Pickering emulsion based on silane coupling agent modified attapulgite as well as preparation method and application of Pickering emulsion
Modifying the concave and concave rock stone by silane coupling agent solves the problems of poor stability and harm to the human environment, and achieves high stability and safety preparation of Pickering emulsion, which is suitable for cosmetic applications.
Patent Information
- Application Number
- CN202410956765.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-01
AI Technical Summary
The existing Pickering emulsion is not stable and depends on auxiliary chemical components such as thickeners. Solid particle modifiers are harmful to the human body and the environment.
The silane coupling agent is used to modify the concave and concave rock stone. The silane groups are grafted onto the concave and concave rock stone through hydrolysis reaction, and its contact angle is adjusted to form a three-dimensional network structure to stabilize the oil-soluble components of cosmetics and reduce the environment and human body. harm.
It achieves high stability and a wide range of oil-water ratios without the need for additional stabilizers, with excellent stability and safety, suitable for cosmetic applications, and comply with green environmental standards.
Smart Images

Figure CN118873459A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of cosmetics, and in particular to a Pickering emulsion based on silane coupling agent-modified attapulgite, and a preparation method and application thereof. Background Art
[0002] Emulsion is the most common dosage form in daily chemical products such as cosmetics. Traditional emulsions are prepared by emulsifying the aqueous phase and the oil phase with the help of surfactants. Although this technical process is relatively mature in the cosmetics industry, chemically synthesized surfactants have toxic side effects such as irritation, which may cause adverse reactions such as skin discomfort, redness, swelling, and itching during application. Long-term contact may aggravate skin sensitivity and pose potential risks to human health. Cosmetics contain a variety of oil-soluble functional ingredients, such as plant essential oils, animal fats, mineral oils, sunscreens, and pigments, which are essential for the efficacy of the products. However, these oil-soluble ingredients are often less stable and easily degraded and volatilized, so effective measures need to be taken to ensure their stability in emulsions. In order to stabilize these oil-soluble ingredients, the cosmetics industry usually adopts the method of adding excipients such as emulsifiers, thickeners, and antioxidants. However, the addition of these additives can also irritate human skin (especially infants and young children with incomplete skin barrier function and people with sensitive skin), destroy the skin barrier, and cause many skin problems. Moreover, many chemical synthetic emulsifiers are prone to produce toxic by-products during production, which have a negative impact on the environment.
[0003] Pickering emulsion is a new type of formulation that uses micron or nanometer solid particles to replace traditional surfactants to prepare stable emulsions. Solid particles with specific wettability (can form a stable adsorption layer at the oil-water interface) can be irreversibly adsorbed at the oil-water interface, which not only effectively prevents the spatial collision and aggregation of emulsion droplets, but also gives the emulsion excellent stability by enhancing the electrostatic repulsion and steric effect between emulsion droplets. Pickering emulsions show a number of unique properties on the basis of maintaining the basic characteristics of classic emulsions. First, high responsiveness, can respond to external stimuli such as pH, temperature, light intensity and magnetic field, so as to achieve dynamic regulation of emulsion properties. Second, extremely excellent stability, the desorption energy of solid particles from the water / oil interface is much higher than thermal energy, ensuring that the emulsion can maintain long-term stability under various conditions. Finally, excellent biosafety, the solid particles used in Pickering emulsions are usually not easy to irritate the human body, and some natural solid emulsifiers are also environmentally friendly, meet green environmental protection standards, and have no environmental pollution risks. Therefore, surfactant-free Pickering emulsions have received great attention and favor in the cosmetic and pharmaceutical fields. Compared with traditional emulsions, Pickering emulsions have the advantages of good safety, low cost and high stability.
[0004] Attapulgite is a water-rich magnesium-aluminum silicate clay mineral. Its unique nano-scale microstructure and ecological mineral material matrix give it a variety of excellent properties, such as excellent ion exchange capacity, adsorption performance, rheological regulation and carrier function. Relevant studies have shown that the preparation of Pickering emulsions using natural attapulgite directly as a solid agent has problems such as high addition amount, poor emulsion stability, and large droplet size distribution. However, the surface of attapulgite contains a large number of Si-OH groups and is highly active. Other groups can be added to its surface through chemical reactions to change the hydrophilicity and hydrophobicity of attapulgite, which can be used as a new solid emulsifier to stabilize Pickering emulsions.
[0005] Chinese patent CN114540045A discloses a method for preparing a soapberry-modified attapulgite and its plant essential oil O / W Pickering emulsion, wherein the attapulgite is hydrophilic and hydrophobic modified by soapberry saponin, and the surface wettability of the soapberry-modified attapulgite is less affected by the modification result, and the contact angle (θ) only rises from 23° to 32°, which is not conducive to the encapsulation of hydrophobic essential oil. And the soapberry saponin extraction process is relatively complicated, the cost is high, and the production process will produce a large amount of waste to cause environmental pollution. At the same time, the emulsion system stability is not strong, and xanthan gum needs to be used in combination as a thickener to enhance the stability of the system.
[0006] Chinese patent CN114632478A discloses a method for preparing a Pickering emulsion gel based on modified attapulgite clay, wherein octenyl succinic anhydride (OSA) is used as a modifier to impart specific properties to the emulsion gel. As a chemical synthetic product, octenyl succinic anhydride has a relatively high cost. In addition, the experimental operation process in this method is complicated, freeze drying is required, the reaction conditions are high, and the time consumption is long, which limits its practicality in large-scale production and industrial application.
[0007] Chinese patent CN106214638A discloses a modified montmorillonite-stabilized curcumin-loaded Pickering emulsion and its preparation method, Chinese patent CN109704352A discloses a preparation method of a kaolinite-stabilized Pickering emulsion based on a lock-type structure, and CN117898970A discloses the use of composite nanoparticles in stabilizing Pickering emulsions, Pickering emulsions and preparation methods. Although the montmorillonite and kaolin used in the above patents have a wide range of raw material sources and are natural and non-irritating, they are clays with layered structures. The uneven morphology between layers will cause solid particles to fall off, which has significant structural and morphological differences from the chain-like fibrous clay attapulgite used in the present invention, and the modification method is also different.
[0008] Chinese patent CN110859763A discloses a Pickering emulsion loaded with fat-soluble active ingredients, a preparation method and cosmetics. PLGA / PSS nanoparticle freeze-dried powder is used as an emulsifier to prepare an emulsion loaded with fat-soluble active ingredients. The prepared emulsion has good storage stability, pH stability and radiation stability. However, the experimental preparation process is complicated and requires ultrasound and freeze drying. In addition, acetone is used as an organic solvent in the experimental process, which is harmful to the human body and the environment. At the same time, the stability of the emulsion system is not high, and xanthan gum thickener needs to be added to enhance the stability of the system.
[0009] Chinese patent CN109776881A discloses the preparation of a carboxymethyl starch / chitosan hydrochloride nanogel and its application in the preparation of a stable Pickering emulsion. The contact angle (θ) of the modified nanogel is 90.3°, and the particles have neutral wettability, which is conducive to the formation of a stable Pickering emulsion. However, the volume fraction range of the emulsion oil phase is too narrow (10-50%), and within this volume fraction range, the change in the emulsion particle size shows an increasing trend; the emulsion pH range is relatively narrow (pH2-6), and it only tends to be an acidic emulsion. In addition, the chloroacetic acid used in the modification process of modified starch is severely corrosive and irritating, and ingestion or skin contact will cause poisoning. It is extremely toxic to aquatic organisms and poses potential hazards to humans and the environment.
[0010] Based on this, it is very important to provide a Pickering emulsion with good stability and safety and wide application. Summary of the invention
[0011] The purpose of the present invention is to provide a Pickering emulsion based on silane coupling agent modified attapulgite and its preparation method and application, so as to solve the technical problems in the prior art that the Pickering emulsion is not stable, relies on auxiliary chemical components such as thickeners, the solid particle modifier is not a cosmetic raw material, and is harmful to the human body and the environment.
[0012] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0013] The present invention provides a method for preparing a Pickering emulsion based on silane coupling agent-modified attapulgite, comprising the following steps:
[0014] (1) mixing attapulgite, sodium pyrophosphate and water to obtain pretreated attapulgite;
[0015] (2) dispersing the pretreated attapulgite in an ethanol aqueous solution, and then adding a silane coupling agent for hydrolysis modification to obtain modified attapulgite;
[0016] (3) The modified attapulgite, the aqueous phase and the oil-soluble functional component are mixed and homogenized to obtain a Pickering emulsion.
[0017] Furthermore, in the step (1), the dosage ratio of attapulgite, sodium pyrophosphate and water is 5-30 g: 0.1-10 g: 200-400 mL;
[0018] The purity of the attapulgite is 50-99%.
[0019] Furthermore, in the step (2), the dosage ratio of the pretreated attapulgite, ethanol aqueous solution and silane coupling agent is 0.05-2 g: 50 mL: 0.01-10 mL.
[0020] Furthermore, in step (2), the volume concentration of the ethanol aqueous solution is 30 to 90%;
[0021] The silane coupling agent includes one or more of γ-methacryloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane, n-octyltriethoxysilane, n-decyltriethoxysilane, dodecyltriethoxysilane and octadecyltriethoxysilane.
[0022] Furthermore, in the step (2), the temperature of the hydrolysis modification is 20 to 40° C., and the time of the hydrolysis modification is 1 to 3 hours;
[0023] The pH value of the hydrolysis modification is 2 to 14;
[0024] The hydrolysis modification is carried out under stirring, and the stirring speed is 200-600 rpm;
[0025] The particle size of the modified attapulgite is 100 to 500 meshes.
[0026] Furthermore, in the step (3), the usage ratio of the modified attapulgite, the aqueous phase and the oil-soluble functional ingredient is 0.05-2 g: 4-8 mL: 2-5 mL;
[0027] The homogenizing speed is 5000-18000 rpm, and the homogenizing time is 1-8 min.
[0028] Furthermore, in step (3), the oil-soluble functional ingredients include one or more of vegetable oil, animal oil, mineral oil, antibacterial agent, antioxidant, colorant and sunscreen;
[0029] The vegetable oil includes one or more of olive oil, almond oil and peony seed oil;
[0030] The animal oil includes sheep oil and / or bird's nest oil;
[0031] The mineral oil includes white oil and / or silicone oil.
[0032] Further, the antibacterial agent includes tea tree essential oil, angustifolia essential oil, lavender essential oil, forsythia essential oil, prickly ash essential oil, eucalyptus essential oil, peppermint essential oil, clove essential oil, rosemary essential oil, cinnamon essential oil, lemon balm essential oil, frankincense essential oil, eucalyptus essential oil, sage essential oil, magnolia bark extract or sophora flavescens extract;
[0033] The antioxidant includes astaxanthin, lutein, vitamin E, butylated hydroxyanisole, 2,6-di-tert-butylated cresol, propyl gallate, tocopherol acetate, lipoic acid or coenzyme Q10;
[0034] The colorant includes curcumin, capsanthin, hematoxylin, guaiazulene, carotenoids, cochineal, persimmon, smoky blue or squalane pigment;
[0035] The sunscreen includes ethylhexyl methoxycinnamate, isoamyl methoxycinnamate, ethylhexyl dimethylparaaminobenzoate, phenylbenzimidazole sulfonic acid, octocrylene, butyl methoxydibenzoylmethane or ethyl triazone.
[0036] The invention provides a Pickering emulsion prepared by the method for preparing the Pickering emulsion based on silane coupling agent modified attapulgite.
[0037] The present invention also provides an application of the Pickering emulsion in preparing daily chemical products, wherein the daily chemical products include one or more of fragrances, gels, perfumes, solid ointments, detergents, isolation creams, foundation creams, makeup, acne patches, mosquito repellent patches and disinfectants.
[0038] Beneficial effects of the present invention:
[0039] (1) The preparation method of the present invention modifies attapulgite by a silane coupling agent. The attapulgite has the characteristics of large specific surface area, porous structure and abundant hydroxyl groups. The silane coupling agent is hydrolyzed to make the silanol group and the single bond on the surface of the attapulgite undergo aldol condensation reaction, so that the silane group is grafted to the attapulgite, and then the contact angle (θ) thereof is adjusted to be close to 90°, which is conducive to encapsulating and stabilizing a variety of cosmetic oil-soluble functional ingredients, especially natural plant essential oils and plant pigments. The attapulgite crystals interact with each other through van der Waals forces to form a three-dimensional network structure, so that the dispersion system containing attapulgite is more stable. The prepared Pickering emulsion does not need to add additional stabilizers and thickeners, and the volume fraction of oil-soluble functional ingredients is wider than that of traditional emulsions, the pH range is larger, and it is not easily affected by ions and temperature. Compared with traditional surfactant emulsions, the Pickering emulsion of the present invention has excellent stability and safety.
[0040] (2) The present invention uses silane coupling agent as a modifier, the raw materials are relatively easy to obtain, and the preparation process is mature. At the same time, the silane coupling agent itself is inexpensive, non-toxic and tasteless, and has no adverse effects on the human body and the environment during use, further ensuring the safety and compliance of its modified raw materials in daily chemical products such as cosmetics that are in close contact with the human body.
[0041] (3) The modified attapulgite Pickering emulsion prepared by the present invention can be added to a gel matrix such as chitosan, hydroxyethyl cellulose, polyvinyl pyrrolidone (PVP), gelatin, polyvinyl alcohol, collagen, chitin, sodium trehalose, hyaluronic acid, polyacrylic acid, sodium alginate, etc., and can be used to prepare daily chemical products such as gel patches, solid ointments, foundation makeup, etc., and the usage scenarios are more diversified.
[0042] (4) The Pickering emulsion prepared by the present invention has a simple preparation method and does not require complex and expensive equipment. In addition, the mineral raw materials are abundant in my country (ranking first in the world). The prepared formula does not contain irritating ingredients such as surfactants, is friendly to the human body and the environment, and is green and environmentally friendly. It meets the requirements of "pure beauty" for daily chemical products to be "green, safe, natural, and non-toxic." BRIEF DESCRIPTION OF THE DRAWINGS
[0043] Figure 1 A schematic diagram of the structure of the Pickering emulsion prepared in the present invention;
[0044] Figure 2 It is a comparison diagram of Fourier infrared spectra of attapulgite, pretreated attapulgite and modified attapulgite;
[0045] Figure 3 is the particle size distribution diagram of the Pickering emulsion prepared in Example 1;
[0046] Figure 4 An inverted fluorescence microscope image of the Pickering emulsion prepared in Example 1;
[0047] Figure 5 The appearance of Pickering emulsions with different volume fractions in Example 1;
[0048] Figure 6 The appearance of Pickering emulsions with different particle concentrations in Example 1;
[0049] Figure 7 This is a comparison diagram of the particle size distribution of the tea tree essential oil Pickering emulsion at different pH values in Example 1;
[0050] Figure 8 is the UV stability graph of the Pickering emulsion prepared in Example 2;
[0051] Fig. 9 The thermal stability diagram of the Pickering emulsion prepared in Example 2;
[0052] Fig.10 This is the appearance of the Pickering emulsion prepared in Example 3;
[0053] Fig.11 is the particle size distribution diagram of the Pickering emulsion prepared in Example 3;
[0054] Fig.12 This is a graph showing the essential oil release of the Pickering emulsion prepared in Example 3;
[0055] Fig.13 The cross-sectional scanning electron microscope images of the acne patches prepared in Comparative Example 1, Example 1 and Examples 4 to 5;
[0056] Fig.14 1 is a human efficacy comparison chart of the acne patch prepared by Example 1, Examples 4 to 5, and Comparative Example 1, wherein 1 is a human efficacy comparison chart of the acne patch prepared by Comparative Example 1, 2 is a human efficacy comparison chart of the acne patch prepared by Example 1, 3 is a human efficacy comparison chart of the acne patch prepared by Example 4, 4 is a human efficacy comparison chart of the acne patch prepared by Example 5, and 5 is a blank human efficacy comparison chart. DETAILED DESCRIPTION
[0057] The present invention provides a method for preparing a Pickering emulsion based on silane coupling agent-modified attapulgite, comprising the following steps:
[0058] (1) mixing attapulgite, sodium pyrophosphate and water to obtain pretreated attapulgite;
[0059] (2) dispersing the pretreated attapulgite in an ethanol aqueous solution, and then adding a silane coupling agent for hydrolysis modification to obtain modified attapulgite;
[0060] (3) The modified attapulgite, the aqueous phase and the oil-soluble functional component are stirred and homogenized to obtain a Pickering emulsion.
[0061] In the present invention, in the step (1), the dosage ratio of attapulgite, sodium pyrophosphate and water is 5-30 g: 0.1-10 g: 200-400 mL, preferably 6-28 g: 0.2-9 g: 220-380 mL, and more preferably 8-25 g: 0.5-8 g: 250-350 mL.
[0062] In the present invention, the purity of the attapulgite is 50 to 99%, preferably 55 to 98%, and more preferably 60 to 95%.
[0063] In the present invention, in the step (1), after mixing, the mixture is preferably stirred for 1 to 6 hours, and after standing for 1 to 6 hours, the upper suspension is filtered, and then centrifuged at 8000 rpm for 5 minutes. After the centrifugation, the mixture is washed with water until neutral, and finally dried at 100°C, crushed, and sieved through a 100-mesh sieve to obtain the pretreated attapulgite.
[0064] In the present invention, in the step (2), the dosage ratio of the pretreated attapulgite, ethanol aqueous solution and silane coupling agent is 0.05-2 g:50 mL:0.01-10 mL, preferably 0.08-1.5 g:50 mL:0.03-9 mL, and more preferably 1 g:50 mL:0.05-8 mL.
[0065] In the present invention, in step (2), the volume concentration of the ethanol aqueous solution is 30 to 90%, preferably 35 to 85%, and more preferably 40 to 80%.
[0066] In the present invention, in the step (2), the silane coupling agent includes one or more of γ-methacryloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane, n-octyltriethoxysilane, n-decyltriethoxysilane, dodecyltriethoxysilane and octadecyltriethoxysilane, preferably one or more of γ-aminopropyltriethoxysilane, n-octyltriethoxysilane, n-decyltriethoxysilane, dodecyltriethoxysilane and octadecyltriethoxysilane, and further preferably one or more of n-decyltriethoxysilane, dodecyltriethoxysilane and octadecyltriethoxysilane.
[0067] In the present invention, in the step (2), the temperature of the hydrolysis modification is 20 to 40°C, preferably 22 to 38°C, and more preferably 25 to 35°C; the time of the hydrolysis modification is 1 to 3 hours, preferably 1.5 to 2.5 hours, and more preferably 2 hours.
[0068] In the present invention, in step (2), the pH value of the hydrolysis modification is 2 to 14, preferably 3 to 12, and more preferably 4 to 10;
[0069] The reagent used to adjust the pH value is preferably hydrochloric acid, and the molar concentration of the hydrochloric acid is 0.1 to 5 mol / L, preferably 0.5 to 4 mol / L, and more preferably 1 to 3 mol / L;
[0070] The amount of hydrochloric acid used is 50 to 200 μL.
[0071] In the present invention, in the step (2), the hydrolysis modification is carried out under stirring, the stirring speed is 200 to 600 rpm, preferably 250 to 550 rpm, and more preferably 300 to 500 rpm; the stirring time is 2 to 6 hours, preferably 3 to 5 hours, and more preferably 4 hours.
[0072] In the present invention, in the step (2), centrifugation is preferably performed after the hydrolysis modification is completed, the centrifugal speed is 5000-18000 rpm, the centrifugal time is 5-15 min, and after the centrifugation is completed, the solid precipitate after centrifugation is washed with anhydrous ethanol and pure water for 2-5 times, then dried at 100°C for 2h, and sieved to obtain modified attapulgite.
[0073] In the present invention, in the step (2), the particle size of the modified attapulgite is 100 to 500 meshes, preferably 150 to 450 meshes, and more preferably 200 to 400 meshes.
[0074] In the present invention, in the step (3), the usage ratio of the modified attapulgite, the aqueous phase and the oil-soluble functional ingredient is 0.05-2g:4-8mL:2-5mL, preferably 0.08-1.5g:5-7mL:3-4.5mL, and more preferably 1g:6mL:4mL.
[0075] In the present invention, the aqueous phase includes water and / or hydrosol, preferably water.
[0076] In the present invention, the preparation method of the hydrosol is as follows: soaking the plant in a mixed solution prepared by a polyvinyl alcohol solution with a mass fraction of 0.1% and a sodium chloride solution with a mass fraction of 2.5%, the soaking time is 0.5 to 2 hours, the solid-liquid ratio is 1:4, and then continuously distilling for 2 to 5 hours by steam distillation, collecting the distillate, placing the distillate in a separatory funnel, adding 2.5 mL of saturated sodium chloride, extracting with ether, adding anhydrous sodium sulfate to dry, concentrating the extract, obtaining plant essential oil on the upper layer, and obtaining plant hydrosol on the lower layer.
[0077] In the present invention, in step (3), the oil-soluble functional ingredients include one or more of vegetable oil, animal oil, mineral oil, antibacterial agent, antioxidant, colorant and sunscreen, preferably one or more of vegetable oil, animal oil, antibacterial agent, antioxidant and colorant, and more preferably one or more of vegetable oil, antibacterial agent and colorant.
[0078] In the present invention, the vegetable oil includes one or more of olive oil, almond oil and peony seed oil, preferably olive oil and / or almond oil, and more preferably olive oil.
[0079] In the present invention, the animal oil includes sheep oil and / or bird's nest oil, preferably sheep oil.
[0080] In the present invention, the mineral oil includes white oil and / or silicone oil, preferably white oil.
[0081] In the present invention, the antibacterial agent includes tea tree essential oil, elaeagnus angustifolia flower essential oil, lavender essential oil, forsythia essential oil, peppermint essential oil, eucalyptus essential oil, mint essential oil, rosemary essential oil, clove essential oil, cinnamon essential oil, lemon balm essential oil, frankincense essential oil, eucalyptus essential oil, sage essential oil, Magnolia bark extract or Sophora flavescens extract, preferably tea tree essential oil, elaeagnus angustifolia flower essential oil, lavender essential oil, forsythia essential oil, peppermint essential oil, eucalyptus essential oil, mint essential oil, clove essential oil, rosemary essential oil, cinnamon essential oil, sage essential oil, Magnolia bark extract or Sophora flavescens extract, further preferably tea tree essential oil, elaeagnus angustifolia flower essential oil, lavender essential oil, forsythia essential oil, peppermint essential oil, eucalyptus essential oil, mint essential oil, clove essential oil, cinnamon essential oil, sage essential oil, Magnolia bark extract or Sophora flavescens extract.
[0082] In the present invention, the antioxidant includes astaxanthin, lutein, vitamin E, butylated hydroxyanisole, 2,6-di-tert-butylated cresol, propyl gallate, tocopherol acetate, lipoic acid or coenzyme Q10, preferably astaxanthin, lutein, vitamin E, butylated hydroxyanisole, 2,6-di-tert-butylated cresol, tocopherol acetate, lipoic acid or coenzyme Q10, further preferably astaxanthin, lutein, vitamin E, butylated hydroxyanisole, 2,6-di-tert-butylated cresol, lipoic acid or coenzyme Q10.
[0083] In the present invention, the colorant includes curcumin, capsanthin, hematoxylin, guaiazulene, carotenoids, cochineal, persimmon, smoky blue or squalane pigment, preferably curcumin, capsanthin, hematoxylin, carotenoids, cochineal, persimmon, smoky blue or squalane pigment, further preferably curcumin, capsanthin, hematoxylin, carotenoids, persimmon, smoky blue or squalane pigment.
[0084] In the present invention, the sunscreen includes ethylhexyl methoxycinnamate, isopentyl methoxycinnamate, ethylhexyl dimethylpara-aminobenzoate, phenylbenzimidazole sulfonic acid, octocrylene, butyl methoxydibenzoylmethane or ethyl triazone, preferably ethylhexyl methoxycinnamate, isopentyl methoxycinnamate, ethylhexyl dimethylpara-aminobenzoate, phenylbenzimidazole sulfonic acid or ethyl triazone, further preferably ethylhexyl methoxycinnamate, isopentyl methoxycinnamate, phenylbenzimidazole sulfonic acid or ethyl triazone.
[0085] In the present invention, in the step (3), the homogenization is carried out in a high-speed shear homogenizer, and the speed of the homogenization is 5000 to 18000 rpm, preferably 8000 to 16000 rpm, and more preferably 10000 to 15000 rpm;
[0086] The homogenization time is 1 to 8 minutes, preferably 2 to 7 minutes, and more preferably 3 to 6 minutes.
[0087] The invention provides a Pickering emulsion prepared by the method for preparing the Pickering emulsion based on silane coupling agent modified attapulgite.
[0088] The present invention also provides an application of the Pickering emulsion in preparing daily chemical products, wherein the daily chemical products include one or more of fragrances, gels, perfumes, solid ointments, detergents, isolation creams, foundation creams, makeup, acne patches, mosquito repellent patches and disinfectants.
[0089] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.
[0090] Example 1
[0091] 30 g of attapulgite with a purity of 90% and 0.17 g of sodium pyrophosphate were added to 300 mL of pure water and stirred for 2 h, then allowed to stand for 2.5 h, the upper suspension was filtered, and then centrifuged at 8000 rpm for 5 min. After the centrifugation, it was washed with water until neutral, then dried at 100 ° C, and finally crushed and passed through a 100 mesh sieve to obtain pretreated attapulgite;
[0092] 1 g of pretreated attapulgite was dispersed in an ethanol aqueous solution (the ethanol aqueous solution was prepared by 40 mL of ethanol and 10 mL of pure water) and stirred to dissolve, 0.05 mL of dodecyltriethoxysilane was added for hydrolysis modification, 100 μL of hydrochloric acid with a molar concentration of 1 mol / L was used to adjust the pH value to 4, stirred at 30° C. for 2 h, centrifuged at 8000 rpm for 5 min, and the solid precipitate after centrifugation was washed twice with anhydrous ethanol and pure water respectively, and dried at 100° C. for 2 h after washing, and finally passed through a 200-mesh sieve to obtain modified attapulgite;
[0093] 1 g of modified attapulgite was added to 6 mL of pure water and stirred evenly, and then 4 mL of tea tree essential oil was added and stirred, and the mixture was homogenized in a high-speed shear homogenizer at a speed of 10,000 rpm for 2 minutes to obtain a Pickering emulsion.
[0094] The infrared spectra (FTIR) of pretreated attapulgite (purified by sodium pyrophosphate) and modified attapulgite were tested by Fourier transform infrared spectrometer to study the types of functional groups. The test method is: the sample is ground with KBr and pressed into a tablet, and then measured with a scanning range of 4000cm -1 ~400cm -1 The test results are as follows: Figure 2 shown. Figure 2 The following is a comparison of Fourier transform infrared spectra of the attapulgite of Example 1, the pretreated attapulgite and the modified attapulgite. Figure 2 It can be seen that the FTIR spectrum of the pretreated attapulgite shows a peak at 3700-3200 cm -1 The typical bands of the attapulgite structure are in the range of 3399 cm-1, which are related to the stretching and contraction vibration bands of -OH and crystal water. -1 The broad band at 1656 cm is the stretching vibration peak of coordinated water and zeolite water in PAL. -1 The peaks at 1196cm are the bending vibration peaks of adsorbed water and zeolite water; -1 The peak at 1656cm is the stretching vibration peak of Si-O-Si bond. -1 1196cm -1 The absorption peak of 2924cm -1 and 2856cm -1 The new peak nearby is attributed to the CH bond stretching vibration of the grafted silane, indicating that the silane groups are successfully grafted onto the attapulgite.
[0095] According to the method of Example 1, different types of silane coupling agents were used to modify the attapulgite to obtain modified attapulgite. Weigh 0.06g of the modified attapulgite sample, press it with a tablet press for 2min at 15MPa to make it into a sheet. The contact angle of the modified attapulgite was tested. The contact angle was measured by the micro-optical contact angle measurement system of the drop shape analyzer, using a 5μL water droplet as the test index, and measuring 3 points for each sample to take the average value. The test results are shown in Table 1.
[0096] Table 1 Contact angle of modified attapulgite
[0097] Silane coupling agent Contact Angle / 0 γ-Methacryloyloxypropyltrimethoxysilane 36.15±0.34 n-Octyltriethoxysilane 60.88±0.86 n-Decyltriethoxysilane 85.70±0.39 Dodecyltriethoxysilane 96.35±0.93 Octadecyltriethoxydecane 61.15±0.42
[0098] It can be seen from Table 1 that the natural attapulgite has strong hydrophilicity. After modification by the modifier, the contact angle increases and the hydrophobicity is enhanced. Among them, the modification effect of triethoxysilane with different carbon chains is the best.
[0099] The position of modified attapulgite in Pickering emulsion was marked by rhodamine B. First, rhodamine B (<1×10 -6 mol / L) was dissolved in a modified attapulgite aqueous solution to label the particles, and then the fluorescently labeled modified attapulgite solution was used as an emulsifier to prepare an emulsion. The particles were placed on a microscope slide, covered with a cover glass, and the microstructure of the Pickering emulsion was photographed using an inverted fluorescence microscope. The results are shown in Figure 4 shown. Figure 4 This is an inverted fluorescence microscope image of the Pickering emulsion prepared in Example 1. Figure 4 It can be seen that a yellow circle is observed around the oil droplets. This indicates that a large amount of attapulgite is adsorbed on the surface of the oil droplets, and the particles can form a strong rigid film around the oil droplets, providing a strong physical barrier to prevent the droplets from agglomerating, thereby improving the stability of the emulsion. In addition, fluorescence signals are also observed in the continuous phase, which indicates that the solid particles adsorbed at the oil-water interface form a three-dimensional network structure with the modified attapulgite particles in the continuous phase, effectively preventing the oil droplets from agglomerating and condensing.
[0100] Pickering emulsions with different volume fractions (oil-soluble active ingredient: water phase ratio of 3:7, 4:6, 5:5 and 6:4 respectively) and different solid particle concentrations (solid particle concentration of 2%, 2.5% and 3%) were prepared, and the stability of the prepared Pickering emulsions was tested. Figures 5-6 shown. Figure 5 The appearance of Pickering emulsions with different volume fractions; Figure 6 The appearance of Pickering emulsions with different particle concentrations. Figures 5-6 It can be seen that the emulsion systems prepared under different oil-water ratios and different particle concentrations are uniform and do not show stratification, indicating that a stable Pickering emulsion can be prepared when the volume fraction of the oil-soluble active ingredient is 30 to 60% and the solid particle concentration is in the range of 2.0wt% to 3.0wt%.
[0101] Figure 3 This is the particle size distribution diagram of the Pickering emulsion prepared in Example 1. Figures 3 to 6 It can be seen that the Pickering emulsion prepared in Example 1 is milky white, the emulsion droplets are spherical particles, the particle size distribution is uniform, and it has good stability.
[0102] The acid-base stability of the Pickering emulsion prepared in Example 1 was tested by adjusting the pH of the Pickering emulsion to 3.0, 5.0, 7.0, 9.0 and 11.0 respectively with 1 mol / L hydrochloric acid solution or sodium hydroxide solution, and measuring the emulsion particle size at each pH value. The test results are shown in FIG. Figure 7 shown.
[0103] Figure 7The figure is a comparison of the particle size distribution of the tea tree essential oil Pickering emulsion at different pH values in Example 1. Figure 7 It can be seen that when the pH value is 3-11, the particle size remains basically unchanged at about 8 μm, indicating that the Pickering emulsion of the present invention has a good pH value of acid-base stability.
[0104] The Pickering emulsion prepared in Example 1 was used to prepare an acne patch. The specific preparation method was as follows: 1 g of chitosan was dispersed in 30 mL of pure water, and 0.5 mL of acetic acid was added to dissolve the chitosan solution; 1 g of a film matrix precursor was dispersed in 70 mL of pure water, and stirred until transparent to obtain a film matrix precursor solution; the chitosan solution and the film matrix precursor solution were blended, 5% glycerol was added for plasticization, and the mixture was stirred for 2 to 3 hours, and allowed to stand for defoaming to obtain a film matrix;
[0105] Mix 0.75g of Pickering emulsion with 14.25g of film matrix to obtain a mixed solution, keep the film-forming solution at 15g, stir for 1 to 2 hours at room temperature, introduce the mixed solution into a culture dish with a diameter of 90mm by a cast film method, and dry it at 45°C for 4.5 hours to obtain an acne patch.
[0106] Example 2
[0107] 30 g of attapulgite with a purity of 90% and 0.17 g of sodium pyrophosphate were added to 300 mL of pure water and stirred for 2 h, then allowed to stand for 2.5 h, the upper suspension was filtered, and then centrifuged at 8000 rpm for 5 min. After the centrifugation, it was washed with water until neutral, then dried at 100 ° C, and finally crushed and passed through a 100 mesh sieve to obtain pretreated attapulgite;
[0108] 1 g of pretreated attapulgite was dispersed in an ethanol aqueous solution (the ethanol aqueous solution was prepared by 40 mL of ethanol and 10 mL of pure water) and stirred to dissolve, 0.05 mL of dodecyltriethoxysilane was added for hydrolysis modification, 100 μL of hydrochloric acid with a molar concentration of 1 mol / L was used to adjust the pH value to 4, stirred at 30° C. for 2 h, centrifuged at 8000 rpm for 5 min, and the solid precipitate after centrifugation was washed twice with anhydrous ethanol and pure water respectively, and dried at 100° C. for 2 h after washing, and finally passed through a 200-mesh sieve to obtain modified attapulgite;
[0109] Dissolve 0.01 g of curcumin in 10 mL of caprylic / capric triglyceride (GTCC) and stir evenly to obtain a natural pigment oil-soluble functional ingredient solution with a mass concentration of 1 g / L;
[0110] 1 g of modified attapulgite was added to 6 mL of pure water and stirred evenly, and then 4 mL of natural pigment oil-soluble functional ingredient solution was added and stirred, and homogenized in a high-speed shear homogenizer with a speed of 10,000 rpm and a homogenization time of 2 min to obtain a Pickering emulsion.
[0111] The UV stability of the Pickering emulsion prepared in Example 2 was tested as follows: 1.5 mL of the Pickering emulsion was placed in a quartz cuvette and illuminated with a UVA lamp (2.5 mW / cm 2 ) Continuously irradiate for 12 hours, take samples at intervals to determine the residual amount of pigment in the emulsion to evaluate the UVA protection effect of the emulsion on the pigment. Before each sampling, the emulsion needs to be shaken evenly. Take 20 μL of the emulsion each time, add 4 mL of anhydrous ethanol, vortex to break the emulsion to extract the pigment in the emulsion, use anhydrous ethanol as the blank control solution, and use an ultraviolet spectrophotometer to determine the absorbance value. The retention rate is the ratio of the pigment content at different time points during ultraviolet irradiation to the pigment content in the emulsion at the time of initial preparation (0h), and the emulsion prepared with Tween 80 as the emulsifier under the same conditions is used as a comparative experiment. The retention rate (RR, %) is calculated using the following formula: RR = T t / T0×100%,
[0112] Among them, T t is the content of pigment at different irradiation time points, and T0 is the total content of pigment when the emulsion is initially prepared. Figure 8 shown.
[0113] Figure 8 The UV stability diagram of the Pickering emulsion prepared in Example 2. Figure 8 It can be seen that with the increase of irradiation time, the curcumin retention rate in the emulsion of Example 2 shows a downward trend, but the pigment retention rate of the Pickering emulsion in Example 2 is greater than the pigment retention rate of the Pickering emulsion prepared with Tween 80 as an emulsifier. The modified attapulgite in Example 2 can be adsorbed on the surface of the essential oil in which the pigment is dissolved to form a physical barrier, which to a certain extent blocks the direct contact of ultraviolet rays with the pigment oil droplets and reduces the degradation of the pigment.
[0114] The thermal stability of the Pickering emulsion prepared in Example 2 was tested: the Pickering emulsion of Example 2 was heated in an oven at 80°C, 50 μL of the curcumin emulsion was taken into a centrifuge tube each time, 3 mL of anhydrous ethanol was added, vortexed to break the emulsion to extract the pigment in the emulsion, and centrifuged at 6000 r / min for 3 minutes. Anhydrous ethanol was used as the blank control solution at 0, 1, 3, 4, and 5 hours, and the supernatant was taken to measure the absorbance value by ultraviolet spectrophotometer at a wavelength of 425 nm. The retention rate is the ratio of the content of the pigment at different time points during the heating period to the content of the pigment in the emulsion at the time of initial preparation (0h). The emulsion prepared with Tween 80 as the emulsifier was used as a comparative experiment under the same conditions. The retention rate (RR, %) is calculated using the following formula: RR = T t / T0×100%,
[0115] Among them, T t is the content of pigment at different heating time points, and T0 is the total content of pigment when the emulsion is initially prepared. Fig. 9 as shown.
[0116] Fig. 9 The thermal stability diagram of the Pickering emulsion prepared in Example 2. Fig. 9 It can be seen that with the increase of heating time, the retention rate of curcumin in the Pickering emulsion prepared in Example 2 shows a downward trend, but the pigment retention rate of the emulsion of curcumin stabilized by modified attapulgite in Example 2 is greater than that of the emulsion of curcumin stabilized by Tween 80. The modified attapulgite can be adsorbed on the surface of the essential oil that dissolves the pigment, forming a physical barrier to protect the pigment from external influences and reduce the degradation of the pigment. It shows that the emulsion encapsulating curcumin prepared by the technology of the present invention has better thermal stability.
[0117] Example 3
[0118] 30 g of attapulgite with a purity of 90% and 0.17 g of sodium pyrophosphate were added to 300 mL of pure water and stirred for 2 h, then allowed to stand for 2.5 h, the upper suspension was filtered, and then centrifuged at 8000 rpm for 5 min. After the centrifugation, it was washed with water until neutral, then dried at 100 ° C, and finally crushed and passed through a 100 mesh sieve to obtain pretreated attapulgite;
[0119] 1 g of pretreated attapulgite was dispersed in an ethanol aqueous solution (the ethanol aqueous solution was prepared by 40 mL of ethanol and 10 mL of pure water) and stirred to dissolve, 0.05 mL of dodecyltriethoxysilane was added for hydrolysis modification, 100 μL of hydrochloric acid with a molar concentration of 1 mol / L was used to adjust the pH value to 4, stirred at 30° C. for 2 h, centrifuged at 8000 rpm for 5 min, and the solid precipitate after centrifugation was washed twice with anhydrous ethanol and pure water respectively, and dried at 100° C. for 2 h after washing, and finally passed through a 200-mesh sieve to obtain modified attapulgite;
[0120] Soak 30g of crushed Elaeagnus angustifolia flowers in a mixed solution prepared by a polyvinyl alcohol solution with a mass fraction of 0.1% and a sodium chloride solution with a mass fraction of 2.5% for 1h, and then use steam distillation to continuously distill for 3h, collect the distillate, put the distillate in a separatory funnel, add 2.5mL of saturated sodium chloride, extract with ether, add anhydrous sodium sulfate to dry, concentrate the extract, and obtain Elaeagnus angustifolia flower essential oil on the upper layer and Elaeagnus angustifolia flower hydrosol on the lower layer;
[0121] Add 1 g of modified attapulgite to 6 mL of Elaeagnus angustifolia flower hydrosol, stir evenly, then add 4 mL of Elaeagnus angustifolia flower essential oil and stir, and homogenize in a high-speed shear homogenizer with a speed of 10,000 rpm and a homogenization time of 2 min to obtain Pickering emulsion.
[0122] Fig.10 This is the appearance of the Pickering emulsion prepared in Example 3; Fig.11 The particle size distribution diagram of the Pickering emulsion prepared in Example 3. Figures 10-11 It can be seen that the Pickering emulsion prepared in Example 3 is milky white, has a uniform particle size distribution, and has good stability.
[0123] The release amount of the essential oil of Elaeagnus angustifolia in the Pickering emulsion prepared in Example 3 was tested. The test method was as follows: 500 mg of Example 3 was placed in a dialysis bag and soaked in 50 mL of phosphate buffer solution (PBS, pH 5.4), and maintained at 32°C to simulate the physiological conditions of human skin to measure the release curve of the essential oil of Elaeagnus angustifolia. Take 2 mL of the same amount, sample it every hour, and replenish it with an equal amount of fresh buffer, measure the release amount of the essential oil of Elaeagnus angustifolia in the Pickering emulsion, and calculate the release rate of the essential oil of Elaeagnus angustifolia by comparing the content of the essential oil of Elaeagnus angustifolia after complete release. The test results are as follows: Fig.12 shown.
[0124] Fig.12 This is the essential oil release curve of the Pickering emulsion prepared in Example 3. Fig.12It can be seen that the essential oil of Elaeagnus angustifolia flower in the Pickering emulsion prepared in Example 3 is rapidly released within the first 10 hours, and then slowly released with a long release time, indicating that the Pickering emulsion prepared by the present invention has a good fragrance retention effect.
[0125] Example 4
[0126] The only difference from Example 1 is that 1.5 g of Pickering emulsion is mixed with 13.5 g of film base, keeping the film-forming solution at 15 g.
[0127] Example 5
[0128] The only difference from Example 1 is that 2.25 g of Pickering emulsion is mixed with 12.75 g of film base, and the film-forming solution is kept at 15 g.
[0129] Comparative Example 1
[0130] The only difference from Example 1 is that the pretreated film substrate is directly poured into the culture dish and the film-forming solution is kept at 15 g.
[0131] The acne patches prepared in Comparative Example 1, Example 1 and Examples 4-5 were cut into appropriate sizes, attached to conductive tape, sprayed with a layer of gold before observation, and the accelerating voltage was set to 5.0 kV. Frozen fracture was performed in liquid nitrogen, and cross-sectional analysis was performed. The results are shown in FIG. Fig.13 shown.
[0132] Fig.13 The following are scanning electron microscope images of the cross sections of the acne patches prepared in Comparative Example 1, Example 1, and Examples 4 to 5. Fig.13 It can be seen that the surface of comparative example 1 is smooth and presents a continuous structure without any phase separation, which is due to the good compatibility of chitosan with the patch matrix. The cross-sectional images of Examples 1 and Examples 4-5 show a less continuous structure. The presence of tea tree oil Pickering emulsion can be seen on the cross-section of the acne patch, and there are some holes in the structure. After adding tea tree oil Pickering emulsion, some regular spheres of almost the same size can be seen in the entire patch. The tea tree oil emulsion is well distributed in the entire patch matrix, indicating good compatibility between the dispersed phase and the continuous phase.
[0133] The antibacterial patch prepared in Example 1, Examples 4-5 and Comparative Example 1 was subjected to an in vitro antibacterial test. The test method was as follows: the antibacterial performance of the composite antibacterial patch against Staphylococcus aureus and Propionibacterium acnes was determined by the antibacterial zone method. The antibacterial activity of Comparative Example 1 and Example 1, Examples 4-5 against Staphylococcus aureus and Propionibacterium acnes was evaluated by measuring the antibacterial inhibition zone. As shown in Table 2.
[0134] Table 2 Diameters of inhibition zones of different bacteria under the action of composite films
[0135] sample Staphylococcus aureus (mm) Propionibacterium acnes (mm) Comparative Example 1 5 17.83±0.58 Example 1 10.23±0.25 20.33±0.76 Example 4 17.7±2.08 22.67±0.58 Example 5 19.83±1.26 23.17±0.76
[0136] As shown in Table 2, Comparative Example 1 has no obvious antibacterial zone against Staphylococcus aureus, while Examples 1 and Examples 4-5 have obvious inhibitory effects on Staphylococcus aureus and Propionibacterium acnes. The antibacterial ability of the acne patch increases with the increase of the content of Pickering emulsion, and the antibacterial ability against Propionibacterium acnes is better than that against Staphylococcus aureus, which indicates that the acne patch prepared by the present invention has excellent antibacterial performance.
[0137] The acne patches of Example 1, Examples 4-5 and Comparative Example 1 were used for human skin patch testing: human safety testing was performed with reference to the human skin patch test method in the "Technical Specifications for Safety of Cosmetics". Test method: Select an area not exceeding 50mm 2 , a qualified spot test device with a depth of about 1mm, put the acne patches of Example 1, Examples 4-5 and Comparative Example 1 into the small chamber of the spot tester, and the dosage is about 0.020g-0.025g. The negative control well is a blank control (no substance is placed). The spot tester with the acne patches of Example 1, Examples 4-5 and Comparative Example 1 is applied to the back or curved side of the forearm of the subject with a low-allergenic tape, and gently pressed with the palm of the hand to evenly apply it on the skin for 24 hours. Observe the skin reaction 30 minutes (after the indentation disappears), 24 hours and 48 hours after removing the spot tester of the acne patches of Example 1, Examples 4-5 and Comparative Example 1, and record the observation results. The test results are shown in Table 3.
[0138] Table 3 Human patch test results
[0139]
[0140] According to the "Technical Specifications for Safety of Cosmetics", if more than 5 cases of grade 1 adverse skin reactions or more than 2 cases of grade 2 adverse skin reactions occur among 30 subjects, or any grade 3 or above adverse skin reactions occur, the test substance is judged to have obvious adverse reactions to the human body. The results show that Example 1, Examples 4 to 5 and Comparative Example 1 were all negative during the entire test period and no adverse reactions occurred. The acne patch prepared by the present invention has no potential adverse effects on human skin and has good safety.
[0141] Efficacy index for human body: Determine the acne removal efficacy of the acne patch. The test method is: select 10 volunteers, including 4 male and 6 female volunteers with an average age of 23±1.5 years old. For each volunteer, randomly select 5 inflamed acne, and use comparative example 1 (circle 1), embodiment 1 (circle 2), embodiment 4 (circle 3), embodiment 5 (circle 4), and blank (circle 5) for treatment respectively. Through facial image analysis, the subjects cleaned their faces for 30 minutes and then took facial images with VISIA-CR skin image analyzer. The results are as follows Fig.14 shown.
[0142] Fig.14 The following are the human efficacy comparison diagrams of the acne patches prepared using Example 1, Examples 4-5 and Comparative Example 1, wherein 1 is the human efficacy comparison diagram of the acne patch prepared using Comparative Example 1, 2 is the human efficacy comparison diagram of the acne patch prepared using Example 1, 3 is the human efficacy comparison diagram of the acne patch prepared using Example 4, 4 is the human efficacy comparison diagram of the acne patch prepared using Example 5, and 5 is a blank human efficacy comparison diagram. Fig.14 It can be seen that the acne area on the face was obviously red, swollen and inflamed before use, and the size of the acne lesions was significantly reduced after using the acne patches of Example 1 and Examples 4-5 for seven days, and the acne removal effects of Example 1 and Examples 4-5 were significantly better than those of Comparative Example 1. For acne containing pus, the pus was significantly eliminated, which shows that the acne patch prepared by the present invention has a good therapeutic effect on acne.
[0143] As can be seen from the above embodiments, the present invention provides a Pickering emulsion based on silane coupling agent modified attapulgite and its preparation method and application, wherein attapulgite is pretreated with sodium pyrophosphate, the pretreated attapulgite is dispersed in an ethanol aqueous solution, and then a silane coupling agent is added for hydrolysis modification to obtain modified attapulgite, and the modified attapulgite, aqueous phase and oil-soluble functional ingredients are mixed and homogenized to obtain Pickering emulsion. The attapulgite mineral raw material used in the present invention has abundant reserves, is natural and non-toxic, has a simple and efficient preparation process, and is green and environmentally friendly. Compared with traditional emulsions based on surfactants, the prepared Pickering emulsion can more effectively stabilize a variety of cosmetic oil-soluble functional ingredients, and is mild and non-irritating to human skin, and is particularly suitable for application in green, environmentally friendly and mild "pure beauty" products.
[0144] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for preparing a Pickering emulsion based on silane coupling agent modified attapulgite, characterized in that: The steps include: (1) mixing attapulgite, sodium pyrophosphate and water to obtain pretreated attapulgite; (2) dispersing the pretreated attapulgite in an ethanol aqueous solution, and then adding a silane coupling agent for hydrolysis modification to obtain modified attapulgite; (3) The modified attapulgite, the aqueous phase and the oil-soluble functional component are mixed and homogenized to obtain a Pickering emulsion.
2. The method for preparing the Pickering emulsion based on silane coupling agent modified attapulgite according to claim 1, characterized in that: In the step (1), the dosage ratio of attapulgite, sodium pyrophosphate and water is 5-30 g: 0.1-10 g: 200-400 mL; The purity of the attapulgite is 50-99%.
3. The method for preparing the Pickering emulsion based on silane coupling agent modified attapulgite according to claim 1 or 2, characterized in that: In the step (2), the dosage ratio of the pretreated attapulgite, ethanol aqueous solution and silane coupling agent is 0.05-2 g: 50 mL: 0.01-10 mL.
4. The method for preparing the Pickering emulsion based on silane coupling agent modified attapulgite according to claim 3, characterized in that: In the step (2), the volume concentration of the ethanol aqueous solution is 30 to 90%; The silane coupling agent includes one or more of γ-methacryloxypropyltrimethoxysilane, γ-aminopropyltriethoxysilane, n-octyltriethoxysilane, n-decyltriethoxysilane, dodecyltriethoxysilane and octadecyltriethoxysilane.
5. The method for preparing the Pickering emulsion based on silane coupling agent modified attapulgite according to claim 4, characterized in that: In the step (2), the temperature of the hydrolysis modification is 20 to 40° C., and the time of the hydrolysis modification is 1 to 3 hours; The pH value of the hydrolysis modification is 2 to 14; The hydrolysis modification is carried out under stirring, and the stirring speed is 200-600 rpm; The particle size of the modified attapulgite is 100 to 500 meshes.
6. The method for preparing the Pickering emulsion based on silane coupling agent modified attapulgite according to claim 1, 4 or 5, characterized in that: In the step (3), the modified attapulgite, the aqueous phase and the oil-soluble functional ingredient are used in a ratio of 0.05-2 g: 4-8 mL: 2-5 mL; The homogenization speed is 5000-18000 rpm, and the homogenization time is 1-8 minutes. 。 7. The method for preparing the Pickering emulsion based on silane coupling agent modified attapulgite according to claim 6, characterized in that: In the step (3), the oil-soluble functional ingredients include one or more of vegetable oil, animal oil, mineral oil, antibacterial agent, antioxidant, colorant and sunscreen; The vegetable oil includes one or more of olive oil, almond oil and peony seed oil; The animal oil includes sheep oil and / or bird's nest oil; The mineral oil includes white oil and / or silicone oil.
8. The method for preparing the Pickering emulsion based on silane coupling agent modified attapulgite according to claim 7, characterized in that: The antibacterial agent includes tea tree essential oil, angustifolia essential oil, lavender essential oil, forsythia essential oil, prickly ash essential oil, eucalyptus essential oil, peppermint essential oil, clove essential oil, rosemary essential oil, cinnamon essential oil, lemon balm essential oil, frankincense essential oil, eucalyptus essential oil, sage essential oil, magnolia bark extract or sophora flavescens extract; The antioxidant includes astaxanthin, lutein, vitamin E, butylated hydroxyanisole, 2,6-di-tert-butylated cresol, propyl gallate, tocopherol acetate, lipoic acid or coenzyme Q10; The colorant includes curcumin, capsanthin, hematoxylin, guaiazulene, carotenoids, cochineal, persimmon, smoky blue or squalane pigment; The sunscreen includes ethylhexyl methoxycinnamate, isoamyl methoxycinnamate, ethylhexyl dimethylparaaminobenzoate, phenylbenzimidazole sulfonic acid, octocrylene, butyl methoxydibenzoylmethane or ethyl triazone.
9. The Pickering emulsion prepared by the method for preparing the Pickering emulsion based on silane coupling agent modified attapulgite according to any one of claims 1 to 8.
10. The use of the Pickering emulsion according to claim 9 in the preparation of daily chemical products, characterized in that: The daily chemical products include one or more of fragrances, gels, perfumes, solid ointments, detergents, isolation creams, foundation creams, makeup, acne patches, mosquito repellent patches and disinfectants.
Citation Information
Patent Citations
Modified attapulgite nano particles and preparation method thereof
CN106006656A
Preparation method of Chinese soapberry modified attapulgite and plant essential oil O / W type Pickering emulsion of Chinese soapberry modified attapulgite
CN114540045A
One-step process for purification and organic modification of attapulgite
CN116730350A
Method for preparing silane coupler modified attapulgite
CN1843911A