Self-cleaning film as well as preparation method and application thereof
By applying gel materials of phenolic resin and Mxene nanosheets on the surface of the film, photocatalytic degradation of pollutants is used to solve the problem of biological contamination in membrane separation technology, the self-cleaning and antibacterial properties of the film are achieved, and the water effluent is improved. Removal effect.
Patent Information
- Application Number
- CN202410932100.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-01
AI Technical Summary
In membrane separation technology, membrane pollution caused by biological contamination is difficult to remove, resulting in a decrease in water effluent, and the existing cleaning methods are of limited effect.
The base film surface is coated with gel material composed of phenolic resin and Mxene nanosheets, and the visible light irradiation produces H2O2 and photothermal effect to degrade pollutants, and has antibacterial properties.
It effectively avoids membrane pollution, improves the self-cleaning performance and antibacterial ability of the membrane, and maintains high throughput and pollutant removal effects.
Smart Images

Figure CN118874235A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the technical field of membrane materials, and specifically relates to a self-cleaning membrane and a preparation method and application thereof. Background Art
[0002] Wastewater treatment is one of the important means to solve the problems of water shortage and water pollution. Membrane separation technology is widely used in deep treatment of wastewater and water purification due to its advantages such as simple equipment, energy saving, no phase change, no secondary pollution, and strong adaptability. However, membrane fouling is an unavoidable problem in the membrane separation process, among which biological fouling is the main cause of microfiltration membrane fouling. Due to its high adhesion and stability, it is difficult to remove it through simple physical and / or chemical cleaning, resulting in a significant decrease in water output.
[0003] Therefore, it is necessary to provide a self-cleaning membrane and a preparation method and application thereof to solve the problems raised in the above background technology. Summary of the invention
[0004] The present application provides a self-cleaning film and a preparation method and application thereof, wherein a gel material is coated on the surface of a base film, and H generated by a phenolic resin on the surface of the gel is used to generate a self-cleaning film under visible light irradiation. 2 O 2 The photothermal effect of MXene can degrade and remove pollutants on the membrane surface, effectively avoiding membrane pollution; at the same time, it can also kill bacteria in the water and has certain antibacterial properties.
[0005] In order to solve the above technical problems, the technical solution of this application is:
[0006] A method for preparing a self-cleaning membrane comprises the following steps:
[0007] Step S1, providing a basement membrane, placing the basement membrane in a dopamine solution, and cross-linking to obtain a modified basement membrane;
[0008] Step S2, adding resorcinol and formaldehyde into oxalic acid solution at a mass ratio of 1:2, stirring and dissolving, adding Mxene nanosheets into the solution, reacting in a high-temperature reactor, and filtering after the reaction to obtain Mxene@phenolic resin;
[0009] Step S3, adding acrylic acid, ammonium persulfate, and a cross-linking agent into an aqueous solution, and after fully dissolving, adding the Mxene@phenolic resin prepared in step S2 to obtain a gel solution;
[0010] Step S4, coating the gel solution prepared in step S3 on the surface of the modified base film, and freeze-drying the gel after solidification to obtain a self-cleaning film.
[0011] As an improvement, in step S1, the base film is selected from any one of PVDF film, CPVC film, PP film, and ceramic film; the concentration of the dopamine solution is 0.2-2%, and the cross-linking time is 10-60 min.
[0012] As an improvement, in step S2, the amount of Mxene nanosheets added is 1%-5% of resorcinol; and the concentration of the oxalic acid solution is 0.1 mol / L.
[0013] As an improvement, in step S2, the reaction temperature in the high temperature reactor is 200-250°C.
[0014] As an improvement, in step S3, the crosslinking agent is N,N′-methylenebisacrylamide, and the added amount is 0.2-0.6% of the added amount of acrylic acid; the added amount of ammonium persulfate is 0.8-1.4% of the added amount of acrylic acid, the added amount of water is 5 times the added amount of acrylic acid, and the added amount of Mxene@phenolic resin is 0.5%-2% of the added amount of acrylic acid.
[0015] As an improvement, step S4 specifically includes the following process:
[0016] The gel solution was sprayed on the surface of the modified base film with a spray gun, and then placed in a water bath at 60° C. After the gel solidified, it was taken out and freeze-dried to obtain a self-cleaning film.
[0017] The present application also provides a self-cleaning membrane, which is prepared using the above-mentioned method for preparing the self-cleaning membrane.
[0018] The present application also provides an application of the above-mentioned self-cleaning membrane, which is used as a sewage treatment membrane under visible light conditions.
[0019] The beneficial effects of this application are:
[0020] The base film was modified with dopamine, and then Mxene@phenolic resin was prepared with resorcinol, formaldehyde and Mxene nanosheets. The Mxene@phenolic resin was cross-linked with acrylic acid, a cross-linking agent and ammonium persulfate to obtain a gel solution. Finally, the gel solution was coated on the surface of the modified substrate to obtain a self-cleaning film. The H generated by the phenolic resin on the gel surface under visible light irradiation was used to 2 O 2 The photothermal effect of MXene can degrade and remove pollutants on the membrane surface, effectively avoiding membrane pollution; at the same time, it can also kill bacteria in the water and has certain antibacterial properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments are briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work, among which:
[0022] Figure 1 The surface SEM image of the self-cleaning membrane prepared in Example 2 is shown. DETAILED DESCRIPTION
[0023] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0024] See also Figure 1 The present application provides a method for preparing a self-cleaning membrane, comprising the following steps:
[0025] Step S1, providing a basement membrane, placing the basement membrane in a dopamine solution, and cross-linking to obtain a modified basement membrane;
[0026] Step S2, adding resorcinol and formaldehyde in a mass ratio of 1:2 to an oxalic acid solution, stirring and dissolving, adding Mxene nanosheets to the solution, reacting under high temperature and high pressure conditions, and filtering after the reaction to obtain Mxene@phenolic resin;
[0027] Step S3, adding acrylic acid, ammonium persulfate, and a cross-linking agent into an aqueous solution, and adding the Mxene@phenolic resin after fully dissolving to obtain a gel solution;
[0028] Step S4, coating the gel solution on the surface of the modified base film, and freeze-drying the gel after solidification to obtain a self-cleaning film.
[0029] In step S1, the base film is selected from any one of PVDF film, CPVC film, PP film and ceramic film; the concentration of the dopamine solution is 0.2-2%, and the cross-linking time is 10-60 minutes.
[0030] In step S2, the amount of MXene nanosheets added is 1%-5% of resorcinol, the concentration of oxalic acid solution is 0.1 mol / L, and the reaction temperature in the high temperature reactor is 200-250°C.
[0031] In step S3, the crosslinking agent is N,N′-methylenebisacrylamide, and the addition amount is 0.2-0.6% of the addition amount of acrylic acid; the addition amount of ammonium persulfate is 0.8-1.4% of the addition amount of acrylic acid; the addition amount of water is 5 times the addition amount of acrylic acid; the addition amount of Mxene@phenolic resin is 0.5%-2% of the addition amount of acrylic acid.
[0032] Step S4 specifically includes the following process:
[0033] The gel solution was sprayed on the surface of the modified base film with a spray gun, and then placed in a water bath at 60° C. After the gel solidified, it was taken out and freeze-dried to obtain a self-cleaning film.
[0034] The present application also provides a self-cleaning membrane, which is prepared using the above-mentioned method for preparing the self-cleaning membrane.
[0035] The present application also provides an application of the above-mentioned self-cleaning membrane, which is used as a sewage treatment membrane under visible light conditions.
[0036] Example 1
[0037] The PVDF base membrane with an average pore size of 0.1 μm was immersed in ethanol for 1 hour, taken out, washed with water, placed in 2 mg / mL dopamine tris buffer (pH=8.5), and allowed to stand for 30 minutes to obtain a modified base membrane.
[0038] Example 2
[0039] 0.400 g of resorcinol, 0.56 mL of formaldehyde, and 300 μL of 1 mol / L oxalic acid were placed in a beaker, stirred to dissolve, and then 50 mg of Mxene nanosheets were added. After reacting in a reactor at 250 °C for 12 h, the mixture was taken out and filtered to obtain Mxene@phenolic resin.
[0040] 2.0 g of acrylic acid, 0.06 g of ammonium persulfate, and 0.01 g of a cross-linking agent were added to 10 mL of an aqueous solution, and after magnetic stirring for 1 h, 5 mg of the prepared Mxene@phenolic resin was added and stirred evenly to obtain a hydrogel solution;
[0041] The hydrogel solution was loaded into a spray gun and sprayed onto the surface of the modified base film prepared in Example 1 with a diameter of 47 mm, and then placed in a 60° C. water bath for reaction for 30 minutes. The film was taken out and freeze-dried to obtain a self-cleaning film.
[0042] The surface SEM image of the self-cleaning membrane prepared in this example is as follows: Figure 1 As shown, from Figure 1 It can be seen that the gel material forms a 3D porous structure on the membrane surface, which does not affect the flux of the membrane; at the same time, the hydrogen bonds formed between the catalyst and the gel make it evenly distributed on the gel skeleton, avoiding the fall-off of the catalyst.
[0043] Example 3
[0044] 2.0 g of acrylic acid, 0.06 g of ammonium persulfate, and 0.01 g of a cross-linking agent were added to 10 mL of an aqueous solution, and after magnetic stirring for 1 h, 5 mg of Mxene nanosheets were added and stirred evenly to obtain a hydrogel solution;
[0045] The hydrogel solution was loaded into a spray gun and sprayed onto the surface of the modified base film prepared in Example 1 with a diameter of 47 mm, and then placed in a 60° C. water bath for reaction for 30 minutes. The film was taken out and freeze-dried to obtain a self-cleaning film.
[0046] Example 4
[0047] 2.0 g of acrylic acid, 0.06 g of ammonium persulfate, and 0.01 g of a cross-linking agent were added to 10 mL of an aqueous solution, and after magnetic stirring for 1 h, 5 mg of a phenolic resin was added and stirred evenly to obtain a hydrogel solution;
[0048] The hydrogel solution was loaded into a spray gun and sprayed onto the surface of the modified base film prepared in Example 1 with a diameter of 47 mm, and then placed in a water bath at 60° C. to react for 30 minutes. The film was taken out and freeze-dried to obtain a self-cleaning film.
[0049] Example 5
[0050] 0.400 g of resorcinol, 0.56 mL of formaldehyde, and 300 μL of 1 mol / L oxalic acid were placed in a beaker, stirred and dissolved, and 10 mg of Mxene nanosheets were added. After reacting in a reactor at 250 °C for 12 h, the mixture was taken out and filtered to obtain Mxene@phenolic resin.
[0051] 2.0 g of acrylic acid, 0.06 g of ammonium persulfate, and 0.01 g of a cross-linking agent were added to 10 mL of an aqueous solution, and after magnetic stirring for 1 h, 5 mg of the prepared Mxene@phenolic resin was added and stirred evenly to obtain a hydrogel solution;
[0052] The hydrogel solution was loaded into a spray gun and sprayed onto the surface of the modified base film prepared in Example 1 with a diameter of 47 mm, and then placed in a 60° C. water bath for reaction for 30 minutes. The film was taken out and freeze-dried to obtain a self-cleaning film.
[0053] Example 6
[0054] 0.400 g of resorcinol, 0.56 mL of formaldehyde, and 300 μL of 1 mol / L oxalic acid were placed in a beaker, stirred and dissolved, and 100 mg of Mxene nanosheets were added. After reacting in a reactor at 250 °C for 12 h, the mixture was taken out and filtered to obtain Mxene@phenolic resin.
[0055] 2.0 g of acrylic acid, 0.06 g of ammonium persulfate, and 0.01 g of a cross-linking agent were added to 10 mL of an aqueous solution. After magnetic stirring for 1 h, 5 mg of the prepared Mxene@phenolic resin was added and stirred evenly.
[0056] The hydrogel solution was loaded into a spray gun and sprayed onto the surface of the modified base film prepared in Example 1 with a diameter of 47 mm, and then placed in a 60° C. water bath for reaction for 30 minutes. The film was taken out and freeze-dried to obtain a self-cleaning film.
[0057] Example 7
[0058] Take 0.400 g of resorcinol and 0.56 mL of formaldehyde, add 300 μL of 1 mol / L oxalic acid and put them in a beaker. After stirring to dissolve, add 100 mg of Mxene nanosheets and react in a reactor at 250 °C for 12 h. Then take out and filter to obtain Mxene@phenolic resin.
[0059] Take 2.0g acrylic acid, 0.06g ammonium persulfate, and 0.01g cross-linking agent and add them to 10mL aqueous solution. After magnetic stirring for 1h, add 10mg Mxene@phenolic resin and stir evenly.
[0060] The hydrogel solution was loaded into a spray gun and sprayed onto the surface of the modified base film prepared in Example 1 with a diameter of 47 mm, and then placed in a 60° C. water bath for reaction for 30 minutes. The film was taken out and freeze-dried to obtain a self-cleaning film.
[0061] Example 8
[0062] Take 0.400 g of resorcinol and 0.56 mL of formaldehyde, add 300 μL of 1 mol / L oxalic acid and put them in a beaker. After stirring to dissolve, add 100 mg of Mxene nanosheets and react in a reactor at 250 °C for 12 h. Then take out and filter to obtain Mxene@phenolic resin.
[0063] Take 2.0g acrylic acid, 0.06g ammonium persulfate, and 0.01g cross-linking agent and add them to 10mL aqueous solution. After magnetic stirring for 1h, add 15mg Mxene@phenolic resin and stir evenly.
[0064] The hydrogel solution was loaded into a spray gun and sprayed onto the surface of the modified base film prepared in Example 1 with a diameter of 47 mm, and then placed in a 60° C. water bath for reaction for 30 minutes. The film was taken out and freeze-dried to obtain a self-cleaning film.
[0065] The membranes obtained in Examples 1-8 were tested for photocatalytic degradation, flux recovery rate and antibacterial performance using 10 mg / L bovine serum albumin (BSA) as a model pollutant.
[0066] Photocatalytic degradation performance test: The film prepared in Examples 1-8 was placed in a model pollutant solution and stirred for 30 minutes in the dark to reach adsorption equilibrium. Under irradiation with a 300W xenon lamp (with a 420nm filter), the change of BSA concentration over time was recorded. The test results are summarized in Table 1.
[0067] Self-cleaning performance test: The membrane body prepared in Examples 1-8 was fixed on a cross-flow filtration device. After stabilization under a transmembrane pressure difference of 0.2Mpa, the Pseudomonas aeruginosa suspension experiment was continuously performed for 60 minutes, and then the membrane surface was washed with deionized water to calculate the pure water flux. The cleaned membrane body was placed in a groove with a quartz window, and under the irradiation of a 300w xenon lamp (with a 420nm filter), pure water was continuously filtered for 60 minutes, the membrane was cleaned, and the pure water flux was calculated. According to the pure water flux test method, the pure water flux recovery rate was tested, and the test results are summarized in Table 1.
[0068] Antibacterial performance test: The glassware and culture medium solution were sterilized at 121°C for 20 min. The antibacterial activity of the membrane against Pseudomonas aeruginosa was determined by the dilution plate count method. First, 50 μL of 10 8 CFU / mL of Pseudomonas aeruginosa suspension was dispersed on nutrient agar medium. Then, the membrane was placed in nutrient agar medium. Finally, the plate was incubated in the dark at 37°C for 24 hours. Irradiate under visible light (wavelength > 420nm) for 1 hour. Remove the upper bacterial liquid, take out the membrane with bacteria on the surface, and rinse the bacteria off the membrane surface with physiological saline. Take 1mL of the bacterial suspension on the membrane surface and inoculate it on the surface of the solid culture medium. After constant temperature culture at 37°C for 24 hours, the number of bacteria was counted and the inhibition rate was calculated. The test results are summarized in Table 1.
[0069] Table 1 Test results of photocatalytic degradation performance, self-cleaning performance and antibacterial performance of various embodiments
[0070]
[0071]
[0072] From Table 1 we can see that:
[0073] In the photocatalytic degradation performance experiment, the modified base membrane of Example 1 has the lowest removal rate of BSA, which is only 53%, indicating that the base membrane modified by dopamine alone has a poor removal effect on pollutants; by comparing Implementation 2-4, it can be seen that the addition of phenolic resin and Mxene nanosheets can improve the removal effect of the membrane on pollutants, and the removal rate of Implementation 2 is greatly improved compared with Implementation 3 and Implementation 4, indicating that the self-cleaning membrane prepared by the method of the present application can obtain excellent pollutant removal effect and effectively avoid membrane pollution; comprehensive comparison of Examples 5-8 shows that the removal rate is affected by the addition amount of phenolic resin and Mxene nanosheets, among which Example 8 achieves the highest removal rate, indicating that the addition amount in Implementation 8 is the optimal addition amount, which can be used to guide actual production.
[0074] In the cross-flow filtration experiment of the self-cleaning performance test, the membrane flux of Example 1 decayed sharply within 1 hour, the membrane flux of Example 2 decreased the slowest, and the flux was always greater than the flux of the membrane of Example 1 after 24 hours of operation; the membrane flux of Examples 3-8 was basically the same as that of Example 2, and all maintained above 90%, indicating that in the self-cleaning membrane prepared in the present application, the 3D porous structure of the gel material can not only firmly and evenly distribute the catalyst on the gel skeleton, but also has little effect on the membrane flux.
[0075] In the antibacterial performance test, Example 1 had no obvious inhibitory effect on Pseudomonas aeruginosa, while Examples 2-8 had a good inhibitory effect on Pseudomonas aeruginosa, indicating that the self-cleaning membrane prepared in the present application can kill bacteria in water under visible light irradiation and has certain antibacterial properties.
[0076] The embodiments of the present application are described above in conjunction with the accompanying drawings, but the present application is not limited to the above-mentioned specific implementation methods. The above-mentioned specific implementation methods are merely illustrative and not restrictive. Under the guidance of the present application, ordinary technicians in this field can also make many forms without departing from the purpose of the present application and the scope of protection of the claims, all of which are within the protection of the present application.
Claims
1. A method for preparing a self-cleaning membrane, characterized in that: The steps include: Step S1, providing a basement membrane, placing the basement membrane in a dopamine solution, and cross-linking to obtain a modified basement membrane; Step S2, adding resorcinol and formaldehyde into oxalic acid solution at a mass ratio of 1:2, stirring and dissolving, adding Mxene nanosheets into the solution, reacting in a high-temperature reactor, and filtering after the reaction to obtain Mxene@phenolic resin; Step S3, adding acrylic acid, ammonium persulfate, and a cross-linking agent into an aqueous solution, and after fully dissolving, adding the Mxene@phenolic resin prepared in step S2 to obtain a gel solution; Step S4, coating the gel solution prepared in step S3 on the surface of the modified base film, and freeze-drying the gel after solidification to obtain a self-cleaning film.
2. The method for preparing a self-cleaning film according to claim 1, characterized in that: In step S1, the base film is selected from any one of PVDF film, CPVC film, PP film and ceramic film; the concentration of the dopamine solution is 0.2-2%, and the cross-linking time is 10-60 minutes.
3. The method for preparing the self-cleaning film according to claim 1, characterized in that: In step S2, the added amount of Mxene nanosheets is 1%-5% of resorcinol; and the concentration of the oxalic acid solution is 0.1 mol / L.
4. The method for preparing a self-cleaning film according to claim 1, characterized in that: In step S2, the reaction temperature in the high temperature reactor is 200-250°C.
5. The method for preparing a self-cleaning film according to claim 1, characterized in that: In step S3, the crosslinking agent is N,N′-methylenebisacrylamide, and the addition amount is 0.2-0.6% of the addition amount of acrylic acid; the addition amount of ammonium persulfate is 0.8-1.4% of the addition amount of acrylic acid; the addition amount of water is 5 times the addition amount of acrylic acid; the addition amount of Mxene@phenolic resin is 0.5%-2% of the addition amount of acrylic acid.
6. The method for preparing a self-cleaning film according to claim 1, characterized in that: Step S4 specifically includes the following process: The gel solution was sprayed on the surface of the modified base film with a spray gun, and then placed in a water bath at 60° C. After the gel solidified, it was taken out and freeze-dried to obtain a self-cleaning film.
7. A self-cleaning membrane, characterized in that: The self-cleaning film is prepared by the preparation method of any one of claims 1 to 6.