Catalyst for preparing adipic acid through selective oxidation of cyclohexanone as well as preparation method and application of catalyst

Through the hydrothermal method of the manganese salt-modified carbon material catalyst, adipic acid is prepared by molecular oxygen oxidation cyclohexanone, which solves the pollution and cost problems of the cyclohexanone oxidation process in the prior art, and achieves high selectivity and clean production. And the catalyst has good stability and cycle performance.

CN118874458AActive Publication Date: 2024-11-01HUNAN NORMAL UNIVERSITY

Patent Information

Application Number
CN202411028117.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-11-01
Estimated Expiration
2044-07-30

AI Technical Summary

Technical Problem

The prior art has problems such as high pollution, equipment corrosion, high oxidant cost, difficult reaction rate and difficult catalyst separation in the process of oxidation of cyclohexanone, and the cyclohexanone cleaning oxidation method cannot be effectively used.

Method used

Using manganese salt modified carbon material as catalyst, x%Mn/C catalyst is prepared by hydrothermal method, molecular oxygen is used as oxidant, and cyclohexanone is selected for oxidation of cyclohexanone to form a stable heterogeneous catalyst to ensure the catalyst hydrothermal stability and recycling performance.

Benefits of technology

Highly selective, clean and pollution-free production of adipic acid is achieved. The catalyst has good hydrothermal stability and recycling performance, which reduces production costs and avoids the use of NOx and high-value oxidants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874458A_ABST
    Figure CN118874458A_ABST
Patent Text Reader

Abstract

The invention discloses a catalyst for preparing adipic acid by selective oxidation of cyclohexanone as well as a preparation method and application of the catalyst, and relates to manganese salt modified organic carboxylic acid. The preparation method of the catalyst for preparing adipic acid through selective oxidation of cyclohexanone comprises the following steps: dissolving manganese salt in a mixed solution of ethanol and deionized water, stirring to be uniform, adding organic carboxylic acid, dissolving, stirring for more than 12 hours, drying, and calcining in N2 atmosphere. The application of the catalyst for preparing adipic acid through selective oxidation of cyclohexanone comprises the following operation steps: mixing the catalyst, acetic acid and cyclohexanone, heating to a reaction temperature, continuously introducing oxygen, pressurizing, starting a reaction, and cooling to room temperature after the reaction is finished, so as to obtain the catalyst for preparing adipic acid through selective oxidation of cyclohexanone. The catalyst is good in hydrothermal stability, convenient to filter and separate and good in recycling performance, the preparation method is stable, controllable and good in reproducibility, the adipic acid selectivity is high, and the production process is clean and free of pollution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of catalyst preparation, and in particular to a catalyst for preparing adipic acid by selective oxidation of cyclohexanone, and a preparation method and application thereof. Background Art

[0002] Adipic acid (AA) is a hexacarbonyl dibasic acid with the molecular formula C6H 10O4, white crystalline powder, odorless, is an aliphatic dibasic acid with important application value. It can undergo salt formation, esterification, aminoacyl and other reactions. At the same time, adipic acid can also undergo polycondensation with diamines and diols to produce high molecular polymers. The application of adipic acid is divided into two categories: nylon and non-nylon: the application of adipic acid in nylon products is mainly to manufacture nylon 66 salt (about 75%), and nylon 66 salt polycondensation produces nylon 66 resin and nylon 66 fiber; the application in non-nylon is mainly to produce polyester polyols, and then produce polyurethane products, such as polyurethane synthetic leather resin, polyurethane sole resin, thermoplastic polyurethane (TPU), polyurethane adhesive, polyurethane rubber and polyurethane foam plastics. It can be used to manufacture polyvinyl chloride, which is the third most widely produced synthetic plastic polymer in the world. In addition, adipic acid is also widely used in medicine, fragrances, pesticides, coatings, food, adhesives and dyes (see [1] Cui Xiaoming. Market status and development prospects of adipic acid at home and abroad [J]. Fine and Specialty Chemicals, 2013, 21(1): 6-16. and [2] Yang Yansong, Jian Jian, You Kuiyi et al. Research progress in synthetic adipic acid technology [J]. Chemical Industry Progress, 2013, 32(11): 2638-2643.). There are many methods for producing adipic acid: preparing adipic acid from cyclohexene as raw material, preparing adipic acid from cyclohexanone as raw material, preparing adipic acid from cyclohexane as raw material, and preparing adipic acid from renewable resources such as starch or cellulose as raw materials (currently in the research stage). The global annual production of AA exceeds 3 million tons, growing at an annual rate of 3-5%. It is estimated that by 2025, the global AA market will exceed US$8 billion (see [3] Skoog E, Shin JH, Saez-Jimenez V, et al. Biobased adipic acid-The challenge of developing the production host[J]. Biotechnology advances, 2018, 36(8): 2248-2263. and [4] Adipic Acid Market Size Worth $8.0 Billion By 2024 CAGR 4.7%. [cited 2020 Jan 22]. and [5] Bart JCJ, Cavallaro S. Transiting from adipic acid to bioadipic acid. 1, Petroleum-based processes[J]. Industrial & Engineering Chemistry Research, 2015, 54(1): 1-46.). In recent years, researchers have been committed to the study of green synthesis technology of adipic acid, and new catalysts have become a research hotspot.The more common catalysts include heteropolyacids and heteropolyacid salts, tungstic acid and tungstates, molecular sieve catalysts, supported catalysts and other new catalysts (see [6] Ren Shuiying, Xie Zhengfeng, Xie Xiaopeng, et al. Clean method for catalytic oxidation synthesis of adipic acid [J]. Progress in Chemistry, 2009, 21(4): 663-671. and [7] Di Dapeng, Lu Jie, Lou Yang, et al. Adipic acid production process technology and research progress [J]. Petroleum Refining and Chemical Engineering, 2013, 24(5): 10-12.). In view of the growing demand for AA and the desire to reduce its negative impact on the environment, a lot of efforts have been made to develop more sustainable processes. The focus of petroleum-based raw materials is on NO. x Mitigation strategies and NO generation x Cyclohexanone is an intermediate product of cyclohexane oxidation. In industry, nitric acid is usually used to oxidize cyclohexanone to produce adipic acid (industrial process as shown in the attached Figure 1 ), although it can achieve a conversion rate of up to 90% and a selectivity of about 70% for adipic acid, it will also release a large amount of toxic gases such as nitrogen oxides, which seriously pollute the environment. In addition, concentrated nitric acid is highly corrosive and causes serious corrosion to equipment. The clean oxidation of cyclohexanone has always been a research hotspot in the industry.

[0003] An environmentally friendly cyclohexanone oxidation method has been developed (Y.Usui, A green method of adipicacid synthesis: organic solvent-and halide-free oxidation of cycloalkanoneswith 30% hydrogen peroxide. Green Chem. 2003, 5, 373-375.), which can convert cyclohexanone into adipic acid at 90°C. This process uses H2WO4 as a catalyst and reacts with 3.3 mol of 30% hydrogen peroxide (H2O2) in a halide and organic solvent. H2WO4 acts as a precatalyst in the reaction, but it is easily further oxidized by H2O2 to produce water-soluble H2[WO(O2)2(OH)2]. It is worth noting that this multiphase reaction shows higher activity under solvent-free conditions. When solvents are used, such as tert-butyl alcohol and dioxane, their presence significantly reduces the efficiency of cyclohexanone conversion to adipic acid, with yields of 31% and 52%, respectively. This method uses H2O2 as an oxidant, which is costly and has certain safety risks.

[0004] CN104276937 discloses a technology for extracting adipic acid and C-5 dibasic acid from the byproducts of cyclohexane oxidation reaction. The technology uses washing water to separate oil and water from cyclohexane oxidation liquid, then concentrates the washing water, and obtains the target compound through nitric acid oxidation and cooling crystallization process. However, this method is only applicable to cyclohexane oxidation liquid that does not contain acetic acid as a solvent. It uses the extraction ability of water to concentrate organic matter in the oil phase and recovers byproducts through oxidation. This method requires the use of nitric acid and has high requirements on the material of the equipment. In addition, it cannot effectively separate and utilize tar impurities in the system.

[0005] CN102850205B discloses a zinc-modified titanium silicon molecular sieve catalyst, which is used to produce 1,2-cyclohexanediol and adipic acid in the oxidation process of cyclohexene. The preparation process is simple, and the catalyst can be obtained by roasting a zinc compound and a heteroatom molecular sieve. Under mild conditions, adipic acid can be effectively synthesized using hydrogen peroxide as an oxidant. However, this method uses organic solvents such as methanol, acetone and acetonitrile in the production process, which may have a negative impact on the environment.

[0006] The production technology of adipic acid needs to be further improved, production efficiency needs to be increased, and production costs need to be reduced. Using H2O2 as an oxidant may seem greener, but in fact, the water produced after the hydrogen peroxide reaction will dissolve with the reactants, and the industry needs to spend a huge amount of money to separate the water. At the same time, H2O2 is a violent oxidant, and the reaction rate is difficult to control, and there is even a risk of explosion. Using nitric acid as an oxidant not only has high requirements on the material and quality of the equipment, but also produces NO x The cost is high in subsequent treatment; using ozone O3 as a green oxidant to obtain a higher adipic acid yield, which does achieve the requirements of environmental friendliness and low pollution, but ozone is not cheap and is difficult to achieve in industrial production.

[0007] Therefore, it is urgent to develop an excellent heterogeneous catalyst that can reduce the difficulty of catalyst separation and increase its service life while ensuring a high adipic acid yield. At the same time, molecular oxygen is used as the oxidant to avoid NO generated by concentrated nitric acid. x And the high cost of H2O2 or other oxidants. Summary of the invention

[0008] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a catalyst for preparing adipic acid by selective oxidation of cyclohexanone and a preparation method and application thereof. The catalyst has good hydrothermal stability and good recycling performance, the preparation method is stable, controllable and reproducible, the selectivity of adipic acid is high, and the production process is clean and pollution-free.

[0009] The technical solution adopted by the present invention to solve its technical problem is to use a catalyst for selective oxidation of cyclohexanone to prepare adipic acid, select a manganese salt to modify a carbon material, the carbon material is an organic carboxylic acid, and the catalyst is expressed as x% Mn / C, where x% is the mass ratio of metallic manganese to the organic carboxylic acid.

[0010] Furthermore, x% is 5 to 9%, and can be selected from 5%, 6%, 7%, 8%, and 9%.

[0011] Furthermore, the manganese salt is selected from at least one of manganese acetate, manganese acetylacetonate, manganese oxalate and manganese chloride.

[0012] Furthermore, the selected organic carboxylic acid is selected from one or more of phthalic acid, isophthalic acid, terephthalic acid, phthalic acid, adipic acid, citric acid, and salicylic acid. Studies have shown that the carboxylic acids selected in the present invention are all polycarboxylic acids, containing two or more carboxyl groups, which are convenient for coordination with manganese ions in manganese salts, and their longer carbon chains can serve as templates to guide the formation of carbon materials, forming an ordered structure through intermolecular interactions.

[0013] The method for preparing a catalyst for preparing adipic acid by selective oxidation of cyclohexanone comprises the following steps:

[0014] The manganese salt is dissolved in a mixed solution of ethanol and deionized water, stirred until uniform, and then an organic carboxylic acid is added to dissolve, stirred for more than 12 hours, and then dried and calcined under a N2 atmosphere to obtain the product.

[0015] Furthermore, the amount of the mixed solution of ethanol and deionized water used is sufficient to dissolve both the manganese salt and the organic carboxylic acid.

[0016] Furthermore, the mixed solution of ethanol and deionized water is a solution in which ethanol and deionized water are mixed in a volume ratio of 1: 1. Studies have shown that when ethanol and deionized water are in a ratio of 1: 1, the polarity of the solution is conducive to uniform mixing of manganese salt and polycarboxylic acid.

[0017] Furthermore, the drying temperature is 70-100° C. Drying is to remove ethanol and deionized water. If the drying temperature is too low, it is easy to cause incomplete drying, and there will still be residual solution in the obtained solid powder, which will affect the catalyst structure formation. If the drying temperature is too high, the polycarboxylic acid will recrystallize into needle-shaped crystals, and finally make the catalyst uneven. The drying time is preferably 4-8 hours, and more preferably 6 hours.

[0018] Furthermore, the calcination temperature is 300°C to 600°C. If the calcination temperature is too low, the coordination between the carboxylic acid anion and the manganese ion is incomplete, so that the manganese ion cannot be firmly anchored on the surface of the carbon material, which ultimately affects the activity of the catalyst in the reaction; if the calcination temperature is too high, it is easy to destroy the formed ordered structure. An inert gas such as N2 is used as a protective gas to ensure that the structure of the carbon material is not destroyed by high temperature.

[0019] Furthermore, the calcination heating rate is 4-6°C / min (preferably 5°C / min). If the heating rate is too slow, the coordination between the carboxylic acid anion and the manganese ion is incomplete, so that the manganese ion cannot be firmly anchored on the surface of the carbon material, which ultimately affects the activity of the catalyst in the reaction; if the heating rate is too fast, it is easy to destroy the formed ordered structure.

[0020] Furthermore, the calcination time is 4 to 8 hours. If the calcination time is too short, the coordination between the carboxylic acid anion and the manganese ion is incomplete, so that the manganese ion cannot be firmly anchored on the surface of the carbon material, which ultimately affects the activity of the catalyst in the reaction; if the calcination time is too long, the formed ordered structure is easily destroyed.

[0021] The application of the catalyst for preparing adipic acid by selective oxidation of cyclohexanone is a method for preparing adipic acid by selective oxidation of cyclohexanone by the catalyst, and the operation steps are as follows:

[0022] The catalyst, acetic acid and cyclohexanone are mixed, heated to the reaction temperature, oxygen is continuously introduced and pressurized to start the reaction. After the reaction is completed, the mixture is cooled to room temperature to obtain the product.

[0023] Furthermore, the mass ratio of catalyst, acetic acid and cyclohexanone is 0.5-2:10-30:100 (preferably 1:20:100). The conversion of cyclohexanone to the enol form in the presence of a trace amount of acetic acid can reduce the reaction energy barrier and accelerate the reaction rate. Too little or too much acetic acid will reduce the selectivity of adipic acid, and too little or too much catalyst will reduce the selectivity of adipic acid.

[0024] Furthermore, oxygen was continuously introduced and pressurized, and the reaction pressure was 0.5-0.8 MPa.

[0025] Furthermore, the reaction temperature is 60 to 80°C (preferably 65 to 75°C).

[0026] Furthermore, the reaction time is 4 to 10 h (preferably 5 to 8 h).

[0027] Furthermore, stirring is maintained throughout the entire reaction process from the addition of materials to the end of the reaction, with a stirring speed of 300 to 600 r / min.

[0028] Recycling application of catalyst for selective oxidation of cyclohexanone to produce adipic acid:

[0029] After filtering the catalyst in the reaction solution, use deionized water and anhydrous ethanol to wash away the organic matter on the catalyst surface, dry it, and re-calcine it under N2 atmosphere using the same calcination conditions as in the catalyst preparation method (the obtained catalyst is recorded as Rz-x%Mn / C, z is the number of catalyst cycle reactions, which can be 2, 3, 4, 5, etc.). New reactants can be added to react under the same conditions.

[0030] Beneficial effects of the present invention:

[0031] The catalyst provided by the invention, in the impregnation process, the manganese salt and the organic carboxylic acid are evenly mixed to ensure that the two are fully in contact. Subsequently, in the calcination process, the carboxyl (-COOH) in the organic carboxylic acid molecule undergoes a deprotonation reaction to form a carboxylic anion (COO-). The oxygen atoms in these carboxylic anions form a coordination bond with the manganese ion in the manganese salt, i.e., an Mn-O bond. This coordination firmly anchors the manganese ion on the skeleton of the carbon material to form a stable composite structure catalyst, which has a good catalytic effect for the reaction. Using molecular oxygen as an oxidant, cyclohexanone can be oxidized to produce adipic acid in one step.

[0032] The Mn / C heterogeneous catalyst of the present invention has the advantages of good hydrothermal stability, easy separation, good recycling performance, etc. The preparation method is stable, controllable, reproducible, and has high selectivity for adipic acid. No three wastes are generated in the production process, and it has the advantages of being clean and pollution-free. The catalyst of the present invention has good hydrothermal stability, can maintain its structural stability and catalytic activity under high temperature and high pressure conditions, the heterogeneous catalyst is easy to filter and separate, has good recycling performance, the preparation method is stable, controllable, reproducible, has high selectivity for adipic acid, and the production process is clean and pollution-free. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 The present invention is a common industrial flow chart for preparing adipic acid by oxidizing cyclohexanone with nitric acid. DETAILED DESCRIPTION

[0034] The present invention is further described in detail below in conjunction with specific embodiments.

[0035] In this specification, unless otherwise specified, the percentages are by mass.

[0036] In the actual production of adipic acid by selective oxidation of cyclohexanone, the selectivity of the target product adipic acid is given priority. The higher the selectivity of adipic acid, the easier the subsequent separation is and the lower the cost is.

[0037] Embodiment 1:

[0038] The application of the catalyst for preparing adipic acid by selective oxidation of cyclohexanone in this embodiment is a method for preparing adipic acid by selective oxidation of cyclohexanone using the catalyst, and the operation steps are as follows:

[0039] 0.20g of catalyst 5% Mn / C, 20g of cyclohexanone and 4g of acetic acid were added to the reactor, and then O2 was introduced three times to remove air. When the reaction temperature rose to 70°C, O2 was pressurized to 0.6MPa under stirring (stirring speed was 500r / min during the entire reaction process). After 8h of reaction, ventilation was stopped and the reactor was placed in a cold water bath to cool to room temperature.

[0040] The reaction product was completely dissolved with anhydrous ethanol and transferred to a volumetric flask to adjust the volume. Then, a gas chromatography-mass spectrometer (Shimadzu QP2010 GC-MS) was used for qualitative analysis, and a high performance liquid chromatography (Agilent 1200 HPLC) was used for quantitative analysis.

[0041] Preparation method of the 5% Mn / C catalyst:

[0042] 1.115 g of manganese acetate tetrahydrate was added to a mixed solution, which was a mixture of 30 mL of ethanol and 30 mL of deionized water, and stirred until uniform. Then 5 g of phthalic acid was added to dissolve, stirred for 12 h, and dried at 90 ° C for 6 h. The obtained catalyst powder was calcined at 400 ° C (calcination heating rate of 5 ° C / min) for 5 h under N2 atmosphere to obtain the catalyst powder.

[0043] The cyclohexanone conversion rate of this example is 31.2%, and the adipic acid selectivity is 92.4%.

[0044] Example 2: The steps and parameters of this example are the same as those of Example 1, except that the catalyst is 6% Mn / C. The cyclohexanone conversion rate of this example is 29.4% and the adipic acid selectivity is 87.6%.

[0045] Preparation method of the 6% Mn / C catalyst:

[0046] 1.338 g of manganese acetate tetrahydrate was added to a mixed solution, which was a mixture of 30 mL of ethanol and 30 mL of deionized water, and stirred until uniform. Then 5 g of phthalic acid was added to dissolve, stirred for 12 hours, and dried at 90° C. for 6 hours. The obtained catalyst powder was calcined at 400° C. (calcination heating rate of 5° C. / min) for 5 hours under N2 atmosphere to obtain the catalyst powder.

[0047] Example 3: The steps are the same as those of Example 1, except that the catalyst is 7% Mn / C. The cyclohexanone conversion rate of this example is 29.7% and the adipic acid selectivity is 84.6%.

[0048] Preparation method of the 7% Mn / C catalyst:

[0049] 1.561 g of manganese acetate tetrahydrate was added to a mixed solution, which was a mixture of 30 mL of ethanol and 30 mL of deionized water, and stirred until uniform. Then 5 g of phthalic acid was added to dissolve, stirred for 12 hours, and dried at 90°C for 6 hours. The obtained catalyst powder was calcined at 400°C (calcination heating rate of 5°C / min) for 5 hours under N2 atmosphere to obtain the catalyst powder.

[0050] Example 4: The steps are the same as those of Example 1, except that the catalyst is 9% Mn / C. The cyclohexanone conversion rate of this example is 28.4% and the adipic acid selectivity is 83.5%.

[0051] Preparation method of the 9% Mn / C catalyst:

[0052] 2.007 g of manganese acetate tetrahydrate was added to a mixed solution, which was a mixture of 30 mL of ethanol and 30 mL of deionized water, and stirred until uniform. Then 5 g of phthalic acid was added to dissolve, stirred for 12 h, and dried at 90 ° C for 6 h. The obtained catalyst powder was calcined at 400 ° C (calcination heating rate of 5 ° C / min) for 5 h under N2 atmosphere to obtain the catalyst powder.

[0053] Example 5: The steps are the same as those of Example 1, except that the calcination temperature in the catalyst preparation method is 300°C. The cyclohexanone conversion rate of this example is 26.1%, and the adipic acid selectivity is 75.2%.

[0054] Example 6: The steps are the same as those of Example 1, except that the calcination temperature in the catalyst preparation method is 500°C. The cyclohexanone conversion rate of this example is 35.6%, and the adipic acid selectivity is 85.6%.

[0055] Example 7: The steps are the same as those of Example 1, except that the calcination temperature in the catalyst preparation method is 600°C. The cyclohexanone conversion rate of this example is 46.4%, and the adipic acid selectivity is 76.7%.

[0056] Comparative Example 1: The steps are the same as those of Example 1, except that the calcination temperature in the catalyst preparation method is 700° C. The cyclohexanone conversion rate of this example is 39.7%, and the adipic acid selectivity is 61.9%.

[0057] Example 8: The steps are the same as those of Example 1, except that the organic carboxylic acid used to prepare the catalyst is adipic acid. The cyclohexanone conversion rate of this example is 30.6%, and the adipic acid selectivity is 87.0%.

[0058] Example 9: The steps are the same as those of Example 1, except that the organic carboxylic acid used to prepare the catalyst is isophthalic acid. The cyclohexanone conversion rate of this example is 47.9%, and the adipic acid selectivity is 71.3%.

[0059] Example 10: The steps are the same as those of Example 1, except that the organic carboxylic acid used to prepare the catalyst is terephthalic acid. The cyclohexanone conversion rate of this example is 46.5%, and the adipic acid selectivity is 70.2%.

[0060] Example 11: The steps are the same as those of Example 1, except that the organic carboxylic acid used to prepare the catalyst is trimesic acid. The cyclohexanone conversion rate of this example is 43.8%, and the adipic acid selectivity is 69.1%.

[0061] Example 12: The steps are the same as those of Example 1, except that the organic carboxylic acid used to prepare the catalyst is citric acid. The cyclohexanone conversion rate of this example is 36.2%, and the adipic acid selectivity is 78.2%.

[0062] Example 13: The steps are the same as those of Example 1, except that the organic carboxylic acid used to prepare the catalyst is salicylic acid. The cyclohexanone conversion rate of this example is 39.0%, and the adipic acid selectivity is 69.5%.

[0063] Comparative Example 2: The steps are the same as those of Example 1, except that the organic carboxylic acid used to prepare the catalyst is glutaric acid. The cyclohexanone conversion rate of this example is 29.5%, and the adipic acid selectivity is 48.0%.

[0064] Example 14: The steps are the same as those of Example 1, except that the manganese salt used to prepare the catalyst is manganese oxalate. The cyclohexanone conversion rate of this example is 34.4%, and the adipic acid selectivity is 71.2%.

[0065] Example 15: The steps are the same as those of Example 1, except that the manganese salt used to prepare the catalyst is manganese acetylacetonate. The cyclohexanone conversion rate of this example is 32.3%, and the adipic acid selectivity is 86.6%.

[0066] Comparative Example 3: The steps are the same as those of Example 1, except that the manganese salt used to prepare the catalyst is manganese nitrate. The cyclohexanone conversion rate of this example is 23.6%, and the adipic acid selectivity is 32.9%.

[0067] Example 16: The steps are the same as those of Example 1, except that the manganese salt used to prepare the catalyst is manganese chloride. The cyclohexanone conversion rate of this example is 14.9%, and the adipic acid selectivity is 69.8%.

[0068] Comparative Example 4: The steps are the same as those of Example 1, except that the reaction pressure is 0.4 MPa. The cyclohexanone conversion rate of this example is 22.6%, and the adipic acid selectivity is 58.9%.

[0069] Example 17: The steps are the same as those of Example 1, except that the reaction pressure is 0.5 MPa. The cyclohexanone conversion rate of this example is 26.8% and the adipic acid selectivity is 68.3%.

[0070] Example 18: The steps are the same as those of Example 1, except that the reaction pressure is 0.8 MPa. The cyclohexanone conversion rate of this example is 31.1% and the adipic acid selectivity is 87.3%.

[0071] Comparative Example 5: The steps are the same as those of Example 1, except that the reaction pressure is 1.0 MPa. The cyclohexanone conversion rate of this example is 38.4%, and the adipic acid selectivity is 57.6%.

[0072] Example 19: The steps are the same as those of Example 1, except that the reaction temperature is 65°C. The cyclohexanone conversion rate of this example is 25.0% and the adipic acid selectivity is 84.8%.

[0073] Example 20: The steps are the same as those of Example 1, except that the reaction temperature is 75°C. The cyclohexanone conversion rate of this example is 32.3% and the adipic acid selectivity is 88.8%.

[0074] Example 21: The steps are the same as those of Example 1, except that the reaction temperature is 60°C. The cyclohexanone conversion rate of this example is 16.5% and the adipic acid selectivity is 78.5%.

[0075] Example 22: The steps are the same as those of Example 1, except that the reaction temperature is 80°C. The cyclohexanone conversion rate of this example is 32.5% and the adipic acid selectivity is 72.2%.

[0076] Example 23: The steps are the same as those of Example 1, except that the reaction time is 5 hours. The cyclohexanone conversion rate of this example is 13.6% and the adipic acid selectivity is 82.4%.

[0077] Example 24: The steps are the same as those of Example 1, except that the reaction time is 6 hours. The cyclohexanone conversion rate of this example is 15.0% and the adipic acid selectivity is 86.5%.

[0078] Example 25: The steps are the same as those of Example 1, except that the reaction time is 7 hours. The cyclohexanone conversion rate of this example is 22.9% and the adipic acid selectivity is 88.8%.

[0079] Example 26: The steps are the same as those of Example 1, except that the reaction time is 9 hours. The cyclohexanone conversion rate of this example is 32.3% and the adipic acid selectivity is 76.6%.

[0080] Example 27: The steps are the same as those of Example 1, except that the reaction time is 10 h. The cyclohexanone conversion rate of this example is 35.0% and the adipic acid selectivity is 74.2%.

[0081] Example 28: The steps are the same as those of Example 1, except that the catalyst is R2-5% Mn / C. The cyclohexanone conversion rate of this example is 30.1% and the adipic acid selectivity is 90.4%.

[0082] After filtering the catalyst in the reaction solution in Example 1, deionized water and anhydrous ethanol were used to wash away organic matter on the catalyst surface, and after drying, the catalyst was re-calcined under the same calcination conditions as in the catalyst preparation method under N2 atmosphere (the obtained catalyst was recorded as R2-5% Mn / C). New reactants can be added to react under the same conditions.

[0083] Example 29: The steps are the same as those of Example 1, except that the catalyst is R3-5% Mn / C. The cyclohexanone conversion rate of this example is 30.1% and the adipic acid selectivity is 90.4%.

[0084] After filtering the catalyst R2-5% Mn / C in the reaction solution, the organic matter on the catalyst surface is washed off with deionized water and anhydrous ethanol, and after drying, it is re-calcined under N2 atmosphere using the same calcination conditions as in the catalyst preparation method (the obtained catalyst is recorded as R3-5% Mn / C). New reactants can be added to react under the same conditions.

[0085] Example 30: The steps are the same as those of Example 1, except that the catalyst is R4-5% Mn / C. The cyclohexanone conversion rate of this example is 30.6% and the adipic acid selectivity is 90.3%.

[0086] After filtering the catalyst R3-5% Mn / C in the reaction solution, the organic matter on the catalyst surface is washed off with deionized water and anhydrous ethanol, and after drying, it is re-calcined under N2 atmosphere using the same calcination conditions as in the catalyst preparation method (the obtained catalyst is recorded as R4-5% Mn / C). New reactants can be added to react under the same conditions.

[0087] Example 31: The steps are the same as Example 1, except that the catalyst is R8-5% Mn / C. The cyclohexanone conversion rate of this example is 29.4% and the adipic acid selectivity is 90.8%.

[0088] The catalyst R7-5% Mn / C in the reaction solution was recycled for 7 times, filtered, and organic matter on the catalyst surface was washed off with deionized water and anhydrous ethanol. After drying, it was re-calcined under N2 atmosphere under the same calcination conditions as in the catalyst preparation method (the obtained catalyst was recorded as R8-5% Mn / C). New reactants can be added to react under the same conditions.

Claims

1. A catalyst for preparing adipic acid by selective oxidation of cyclohexanone, characterized in that: A manganese salt-modified carbon material is selected, the carbon material is an organic carboxylic acid, and the catalyst is expressed as x%Mn / C, where x% is the mass ratio of metallic manganese to the organic carboxylic acid.

2. The catalyst for preparing adipic acid by selective oxidation of cyclohexanone according to claim 1, characterized in that: x% is 5-9%; and / or the manganese salt is selected from at least one of manganese acetate, manganese acetylacetonate, manganese oxalate, and manganese chloride; and / or the selected organic carboxylic acid is selected from one or more of phthalic acid, isophthalic acid, terephthalic acid, phthalic acid, adipic acid, citric acid, and salicylic acid.

3. The method for preparing a catalyst for preparing adipic acid by selective oxidation of cyclohexanone according to claim 1 or 2, characterized in that: The following steps are involved: The manganese salt is dissolved in a mixed solution of ethanol and deionized water, stirred until uniform, and then an organic carboxylic acid is added to dissolve, stirred for more than 12 hours, and then dried and calcined under a N2 atmosphere to obtain the product.

4. The method for preparing a catalyst for preparing adipic acid by selective oxidation of cyclohexanone according to claim 3, characterized in that: The amount of the mixed solution of ethanol and deionized water is such that both the manganese salt and the organic carboxylic acid can be dissolved; and / or the mixed solution of ethanol and deionized water is a solution in which ethanol and deionized water are mixed in a volume ratio of 1:

1.

5. The method for preparing a catalyst for preparing adipic acid by selective oxidation of cyclohexanone according to claim 3 or 4, characterized in that: The drying temperature is 70-100°C; and / or the drying time is 4-8 hours.

6. The method for preparing a catalyst for preparing adipic acid by selective oxidation of cyclohexanone according to claim 3 or 4, characterized in that: The calcination temperature is 300° C. to 600° C.; and / or the calcination heating rate is 4-6° C. / min; and / or the calcination time is 4 to 8 hours.

7. Use of the catalyst for preparing adipic acid by selective oxidation of cyclohexanone as claimed in claim 1 or 2, i.e., a method for preparing adipic acid by selective oxidation of cyclohexanone using the catalyst, characterized in that: The operation steps are: The catalyst, acetic acid and cyclohexanone are mixed, heated to the reaction temperature, oxygen is continuously introduced and pressurized to start the reaction. After the reaction is completed, the mixture is cooled to room temperature to obtain the product.

8. The use of the catalyst for preparing adipic acid by selective oxidation of cyclohexanone according to claim 7, i.e., a method for preparing adipic acid by selective oxidation of cyclohexanone using the catalyst, characterized in that: The mass ratio of the catalyst, acetic acid and cyclohexanone is 0.5-2:10-30:100 (preferably 1:20:100); and / or oxygen is continuously introduced and pressurized, and the reaction pressure is 0.5-0.8 MPa.

9. The use of the catalyst for preparing adipic acid by selective oxidation of cyclohexanone according to claim 7 or 8, i.e., a method for preparing adipic acid by selective oxidation of cyclohexanone using the catalyst, characterized in that: The reaction temperature is 60-80°C (preferably 65-75°C); and / or the reaction time is 4-10 h (preferably 5-8 h); and / or stirring is maintained throughout the entire reaction process from adding the materials to the end of the reaction, and the stirring speed is 300-600 r / min.

10. The use of the catalyst for preparing adipic acid by selective oxidation of cyclohexanone according to claim 7 or 8, i.e., a method for preparing adipic acid by selective oxidation of cyclohexanone using the catalyst, characterized in that: Recycling application of catalyst for selective oxidation of cyclohexanone to prepare adipic acid: After filtering the catalyst in the reaction solution, deionized water and anhydrous ethanol are used to wash away organic matter on the catalyst surface, and after drying, the catalyst is re-calcined under a N2 atmosphere using the same calcination conditions as in the catalyst preparation method.

Citation Information

Patent Citations

  • Method for preparing multilevel porous carbon base composite phase change material

    CN104710965A

  • Process for preparing adipic acid through cleaning catalytic oxidation of cyclohexanone, catalyst, and catalyst preparation method

    CN105622385A

  • Mn base metal organic skeletal catalyst, and preparation method and application thereof in air pollution prevention

    CN106345527A

  • Mn-C catalytic material based on MOFs as well as preparation method and application thereof

    CN111468107A

  • Preparation method and application of two-dimensional flaky manganese oxide / mesoporous carbon catalyst based on Mn-MOF

    CN114042448A

Cited By

  • V2O5 / MnO2 composite oxide catalyst and preparation and application thereof

    CN121571135A