Cooker with graphite core
By adopting a solid-state combination technology of perforated graphite layer and multi-layer metal structure in the cookware, the problem of insufficient weight and thermal performance of the existing cookware is solved, and the lightweight and efficient heating effect of the cookware is achieved.
Patent Information
- Application Number
- CN202411090390.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2019-12-13
- Filing Date
- 2020-12-11
- Publication Date
- 2024-11-01
AI Technical Summary
There is room for improvement in the weight and thermal characteristics of existing multi-layer combined cookware, and traditional roll-in bonding technology is difficult to effectively reduce the weight of the cookware and improve its thermal performance.
Using solid-state combination technology of perforated graphite layer and multi-layer metal structure, metal layers such as aluminum and stainless steel are metallurgically combined through high pressure and high temperature, and using the high thermal conductivity of perforated graphite layer and the lightweight properties of aluminum, it has improved thermal performance and reduced Weight cookware.
The lightweight and improved thermal characteristics of the cookware are achieved, the heating speed and uniform heat distribution of the cooking surface are improved, the material cost is reduced, and the overall performance of the cookware is improved.
Smart Images

Figure CN118873013A_ABST
Abstract
Description
[0001] Related Applications
[0002] This application is a divisional application of the patent application with the application date of December 11, 2020, application number 202080086043.X, and invention name “Cookware with graphite core”.
[0003] CROSS-REFERENCE TO RELATED APPLICATIONS
[0004] This application claims priority to U.S. Application No. 16 / 714,120, filed on December 13, 2019, the entire disclosure of which is hereby incorporated by reference. Technical Field
[0005] The present disclosure relates generally to multi-layer bonded cookware, and more particularly to multi-layer bonded cookware having a perforated graphite core layer between at least two metal layers metallurgically bonded together. A method of making cookware using solid state bonding techniques is also disclosed. Background Art
[0006] It has long been known to make multi-layer bonded composite cookware, in which various materials are bonded together to combine the desired physical properties of each material into a composite. For example, the corrosion resistance of stainless steel is ideal for cooking surfaces and the outer surface of cookware, but the thermal conductivity of stainless steel is relatively low. On the other hand, aluminum and / or copper provide relatively higher thermal conductivity and have been bonded to stainless steel to provide well-known composite cookware products, such as pots, pans, etc. Multi-layer bonded cookware is known in the art, as shown in many patents, such as: U.S. Patents 4,246,045 and 4,167,606 to Ulam; and U.S. Patents 8,133,596 and 6,267,830 to Groll. These references illustrate the manufacture of multi-layer bonded cookware with a stainless steel outer layer bonded to an intermediate layer of aluminum and / or copper of higher conductivity. The bonding between these layers of different materials is usually achieved by conventional roll bonding techniques, using aluminum and / or copper strips that are roll bonded to stainless steel outer strips.
[0007] Groll et al., U.S. Pat. No. 9,078,539, discloses a solid state bonding technique that uses high static pressure and heat applied over time to produce multiple composite billets of a stainless steel-aluminum-stainless steel composition, such as in manufactured cookware. There is a continuing need in the art for producing cookware using improved solid state bonding techniques for reducing weight and improving the thermal properties of the cookware. Summary of the invention
[0008] In view of the present needs in the art, it is desirable to develop new methods for producing cookware using improved solid state bonding techniques. It is also desirable to provide cookware made by these methods, wherein the cookware has reduced weight and improved thermal properties compared to existing cookware made by solid state bonding techniques.
[0009] According to some embodiments or aspects of the present disclosure, a cookware made from a bonded multi-layer billet assembly may have a first metal layer; a second metal layer having a cavity with a plurality of spaced-apart posts protruding from a bottom surface of the cavity; and a perforated graphite layer having a thickness of at least 0.010 inches (0.254 mm) and a plurality of spaced-apart holes formed therethrough. The perforated graphite layer may be located within the cavity of the second metal layer such that the plurality of spaced-apart posts extend through the plurality of spaced-apart holes. The second metal layer may be metallurgically bonded to the first metal layer at least via the plurality of spaced-apart posts.
[0010] According to some embodiments or aspects of the present disclosure, the surface of the second metal layer surrounding the cavity can be metallurgically bonded to the first metal layer. Preferably, the surface is planar. The depth of the cavity can be less than, equal to, or greater than the thickness of the perforated graphite layer. The plurality of spaced-apart pillars can have a circular cross-section or a polygonal cross-section.
[0011] According to some embodiments or aspects of the present disclosure, the perforated graphite layer may be made of anisotropic graphite. The first metal layer may be made of aluminum, stainless steel, or titanium. The second metal layer may be made of aluminum.
[0012] According to some embodiments or aspects of the present disclosure, the third metal layer may be metallurgically bonded to a planar side of the second metal layer opposite the cavity. The third metal layer may be made of stainless steel.
[0013] According to some embodiments or aspects of the present disclosure, the second metal layer may have an outer metal layer and a central metal layer accommodated in a central opening of the outer metal layer. The cavity may be disposed on the central metal layer. The outer metal layer may be thinner than the central metal layer.
[0014] According to some embodiments or aspects of the present disclosure, the first metal layer may have a first sublayer made of aluminum bonded to the spaced-apart posts and a second sublayer made of stainless steel. The second metal layer may be metallurgically bonded to the first sublayer of the first metal layer. The surface of the second metal layer surrounding the cavity may be metallurgically bonded to the first sublayer of the first metal layer. Preferably, the surface is planar.
[0015] According to some embodiments or aspects of the present disclosure, a method for manufacturing cookware may include (a) providing a first metal layer; (b) providing a perforated graphite layer having a thickness of at least 0.010 inches (0.254 mm) and a plurality of spaced-apart holes formed therethrough, (c) providing a second metal layer having a cavity, wherein a plurality of spaced-apart pillars protrude from a bottom surface of the cavity; (d) stacking the layers provided in (a)-(c) in a billet assembly so that the perforated graphite layer is accommodated in the cavity of the second metal layer, whereby the plurality of spaced-apart pillars of the second metal layer are aligned with and pass through the plurality of spaced-apart holes in the perforated graphite layer so that the lower surface of the first metal layer at least contacts the upper surface of the upper ends of the plurality of spaced-apart pillars; and (e) pressing the billet assembly by applying a force in a direction perpendicular to the planes of the layers in the billet assembly, and simultaneously heating the billet assembly to achieve a metallurgical bond between the first metal layer and the second metal layer at least via the plurality of spaced-apart pillars, thereby providing a bonded billet assembly.
[0016] According to some embodiments or aspects of the present disclosure, the method may further include (f) cooling the bonded blank assembly; and (g) forming the bonded blank assembly into a cooker. The first metal layer may be made of aluminum, stainless steel or titanium, and the second metal layer may be made of aluminum.
[0017] According to some embodiments or aspects of the present disclosure, the method may also include (h) providing a third metal layer and stacking the third metal layer with the layers of the blank assembly before pressing the blank assembly so that the third metal layer faces the planar side of the second metal layer opposite to the cavity.
[0018] According to some embodiments or aspects of the present disclosure, the method may further include (i) providing a fourth metal layer, and stacking the fourth metal layer on the first metal layer of the blank assembly before pressing the blank assembly. The third metal layer and the fourth metal layer may be made of stainless steel.
[0019] These and other features and characteristics of the cookware described herein and methods of making such cookware will become more apparent after considering the following description and the appended claims with reference to the accompanying drawings, all of which form a part of this specification, wherein like reference numerals in the various drawings represent corresponding parts. However, it should be clearly understood that the drawings are for illustration and description purposes only. Therefore, specific dimensions and other physical characteristics related to the embodiments disclosed herein should not be considered limiting. In addition, it should be understood that the present disclosure may adopt various alternative variations and step sequences unless expressly stated to the contrary. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1is an exploded side cross-sectional view of a cooker for preparing a blank assembly according to some embodiments or aspects of the present disclosure;
[0021] Figure 2 yes Figure 1 An assembled side cross-sectional view of a blank assembly;
[0022] Figure 3 yes Figure 2 An enlarged view of detail A shown in;
[0023] Figure 4 yes Figure 1 A top view of the middle layer shown in
[0024] Figure 5 Is Figure 1 A cross-sectional view of a shaped frying pan formed from the combined blank components;
[0025] Figure 6 yes Figure 5 An enlarged view of detail B shown in;
[0026] Figure 7 yes Figure 5 An enlarged view of detail C shown in;
[0027] Figure 8 is an exploded side cross-sectional view of a cooker for preparing a blank assembly according to some embodiments or aspects of the present disclosure;
[0028] Fig. 9 yes Figure 8 An assembled side cross-sectional view of a blank assembly;
[0029] Fig.10 yes Fig. 9 An enlarged view of detail D shown in;
[0030] Fig.11 Is Figure 8 A cross-sectional view of a shaped frying pan formed from the combined blank components;
[0031] Fig.12 yes Fig.11 An enlarged view of detail E shown in;
[0032] Fig.13 yes Fig.11 An enlarged view of detail F shown in;
[0033] Fig.14 is an exploded side cross-sectional view of a cooker for preparing a blank assembly according to some embodiments or aspects of the present disclosure;
[0034] Fig.15 yes Fig.14 An assembled side cross-sectional view of a blank assembly;
[0035] Fig.16 yes Fig.15 An enlarged view of detail G shown in;
[0036] Fig.17 Is Fig.14 A cross-sectional view of a shaped frying pan formed from the combined blank components;
[0037] Fig.18 yes Fig.17 An enlarged view of detail H shown in;
[0038] Fig.19 yes Fig.17 an enlarged view of detail I shown in;
[0039] Fig. 20 is an exploded side cross-sectional view of a cooker for preparing a blank assembly according to some embodiments or aspects of the present disclosure;
[0040] Fig.21 yes Fig. 20 An assembled side cross-sectional view of the blank assembly; and
[0041] Fig. 22 yes Fig.21 An enlarged view of detail J shown in;
[0042] exist Figure 1-Figure 22 Unless otherwise specified, the same symbols denote the same components. DETAILED DESCRIPTION
[0043] As used in the specification and claims, the singular form "a," "an," and "the" include plural referents unless the context clearly dictates otherwise.
[0044] For the purpose of the following description, the terms "end", "upper", "lower", "right", "left", "vertical", "horizontal", "top", "bottom", "lateral", "longitudinal" and their derivatives shall be related to the orientation of the present disclosure in the accompanying drawings. However, it should be understood that the present disclosure may adopt various alternative variations and step sequences, unless expressly specified to the contrary.
[0045] All numbers and ranges used in the specification and claims should be understood as being modified in all cases by the term "about". "About" means plus or minus 25 percent of the value, for example plus or minus 10 percent of the value. However, this should not be considered as a limitation on any analysis of values under the doctrine of equivalents.
[0046] Unless otherwise indicated, all ranges or ratios disclosed herein are understood to include starting and ending values and any and all subranges or subratios contained therein. For example, the range or ratio "1 to 10" is considered to include any and all subranges or subratios between a minimum value of 1 and a maximum value of 10 (and including the end value); that is, all subranges or subratios starting with a minimum value of 1 or greater and ending with a maximum value of 10 or less. The ranges and / or ratios disclosed herein represent average values over the specified ranges and / or ratios.
[0047] Unless otherwise noted, all documents, such as but not limited to issued patents and patent applications, mentioned herein are considered to be "incorporated by reference" in their entirety.
[0048] The terms "first", "second", etc. are not intended to refer to any particular sequential or chronological order, but rather to different conditions, characteristics or elements.
[0049] The term "at least" is synonymous with "greater than or equal to."
[0050] As used herein, "at least one" is synonymous with "one or more". For example, the phrase "at least one of A, B, and C" refers to any one of A, B, or C, or any combination of any two or more of A, B, or C. For example, "at least one of A, B, and C" includes only one or more A; or only one or more B; or only one or more C; or one or more A and one or more B; or one or more A and one or more C; or one or more B and one or more C; or one or more all of A, B, and C.
[0051] The term "comprising" is synonymous with "including."
[0052] As used herein, the term "parallel" or "substantially parallel" refers to the relative angle between two objects, such as elongated objects and including a reference line, if extended to a theoretical intersection, i.e., 0° to 5°, or 0° to 3°, or 0° to 2°, or 0° to 1°, or 0° to 0.5°, or 0° to 0.25°, or 0° to 0.1, including the recited values.
[0053] As used herein, the terms "perpendicular" or "substantially perpendicular" means that the relative angle between two objects at their actual or theoretical intersection is 85° to 90°, or 87° to 90°, or 88° to 90°, or 89° to 90°, or 89.5° to 90°, or 89.75° to 90°, or 89.9° to 90°, inclusive of the recited values.
[0054] As used herein, the term "solid state bonding" refers to a process of bonding together two or more stacked layers of metals or metal alloys using high pressure (typically in excess of 5,000 psi (34.5 MPa)) and high temperature (typically in excess of 600°F (315°C)), wherein the high pressure is applied in a normal or perpendicular direction, i.e., at 90° relative to the plane of the stacked layers.
[0055] As used herein, the term "metallurgical bond" or "metallurgically bonded" refers to a bond formed between similar or dissimilar metallic materials that has no voids or discontinuities at the bonding surfaces.
[0056] With reference to the accompanying drawings, Figure 1-Figure 3 Various views of blank assemblies 100 for making some embodiments of cookware described in the present disclosure are shown. In some embodiments or aspects, each blank assembly 100 can be used to form a piece of cookware, such as Figure 5-Figure 7 . As described herein, the blank assembly 100 is formed by a plurality of stacked discs or layers that are metallurgically bonded together to form the integral blank assembly 100. In some embodiments or aspects, a plurality of stacked discs or layers may be stacked so that the individual discs are substantially parallel to each other. The stacked disc or layer assembly may then be bonded together using a solid-state bonding technique, wherein high pressure (typically in excess of 5,000 psi (34.5 MPa)) and high temperature (typically in excess of 600°F (315°C)) are used to bond the stacked discs or layers. Desirably, the high pressure is applied in a vertical direction, i.e., at 90° relative to the plane of the stacked discs or layers. The bonded discs or layers constitute a bonded multilayer blank assembly 100. Figure 2-Figure 3 A bonded multi-layer blank assembly 100 is shown.
[0057] Continue to refer Figure 1-Figure 3 , the blank assembly 100 has at least one upper (first) metal disk or layer 102 (hereinafter referred to as "first metal layer 102") and at least one lower (third) metal disk or layer 104 (hereinafter referred to as "third metal layer 104"). A second disk or layer 106 (hereinafter referred to as "second layer 106") is arranged between the first metal layer 102 and the third metal layer 104. The upper surface or top surface of the first metal layer 102 forms the inner surface of the cookware, and the lower surface or bottom surface of the third metal layer 104 forms the outer surface of the cookware. In some embodiments or aspects, the arrangement of the layers in the blank assembly 100 can be flipped 180° so that the lower surface or bottom surface of the first metal layer 102 forms the outer surface of the cookware, and the upper surface or top surface of the third metal layer 104 forms the inner surface of the cookware.
[0058] Continue to refer Figure 1-Figure 3, the material of the first metal layer 102 is selected to have the desired scratch resistance, wear resistance and thermal performance required for the cooking surface of the cooker. In some embodiments or aspects, the first metal layer 102 can be formed by food grade stainless steel. The stainless steel of the first metal layer 102 can be, for example, 400 series stainless steel, such as 436 stainless steel, or 300 series stainless steel, such as 304 stainless steel. In some embodiments or aspects, the stainless steel of the first metal layer 102 can be any corrosion-resistant stainless steel alloy suitable for use as a food preparation surface. In other embodiments or aspects, the first metal layer 102 can be made of a titanium alloy suitable for use as a food preparation surface. In other embodiments or aspects, the material of the first metal layer 102 can include aluminum. In some embodiments or aspects, the material of the first metal layer 102 can be, for example, high purity aluminum, or an alloy aluminum material coated with a thin pure aluminum layer on one or both sides to adapt to metallurgical bonding. In some embodiments or aspects, the material of the first metal layer 102 can be a 1000 series aluminum alloy, such as a 1100 aluminum alloy.
[0059] In some embodiments or aspects, the first metal layer 102 can be a disk having a diameter of about 14 inches (355.6 mm) to form a nearly net-sized blank having a diameter of 10 inches (254 mm) for making cookware (e.g., a frying pan). In other embodiments or aspects, the first metal layer 102 can be a disk having a diameter of about 5 inches to about 20 inches (127 mm to 508 mm) to form cookware of various sizes. The diameter of the first metal layer 102 is selected to be large enough to form the bottom, sidewalls, and edges of the finished cookware. The diameter of the first metal layer 102 is selected so that it matches the diameter of at least one of the second layer 106 and the third metal layer 104. In some embodiments or aspects, the thickness of the first metal layer 102 can be about 0.010 inches (0.25 mm) to about 0.025 inches (0.65 mm), for example, about 0.015 inches (0.40 mm). One of ordinary skill in the art will readily appreciate that the diameter and thickness of the first metal layer 102 may be increased or decreased to produce cookware with a larger or smaller diameter and thickness, respectively.
[0060] In some embodiments or aspects, for example Figure 20-Figure 22 As shown, the blank assembly 100 may include a fourth metal layer 140 stacked on the first metal layer 102. As discussed herein, the first metal layer 102 may be made of a material having a bonding affinity to the metal materials of the fourth metal layer 140 and the second layer 106. In further embodiments or aspects, the blank assembly 200, 300 (in Figure 8-Figure 10 and Figure 14-16202, 302) may also include a fourth metal layer (not shown) stacked on the first metal layer 202, 302. The material of the first metal layer 102, 202, 302 may be aluminum. In some embodiments or aspects, the material of the first metal layer 102, 202, 302 may be, for example, high-purity aluminum, or an alloy aluminum material coated with a thin pure aluminum layer on either side to accommodate metallurgical bonding. In some embodiments or aspects, the material of the first metal layer 102, 202, 302 may be a 1000 series aluminum alloy, such as a 1100 aluminum alloy. In some embodiments or aspects, the thickness of the first metal layer 102, 202, 302 may be about 0.020 inches (0.5 mm) to about 0.100 inches (2.5 mm), for example, about 0.040 inches (1.0 mm).
[0061] Continue to refer Figure 20-Figure 22 , the material of the fourth metal layer 140 is selected to have the desired scratch resistance, wear resistance and thermal properties required for the cooking surface of the cooker. In some embodiments or aspects, the material of the fourth metal layer 140 can be food grade stainless steel. The stainless steel of the fourth metal layer 140 can be, for example, 400 series stainless steel, such as 436 stainless steel, or 300 series stainless steel, such as 304 stainless steel. In some embodiments or aspects, the stainless steel of the fourth metal layer 140 can be any corrosion-resistant stainless steel alloy suitable for use as a food preparation surface. In other embodiments or aspects, the fourth metal layer 140 can be made of a titanium alloy suitable for use as a food preparation surface. In some embodiments or aspects, the thickness of the fourth metal layer 140 can be about 0.010 inches (0.25mm) to about 0.025 inches (0.65mm), for example about 0.015 inches (0.4mm).
[0062] In some embodiments or aspects, the third metal layer 104 can be made of a material having the desired scratch resistance, wear resistance and thermal properties required for the outer surface of the cookware. As discussed herein, the material of the third metal layer 104 is selected so that it has a binding affinity to the metal material of at least a portion of the second layer 106. In some embodiments or aspects, the third metal layer 104 can be made of ferromagnetic stainless steel, such as 400 grade stainless steel, so that the finished cookware is suitable for use on induction cooking equipment. The stainless steel of the third metal layer 104 can be, for example, magnetic grade stainless steel, such as 430 stainless steel. In some embodiments or aspects, the stainless steel of the third metal layer 104 can be any stainless steel alloy suitable for use as a food preparation surface. In other embodiments or aspects, the third metal layer 104 can be made of a titanium alloy suitable for use as a food preparation surface. The material of the third metal layer 104 can be selected to have a material property similar to or identical to the material property of the first metal layer 102.
[0063] In some embodiments or aspects, the third metal layer 104 can be a disk having a diameter of about 14 inches (355.6 mm) to form a nearly net-sized blank having a diameter of 10 inches (254 mm) for making cookware (e.g., a frying pan). In other embodiments or aspects, the third metal layer 104 can be a disk having a diameter of about 5 inches to about 20 inches (127 mm to 508 mm) to form cookware of various sizes. The diameter of the third metal layer 104 is selected to be large enough to form the bottom, sidewalls, and edges of the finished cookware. In some embodiments or aspects, the thickness of the third metal layer 104 can be about 0.010 inches (0.25 mm) to about 0.025 inches (0.6 mm), for example, about 0.015 inches (0.4 mm). It will be readily understood by those of ordinary skill in the art that the diameter and thickness of the third metal layer 104 can be increased or decreased to manufacture cookware of larger or smaller diameter and thickness, respectively. The bottom surface 124 of the third metal layer 104 may be substantially flat and without any protrusions or depressions.
[0064] Continue to refer Figure 1-Figure 3 , the second layer 106 is disposed between the first metal layer 102 and the third metal layer 104. The second layer 106 has a perforated graphite disk or layer 108 (hereinafter referred to as "perforated graphite layer 108") having a plurality of spaced-apart holes 114 formed therethrough. The second layer 106 also has a second metal disk or layer 110 (hereinafter referred to as "second metal layer 110") having a cavity 112 configured to accommodate the perforated graphite layer 108.
[0065] In some embodiments or aspects, the second metal layer 110 can be made of a material having a bonding affinity to the metal materials of the first metal layer 102 and the third metal layer 104, as discussed herein. The material of the second metal layer 110 can be aluminum. In some examples or aspects, the second metal layer 110 can be made of high purity aluminum or an alloy aluminum material coated with a thin pure aluminum layer on either side to accommodate metallurgical bonding. In some embodiments or aspects, the second metal layer 110 can be made of, for example, a 1000 series aluminum alloy, such as 1100 aluminum alloy.
[0066] In some embodiments or aspects, the second metal layer 110 can be a disk having a diameter of about 14 inches (355.6 mm) to form a nearly net-sized blank having a diameter of 10 inches (254 mm) for making cookware (e.g., a frying pan). In other embodiments or aspects, the second metal layer 110 can be a disk having a diameter of about 5 inches to about 20 inches (127 mm to 508 mm) to form cookware of various sizes. The diameter of the second metal layer 110 is selected to be large enough to form the bottom, sidewalls, and edges of the finished cookware. In some embodiments or aspects, the thickness of the second metal layer 110 can be about 0.020 inches (0.5 mm) to about 0.200 inches (5.0 mm), for example, about 0.040 inches (1.0 mm). It will be readily understood by those of ordinary skill in the art that the diameter and thickness of the second metal layer 110 can be increased or decreased to manufacture cookware of larger or smaller diameter and thickness, respectively. The bottom surface 126 of the second metal layer 110 may be substantially flat without any protrusions or depressions.
[0067] In some embodiments or aspects, the cavity 112 may have a circular shape having a diameter that is the same as or slightly larger than the diameter of the circular-shaped perforated graphite layer 108. For example, the cavity 112 may have a diameter of about 3 inches (76.2 mm) to about 12 inches (305 mm), such as about 7 inches (178 mm). The perforated graphite layer 108 may have a corresponding diameter that is about 90-99.9% of the diameter of the cavity 112. In other embodiments or aspects, the cavity 112 may have any desired geometry corresponding to the perforated graphite layer 108. The cavity 112 may have a depth (i.e., the distance that the cavity 112 is recessed relative to the upper surface 120 of the second metal layer 110) of about 0.010 inches (0.25 mm) to about 0.100 inches (2.5 mm), such as about 0.020 inches (0.5 mm). The cavity may have a uniform depth or a non-uniform depth, where the depth varies across at least a portion of the cavity 112. In some embodiments or aspects, the cavity 112 may be centered on the second metal layer 110 such that the cavity 112 and the second metal layer 110 share a common axis. One of ordinary skill in the art will readily appreciate that the diameter and depth of the cavity 112 may be increased or decreased to accommodate larger and thicker perforated graphite layers 108, respectively.
[0068] The second metal layer 110 has a plurality of upwardly protruding, spaced-apart pillars 116 (hereinafter referred to as “pillars 116”) in the cavity 112. The pillars 116 extend upward from a bottom surface 118 of the cavity 112 that is recessed relative to an upper surface 120 of the second metal layer 110. Figure 4As shown, the columns 116 can be arranged in an ordered array or randomly distributed within the cavity 112. For example, the columns 116 can be arranged in a circular array with equal or unequal spacing between adjacent columns 116. In various embodiments or aspects, the density of the columns 116 (i.e., the number of columns 116 per unit area) can be uniform across the cavity 112, or it can vary between different portions of the cavity. For example, the density of the columns 116 can increase or decrease in the radial direction of the cavity 112. In some embodiments or aspects, the columns 116 can be arranged in one or more groups of columns 116. The columns 116 can have the same size (i.e., diameter) or different sizes relative to each other.
[0069] refer to Figure 4 The cavity 112 and the pillar 116 can be formed by removing material from the upper surface 120 of the second metal layer 110, such as by milling. In some embodiments or aspects, a mold can be used to cast the cavity 112 and the pillar 116. The pillar 116 can have a circular cross-sectional shape, a polygonal shape (e.g., a hexagonal shape), or any other geometric shape.
[0070] In some embodiments or aspects, pillars 116 may have a height above bottom surface 118 of cavity 112 of about 0.010 inches (0.254 mm) to about 0.100 inches (2.54 mm), such as about 0.020 inches (0.508 mm). In some embodiments or aspects, the height of pillars 116 is selected to be slightly higher than the thickness of perforated graphite layer 108 so that the peaks of pillars 116 protrude through the holes in perforated graphite layer 108, as described herein. In embodiments or aspects where pillars 116 have a circular shape, pillars 116 may have a diameter of about 0.050 inches (1.27 mm) to about 0.250 inches (6.35 mm), such as about 0.125 inches (3.175 mm). In other embodiments or aspects where pillars 116 have a non-circular shape, pillars 116 may have a diameter of about 0.002 square inches (1.3 mm 2 ) to about 0.050 square inches (32mm 2 ), for example, about 0.12 square inches (7.9 mm 2 ). In some embodiments or aspects, the posts 116 can have a uniform width or diameter along their longitudinal length measured in a direction from the bottom surface 118 of the cavity 112 toward the upper surface 120. In other embodiments or aspects, the width or diameter of the posts can narrow or widen in a direction from the bottom surface 118 of the cavity 112 toward the upper surface 120.
[0071] In some embodiments or aspects, the perforated graphite layer 108 may be made of anisotropic graphite, which is configured to transfer thermal energy primarily in the radial (rather than axial) direction. In this way, the cooking surface can be heated evenly while avoiding hot spots. Graphite is preferably selected because it has a high thermal conductivity (about 500-1500 W / mK, while aluminum is about 220 W / mK and copper is about 340 W / mK). Anisotropic graphite has a thermal conductivity of about 2-6 times that of copper in the direction of the XY plane defining the cooking surface. Anisotropic graphite is also about 1 / 6 times the weight of copper and acts as an insulator in the Z direction (i.e., substantially perpendicular to the cooking surface) compared to copper. The low conductivity in the Z direction (about 100 times lower than in the XY plane) acts as a thermal barrier that temporarily blocks heat from the heat source from flowing directly through the food preparation surface, thereby giving the thermal energy additional time to spread evenly along the cooking surface. The perforated graphite layer 108 effectively spreads heat evenly over the cooking surface while resisting heat flow in a direction perpendicular to the cooking surface. Without being bound by theory, it has been found that the presence of the perforated graphite layer 108 increases resistance to electrical current, thereby increasing the effectiveness of induction heating compared to cookware without the perforated graphite layer 108.
[0072] In some embodiments or aspects, the perforated graphite layer 108 may have a circular shape with a diameter of about 3 inches (76.2 mm) to about 12 inches (305 mm), such as about 7 inches (178 mm). As described herein, the perforated graphite layer 108 may have a corresponding diameter of about 90-99.9% of the diameter of the cavity 112. In other embodiments or aspects, the perforated graphite layer 108 may have any desired geometry corresponding to the cavity 112. The perforated graphite layer 108 may have a thickness of about 0.010 inches (0.25 mm) to about 0.100 inches (2.5 mm), such as about 0.020 inches (0.5 mm). The perforated graphite layer 108 may have a minimum thickness of about 0.010 inches (0.25 mm). Without being bound by theory, it has been found that a perforated graphite layer 108 having a thickness less than the minimum thickness may be damaged during the solid state bonding process, thereby compromising its ability to evenly distribute heat along the cooking surface of the cookware. In addition, a perforated graphite layer 108 having at least the minimum thickness is easier to handle and cheaper to manufacture than a perforated graphite layer having less than the minimum thickness, thereby reducing the overall cost of the cookware. In addition, a perforated graphite layer 108 having at least the minimum thickness is configured to move more energy in a plane defining the cooking surface than a perforated graphite layer having less than the minimum thickness. In some embodiments or aspects, the thickness of the perforated graphite layer 108 is selected to be less than the height of the pillars 116 of the second metal layer 110. In this way, the upper surface of the perforated graphite layer 108 can be recessed within the cavity 112 relative to the upper surface 120 of the second metal layer 110 and the peaks of the pillars 116.
[0073] In some embodiments or aspects, the thickness of the perforated graphite layer 108 is selected to be less than the height of the pillars 116 of the second metal layer 110 / the depth of the cavity 112. In this way, the upper surface of the perforated graphite layer 108 can be recessed within the cavity 112 relative to the upper surface 120 of the second metal layer 110 and the peaks of the pillars 116. In other embodiments or aspects, the thickness of the perforated graphite layer 108 is selected to be the same as the height of the pillars 116 / the depth of the cavity 112. In further embodiments or aspects, the thickness of the perforated graphite layer 108 can be selected to be slightly greater than the height of the pillars 116 of the second metal layer 110 / the depth of the cavity 112. In this way, the upper surface of the perforated graphite layer 108 can protrude slightly from the cavity 112 relative to the upper surface 120 of the second metal layer 110 and the peaks of the pillars 116. Since perforated graphite layer 108 is more compressible than first metal layer 102 and second metal layer 110 , perforated graphite layer 108 is compressed into cavity 112 during the solid state bonding process.
[0074] Continue to refer Figure 1-Figure 3 , each hole 114 extends through the material between the upper surface and the lower surface of the perforated graphite layer 108. The size and arrangement of the holes 114 in the perforated graphite layer 108 are selected to correspond to the size and arrangement of the pillars 116 on the second metal layer 110. In this way, the pillars 116 can be arranged so that all of the pillars 116 are aligned (i.e., aligned) with all of the holes 114, wherein each pillar 116 is accommodated in a corresponding hole 114. For example, in an embodiment where the pillars 116 are arranged in a circular array and the pillars 116 have uniform spacing on the cavity 112 of the second metal layer 110, the holes 114 have a corresponding circular array arrangement so that the pillars 116 can be accommodated in the holes 114. The shape of the holes 114 is such that a single pillar 116 can be accommodated in a single hole 114. In some embodiments or aspects, multiple pillars 116 can be accommodated in a single hole 114. In further embodiments or aspects, the number of holes 114 may be greater than the number of posts 116 , such that some holes 114 do not have posts 116 therein.
[0075] The holes 114 can have the same or different shapes as the posts 116. For example, the holes 114 can have a circular shape to accommodate circular or non-circular posts 116. In embodiments or aspects where the holes 114 have a circular shape, the holes 114 can have a diameter of about 0.050 inches (1.27 mm) to about 0.250 inches (6.35 mm), such as about 0.125 inches (3.175 mm). The holes 114 can have the same or different sizes and shapes.
[0076] Reference Figure 8-Figure 10 , shows a blank assembly 200 according to another embodiment or aspect of the present disclosure. Figure 8-Figure 10 The components of the blank assembly 200 shown are similar to those described herein with reference Figure 1-Figure 3 The components of the blank assembly 100 are substantially similar. Figure 8-Figure 10 The reference numerals in the figure are used to illustrate the Figure 1-Figure 3 The same components as in the corresponding reference numerals are shown in the figure except that the first digit of each reference numeral is replaced by the number 2. For example, although Figure 1-Figure 3 The first metal layer shown in FIG. 1 is identified by reference numeral 102, but Figure 8-Figure 10 The same first metal layer shown in FIG. 1 is identified by reference numeral 202. Figure 1-Figure 3 The foregoing discussion of the components of the blank assembly 100 generally shown in FIG. Figure 8-Figure 10 The blank assembly 200 is shown in FIG. 2 , and therefore only the relative differences between the two blank assemblies are discussed below. Figure 9-10 A bonded multi-layer blank assembly 200 is shown.
[0077] refer to Figure 8-Figure 10 , the blank component 200 has at least one upper (first) metal disk or layer 202 (hereinafter referred to as "first metal layer 202") and at least one lower (second) metal disk or layer 210 (hereinafter referred to as "second metal layer 210"). A core disk or layer 206 (hereinafter referred to as "core layer 206") is disposed between the first metal layer 202 and the second metal layer 210. The upper surface or top surface of the first metal layer 202 forms the inner surface of the cookware, and the lower surface or bottom surface of the second metal layer 210 forms the outer surface of the cookware.
[0078] The first metal layer 202 may be made of food grade stainless steel, such as 400 series stainless steel, such as 436 stainless steel, or 300 series stainless steel, such as 304 stainless steel, or formed by a titanium alloy suitable for use as a food preparation surface. The material of the first metal layer 202 may be aluminum. In some embodiments or aspects, the first metal layer 202 may be formed of an alloy aluminum material coated with a thin pure aluminum layer on either side, to adapt to metallurgical bonding. In some embodiments or aspects, the first metal layer 202 may be made of, for example, a 1000 series aluminum alloy, such as a 1100 aluminum alloy. The material of the second metal layer 210 is selected so that it has a bonding affinity with the metal material of the first metal layer 202. The material of the second metal layer 210 may include aluminum. In some embodiments or aspects, the second metal layer 210 may be made of, for example, high purity aluminum or an alloy aluminum material coated with a thin pure aluminum layer on either side, to adapt to metallurgical bonding. In some embodiments or aspects, the second metal layer 210 may be made of, for example, a 1000 series aluminum alloy, such as a 1100 aluminum alloy. The bottom surface 224 of the second metal layer 210 may be substantially flat without any protrusions or depressions.
[0079] Continue to refer Figure 8-Figure 10, a core layer 206 is disposed between the first metal layer 202 and the second metal layer 210. The core layer 206 is a perforated graphite disk or layer 208 (hereinafter referred to as "perforated graphite layer 208") having a plurality of spaced-apart holes 214 formed therethrough. Figure 1-Figure 3 The second layer 106 in the embodiment has a second metal layer 110 and a perforated graphite layer 108 accommodated in a cavity 112 on the second metal layer 110, but Figure 8-Figure 10 The core layer 206 in the embodiment has only the perforated graphite layer 208 . The perforated graphite layer 208 is configured to be accommodated in a cavity 212 that is recessed relative to the upper surface 220 of the second metal layer 210 .
[0080] In some embodiments or aspects, the cavity 212 can have a circular shape having a diameter that is the same as or slightly larger than the diameter of the circular shaped perforated graphite layer 208. In other embodiments or aspects, the cavity 212 can have any desired geometry corresponding to the perforated graphite layer 208. In some embodiments or aspects, the cavity 212 can be centered on the second metal layer 210 such that the cavity 212 and the second metal layer 210 share a common axis.
[0081] Continue to refer Figure 8-Figure 10 , a plurality of spaced-apart pillars 216 (hereinafter referred to as "pillars 216") protrude upward from a bottom surface 218 of the cavity 212. Figure 4 Similar to the illustrated pillars 116, pillars 216 may be arranged in an ordered array or randomly distributed within cavity 212. Pillars 216 may have a circular cross-sectional shape, a polygonal shape (eg, a hexagonal shape), or any other geometric shape.
[0082] In some embodiments or aspects, the perforated graphite layer 208 may be made of anisotropic graphite that is configured to transfer thermal energy primarily in the radial (rather than axial) direction. In this way, the cooking surface may be heated evenly while avoiding hot spots. Figure 1-Figure 4As described in the embodiment shown in , the perforated graphite layer 208 may have a minimum thickness of about 0.010 inches (0.25 mm). Without being bound by theory, it has been found that a perforated graphite layer 208 having a thickness less than the minimum thickness may be damaged during the solid-state bonding process, thereby compromising its ability to evenly distribute heat along the cooking surface of the cookware. In addition, a perforated graphite layer 208 having at least the minimum thickness is easier to handle and cheaper to manufacture than a perforated graphite layer having less than the minimum thickness, thereby reducing the overall cost of the cookware. In addition, the perforated graphite layer 208 having at least the minimum thickness is configured to move more energy in a plane defining the cooking surface than a perforated graphite layer having less than the minimum thickness. In some embodiments or aspects, the thickness of the perforated graphite layer 208 is selected to be less than the height of the pillars 216 of the second metal layer 210 / the depth of the cavity 212. In this way, the upper surface of the perforated graphite layer 208 can be recessed within the cavity 212 relative to the upper surface 220 of the second metal layer 210 and the peaks of the pillars 216. In other embodiments or aspects, the thickness of the perforated graphite layer 208 is selected to be the same as the height of the pillars 216 / the depth of the cavity 212. In further embodiments or aspects, the thickness of the perforated graphite layer 208 can be selected to be slightly greater than the height of the pillars 216 of the second metal layer 210 / the depth of the cavity 212. In this way, the upper surface of the perforated graphite layer 208 can be slightly protruding from the cavity 212 relative to the upper surface 220 of the second metal layer 210 and the peaks of the pillars 216. Since the perforated graphite layer 208 is more compressible than the first metal layer 202 and the second metal layer 210, the perforated graphite layer 208 is compressed into the cavity 212 during the solid state bonding process.
[0083] Continue to refer Figure 8-Figure 10 , each hole 214 extends through the material between the upper surface and the lower surface of the perforated graphite layer 208. The size and arrangement of the holes 214 in the perforated graphite layer 208 are selected to correspond to the size and arrangement of the pillars 216 on the second metal layer 210. In this way, the pillars 216 can be arranged so that all of the pillars 216 are aligned (i.e., aligned) with all of the holes 214, wherein each pillar 216 is received in a corresponding hole 214. In some embodiments or aspects, multiple pillars 216 can be received in a single hole 214. In other embodiments or aspects, the number of holes 214 can be greater than the number of pillars 216, so that some holes 214 do not have a pillar 216. The hole 214 can have the same or different shape as the pillar 216.
[0084] Reference Figure 14-16 , shows a blank assembly 300 according to another embodiment or aspect of the present disclosure. Figure 14-16 The components of the blank assembly 300 shown are similar to those described herein with reference Figure 1-Figure 3 The components of the blank assembly 100 are substantially similar. Figure 14-16The reference numerals in the figure are used to illustrate the Figure 1-Figure 3 The same components as in the corresponding reference numerals are shown in the figure except that the first digit of each reference numeral is replaced by the number 3. For example, although Figure 1-Figure 3 The first metal layer shown in FIG. 1 is identified by reference numeral 102, but Figure 14-16 The same first metal layer shown in FIG. 1 is identified by reference numeral 302. Figure 1-Figure 3 The foregoing discussion of the components of the blank assembly 100 generally shown in FIG. Figure 14-16 The blank assembly 300 is shown in FIG. 1 , and therefore only the relative differences between the two blank assemblies are discussed below. Figure 15-16 A bonded multi-layer blank assembly 300 is shown.
[0085] refer to Figure 14-16 , the blank component 300 has at least one upper (first) metal disk or layer 302 (hereinafter referred to as "first metal layer 302") and at least one lower (third) metal disk or layer 304 (hereinafter referred to as "third metal layer 304"). A second disk or layer 306 (hereinafter referred to as "second layer 306") is disposed between the first metal layer 302 and the third metal layer 304. The upper surface or top surface of the first metal layer 302 forms the inner surface of the cookware, and the lower surface or bottom surface of the third metal layer 304 forms the outer surface of the cookware.
[0086] The first metal layer 302 can be made of food grade stainless steel, such as 400 or 436 series stainless steel, or formed by a titanium alloy suitable for use as a food preparation surface. As discussed herein, the material of the third metal layer 304 is selected so that it has a binding affinity to the metal material of at least a portion of the second layer 306. In some embodiments or aspects, the third metal layer 304 can be made of food grade stainless steel, such as 400 or 436 series stainless steel, or made of a titanium alloy. The material of the third metal layer 304 can include aluminum. In some embodiments or aspects, the material of the third metal layer 304 can be, for example, high purity aluminum, or an alloy aluminum material coated with a thin pure aluminum layer on either side to accommodate metallurgical bonding. In some embodiments or aspects, the material of the third metal layer 304 can be a 1000 series aluminum alloy, such as a 1100 aluminum alloy. The bottom surface 324 of the third metal layer 304 can be substantially flat, and without any protrusions or depressions.
[0087] Continue to refer Figure 14-16 , the second layer 306 is arranged between the first metal layer 302 and the third metal layer 304. Figure 1-Figure 3 The second layer 106 in the embodiment has a second metal layer 110 and a perforated graphite layer 108 accommodated in a cavity 112 of the second metal layer 110, but Figure 14-16The second layer 306 in the embodiment includes a second metal layer 310 and a perforated graphite disk or layer 308 (hereinafter referred to as "perforated graphite layer 308"). The second metal layer 310 has a central metal core disk or layer 310a (hereinafter referred to as "central metal layer 310a"), an annular outer core metal disk or layer 310b (hereinafter referred to as "outer metal layer 310b") surrounding the central metal layer 310a. The perforated graphite layer 308 is accommodated in a cavity 312 of the second metal layer 310. The cavity 312 is formed on the central metal layer 310a. The material of the outer metal layer 310a and / or the intermediate metal layer 310b may be aluminum. In some embodiments or aspects, the material of the outer metal layer 310a and / or the central metal layer 310b may be, for example, high purity aluminum, or an alloy aluminum material coated with a thin pure aluminum layer on either side to accommodate metallurgical bonding. In some embodiments or aspects, the material of the outer metal layer 310a and / or the central metal layer 310b may be a 1000 series aluminum alloy, such as 1100 aluminum alloy. Therefore, the material of the second metal layer 310 may be aluminum.
[0088] The outer metal layer 310b has a central opening 322, which is shaped to accommodate the central metal layer 310a therein. In some embodiments or aspects, the central opening 322 may have a circular shape, and its diameter is equal to or slightly larger than the diameter of the central metal layer 310a of the circular shape. For example, the central opening 322 may have a diameter of about 3 inches (76.2mm) to about 12 inches (305mm), such as about 7 inches (178mm). The thickness of the central metal layer 310a may be the same or different from the thickness of the outer metal layer 310b. For example, the central metal layer 310a may be thinner or thicker than the outer metal layer 310b. In some embodiments or aspects, the central metal layer 310a is thicker than the outer metal layer 310b (e.g., 0.004 inches (0.1mm) thick). In this way, the additional material of the central metal layer 310a can be compressed during solid-state bonding so that the upper and lower surfaces of the central metal layer 310a and the outer metal layer 310b are substantially planar. The compression of the additional material of the central metal layer 310a facilitates a stronger bond with the perforated graphite layer 308 during solid state bonding. The bottom surfaces 326a, 326b of the central metal layer 310a and the outer metal layers 310b may be substantially flat and without any protrusions or depressions.
[0089] Continue to refer Figure 14-16 , the cavity 312 can have a circular shape with a diameter equal to or slightly larger than the diameter of the circular perforated graphite layer 308. In other embodiments or aspects, the cavity 312 can have any desired geometry corresponding to the perforated graphite layer 308. In some embodiments or aspects, the cavity 312 can be centered on the central metal layer 310a such that the cavity 312 and the central metal layer 310a share a common axis.
[0090] Continue to refer Figure 14-16 , a plurality of spaced-apart pillars 316 (hereinafter referred to as "pillars 316") protrude upward from a bottom surface 318 of the cavity 312. Figure 4 Similar to the illustrated pillars 116, pillars 316 may be arranged in an ordered array or randomly distributed within cavity 312. Pillars 316 may have a circular cross-sectional shape, a polygonal shape (eg, a hexagonal shape), or any other geometric shape.
[0091] In some embodiments or aspects, the perforated graphite layer 308 has a plurality of spaced apart holes 314 formed therethrough. Each hole 314 extends through the material between the upper and lower surfaces of the perforated graphite layer 308. The size and arrangement of the holes 314 in the perforated graphite layer 308 are selected to correspond to the size and arrangement of the posts 316 on the central metal layer 310a. In this way, the posts 316 can be arranged so that all of the posts 316 are aligned (i.e., aligned) with all of the holes 314, wherein each post 316 is accommodated in a corresponding hole 314. In some embodiments or aspects, a plurality of posts 316 can be accommodated in a single hole 314. In other embodiments or aspects, the number of holes 314 can be greater than the number of posts 316, so that some of the holes 314 do not have posts 316. The holes 314 can have the same or different shapes as the posts 316.
[0092] The perforated graphite layer 308 may be made of anisotropic graphite that is configured to transfer thermal energy primarily in a radial (rather than axial) direction. In this way, the cooking surface can be heated evenly while avoiding hot spots. As described herein, the perforated graphite layer 308 may have a minimum thickness of about 0.010 inches (0.25 mm). Without being bound by theory, it has been found that a perforated graphite layer 308 having a thickness less than the minimum thickness may be damaged during the solid-state bonding process, thereby compromising its ability to evenly distribute heat along the cooking surface of the cookware. In addition, a perforated graphite layer 308 having at least the minimum thickness is easier to handle and cheaper to manufacture than a perforated graphite layer having a smaller thickness, thereby reducing the overall cost of the cookware. In addition, the perforated graphite layer 308 having the minimum thickness is configured to move more energy in the plane defining the cooking surface than a perforated graphite layer having a smaller thickness. In some embodiments or aspects, the thickness of the perforated graphite layer 308 is selected to be less than the height of the pillars 316 of the central metal layer 310a. In this way, the upper surface of the perforated graphite layer 308 can be recessed within the cavity 312 relative to the upper surface 320 of the central metal layer 310a and the peaks of the pillars 316. In other embodiments or aspects, the thickness of the perforated graphite layer 308 is selected to be the same as the height of the pillars 316 / the depth of the cavity 312. In further embodiments or aspects, the thickness of the perforated graphite layer 308 can be selected to be slightly greater than the height of the pillars 316 of the second metal layer 310 / the depth of the cavity 312. In this way, the upper surface of the perforated graphite layer 308 can protrude slightly from the cavity 312 relative to the upper surface 320 of the second metal layer 310 and the peaks of the pillars 316. Since perforated graphite layer 308 is more compressible than first metal layer 302 and second metal layer 310 , perforated graphite layer 308 is compressed into cavity 312 during the solid state bonding process.
[0093] Having described the structure of the blank assembly 100, 200, 300 according to various embodiments or aspects of the present disclosure, the method of manufacturing cookware using the bonded multi-layer blank assembly 100, 200, 300 will now be described. Before bonding, the layers of the blank assembly 100, 200, 300 undergo appropriate surface treatment steps, such as degreasing, surface abrasion by chemical or mechanical methods, etc. After appropriate surface preparation, unbonded blank assemblies 100, 200, 300 are formed by stacking the layers on each other. Desirably, the layers are aligned so that the centers of the layers share a common axis. In some embodiments or aspects, the layers can be stacked so that their centers are offset from each other. For manufacturing efficiency, multiple unbonded blank assemblies 100, 200, 300 can be stacked on top of each other with or without spacer layers between adjacent blank assemblies 100, 200, 300.
[0094] exist Figure 1-Figure 3In the case of the blank assembly 100 shown, the second layer 106 is stacked on the upper surface of the third metal layer 104. The perforated graphite layer 108 of the second layer 106 is arranged in the cavity 112 of the second metal layer 110 so that the holes 114 in the perforated graphite layer 108 are aligned with the pillars 116 in the cavity 112. When the pillars 116 are received in the holes 114 of the perforated graphite layer 108, the peaks of the pillars 116 are configured to be at the same height or extend above the upper surface of the perforated graphite layer 108. The first metal layer 102 is stacked above the second layer 106 so that the lower surface of the first metal layer 102 is opposite to the upper surfaces of the second metal layer 110 and the perforated graphite layer 108. When stacked, the first metal layer 102, the second layer 106, and the third metal layer 104 are substantially parallel to each other. For manufacturing efficiency, multiple unbonded blank assemblies 100 can be stacked on top of each other with or without spacer layers between adjacent blank assemblies 100.
[0095] exist Figure 8-Figure 10 In the case of the billet assembly 200 shown, the core layer 206 (i.e., the perforated graphite layer 208) is disposed within the cavity 212 of the second metal layer 210 such that the holes 214 in the perforated graphite layer 208 are aligned with the pillars 216 in the cavity 212. When the pillars 216 are received within the holes 214 of the perforated graphite layer 208, the peaks of the pillars 216 are configured to be at the same height or extend above the upper surface of the perforated graphite layer 208. The first metal layer 202 is stacked over the core layer 206 and the second metal layer 210 such that the lower surface of the first metal layer 202 is positioned opposite the upper surface 220 of the second metal layer 210 and the perforated graphite layer 208. When stacked, the upper metal layer 22, the perforated graphite layer 208, and the second metal layer 210 are substantially parallel to each other.
[0096] exist Figure 14-16 In the case of the blank assembly 300 shown, the central metal layer 310a and the outer metal layer 310b are positioned on the upper surface of the third metal layer 304 such that the central metal layer 310a is received within the central opening 322 of the outer metal layer 310b. The perforated graphite layer 308 is disposed within the cavity 312 of the central metal layer 310a such that the holes 314 in the perforated graphite layer 308 are aligned with the posts 316 in the cavity 312. When the posts 316 are received within the holes 314 of the perforated graphite layer 308, the peaks of the posts 316 are configured to be at the same height or extend above the upper surface of the graphite layer 308. The first metal layer 302 is stacked over the second layer 306 (i.e., the central metal layer 310a, the outer metal layer 310b, and the perforated graphite layer 308) such that the lower surface of the first metal layer 302 is positioned opposite the upper surfaces of the central metal layer 310a, the outer metal layer 310b, and the perforated graphite layer 108. When stacked, the first metal layer 302, the second layer 306, and the third metal layer 304 are substantially parallel to each other.
[0097] The blank assembly 100, 200, 300 or a plurality of stacked blank assemblies 100, 200, 300 are then placed in a press apparatus (not shown) to apply a load or pressure in a normal or perpendicular direction relative to the plane of the layers in the blank assembly 100, 200, 300 via a solid state bonding technique. The solid state bonding technique of bonding pre-cut near net shape sheet blanks not only reduces the waste losses encountered in conventional roll bonding to date in the manufacture of composite cookware, but also allows the use of other materials to manufacture multiple composite materials, which have proven to be difficult, impossible and / or expensive for roll bonding. For example, solid state bonding allows the use of stainless steel of a different grade than other possible stainless steel in conventional roll bonding in order to reduce material costs. In addition, solid state bonding also allows encapsulation of materials such as graphite, which otherwise cannot be bonded to stainless steel.
[0098] Heat is applied to the one or more billet assemblies 100, 200, 300 at between about 500°F and 1,000°F (260-538°C) while under a pressure between 5,000 and 20,000 psi (34.5-137.9 MPa) for a sufficient time (about 1-4 hours) to achieve a solid state bond (i.e., a metallurgical bond) between the metal layers in the one or more billet assemblies 100, 200, 300. During the solid state bonding process, air that may be present between the pillars of the core metal layer and the perforated graphite layer due to the size difference between the core metal layer and the perforated graphite layer is pressed out of the billet assemblies 100, 200, 300.
[0099] exist Figure 1-Figure 3 In the case of the blank assembly 100 shown, during the solid state bonding process, the lower surface of the second metal layer 110 is metallurgically bonded to the upper surface of the third metal layer 104. The upper surface of the second metal layer 110 and the posts 116 are metallurgically bonded to the lower surface of the first metal layer 102. The perforated graphite layer 108 is completely encapsulated between the second metal layer 110 and the first metal layer 102, wherein the cavity 112 of the second metal layer 110 completely surrounds the perforated graphite layer 108 on its lower and side sides, and the first metal layer 102 surrounds its upper side.
[0100] Each blank assembly 100, 200, 300 is then removed from the press apparatus and allowed to cool. In some embodiments or aspects, cooling can be achieved by exposure to ambient air or by using a coolant, such as forced air or liquid.
[0101] After solid state bonding, the bonded blank assembly 100, 200, 300 is formed into the desired shape of the cookware 400 in a draw press, spin forming or hydroforming machine (not shown), for example Figure 5-Figure 7 , Figure 11-13 and Figure 17-Figure 194. While the bonded blank assembly 100, 200, 300 may be oriented so that the first metal layer 102, 202, 302 forms the inner surface of the cookware 400 and the second metal layer 210 or the third metal layer 104, 304 forms the outer surface of the cookware 400, the bonded blank assembly 100, 200, 300 may be flipped 180° so that the first metal layer 102, 202, 302 forms the outer surface of the cookware 400 and the second metal layer 210 or the third metal layer 104, 304 forms the inner surface of the cookware 400. The cookware 400 has a substantially flat cooking surface 402, and a raised sidewall 404 surrounding and protruding vertically above the cooking surface 402. The sidewall 404 has a rounded portion 406 connected to the cooking surface 402 and an edge 408 at its free end. One or more handles (not shown) may be connected to the cookware in a known manner. In further embodiments or aspects, a non-stick coating can be applied to the cooking surface 402 of the cookware 400. Due to the use of lightweight graphite and aluminum materials, the cookware 400 formed using the blank assembly 100, 200, 300 described herein has a reduced weight compared to conventional cookware, for example, about 30% less weight. In addition, because the perforated graphite layer promotes increased heating speed and uniform heat distribution on the cooking surface, the cookware 400 has improved performance compared to conventional cookware.
[0102] In various embodiments, the present disclosure may be further characterized by one or more of the following clauses:
[0103] Clause 1. A cookware 400 made from a bonded multi-layer billet assembly 100; 200; 300, the cookware 400 comprising: a first metal layer 102; 202; 302; a second metal layer 110; 210; 310 having a cavity 112; 212; 312 having a plurality of spaced-apart posts 116; 216; 316 protruding from a bottom surface 118; 218; 318 of the cavity 112; 212; 312; and a perforated graphite layer 108; 208; 308 having a thickness of at least 0.010 inch (0. 254mm) thickness and a plurality of spaced-apart holes 114; 214; 314, wherein the perforated graphite layer 108; 208; 308 is positioned within the cavity 112; 212; 312 of the second metal layer so that a plurality of spaced-apart posts 116; 216; 316 extend through the plurality of spaced-apart holes 114; 214; 314, and wherein the second metal layer 110; 210; 310 is metallurgically bonded to the first metal layer 102; 202; 302 at least via the plurality of spaced-apart posts 116; 216; 316.
[0104] Clause 2. The cookware 400 of clause 1, wherein a surface of the second metal layer 110; 210; 310 surrounding the cavity 112; 212; 312 is metallurgically bonded to the first metal layer 102; 202; 302, said surface preferably being planar.
[0105] Clause 3. The cookware 400 of clause 1 or 2, wherein the depth of the cavity 112; 212; 312 is equal to or greater than the thickness of the perforated graphite layer 108; 208; 308.
[0106] Clause 4. The cooker 400 of any of Clauses 1-3, wherein the plurality of spaced-apart posts 116; 216; 316 have a circular cross-section or a polygonal cross-section.
[0107] Clause 5. The cookware 400 of any of Clauses 1-4, wherein the perforated graphite layer 108; 208; 308) is made of anisotropic graphite.
[0108] Clause 6. The cookware 400 of any of Clauses 1-5, wherein the perforated graphite layer 108; 208; 308 has a thickness between 0.010 inches (0.25 mm) and 0.100 inches (2.5 mm).
[0109] Clause 7. The cookware 400 of any of Clauses 1-6, wherein the first metal layer 102; 202; 302 is made of aluminum.
[0110] Clause 8. The cookware 400 of clause 7, wherein the aluminum is 1100 alloy.
[0111] Clause 9. The cookware 400 of any of Clauses 1-6, wherein the first metal layer 102; 202; 302 is made of stainless steel.
[0112] Clause 10. The cookware 400 of any of Clauses 1-6, wherein the first metal layer 102; 202; 302 is made of titanium.
[0113] Clause 11. The cookware 400 of any of Clauses 1-10, wherein the second metal layer 110; 210; 310 is made of titanium.
[0114] Clause 12. The cookware 400 of any of Clauses 1-11, further comprising a third metal layer 104;304 metallurgically bonded to a planar side of the second metal layer 110;310 opposite the cavity 112;312.
[0115] Clause 13. The cookware 400 of Clause 12, wherein the third metal layer 104; 304 is made of aluminum.
[0116] Clause 14. The cookware 400 of clause 13, wherein the aluminum is 1100 alloy.
[0117] Clause 15. The cookware 400 of Clause 12, wherein the third metal layer 104; 304 is made of stainless steel.
[0118] Clause 16. The cookware 400 of Clause 15, wherein the stainless steel is a ferromagnetic grade of stainless steel.
[0119] Clause 17. The cookware 400 of Clause 12, wherein the third metal layer 104; 304 is made of titanium.
[0120] Clause 18. The cookware 400 of any of Clauses 9-17, wherein the second metal layer 310 includes an outer metal layer 310a and a central metal layer 310b received within the central opening 322 of the outer metal layer 310a, and wherein the cavity 312 is disposed on the central metal layer 310b.
[0121] Clause 19. The cookware 400 of Clause 18, wherein the outer metal layer 310a is thinner than the central metal layer 310b.
[0122] Clause 20. The cookware 400 of any of Clauses 1-19, wherein the first metal layer 102 comprises a first sublayer 102a made of aluminum and a second sublayer 102b made of stainless steel, the first sublayer 102a being metallurgically bonded to the spaced-apart posts 116 .
[0123] Clause 21 . The cookware of claim 20 , wherein the second metal layer 110 is metallurgically bonded to the first sublayer 102 a of the first metal layer 102 .
[0124] Clause 22. The cookware 400 of Clause 20, wherein a surface of the second metal layer 110 surrounding the cavity 112 is metallurgically bonded to the first sublayer 102a of the first metal layer 102, said surface preferably being planar.
[0125] Clause 23. The cookware 400 of any of Clauses 1-22, wherein the second metal layer 112; 212; 312 is metallurgically bonded to the planar lower surface of the first metal layer 102; 202; 302.
[0126] Clause 24. The cookware 400 of any of Clauses 1-23, wherein the bottom surface of the second metal layer 110; 210; 310 is planar.
[0127] Clause 25. A method of making a cookware 400, the method comprising: (a) providing a first metal layer 102; 202; 302; (b) providing a perforated graphite layer 108; 208; 308 having a thickness of at least 0.010 inches (0.254 mm) and a plurality of spaced-apart holes 114; 214; 314 formed therethrough, (c) providing a second metal layer 110; 210; 314 having cavities 112; 212; 312 0, wherein a plurality of spaced-apart pillars protrude from a bottom surface 118; 218; 318 of the cavity 112; 212; 312; (d) stacking the layers provided in (a)-(c) in a blank assembly 100; 200; 300 such that the perforated graphite layer 108; 208; 308 is received within the cavity 112; 212; 312 of the second metal layer 110; 210; 310, whereby a plurality of spaced-apart pillars of the second metal layer 110; 210; 310 protrude from a bottom surface 118; 218; 318 of the cavity 112; 212; 312 The plurality of spaced-apart pillars 116; 216; 316 are aligned with and pass through the plurality of spaced-apart holes 114; 214; 314 in the perforated graphite layer 108; 208; 308, so that the lower surface of the first metal layer 102; 202; 302 at least contacts the upper surface of the upper end portions of the plurality of spaced-apart pillars 116; 216; 316; and (e) by passing the plurality of spaced-apart holes 114; 214; 314 in a direction perpendicular to the billet assembly 100 ; 200; 300, applying force in the direction of the plane of the layers in the blank assembly 100; 200; 300, and simultaneously heating the blank assembly 100; 200; 300 to achieve a metallurgical bond between the first metal layer 102; 202; 302 and the second metal layer 110; 210; 310 via at least a plurality of spaced-apart columns 116; 216; 316, thereby providing a bonded multilayer blank assembly 100; 200; 300.
[0128] Clause 26. The method of Clause 25, further comprising: (f) cooling the bonded multi-layer blank assembly 100; 200; 300; and (g) forming the bonded multi-layer blank assembly 100; 200; 300 into a cooker 400.
[0129] Clause 27. The method of clause 25 or 26, wherein the first metal layer 102; 202; 302 is made of aluminum or stainless steel or titanium, and wherein the second metal layer 110; 210; 310 is made of aluminum.
[0130] Item 28. The method of any one of Items 25-27 further includes: (h) providing a third metal layer 104; 304, and stacking the third metal layer 104; 304 with other layers of the blank assembly 100; 300 before pressing the blank assembly 100; 300, so that the third metal layer 104; 304 faces the planar side of the second metal layer 110; 310 opposite to the cavity 114; 314.
[0131] Clause 29. The method of Clause 28, further comprising: (i) providing a fourth metal layer, and stacking the fourth metal layer over the first metal layer of the blank assembly before pressing the blank assembly.
[0132] Clause 30. The method of Clause 29, wherein the third metal layer and the fourth metal layer are made of stainless steel.
[0133] Item 31. Cookware made from a bonded multi-layer billet assembly, the cookware comprising: a first metal layer; a lower metal layer; and a core disposed between the first metal layer and the lower metal layer, the core comprising: a core metal layer made of aluminum, the core metal layer having a cavity with a plurality of spaced-apart posts protruding from a bottom surface of the cavity; and a perforated graphite layer having a plurality of spaced-apart holes formed therethrough, wherein the graphite layer is positioned in the cavity of the core metal layer such that the plurality of posts extend through the plurality of holes, and wherein the core metal layer is metallurgically bonded to the first metal layer at least via the plurality of posts, and to the second metal layer via the bottom surface of the core metal layer.
[0134] Clause 32. The cookware of Clause 31, wherein an upper surface of the core metal layer surrounding the cavity is metallurgically bonded to the first metal layer.
[0135] Clause 33. The cookware of clause 31 or 32, wherein the depth of the cavity is less than, equal to, or greater than the thickness of the graphite layer.
[0136] Clause 34. The cookware of any of Clauses 31-33, wherein the core metal layer is metallurgically bonded to the planar lower surface of the first metal layer.
[0137] Clause 35. The cooker of any of Clauses 31-34, wherein the plurality of posts have a circular cross-section.
[0138] Clause 36. The cooker of any of Clauses 31-35, wherein the plurality of posts have a polygonal cross-section.
[0139] Clause 37. The cookware of any of Clauses 31-36, wherein the bottom surface of the core metal layer is planar.
[0140] Clause 38. The cookware of any of Clauses 31-37, wherein the core metal layer comprises an outer core metal layer and a central core metal layer received within the central opening of the outer core metal layer.
[0141] Clause 39. The cookware of Clause 38, wherein the outer core metal layer has the same thickness as the central core metal layer.
[0142] Clause 40. The cookware of Clause 39, wherein the core metal layer has a smaller thickness than the central core metal layer.
[0143] Clause 41. The cookware of any of Clauses 31-40, wherein the first metal layer is made of stainless steel or titanium.
[0144] Clause 42. The cookware of Clause 41, wherein the stainless steel is a ferromagnetic grade of stainless steel.
[0145] Clause 43. The cookware of any of Clauses 31-42, wherein the lower metal layer is made of stainless steel or titanium.
[0146] Clause 44. The cookware of Clause 43, wherein the stainless steel is a ferromagnetic grade of stainless steel.
[0147] Clause 45. The cookware of any of Clauses 31-44, wherein the core metal layer is made of aluminum.
[0148] Clause 46. The cookware of clause 45, wherein the aluminum is 1100 alloy.
[0149] Clause 47. The cookware of any of Clauses 31-46, wherein the graphite layer is made of anisotropic graphite.
[0150] Clause 48. The cookware of any of Clauses 31-47, wherein the first metal layer comprises a first sublayer made of aluminum and a second sublayer made of stainless steel.
[0151] Clause 49. The cookware of Clause 48, wherein the core metal layer is metallurgically bonded to the first sublayer of the first metal layer.
[0152] Clause 50. The cookware of any of Clauses 31-51, wherein the graphite layer has a thickness between 0.010 inches (0.25 mm) and 0.100 inches (2.5 mm).
[0153] Clause 51. A method of manufacturing a cookware, the method comprising: (a) providing an upper metal disk of stainless steel; (b) providing a perforated graphite disk having a plurality of spaced-apart holes formed therethrough, (c) providing a core metal disk of aluminum having a cavity, wherein a plurality of spaced-apart posts protrude from a bottom surface of the cavity; (d) providing a lower metal disk of stainless steel; (e) stacking the disks provided in steps (a)-(d) in a blank assembly such that the graphite disk is received within the cavity of the core metal disk, whereby a plurality of posts in the core metal disk are aligned with and extend through a plurality of holes in the graphite disk, wherein the plurality of posts have upper end portions extending beyond an upper surface of the graphite disk, such that a lower surface of the upper metal disk contacts an upper surface of an outer portion of the core metal disk and upper end portions of the plurality of posts; and (f)
[0154] The blank assembly is pressed by applying a force in a direction perpendicular to the plane of the disks in the blank assembly, and the blank assembly is heated simultaneously to achieve a metallurgical bond between the metal materials of the disks in the blank assembly to provide a bonded blank assembly.
[0155] Clause 52. The method of Clause 51, further comprising: (g) cooling the bonded blank assembly; and (h) forming the bonded blank assembly into a cookware.
[0156] Item 53. A cookware made from a bonded multi-layer billet assembly, the cookware comprising: a first metal layer; a lower metal layer having a cavity, wherein a plurality of spaced-apart posts protrude from said bottom surface; and a perforated graphite layer, the perforated graphite layer having a plurality of spaced-apart holes formed therethrough; wherein the graphite layer is positioned in the cavity of the core metal layer such that a plurality of posts extend through the plurality of holes, and wherein the lower metal layer is metallurgically bonded to the first metal layer at least via the plurality of posts.
[0157] Clause 54. The cookware of Clause 53, wherein an upper surface of the lower metal layer surrounding the cavity is metallurgically bonded to the first metal layer.
[0158] Clause 55. The cookware of clause 53 or 54, wherein the depth of the cavity is less than, equal to, or greater than the thickness of the graphite layer.
[0159] Clause 56. The cookware of any of Clauses 53-55, wherein the second metal layer is metallurgically bonded to the planar lower surface of the first metal layer.
[0160] Clause 57. The cooker of any of Clauses 53-56, wherein the plurality of posts have a circular cross-section.
[0161] Clause 58. The cooker of any of Clauses 53-57, wherein the plurality of posts have a polygonal cross-section.
[0162] Clause 59. The cookware of any of Clauses 53-58, wherein the bottom surface of the core metal layer is planar.
[0163] Clause 60. The cookware of any of Clauses 53-59, wherein the first metal layer is made of stainless steel or titanium.
[0164] Clause 61. The cookware of Clause 60, wherein the stainless steel is a ferromagnetic grade of stainless steel.
[0165] Clause 62. The cookware of any of Clauses 51-61, wherein the lower metal layer is made of aluminum.
[0166] Clause 63. The cookware of clause 62, wherein the aluminum is 1100 alloy.
[0167] Clause 64. The cookware of any of Clauses 53-63, wherein the graphite layer is made of anisotropic graphite.
[0168] Item 65. A method of manufacturing a cookware, the method comprising: (a) providing an upper metal disk of stainless steel; (b) providing a perforated graphite disk having a plurality of spaced-apart holes formed therethrough, (c) providing a lower metal disk of aluminum having a cavity, wherein a plurality of spaced-apart posts protrude from a bottom surface of the cavity; (d) stacking the disks provided in steps (a)-(c) in a blank assembly such that the graphite disk is received in the cavity of the lower metal disk, whereby a plurality of posts in the lower metal disk are aligned with and pass through a plurality of holes in the graphite disk, wherein the plurality of posts have upper end portions extending beyond an upper surface of the graphite disk, such that a lower surface of the upper metal disk contacts an upper surface of an outer portion of the lower metal disk and upper end portions of the plurality of posts; and (e) pressing the blank assembly by applying a force in a direction perpendicular to the plane of the disks in the blank assembly, and simultaneously heating the blank assembly to achieve a metallurgical bond between the metal materials of the disks in the blank assembly to provide a bonded blank assembly.
[0169] Clause 66. The method of Clause 65, further comprising: (f) cooling the bonded blank assembly; and (g) forming the bonded blank assembly into a cookware.
[0170] The present disclosure has been described with reference to specific details of particular examples of the invention. It is not intended that such details be considered as limitations on the scope of the present disclosure, except to the extent and within the scope of the appended claims.
Claims
1. A cooker made from a combined multi-layer blank assembly, the cooker comprising: A first metal layer; a second metal layer having a cavity with a plurality of spaced-apart posts protruding from a bottom surface of the cavity; as well as a perforated graphite layer having a thickness of at least 0.010 inches (0.254 mm) and a plurality of spaced-apart holes formed therethrough, wherein the perforated graphite layer is positioned within the cavity of the second metal layer such that the plurality of spaced-apart posts extend through the plurality of spaced-apart holes, and Wherein the second metal layer is metallurgically bonded to the first metal layer at least via the plurality of spaced-apart pillars.
2. The cookware of claim 1 further comprising a third metal layer metallurgically bonded to a planar side of the second metal layer opposite the cavity.
3. The cooker according to claim 2, wherein: The third metal layer is made of stainless steel.
4. The cooker according to claim 1, wherein: A surface of the second metal layer surrounding the cavity is metallurgically bonded to the first metal layer.
5. The cooker according to claim 4, wherein: The surface of the second metal layer surrounding the cavity is planar.
6. The cooker according to claim 1, wherein: The depth of the cavity is less than, equal to, or greater than the thickness of the perforated graphite layer.
7. The cooker according to claim 1, wherein: The plurality of spaced-apart pillars have a circular cross-section or a polygonal cross-section.
8. The cooker according to claim 1, wherein: The first metal layer is made of aluminum or stainless steel, the perforated graphite layer is made of anisotropic graphite, and the second metal layer is made of aluminum.
9. The cooker according to claim 1, wherein: The first metal layer includes a first sublayer made of aluminum and a second sublayer made of stainless steel, and the second metal layer is metallurgically bonded to the first sublayer of the first metal layer.
10. The cooker according to claim 1, wherein: The aluminum is an alloyed aluminum material clad with a thin layer of pure aluminum on either side to facilitate metallurgical bonding.
11. A multi-layer blank assembly for manufacturing a cooker, the multi-layer blank assembly comprising: A first metal layer; a second metal layer having a cavity with a plurality of spaced-apart posts protruding from a bottom surface of the cavity; as well as a perforated graphite layer having a thickness of at least 0.010 inches (0.254 mm) and a plurality of spaced-apart holes formed therethrough, wherein the perforated graphite layer is configured to be positioned within the cavity of the second metal layer such that the plurality of spaced-apart posts extend through the plurality of spaced-apart holes, and Wherein the second metal layer is configured to be metallurgically bonded to the first metal layer at least via the plurality of spaced-apart pillars.
12. The multi-layer billet assembly of claim 11, further comprising a third metal layer configured to be metallurgically bonded to a planar side of the second metal layer opposite the cavity.
13. The multi-layer blank assembly according to claim 12, wherein: The third metal layer is made of stainless steel.
14. The multi-layer blank assembly according to claim 11, wherein: A surface of the second metal layer surrounding the cavity is metallurgically bonded to the first metal layer.
15. The multi-layer blank assembly according to claim 11, wherein: The plurality of spaced-apart pillars have a circular cross-section or a polygonal cross-section.
16. The multi-layer blank assembly according to claim 11, wherein: The perforated graphite layer is made of anisotropic graphite, the first metal layer is made of stainless steel, and the second metal layer is made of aluminum.
17. A method for manufacturing a cooker, the method comprising: (a) providing a first metal layer; (b) providing a perforated graphite layer having a thickness of at least 0.010 inches (0.254 mm) and a plurality of spaced-apart holes formed therethrough, (c) providing a second metal layer having a cavity, a plurality of spaced-apart pillars protruding from a bottom surface of the cavity; (d) stacking the layers provided in (a)-(c) in a blank assembly such that the perforated graphite layer is received within the cavities of the second metal layer, whereby the plurality of pillars of the second metal layer are aligned with and pass through the plurality of holes in the perforated graphite layer such that a lower surface of the first metal layer contacts at least upper surfaces of upper ends of the plurality of pillars; as well as (e) compressing the blank assembly by applying a force in a direction perpendicular to the planes of the layers in the blank assembly and simultaneously heating the blank assembly to achieve a metallurgical bond between the first metal layer and the second metal layer, thereby providing a bonded blank assembly.
18. The method according to claim 17, further comprising: (f) providing a third metal layer and stacking the third metal layer with the layers of the blank assembly prior to pressing the blank assembly such that the third metal layer faces a planar side of the second metal layer opposite the cavity.
19. The method according to claim 18, further comprising: (g) cooling the combined blank assembly; as well as (h) forming the combined blank assembly into the cookware.
20. The method according to claim 17, wherein: The first metal layer is made of aluminum or stainless steel, the perforated graphite layer is made of anisotropic graphite, and the second metal layer is made of aluminum.