°C-300°C, 250°C-300°C, 250°C-270°C, 250°C-260°C, 250°C-280°C and 240°C-290°C. The Curie temperature of the nickel-based alloy magnetic conductive layer is within the temperature range of 230°C-300°C. It is formed on the outer surface of the cookware. When used in conjunction with an induction cooker and the temperature is lower than the Curie temperature of the nickel-based alloy magnetic conductive layer, the external heat source is transferred to the inner surface of the cookware through the nickel-based alloy magnetic conductive layer and then through the cookware body, so that the temperature of the inner surface of the cookware can be maintained within the range of 150°C-230°C. In this way, the temperature of the cookware during cooking can be continuously in a stable temperature range, ensuring that the ingredients are not easily burnt, thereby ensuring a good cooking experience.

[0039] According to the present application, the nickel-based alloy magnetic conductive layer of the cookware can be magnetic or non-magnetic according to its own temperature. In the case where the magnetic permeability of the cookware base itself is insufficient, whether the nickel-based alloy magnetic conductive layer is magnetic or not will determine whether the cookware is ferromagnetic. When the cookware is placed on an induction cooker and its own temperature is lower than the Curie temperature, the induction cooker uses current to pass through the coil to generate magnetic lines of force in the magnetic field that can pass through the cookware with the nickel-based alloy magnetic conductive layer, generating eddy currents, thereby causing the cookware to heat up quickly to heat the food in the cookware. When the temperature of the cooker itself is heated to the Curie temperature, the magnetism of the nickel-based alloy magnetic layer disappears. In this case, the entire cooker will not have ferromagnetism, so the magnetic lines cannot penetrate the bottom wall of the cooker to generate eddy currents, so the induction cooker cannot work normally and stops heating. In this way, the nickel-based alloy magnetic layer is equivalent to having an overheating protection component. When the bottom temperature of the cooker is detected to be too high (for example, greater than the Curie temperature), the nickel-based alloy magnetic layer will automatically lose its ferromagnetism and stop the electromagnetic heating function. In this way, the cooker can always be at a suitable temperature when in use, which can avoid the nickel-based alloy magnetic layer of the cooker being at high temperature for a long time, and the low temperature can also ensure that the nickel-based alloy magnetic layer is not burned or deformed, thereby extending the magnetic life of the cooker. In addition, the temperature of the cooker is controllable when in use, which can avoid the temperature from continuing to rise during the cooking process. In this case, even if the user does not control the induction cooker to reduce the power in time or forgets to reduce the power, it will not cause the cooked food to burn, which can avoid fire and other dangers, reduce safety hazards, and ensure the cooking experience.

[0040] According to the present application, the nickel-based alloy material includes nickel, iron and auxiliary elements, wherein the auxiliary elements include at least two of cobalt, chromium, silicon, manganese, molybdenum, vanadium and copper. Nickel and iron are the main constituent elements of the nickel-based alloy material, and their proportion directly affects the matrix structure and performance of the alloy. Among them, in the preparation process of the nickel-based alloy material, auxiliary elements such as cobalt, chromium, silicon, manganese, molybdenum, vanadium and copper are introduced, and by adjusting their content, the phase change behavior and final performance of the alloy, including the Curie temperature, can be significantly affected. Specifically, in the phase change process of forming the nickel-based alloy material, auxiliary elements such as cobalt, chromium, silicon, manganese, molybdenum, vanadium and copper can expand the austenite zone of the material, can affect the austenitization formation temperature of the material, and thereby affect the Curie temperature of the nickel-based alloy material.

[0041] In addition, cobalt (Co) is a strong austenite forming element, which can not only significantly affect the Curie temperature point, but also increase the austenite stability of nickel-based alloy materials, the hardness and corrosion resistance of nickel-based alloy materials. Chromium (Cr) can affect the stability and Curie temperature of the austenite zone, and can improve the corrosion resistance and oxidation resistance of nickel-based alloy materials. Silicon (Si) is mainly used as a deoxidizer and strengthening element in the alloy, which helps to improve the high temperature strength and corrosion resistance of the alloy. Manganese (Mn) Manganese is one of the strong austenite forming elements and can significantly expand the austenite zone. It also helps to improve the strength and toughness of the alloy and has a certain effect on the Curie temperature. Molybdenum (Mo) is an effective solid solution strengthening element that can significantly improve the high temperature strength and corrosion resistance of the alloy. Vanadium (V) is a strong carbide forming element that can refine the grains of the alloy and improve its strength and heat resistance. Copper (Cu) mainly plays a strengthening role in the alloy, which helps to improve the hardness and corrosion resistance of the alloy.

[0042] According to the present application, a nickel-based alloy magnetic conductive layer is formed on the outer surface of the bottom wall of the cookware base. Compared with setting the magnetic conductive layer on the inner surface of the bottom wall, setting the nickel-based alloy magnetic conductive layer on the outer surface can reduce the loss of heat during the transfer process and improve energy utilization efficiency. In addition. Setting the magnetic conductive layer on the outer surface of the bottom wall can ensure that the heat is more evenly transferred to the cookware base, thereby improving the heating effect. Specifically, the magnetic conductive layer generates eddy currents and generates heat under the action of the electromagnetic field. The heat is transferred to the cookware base through the magnetic conductive layer, and then further transferred to the food, so that the temperature of the inner wall of the cookware can be maintained within the range of 150°C-230°C. In this way, the temperature of the cookware during cooking can continue to be in a stable temperature range, ensuring that the ingredients are not easily burnt, and ensuring a good cooking experience.

[0043] In these embodiments, manganese can significantly improve the strength and hardness of the nickel-based alloy material, thereby enhancing the mechanical properties of the nickel-based alloy material, thus improving the durability and deformation resistance of the cookware. Cobalt can slow down the phase change rate of the molten alloy liquid during the cooling process, making the nickel-based alloy material easier to process and shape. In addition, cobalt also has good antioxidant and corrosion resistance, which helps to extend the service life of the nickel-based alloy material. Silicon acts as a deoxidizer and reductant during the smelting process, which helps to remove oxygen and other impurities in the process of forming the nickel-based alloy material. At the same time, silicon can also increase the magnetic permeability of ferrite, thereby indirectly improving the overall magnetic permeability of the nickel-based alloy material. Copper can improve the electrical conductivity and corrosion resistance of the nickel-based alloy material.

[0044] According to the present application, by adjusting the content ratio of nickel and iron in the nickel-based alloy powder, some other alloy elements are added as an auxiliary. Among them, in the phase change process of forming the nickel-based alloy material, auxiliary elements such as cobalt, chromium, silicon, manganese, molybdenum, vanadium and copper can expand the austenite zone of the material and affect the austenitization formation temperature of the material, thereby affecting the Curie temperature of the nickel-based alloy material, so that the nickel-based alloy material of the present application has a predetermined Curie temperature.

[0045] In some embodiments, taking the total weight of the nickel-based alloy material as 100%, the weight of nickel accounts for 30%-50% of the total weight of the nickel-based alloy material, the weight of the auxiliary elements accounts for 5%-30% of the total weight of the nickel-based alloy material, and the remainder is iron. In this way, the formed cookware nickel-based alloy magnetic conductive layer has a Curie temperature in the range of 230°C-300°C. During the cooking process, the nickel-based alloy magnetic conductive layer can control the temperature of the outer wall of the cookware so that it is not too high. In this case, through the heat conduction of the bottom wall, the temperature of the inner wall of the cookware can be maintained in the range of 150°C-230°C. In this way, the temperature of the cookware during cooking can be continuously in a stable temperature range, ensuring that the ingredients are not easy to burn and ensuring a good cooking experience.

[0046] In these embodiments, nickel, iron and auxiliary elements form a nickel-based alloy material with stable performance during the smelting process. These materials not only have excellent magnetic conductivity, but also have good mechanical properties, corrosion resistance and high temperature stability, so that the properties of the magnetic conductive layer of the formed cookware are more excellent and more suitable for the use conditions of the cookware. By controlling the content of auxiliary elements, the austenite stability and austenitization formation temperature of the nickel-based alloy material can be adjusted, thereby indirectly affecting the Curie temperature point.

[0047] Further, the auxiliary elements are silicon and cobalt, wherein the weight of silicon accounts for 0.2%-0.4% of the total weight of the nickel-based alloy material, and the weight of cobalt accounts for 7%-20% of the total weight of the nickel-based alloy material. Preferably, the weight of cobalt accounts for 7%-10% of the total weight of the nickel-based alloy material.

[0048] In these embodiments, the auxiliary elements are silicon and cobalt, and silicon mainly plays a role in improving corrosion resistance and oxidation resistance in nickel-based alloy materials. Although its content is relatively low, the addition of silicon can significantly improve the stability of nickel-based alloy materials in high temperature environments. In addition, silicon also helps to refine the grain structure of nickel-based alloy materials and improve the mechanical properties of nickel-based alloy materials. The addition of cobalt can significantly improve the high temperature resistance, corrosion resistance and hardness of nickel-based alloy materials. Cobalt can also enhance the magnetic properties of nickel-based alloy materials and ensure the ability to maintain the magnetic properties at high temperatures. In this way, the nickel-based alloy material can have good magnetic conductivity, high temperature resistance, corrosion resistance and mechanical strength while meeting the Curie temperature point of the present application.

[0049] In some other embodiments, the nickel-based alloy material includes nickel, iron, manganese, silicon, cobalt and chromium. Taking the total weight of the nickel-based alloy material as 100%, the weight of nickel accounts for 41.5%-42.5% of the total weight of the nickel-based alloy material, the weight of manganese accounts for 0.1%-0.4% of the total weight of the nickel-based alloy material, the weight of silicon accounts for 0.1%-0.3% of the total weight of the nickel-based alloy material, the weight of cobalt accounts for 5%-9.5% of the total weight of the nickel-based alloy material, the weight of chromium accounts for 5.5%-6.3% of the total weight of the nickel-based alloy material, and the balance is iron.

[0050] In these embodiments, the nickel-based alloy material includes nickel, iron, manganese, silicon and chromium, and manganese, silicon and chromium are auxiliary elements, and the content of manganese accounts for 0.1%-0.4% of the total weight of the nickel-based alloy material. Manganese plays a major role in deoxidation and desulfurization in the nickel-based alloy material, which helps to reduce the content of impurity elements in the nickel-based alloy material and improve the purity and performance of the nickel-based alloy material. At the same time, manganese can also enhance the strength and toughness of the nickel-based alloy material and improve its processing performance. The content of manganese within this ratio range can avoid adverse effects on the magnetic conductivity of the nickel-based alloy material, while playing its positive role. Silicon plays a major role in improving corrosion resistance and oxidation resistance in the nickel-based alloy material. Although its content is relatively low, the addition of silicon can significantly improve the stability of the nickel-based alloy material in a high temperature environment. In addition, silicon also helps to refine the grain structure of the nickel-based alloy material and improve the mechanical properties of the nickel-based alloy material. The addition of cobalt can significantly improve the high temperature resistance, corrosion resistance and hardness of the nickel-based alloy material. Cobalt can also enhance the magnetic properties of the nickel-based alloy material and ensure the ability to maintain the magnetic properties at high temperatures. Chromium can form a dense oxide film with oxygen, covering the surface of the nickel-based alloy material, thereby protecting the nickel-based alloy material from corrosion by corrosive media and significantly improving the corrosion resistance of the nickel-based alloy material. In this way, the nickel-based alloy material can have good magnetic conductivity, high temperature resistance, corrosion resistance and mechanical strength while meeting the Curie temperature point of this application.

[0051] According to the present application, the auxiliary elements may also include carbon. In the nickel-based alloy material, the weight proportion of carbon is 0.01%-0.05%. The formed nickel-based alloy material has a certain amount of carbon, so that the hardness and wear resistance of the nickel-based alloy magnetic conductive layer formed by the nickel-based alloy material can be ensured. It should be noted that the raw iron for preparing the nickel-based alloy material of the present application is not necessarily pure iron, but can be iron with a carbon content of 0.01%-0.05%, so that the formed nickel-based alloy material can have a certain amount of carbon.

[0052] As we all know, nickel and iron are both ferromagnetic materials. The Curie temperature of nickel is usually 358°C, and the Curie temperature of iron is usually 770°C. The Curie temperature of nickel and iron is the temperature point at which nickel and iron lose their ferromagnetism.

[0053] According to the present application, in some embodiments, nickel and iron are both ferromagnetic metals. By adjusting the content ratio of nickel and iron in the nickel-based alloy powder and adding some other alloying elements, the Curie temperature of the nickel-based alloy material can be adjusted to be within the range of 230°C-300°C. It can be understood that based on the different contents of each component in the nickel-based alloy material, the nickel-based alloy magnetic conductive layer can have different Curie temperatures. For example, in the above-mentioned embodiment where the auxiliary elements include silicon and cobalt, the Curie temperature of the nickel-based alloy magnetic conductive layer of the cooker is 270°C-300°C. In the above-mentioned embodiment where the nickel-based alloy material includes nickel, iron, manganese, silicon and chromium, the Curie temperature of the nickel-based alloy magnetic conductive layer of the cooker is 230°C-270°C. When in use, when the temperature of the cooker itself reaches the Curie temperature, the nickel-based alloy magnetic conductive layer will not have magnetism. In this case, the induction cooker cannot work normally and the heating function will stop, thereby preventing the induction cooker from affecting the magnetic conductive life due to long-term over-temperature during use.

[0054] Hereinafter, the method for manufacturing the cooker according to the present application will be described in conjunction with specific embodiments.

[0055] Provide cookware base

[0056] According to the present application, the cookware base is made of inorganic non-metallic silicate minerals, specifically, made of ceramics, glass or stone.

[0057] According to the present application, the obtained cookware base has the basic structure of conventional cookware. In some embodiments, the thickness of the cookware base is generally 2.5 mm-3.6 mm, and such a thickness can ensure the overall strength of the formed cookware.

[0058] Pre-treatment

[0059] The manufacturing method of the cookware according to the present application also includes chemically degreasing the cookware base. Specifically, the cookware base can be degreased at a preset temperature for a preset time using a degreasing tank liquid to complete the step of chemically degreasing the cookware base, wherein the degreasing tank liquid includes a mixture of sodium hydroxide, sodium carbonate, and sodium phosphate. According to an exemplary embodiment of the present application, in the degreasing tank liquid, the mass concentration of sodium hydroxide is 15g / L-25g / L, the mass concentration of sodium carbonate is 25g / L-35g / L, and the mass concentration of sodium phosphate is 25g / L-35g / L. The preset temperature is 60℃-80℃; the preset time is 3min-5min.

[0060] The method for manufacturing the cookware according to the present application further comprises the steps of washing and drying the degreased cookware base. Specifically, the degreased cookware base is washed and dried for later use.

[0061] According to one aspect of the present application, the method for manufacturing the cookware further includes the step of roughening the surface to be formed of the cookware base, so as to provide a good bonding foundation for the subsequent step of forming the nickel-based alloy magnetic conductive layer. Specifically, before the step of forming the nickel-based alloy magnetic conductive layer, the surface of the cookware is roughened by sandblasting or shot blasting to form a layer of rough structure (e.g., pattern and roughness) on the cookware base that is conducive to the bonding of the nickel-based alloy magnetic conductive layer. It should be noted that the surface to be formed here can be the outer wall surface of the cookware base. Specifically, the cookware base includes a bottom wall and a side wall connected to the bottom wall, and the surface to be formed can be the outer surface (outer wall surface) of the bottom wall of the cookware base.

[0062] According to one aspect of the present application, the method for manufacturing the cookware further includes performing plasma surface treatment on the cookware substrate before forming the nickel-based alloy magnetic conductive layer to form a rough structure on the surface of the cookware substrate. Specifically, the surface treatment technology of using ions to impact the surface of the cookware substrate to improve its chemical and physical properties can remove surface pollutants and oxide layers, change surface roughness, improve wear resistance, change chemical properties, etc. In this way, the cookware substrate after plasma treatment can be more suitable for the manufacture of the nickel-based alloy magnetic conductive layer and have stronger bonding force.

[0063] Provide nickel-based alloy materials

[0064] According to the present application, the nickel-based alloy material is the nickel-based alloy material provided according to the above-mentioned embodiment.

[0065] In some embodiments, a method for preparing a nickel-based alloy material is provided, wherein the nickel-based alloy material is formed by melting and smelting a mixture of raw material nickel, raw material iron and raw material auxiliary elements. Specifically, the method for preparing a nickel-based alloy material includes preparing raw material nickel, raw material iron and raw material auxiliary elements, mixing the raw material nickel, raw material iron and raw material auxiliary elements in a certain proportion, and melting and smelting at high temperature to form a molten alloy liquid, and the smelting temperature needs to be higher than the melting point of all components in the raw material to ensure that the raw material is completely melted and a uniform molten alloy liquid is formed. At the same time, the smelting time and smelting atmosphere need to be strictly controlled to avoid the formation of harmful phases and the pollution of gas impurities. As an example, the smelting temperature is 1450°C-1600°C, the smelting time is 2h-4h, and the smelting atmosphere is full-flow helium. Under the above conditions, it is possible to ensure that the alloy composition is uniform and avoid the formation of harmful phases. Then, the molten alloy liquid is placed in a vacuum container to reduce the influence of gas impurities on the alloy, while promoting rapid condensation and homogenization of the alloy. By controlling the air pressure in the vacuum container, the air pressure difference or a special gas injection device is used to spray the molten alloy liquid in the form of droplets. The ejected molten alloy droplets cool rapidly and solidify in a vacuum, and are further refined into tiny particles by the impact of the surrounding gas. During the atomization process, the particle size of the particles can be controlled by adjusting the gas flow rate and the atomizing gas pressure. As an example, the gas flow rate is 0.02L / min-30L / min, and the atomizing gas pressure can be 2-5MPa. After the droplets are formed, the droplets can be cooled at a cooling rate of 80℃ / s-120℃ / s. Under the above conditions, fine particles with a particle size of 15 microns to 75 microns can be atomized to form a nickel-based alloy material according to the present application.

[0066] In other embodiments, another method for preparing a nickel-based alloy material is provided, wherein the nickel-based alloy material is formed by melting and smelting a mixture of nickel iron ore and auxiliary elements of raw materials.

[0067] During the process of melting and smelting the mixed material, the components are metallurgically combined to form the nickel-based alloy material according to the present application. Specifically, the atoms of the components diffuse in the melt to form a uniform solid solution or compound. The nickel-based alloy material formed by the above metallurgical combination process has excellent properties, such as high temperature strength, corrosion resistance and good processing performance.

[0068] It should be noted that the raw material nickel can be pure nickel or an alloy with a nickel content in the range of 20wt%-60wt%, and the raw material iron can be pure iron or an alloy with an iron content in the range of 92wt%-94wt%. For example, the raw material iron is a carbon-containing ferroalloy. The raw material auxiliary elements are corresponding metals or non-metals. The raw material nickel, raw material iron and raw material auxiliary elements are not formed into alloys in a molten state during the smelting process by simple physical blending, and then prepared into alloy powder by vacuum atomization as a nickel-based alloy material according to the present application. Nickel iron ore is the main nickel source and iron source. Nickel iron ore contains a certain amount of nickel and iron elements, which is the basis for forming nickel-based alloy materials.

[0069] In some embodiments, the nickel-based alloy material is in a granular form, and the particle size of the nickel-based alloy material is in the range of 15 microns to 75 microns, so as to ensure the compactness of the nickel-based alloy magnetic conductive layer formed by spraying. If the particle size of the nickel-based alloy material is below 15 microns, the utilization rate of the nickel-based alloy material will be low and the loss will be high; if the particle size of the nickel-based alloy material is above 75 microns, a higher power is required to melt the powder, which will cause the nickel-based alloy material to be overburned, affecting the bonding strength between the nickel-based alloy material and the metal substrate, and may also cause the nozzle and the electrode to be ablated.

[0070] Forming a nickel-based alloy magnetic conductive layer

[0071] According to the present application, the nickel-based alloy magnetic conductive layer according to the present application is formed by thermal spraying. Specifically, the thermal spraying is plasma spraying. As an example, the parameters of the plasma spraying include a main gas (argon) flow rate of 1200L / h-1800L / h, a secondary gas (hydrogen) flow rate of 80L / h-150L / h, a voltage of 55V-70V, and a current of 450A-550A.

[0072] The magnetic conductive layer is placed on the induction cooker. The induction cooker uses an alternating current to pass through the coil to generate an alternating magnetic field with a constantly changing direction. Eddy currents will appear inside the magnetic conductive layer in the alternating magnetic field. This is caused by the eddy electric field driving the movement of carriers in the conductor. The Joule heating effect of the eddy currents causes the magnetic conductive layer to heat up, thereby achieving heating. If the thickness of the magnetic conductive layer is too thin, due to the resistance of the conductor itself, the eddy currents formed are not enough to drive the movement of carriers in the magnetic conductive layer, so that the magnetic conductive layer cannot be heated on the induction cooker. A magnetic conductive layer that is too thin is magnetic, but cannot be used on an induction cooker. A magnetic conductive layer that is too thick has weak bonding and is easily damaged.

[0073] According to the present application, the thickness of the nickel-based alloy magnetic conductive layer is 40 microns to 90 microns. Such a thickness has excellent magnetic conductivity efficiency, good bonding strength and low stress with the cookware base, which can further extend the magnetic conductive life of the cookware. If the thickness of the nickel-based alloy magnetic conductive layer is too thin, it will lead to insufficient magnetic conductive power during use, which does not meet the standards for induction cooker trial pots, and the heating temperature of the pot body is not enough; if the thickness of the nickel-based alloy magnetic conductive layer is too thick, it will increase the stress between the nickel-based alloy magnetic conductive layer and the cookware base, affecting the bonding performance, and if the thickness of the magnetic conductive layer is too high, the heat transfer is too slow, which will affect the consumer experience.

[0074] Forming a protective layer

[0075] According to the present application, after the nickel-based alloy magnetic conductive layer is formed, a ceramic protective layer is formed on the outer surface of the nickel-based alloy magnetic conductive layer by air spraying ceramic coating.

[0076] In some embodiments, the ceramic coating may be a ceramic coating with methylsiloxane polymer as the main non-stick component, which can withstand a temperature higher than 250°C, specifically, within the temperature range of 250°C-650°C. In this way, a ceramic protective layer with good temperature resistance can be formed, which itself can withstand high temperatures to better protect the nickel-based alloy magnetic conductive layer.

[0077] In some embodiments, the protective layer is formed by air spraying of a ceramic coating. As an example, the parameters of the air spraying include a spraying distance of 140 mm to 180 mm; an air pressure of 0.2 MPa to 0.4 MPa; and a flow rate of 5 L / min to 10 L / min. After spraying, the cookware with the protective layer may also be sintered, specifically, sintered at a temperature of 200° C. to 300° C. for 8 minutes to 15 minutes, thereby forming a cookware with a nickel-based alloy magnetic conductive layer and a protective layer. The thickness of the protective layer may be in the range of 5 microns to 25 microns.

[0078] Creates a non-stick coating

[0079] According to the present application, after forming the nickel-based alloy magnetic conductive layer, a non-stick coating is formed on the inner surface of the cookware base body by spraying a non-stick coating. As an example, the non-stick coating is a fluorine coating or a ceramic coating.

[0080] In some embodiments, the non-stick coating is formed by air spraying of a ceramic coating. As an example, the parameters of the air spraying include a spraying distance of 140 mm to 180 mm, an air pressure of 0.2 MPa to 0.4 MPa, and a flow rate of 5 L / min to 10 L / min. After spraying, the cookware with the protective layer can also be sintered, specifically, sintered at a temperature of 200° C. to 300° C. for 8 minutes to 15 minutes, thereby forming a cookware with a non-stick coating on the inner surface of the cookware substrate. As an example, the thickness of the non-stick coating can be in the range of 40 microns to 90 microns, which can ensure the non-stick performance of the cookware.

[0081] According to a second aspect of the present application, a cooker is provided. Figure 1 It is a schematic cross-sectional structural diagram of a cooker provided according to an embodiment of the present application. Figure 2 yes Figure 1 The enlarged schematic diagram of point I in the figure. Figure 1 and Figure 2 As shown, the cooker includes a cooker body 10 and a nickel-based alloy magnetic conductive layer 20, the cooker body has the basic structure of a conventional cooker, and the nickel-based alloy magnetic conductive layer 20 is formed of a nickel-based alloy material at least on the outer surface of the bottom wall of the cooker body, wherein the Curie temperature of the nickel-based alloy material is in the range of 230° C.-300° C., and includes nickel, iron and auxiliary elements, wherein the auxiliary elements include at least two of cobalt, chromium, silicon, manganese, molybdenum, vanadium and copper.

[0082] In some embodiments, based on the total weight of the nickel-based alloy material being 100%, the weight of nickel accounts for 32.4%-33.4% of the total weight of the nickel-based alloy material, the weight of the auxiliary elements accounts for 7.2%-8.4% of the total weight of the nickel-based alloy material, and the remainder is iron. In this way, on the one hand, it is convenient to make the Curie temperature of the formed nickel-based alloy magnetic conductive layer within the range of 230°C-300°C, so that the temperature can be controlled when the cooker is used on an induction cooker and the influence of over-temperature on the cooker can be avoided; on the other hand, it can ensure that the nickel-based alloy magnetic conductive layer has sufficient corrosion resistance, hardness and wear resistance while satisfying the magnetic permeability, so that it is suitable as a magnetic conductive layer of a cooker with both high magnetic permeability and good mechanical properties.

[0083] In some embodiments, the auxiliary elements include silicon and cobalt, wherein the weight of silicon accounts for 0.2%-0.4% of the total weight of the nickel-based alloy material, and the weight of cobalt accounts for 7%-20% of the total weight of the nickel-based alloy material.

[0084] In these embodiments, the auxiliary elements include silicon and cobalt, and silicon mainly plays a role in improving corrosion resistance and oxidation resistance in nickel-based alloy materials. Although its content is relatively low, the addition of silicon can significantly improve the stability of nickel-based alloy materials in high temperature environments. In addition, silicon also helps to refine the grain structure of nickel-based alloy materials and improve the mechanical properties of nickel-based alloy materials. The addition of cobalt can significantly improve the high temperature resistance, corrosion resistance and hardness of the alloy. Cobalt can also enhance the magnetic properties of the alloy, especially maintaining good magnetism at high temperatures. In this way, the nickel-based alloy material can have good magnetic conductivity, high temperature resistance, corrosion resistance and mechanical strength while meeting the Curie temperature point of the present application.

[0085] In some other embodiments, the nickel-based alloy material also includes nickel, iron, manganese, silicon and chromium. Taking the total weight of the nickel-based alloy material as 100%, the weight of nickel accounts for 41.5%-42.5% of the total weight of the nickel-based alloy material, the weight of manganese accounts for 0.1%-0.4% of the total weight of the nickel-based alloy material, the weight of silicon accounts for 0.1%-0.3% of the total weight of the nickel-based alloy material, the weight of chromium accounts for 5.5%-6.3% of the total weight of the nickel-based alloy material, and the balance is iron.

[0086] In these embodiments, the auxiliary elements include manganese, silicon and chromium, and the content of manganese accounts for 0.1%-0.4% of the total weight of the nickel-based alloy material. Manganese plays a major role in deoxidation and desulfurization in the nickel-based alloy material, helps to reduce the content of impurity elements in the nickel-based alloy material, and improves the purity and performance of the nickel-based alloy material. At the same time, manganese can also enhance the strength and toughness of the nickel-based alloy material and improve its processing performance. Within this ratio range, the content of manganese is low enough to avoid adverse effects on the magnetic conductivity of the nickel-based alloy material, while playing its positive role. Silicon plays a major role in improving corrosion resistance and oxidation resistance in the nickel-based alloy material. Although its content is relatively low, the addition of silicon can significantly improve the stability of the nickel-based alloy material in a high temperature environment. In addition, silicon also helps to refine the grain structure of the nickel-based alloy material and improve the mechanical properties of the nickel-based alloy material. Chromium can form a dense oxide film with oxygen, covering the surface of the nickel-based alloy material, thereby protecting the nickel-based alloy material from erosion by the corrosive medium and significantly improving the corrosion resistance of the alloy. In this way, the nickel-based alloy material can have good magnetic conductivity, high temperature resistance, corrosion resistance and mechanical strength while meeting the Curie temperature point of the present application.

[0087] In some embodiments, the thickness of the nickel-based alloy magnetic conductive layer is between 40 microns and 90 microns. Within this range, various aspects such as magnetic conductive heating efficiency, cost, and stress can be balanced, and a higher magnetic conductive service life can be achieved. If the thickness of the nickel-based alloy magnetic conductive layer is too thin, the magnetic conductive heating efficiency is affected. If the thickness of the nickel-based alloy magnetic conductive layer is too thick, the cost is too high, stress is increased, and adhesion is reduced.

[0088] In some embodiments, the cooker body 10 includes a bottom wall 12 and a side wall 11 connected to the bottom wall 12, and has a certain magnetic permeability. In this case, the phosphorus alloy magnetic conductive layer can be formed at least on the outer surface of the bottom wall, so that the interference of the cooker body with the magnetic lines of force can be avoided, and the cooker that can meet the magnetic conductivity can be manufactured, the conduction efficiency of the magnetic lines of force can be improved, and the cooker can be ensured to be quickly and evenly heated. It should be noted that when the phosphorus alloy magnetic conductive layer only needs to be formed on part of the cooker body, for example, when only part of the bottom wall area needs to be formed, a coating can be used to cover the other bottom wall areas except for the part of the bottom wall area.

[0089] In some embodiments, the cooker further includes a ceramic protective layer 30 disposed outside the nickel-based alloy magnetic conductive layer, and the ceramic protective layer 30 is formed of a ceramic coating. In this way, the risk of the nickel-based alloy magnetic conductive layer being directly exposed to the outside and being damaged can be reduced, and the magnetic conductive life of the cooker can be further improved.

[0090] In some embodiments, the ceramic coating is a ceramic coating that can withstand temperatures higher than 250°C, specifically, a ceramic coating within the temperature range of 250°C-650°C. In this way, a ceramic protective layer with good temperature resistance can be formed, which itself can withstand high temperatures to better protect the nickel-based alloy magnetic conductive layer.

[0091] In some embodiments, the ceramic protective layer completely covers the nickel-based alloy magnetic conductive layer, specifically, covers the outer surface of the nickel-based alloy magnetic conductive layer, wherein the outer surface may be the side surface and the bottom surface of the nickel-based alloy magnetic conductive layer, thereby avoiding magnetic leakage or damage to the nickel-based alloy magnetic conductive layer.

[0092] According to the present application, the cookware includes a non-stick coating formed on the inner surface of the bottom wall of the cookware body, and thus, the cookware having non-stick performance is obtained.

[0093] In some embodiments, the non-stick coating is formed by spraying a fluorine coating or a ceramic coating, so that the cookware having the non-stick coating will have good non-stick properties; and / or the thickness of the non-stick coating is in the range of 40 microns to 90 microns, so that the non-stick coating has a suitable thickness to ensure the non-stick life of the cookware.

[0094] In an embodiment, the magnetic conductive layer of the cooker is circular, close to the coil diameter of the induction cooker, so as to ensure normal magnetic conductivity. In an exemplary embodiment, the diameter of the magnetic conductive layer is within a circular range of 11 cm-16 cm.

[0095] The above is a detailed description of the manufacturing method and cooker of the inventive concept in combination with exemplary embodiments. In the following, the beneficial effects of the inventive concept will be described in more detail in combination with specific embodiments, but the protection scope of the inventive concept is not limited to the embodiments.

[0096] Example 1

[0097] The cooker according to Example 1 was manufactured by the following method.

[0098] Step S10, providing a cooker base made of ceramic with a thickness of 3 mm.

[0099] Step S20, a nickel-based alloy material with an average particle size of 50 microns is plasma sprayed at least on the outer surface of the bottom wall of the cookware base to form a nickel-based alloy magnetic conductive layer with a thickness of 70 microns, wherein the nickel-based alloy material is composed of nickel, iron, silicon and cobalt, and the total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of silicon accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of cobalt accounts for 19.7% of the total weight of the nickel-based alloy material, and the balance is iron. Parameters of plasma spraying: main gas (argon) flow rate is 1500L / h, secondary gas (hydrogen) flow rate is 120L / h, voltage is 64V, and current is 520A.

[0100] Step S30, a protective layer with a thickness of 20 microns is formed on the outer side of the nickel-based alloy magnetic conductive layer by air spraying using a ceramic coating, wherein the parameters of the air spraying are a spraying distance of 160 mm, an air pressure of 0.3 MPa, and a flow rate of 8 L / min, thereby obtaining the cooker of Example 1.

[0101] Example 2

[0102] The cooker of Example 2 is manufactured by the same method as Example 1, except that in step S20, the thickness of the nickel-based alloy magnetic conductive layer is set to 40 microns.

[0103] Example 3

[0104] The cooker of Example 3 is manufactured by the same method as Example 1, except that in step S20, the thickness of the nickel-based alloy magnetic conductive layer is set to 90 microns.

[0105] Example 4

[0106] The cooker of Example 4 is manufactured by the same method as Example 1, except that in step S20, materials with different particle sizes are used to form a nickel-based alloy magnetic conductive layer with a thickness of 70 microns (the average particle size of the nickel-based alloy material in this embodiment is 15 microns).

[0107] Example 5

[0108] The cooker of Example 5 is manufactured in the same manner as Example 1, except that in step S20, materials with different particle sizes are used to form a nickel-based alloy magnetic conductive layer with a thickness of 70 microns (the average particle size of the nickel-based alloy material in this embodiment is 75 microns).

[0109] Example 6

[0110] The cooker of Example 6 is manufactured by the same method as Example 1, except that in step S30, the spraying thickness of the protective layer is 30 micrometers.

[0111] Example 7

[0112] The cooker of Example 7 is manufactured by the same method as Example 1, except that in step S30, the spraying thickness of the protective layer is 10 micrometers.

[0113] Example 8

[0114] The cooker of Example 8 is manufactured by the same method as Example 1, except that in step S10, a different material is used to form the cooker base (the material in this example is glass).

[0115] Example 9

[0116] The cooker of Example 9 is manufactured by the same method as Example 1, except that in step S10, a different material is used to form the cooker base (the material of this example is granite).

[0117] Example 10

[0118] Except that in step S20, different materials are used to form the nickel-based alloy magnetic conductive layer (the nickel-based alloy material of this embodiment includes nickel, iron, manganese, silicon, cobalt and chromium. Taking the total weight of the nickel-based alloy material as 100%, the weight of nickel accounts for 42% of the total weight of the nickel-based alloy material, the weight of manganese accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of silicon accounts for 0.2% of the total weight of the nickel-based alloy material, the weight of cobalt accounts for 7% of the total weight of the nickel-based alloy material, the weight of chromium accounts for 6% of the total weight of the nickel-based alloy material, and the balance is iron), the cooker of Example 10 is manufactured by the same method as Example 1.

[0119] Embodiment 11

[0120] The cooker of Example 11 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, silicon and molybdenum. Taking the total weight of the nickel-based alloy material as 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of silicon accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of molybdenum accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0121] Example 12

[0122] The cooker of Example 12 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, silicon and chromium. Taking the total weight of the nickel-based alloy material as 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of silicon accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of chromium accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0123] Example 13

[0124] The cooker of Example 13 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, silicon and vanadium. The total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of silicon accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of vanadium accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0125] Embodiment 14

[0126] The cooker of Example 14 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, silicon and copper. The total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of silicon accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of copper accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0127] Embodiment 15

[0128] The cooker of Example 15 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, silicon and manganese. The total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of silicon accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of manganese accounts for 19.7% of the total weight of the nickel-based alloy material, and the balance is iron).

[0129] Example 16

[0130] The cooker of Example 16 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, manganese and molybdenum. The total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of manganese accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of molybdenum accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0131] Embodiment 17

[0132] The cooker of Example 17 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, manganese and chromium. The total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of manganese accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of chromium accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0133] Embodiment 18

[0134] The cooker of Example 18 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, manganese and vanadium. The total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of manganese accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of vanadium accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0135] Embodiment 19

[0136] The cooker of Example 19 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, manganese and copper. The total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of manganese accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of copper accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0137] Embodiment 20

[0138] The cooker of Example 20 is manufactured in the same manner as in Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, manganese and cobalt. Taking the total weight of the nickel-based alloy material as 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of manganese accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of cobalt accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0139] Embodiment 21

[0140] The cooker of Example 21 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, chromium and molybdenum. With the total weight of the nickel-based alloy material as 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of chromium accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of molybdenum accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0141] Embodiment 22

[0142] The cooker of Example 22 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, chromium and cobalt. The total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of chromium accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of cobalt accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0143] Embodiment 23

[0144] The cooker of Example 23 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, chromium and vanadium. The total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of chromium accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of vanadium accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0145] Embodiment 24

[0146] The cooker of Example 24 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, chromium and copper. The total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of chromium accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of copper accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0147] Embodiment 25

[0148] The cooker of Example 25 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, cobalt and molybdenum. The total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of cobalt accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of molybdenum accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0149] Embodiment 26

[0150] The cooker of Example 26 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, cobalt and vanadium. The total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of cobalt accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of vanadium accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0151] Embodiment 27

[0152] The cooker of Example 27 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, cobalt and copper. The total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of cobalt accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of copper accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0153] Embodiment 28

[0154] The cooker of Example 28 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, molybdenum and vanadium. The total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of molybdenum accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of vanadium accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0155] Embodiment 29

[0156] The cooker of Example 29 is manufactured by the same method as in Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, molybdenum and copper. The total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of molybdenum accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of copper accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0157] Embodiment 30

[0158] The cooker of Example 30 is manufactured by the same method as Example 1, except that different materials are used to form the nickel-based alloy magnetic conductive layer in step S20 (the nickel-based alloy material of this embodiment includes nickel, iron, vanadium and copper. The total weight of the nickel-based alloy material is 100%, the weight of nickel accounts for 45% of the total weight of the nickel-based alloy material, the weight of vanadium accounts for 0.3% of the total weight of the nickel-based alloy material, the weight of copper accounts for 19.7% of the total weight of the nickel-based alloy material, and the remainder is iron).

[0159] Comparative Example 1

[0160] The cookware of Comparative Example 1 is manufactured in the same manner as in Example 1, except that in step S20, the magnetic conductive layer is formed in a different manner (in this comparative example, nickel particles with an average particle size of 50 microns are used to form a magnetic conductive layer with a thickness of 70 μm on the cookware substrate by the same plasma spraying method).

[0161] Comparative Example 2

[0162] The cookware of Comparative Example 2 is manufactured in the same manner as in Example 1, except that the magnetic conductive layer is formed in a different manner in step S20 (in this comparative example, iron particles with an average particle size of 50 microns are used to form a magnetic conductive layer with a thickness of 70 μm on the cookware substrate by the same plasma spraying method).

[0163] Comparative Example 3

[0164] Except that in step S20, the magnetic conductive layer is formed in a different manner (in this comparative example, a nickel-iron alloy with an average particle size of 50 μm is used to form a magnetic conductive layer with a thickness of 70 μm on the cookware substrate by the same plasma spraying method, wherein the nickel-iron alloy is 65 wt % nickel and 35 wt % iron), the cookware of comparative example 3 is manufactured by the same method as in embodiment 1. The Curie temperature of the cookware of comparative example 3 is measured to be 530° C.

[0165] Comparative Example 4

[0166] Except that in step S20, the magnetic conductive layer is formed in a different manner (in this comparative example, an alloy with an average particle size of 50 μm is used to form a magnetic conductive layer with a thickness of 70 μm on the cookware substrate by the same plasma spraying method, wherein the alloy is 45 wt % nickel and 55 wt % iron), the cookware of comparative example 4 is manufactured by the same method as in embodiment 1. The Curie temperature of the cookware of comparative example 4 is measured to be 500° C.

[0167] Comparative Example 5

[0168] The cooker of Comparative Example 5 is manufactured in the same manner as in Example 1, except that in step S20, the magnetic conductive layer is formed in a different manner (a stainless steel magnetic conductive sheet with a thickness of 450 μm is attached in this comparative example).

[0169] Performance index test

[0170] The performance of the cookers of Examples 1-30 and Comparative Examples 1-5 were tested using the following test methods, and the results are recorded in Table 1 below.

[0171] The magnetic permeability life, thermal shock resistance and impact resistance of the cookers prepared in the examples and comparative examples were tested.

[0172] The performance of the cookers of Examples 1-30 and Comparative Examples 1-5 was tested using the following test methods, and the results are recorded in Table 1 below:

[0173] (1) Test method and result determination of magnetic conductivity life

[0174] Boil water continuously under the heating power of 2100W in an induction cooker to detect the time it takes for the magnetic layer to be damaged by ablation, collapse, etc. This test time can reflect the magnetic life of the cooker. Generally, the test time of the cooker needs to reach more than 360 hours.

[0175] (2) Impact resistance performance and result judgment

[0176] A 500g steel ball is dropped vertically from a height of 0.3m to hit the magnetic layer of the cooker three times. If the magnetic layer is damaged, record the test height and result; if the magnetic layer is normal, increase the height by 0.5m each time until the magnetic layer is damaged, and record the test height and result. The higher the height, the better the impact resistance test performance, and vice versa.

[0177] (3) Thermal shock test method and judgment rules

[0178] Place the cooker in an oven at 250℃ for 30 minutes, then take it out and immediately immerse it in room temperature water (23±2℃), and repeat 20 times. Under this test condition, if there is no collapse, cracking or other damage, it is qualified; if there is collapse, cracking or other damage, it is unqualified.

[0179] Table 1 Performance index test data of the embodiments of the present application and the comparative examples

[0180]

[0181]

[0182] In summary, the cooker according to the embodiment of the present application has a longer magnetic conductivity life, and it can be seen from the impact resistance test and the heat and cold resistance test that the magnetic conductive layer of the cooker of the present application has a strong bonding force with the cooker body and is not easy to delaminate, thereby improving the user experience.

[0183] The cookers of Comparative Examples 1 to 4 have a nickel layer or an iron layer, so the magnetic conductive layer is easily damaged due to overheating, and thus the magnetic conductive life is short.

[0184] The cooker of Comparative Example 5 has been gradually eliminated from the market due to its poor bonding performance.

[0185] Although the embodiments of the present application have been described in detail above, those skilled in the art may make various modifications and variations to the embodiments of the present application without departing from the spirit and scope of the present application. However, it should be understood that, in the opinion of those skilled in the art, these modifications and variations will still fall within the spirit and scope of the embodiments of the present application defined by the claims.

Claims

1. A cooking utensil, characterized in that: The cooker comprises: A cooker body, wherein the cooker body is made of inorganic non-metallic silicate minerals; The nickel-based alloy magnetic conductive layer is formed at least on the bottom wall of the cooker body by a nickel-based alloy material, wherein the Curie temperature of the nickel-based alloy material is in the range of 230°C-300°C, and the nickel-based alloy material includes nickel, iron and auxiliary elements, wherein the auxiliary elements include at least two of cobalt, chromium, silicon, manganese, molybdenum, vanadium and copper.

2. The cooker according to claim 1, characterized in that: Taking the total weight of the nickel-based alloy material as 100%, the weight of the nickel accounts for 30%-50% of the total weight of the nickel-based alloy material, the weight of the auxiliary elements accounts for 5%-30% of the total weight of the nickel-based alloy material, and the weight of the iron accounts for 20%-45% of the total weight of the nickel-based alloy material.

3. The cooker according to claim 2, characterized in that: The auxiliary elements include silicon and cobalt, the weight of the silicon accounts for 0.2%-0.4% of the total weight of the nickel-based alloy material, and the weight of the cobalt accounts for 7%-20% of the total weight of the nickel-based alloy material.

4. The cooker according to claim 1, characterized in that: The nickel-based alloy material includes nickel, iron, manganese, silicon, cobalt and chromium. Taking the total weight of the nickel-based alloy material as 100%, the weight of the nickel accounts for 41.5%-42.5% of the total weight of the nickel-based alloy material, the weight of the manganese accounts for 0.1%-0.4% of the total weight of the nickel-based alloy material, the weight of the silicon accounts for 0.1%-0.3% of the total weight of the nickel-based alloy material, the weight of the cobalt accounts for 5%-9.5% of the total weight of the nickel-based alloy material, the weight of the chromium accounts for 5.5%-6.3% of the total weight of the nickel-based alloy material, and the balance is iron.

5. The cooker according to claim 1, characterized in that: The thickness of the nickel-based alloy magnetic conductive layer is 40 microns to 90 microns.

6. The cooker according to claim 1, characterized in that: The particle size of the nickel-based alloy material is 15 microns to 75 microns.

7. The cooker according to claim 1, characterized in that: The cooker further comprises a ceramic protective layer arranged outside the nickel-based alloy magnetic conductive layer, wherein the ceramic protective layer is formed by ceramic coating.

8. The cooker according to claim 7, characterized in that: The ceramic coating is a ceramic coating with a temperature tolerance range of 250°C to 650°C.

9. The cooker according to any one of claims 1 to 8, characterized in that: The auxiliary element also includes carbon. In the nickel-based alloy material, the weight proportion of the carbon is 0.01%-0.05%.

10. A method for manufacturing a cooker, characterized in that: The method comprises: Providing a cookware base, wherein the cookware base is made of inorganic non-metallic silicate minerals; The cookware is manufactured by spraying a nickel-based alloy material on at least the bottom wall of the cookware base to form a nickel-based alloy magnetic conductive layer, wherein the Curie temperature of the nickel-based alloy material is in the range of 230° C.-300° C., and the nickel-based alloy material includes nickel, iron and auxiliary elements, wherein the auxiliary elements include at least two of cobalt, chromium, silicon, manganese, molybdenum, vanadium and copper.

11. The method according to claim 10, characterized in that The nickel-based alloy material is formed by melting and smelting a mixture of raw material nickel, raw material iron and raw material auxiliary elements; or is formed by melting and smelting a mixture of raw material iron ore and raw material auxiliary elements.

12. The method according to claim 10, characterized in that Before forming the nickel-based alloy magnetic conductive layer, plasma surface treatment is performed on the cookware substrate to form a rough structure on the surface of the cookware substrate; and / or after forming the nickel-based alloy magnetic conductive layer, the method also includes forming a ceramic protective layer on the outer surface of the nickel-based alloy magnetic conductive layer by air spraying ceramic coating.