Nickel-based alloy catalyst as well as preparation method and application thereof

By introducing indium or gallium into the nickel-based catalyst to form a nickel-based intermetallic alloy, adjusting the nickel atom spacing and performing oxidation and regeneration treatment, the problem of low selectivity and poor stability of nickel-based catalysts in the propane dehydrogenation reaction is solved, and high Selective and long-life catalysts, suitable for industrial applications.

CN118874475AActive Publication Date: 2024-11-01TIANJIN UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411003538.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-25
Publication Date
2024-11-01
Estimated Expiration
2044-07-25

AI Technical Summary

Technical Problem

The existing nickel-based catalysts have low selectivity in the propane dehydrogenation reaction to propylene and are prone to carbon deposits and metal sintering at high temperatures, resulting in poor stability and difficult to be used in industrial use.

Method used

By introducing a second metal atom M (such as indium and gallium) to form a nickel-based intermetal alloy, the nickel atom spacing is regulated, deep dehydrogenation and cracking side reactions are inhibited, and the catalyst life is extended through oxidation and regeneration treatment.

Benefits of technology

It significantly improves propylene selectivity and catalyst stability. The propylene selectivity reaches more than 91%, and the catalyst life is extended by more than 20%, reducing production costs and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874475A_ABST
    Figure CN118874475A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of catalysts, and discloses a nickel-based alloy catalyst and a preparation method and application thereof.The catalyst comprises active metal nickel and a second modification element M, and the second modification element M is at least one of In and Ga; the active metal nickel and the second modification element M form a nickel-based intermetallic alloy, and the nickel-based intermetallic alloy is loaded on the surface of the carrier; the crystal structure of the nickel-based intermetallic alloy is a body-centered cubic structure; the catalyst can be prepared in one step by adopting a conventional impregnation method, and can be used for preparing olefin by dehydrogenation of low-carbon alkane; when the catalyst is applied to propylene preparation through propane dehydrogenation, compared with the existing catalyst, the yield of propylene is increased by 20% or above, the service life of the catalyst is prolonged by 20% or above, the production cost is greatly reduced, and the catalyst has a wide application prospect in industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of catalysts, and in particular, relates to a platinum-based catalyst and a preparation method and application thereof. Background Art

[0002] Propylene is an important chemical raw material, widely used in the production of bulk chemicals such as polypropylene, acrylonitrile, and propylene oxide. With the vigorous development of the chemical industry, traditional propylene production processes such as petroleum cracking and catalytic cracking can no longer meet the growing market demand. Therefore, in recent years, the production of propylene represented by propane dehydrogenation (PDH) has received widespread attention. Compared with other production routes, the PDH process has the advantages of a large price difference between raw materials and products and a simple process, making it one of the propylene preparation technologies with the most industrial prospects.

[0003] At present, the main industrialized PDH processes are ABB Lummus's Catofin technology and UOP's Oleflex technology. These two technologies use chromium oxide-based and platinum-based catalysts respectively, but they also have disadvantages such as large environmental pollution, frequent catalyst regeneration or high prices, and easy carbon deposition and deactivation. Since the PDH reaction is usually carried out at a high temperature of 600-700℃, the development of catalysts with high activity, high selectivity and high stability has become a research focus and technical bottleneck in this field.

[0004] Compared with precious metal platinum, non-precious metal nickel (Ni) has the advantages of low price and abundant reserves, and is expected to replace nickel for PDH reaction. However, existing catalysts such as nickel / alumina and nickel / silicon dioxide generally have problems such as low selectivity for light olefins and poor stability in the process of propane dehydrogenation. For example, methane is the main by-product on nickel / silicon dioxide catalysts, and the selectivity for propylene is only ~3%. At the same time, it quickly deactivates during high-temperature reactions, making it difficult to apply industrially. Summary of the invention

[0005] The present invention aims to solve the technical problems that the nickel-based catalyst prepared by the prior art has low selectivity in the propane dehydrogenation to propylene reaction, and is prone to carbon deposition and metal sintering at high temperature and in the regeneration process, which affects the performance of the catalyst; a nickel-based alloy catalyst and a preparation method and application thereof are provided, and by introducing a second metal atom M (indium, gallium), the spacing between nickel atoms can be effectively increased, and the nickel-carbon interaction can be weakened, thereby inhibiting side reactions such as deep dehydrogenation and cracking; the catalyst is used in the process of propane dehydrogenation to propylene, and by regulating the microenvironment of the nickel atoms in NiM, side reactions such as carbon deposition and deep dehydrogenation can be inhibited, and the catalyst has the advantages of high propylene selectivity, good stability, etc.

[0006] According to one aspect of the present invention, a nickel-based alloy catalyst is provided, comprising active metal nickel and a second modifying element M, wherein the second modifying element M is at least one of In and Ga; the active metal nickel and the second modifying element M form a nickel-based metal alloy and are loaded on a carrier surface; the crystal structure of the nickel-based metal alloy is a body-centered cubic structure.

[0007] Furthermore, based on the mass of the carrier, the mass percentage of the active metal Ni is 0.1%-10%.

[0008] Furthermore, the molar ratio of Ni to M is (0.5-2):1.

[0009] Furthermore, the molar ratio of Ni to M is 1:1.

[0010] According to another aspect of the present invention, there is provided a method for preparing a nickel-based alloy catalyst, comprising the following steps:

[0011] (1) Immersing the support in a Ni and M precursor solution;

[0012] (2) drying the impregnated product obtained in step (1);

[0013] (3) calcining the dried product of step (2) in a reducing atmosphere to obtain a nickel-based intermetallic compound NiM catalyst.

[0014] Furthermore, in step (1), the precursors of Ni and M are both their nitrates, and the solvent is water.

[0015] Furthermore, in step (3), the calcination temperature is 773-973K and the calcination time is 0.5-3 hours.

[0016] According to another aspect of the present invention, there is provided an application of the above nickel-based alloy catalyst for dehydrogenation of low-carbon alkanes to olefins.

[0017] Furthermore, when used for dehydrogenating propane to produce propylene, the reaction temperature of the propane dehydrogenation reaction is 823-923K.

[0018] The beneficial effects of the present invention are:

[0019] The nickel-based alloy catalyst provided by the present invention regulates the microenvironment around nickel atoms by introducing a second modifying element M (indium, gallium) into nickel, thereby increasing the distance between nickel atoms and weakening the nickel-carbon interaction, thereby effectively inhibiting side reactions such as deep dehydrogenation and cracking of propane on nickel, and solving the problem of low propylene selectivity of existing nickel-based catalysts. Taking the nickel-indium catalyst as an example, when reacting at a temperature of 873K, the propylene selectivity is as high as more than 91%, and it is still maintained at more than 91% after 24 hours of reaction, showing excellent reaction stability.

[0020] In the NiM catalyst of the present invention, nickel atoms are isolated by M atoms, which inhibits the agglomeration and sintering of nickel. In addition, by using 1% oxygen and hydrogen for oxidation regeneration and reduction treatment respectively after the reaction, the carbon deposits on the catalyst can be effectively removed, and the catalyst can be reused many times, which greatly improves the service life of the catalyst and solves the problem of poor stability of existing nickel-based catalysts.

[0021] The preparation method of the NiM catalyst provided by the present invention is simple, and is prepared in one step by a conventional impregnation method, and is calcined in a reducing atmosphere, so as to form a thermodynamically stable body-centered cubic structure nickel-based alloy. The precursor used is cheap and easily available, the preparation conditions are mild and controllable, and the product has high purity, which is very suitable for industrial scale-up production.

[0022] The NiM catalyst of the present invention is applied to the propane dehydrogenation to propylene reaction. Compared with the existing catalyst, not only the propylene yield is increased by more than 20%, but also the catalyst life is extended by more than 20%, which greatly reduces the production cost and has broad application prospects in industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 This is a performance result diagram of the catalytic dehydrogenation of propane to propylene using the nickel indium / silicon dioxide (NiIn / SiO2) catalyst and the nickel / silicon dioxide (Ni / SiO2) catalyst in Example 1 of the present invention;

[0024] Figure 2 It is a high-magnification transmission electron micrograph of the nickel indium / silicon dioxide (NiIn / SiO2) catalyst and the nickel / silicon dioxide (Ni / SiO2) catalyst in Example 1 of the present invention. DETAILED DESCRIPTION

[0025] The present invention uses density functional theory calculations to study a series of nickel-based intermetallic compound NiM catalysts. The study found that by introducing a second metal atom M (such as indium, gallium, etc.), the distance between nickel atoms can be effectively increased, and its activation ability for carbon-hydrogen bonds can be weakened, thereby inhibiting side reactions such as deep dehydrogenation and cracking. Experimental results show that nickel indium (NiIn) catalysts with a suitable catalytic microenvironment show >91% propylene selectivity in the PDH reaction, which is much higher than nickel catalysts and comparable to platinum-based catalysts. The NiM catalyst of the present invention has both excellent selectivity and stability, and is expected to replace platinum-based catalysts, providing a new idea for the development of high-performance PDH catalysts. Specifically:

[0026] The present invention provides a nickel-based alloy catalyst, comprising active metal nickel and a second modifying element M, wherein the second modifying element M is at least one of In and Ga; the active metal nickel and the second modifying element M form a nickel-based metal alloy and are loaded on the surface of a carrier; the crystal structure of the nickel-based metal alloy is a body-centered cubic structure.

[0027] According to some preferred embodiments of the present invention, based on the mass of the carrier, the mass percentage of the active metal Ni is preferably 0.1%-10%.

[0028] According to some preferred embodiments of the present invention, the molar ratio of Ni to M is preferably (0.5-2):1, most preferably 1:1.

[0029] The present invention provides a method for preparing a nickel-based alloy catalyst, comprising the following steps:

[0030] (1) Immersing the support in a Ni and M precursor solution;

[0031] (2) drying the impregnated product obtained in step (1);

[0032] (3) calcining the dried product of step (2) in a reducing atmosphere to obtain a nickel-based intermetallic compound NiM catalyst.

[0033] According to some preferred embodiments of the present invention, in step (1), the precursors of Ni and M are both nitrates thereof, and the solvent is water.

[0034] According to some preferred embodiments of the present invention, the calcination temperature in step (3) is 773-973 K and the calcination time is 0.5-3 hours.

[0035] The invention provides an application of a nickel-based alloy catalyst for dehydrogenating low-carbon alkanes to produce olefins.

[0036] According to some preferred embodiments of the present invention, when used for dehydrogenating propane to produce propylene, the reaction temperature of the propane dehydrogenation reaction is 823-923K.

[0037] In order to make the purpose, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments and drawings.

[0038] Example 1

[0039] 1. Preparation of nickel-based intermetallic compound nickel-indium catalyst:

[0040] (1) Mix 300 μL of 0.1 g (Ni) / mL Ni(NO3)2·6H2O aqueous solution and 590 μL of 0.1 g (In) / mL In(NO3)3 aqueous solution, and dilute to the required volume with deionized water to prepare an impregnation solution.

[0041] (2) Take 1 g of SiO2 carrier and impregnate it with an equal volume of the impregnation solution prepared in step (1).

[0042] (3) The impregnated carrier was allowed to stand at room temperature overnight, then dried at 353 K for 12 hours, and then calcined at 873 K in a 10% H2-Ar atmosphere for 1 hour to obtain a NiIn / SiO2 catalyst with SiO2 as the carrier and a Ni loading of 3 wt%.

[0043] 2. Catalyst activity test:

[0044] (1) 200 mg of the NiIn / SiO2 catalyst prepared in step 1 was loaded into a quartz tube fixed bed reactor with an inner diameter of 8 mm and a length of 24 cm. The catalyst pre-granulated to a particle size of 20 to 40 mesh was loaded into the quartz fixed bed reactor, and the catalyst was diluted with quartz sand particles to a total volume of 1 mL. Before the reactivity test, the catalyst was pretreated in a 10% volume fraction H2-Ar atmosphere at a rate of 10 K / min from room temperature to 873 K and maintained for 1 h.

[0045] (2) After pretreatment, a balanced mixture of 16% volume fraction C3H8 and 16% H2 in N2 was switched, and the reaction gas with a volume flow rate of 50 mL / min was introduced into the reaction pipeline to carry out propane dehydrogenation reaction under normal pressure. The product was analyzed by online gas chromatography, in which a flame ionization detector with a Chromosorb 102 column was used to detect carbon-containing compound components, and a thermal conductivity detector with an Al2O3 Plot column was used to detect H2, N2 and other components.

[0046] 3. Catalyst regeneration test:

[0047] (1) After 24 hours of propane dehydrogenation reaction, the catalyst underwent a cooling process under the protection of N2 atmosphere (flow rate of 34 mL / min), and the temperature dropped to 773 K;

[0048] (2) introducing a 1% O2 / N2 mixed gas (40 mL / min) and reacting it for 20 minutes to remove coke;

[0049] (3) Switch the gas flow to N2 and continue for 5 minutes to replace the oxygen in the reaction tube and gas line;

[0050] (4) The gas was switched to 20% H2 / N2 (flow rate of 42 mL / min) and the temperature was raised to 873 K at a heating rate of 10°C / min and kept at that temperature for 1 hour to carry out the next propane dehydrogenation reaction.

[0051] 4. Calculate propane conversion and propylene selectivity:

[0052] Propane conversion (%) = (F[C3H8] 进口 -F[C3H8] 出口 ) / F[C3H8] 进口 ×100%

[0053] Propylene selectivity (%) = F[C3H6] 出口 / (F[C3H8] 进口 -F[C3H8] 出口 )×100%

[0054] where [F] represents the molar flow rate of each substance.

[0055] Example 2

[0056] A nickel catalyst was prepared and the catalyst activity was evaluated by referring to the method of Example 1, except that the impregnation solution contained only 300 μL of 0.1 g (Ni) / mL Ni (NO3) 2 · 6H2O aqueous solution, and the prepared catalyst was recorded as Ni / SiO2.

[0057] Example 3

[0058] The nickel-based intermetallic compound catalyst was prepared and the catalyst activity was evaluated according to the method of Example 1, except that the catalyst prepared by containing 300 μL of 0.1 g (Ni) / mL Ni (NO3) 2 · 6H2O aqueous solution and 295 μL of 0.1 g (In) / mL In (NO3) 3 aqueous solution in the impregnation solution was denoted as NiIn 0.5 / SiO2.

[0059] Example 4

[0060] A nickel-based intermetallic compound catalyst was prepared and the catalyst activity was evaluated by referring to the method of Example 1, except that the impregnation solution contained 300 μL of 0.1 g (Ni) / mL Ni (NO3) 2 · 6H2O aqueous solution and 1180 μL of 0.1 g (In) / mL In (NO3) 3 aqueous solution. The catalyst prepared was recorded as NiIn2 / SiO2.

[0061] Example 5

[0062] A nickel-based intermetallic compound catalyst was prepared and the catalyst activity was evaluated by referring to the method of Example 1, except that the carrier used was Al2O3, denoted as NiIn / Al2O3.

[0063] Example 6

[0064] A nickel-based intermetallic compound catalyst was prepared and the catalyst activity was evaluated by referring to the method of Example 1, except that the impregnation solution contained 300 μL of 0.1 g (Ni) / mL Ni (NO3) 2 · 6H2O aqueous solution and 252.5 μL of 0.1 g (Ga) / mL Ga (NO3) 3 aqueous solution. The catalyst prepared was recorded as NiGa / SiO2.

[0065] Example 7

[0066] A nickel-based intermetallic compound catalyst was prepared and the catalyst activity was evaluated by referring to the method of Example 1, except that the impregnation solution contained 300 μL of 0.1 g (Ni) / mL Ni (NO3) 2 · 6H2O aqueous solution and 269.3 μL of 0.1 g (Zn) / mL Zn (NO3) 2 aqueous solution. The catalyst prepared was recorded as NiZn / / SiO2.

[0067] Example 8

[0068] A nickel-based intermetallic compound catalyst was prepared and the catalyst activity was evaluated by referring to the method of Example 1, except that the impregnation solution contained 300 μL of 0.1 g (Ni) / mL Ni (NO3) 2 · 6H2O aqueous solution and 277.1 μL of 0.1 g (Cu) / mL Cu (NO3) 2 aqueous solution. The catalyst prepared was recorded as NiCu / SiO2.

[0069] Example 9

[0070] A nickel-based intermetallic compound catalyst was prepared and the catalyst activity was evaluated by referring to the method of Example 1, except that the impregnation solution contained 300 μL of 0.1 g (Ni) / mL Ni (NO3) 2 · 6H2O aqueous solution and 320.5 μL of 0.1 g (Mn) / mL Mn (NO3) 2 aqueous solution. The catalyst prepared was recorded as NiMn / SiO2.

[0071] Example 10

[0072] A nickel-based intermetallic compound catalyst was prepared and the catalyst activity was evaluated according to the method of Example 1, except that the calcination temperature was 773K in a reducing atmosphere.

[0073] Embodiment 11

[0074] A nickel-based intermetallic compound catalyst was prepared and the catalyst activity was evaluated according to the method of Example 1, except that the calcination temperature was 973K in a reducing atmosphere.

[0075] Example 12

[0076] A nickel-based intermetallic compound catalyst was prepared and the catalyst activity was evaluated by referring to the method of Example 1, except that a reducing atmosphere was used and the calcination time was 0.5 h.

[0077] Embodiment 13

[0078] A nickel-based intermetallic compound catalyst was prepared and the catalyst activity was evaluated by referring to the method of Example 1, except that a reducing atmosphere was used and the calcination time was 3 h.

[0079] Embodiment 14

[0080] A nickel-based intermetallic compound catalyst was prepared and the catalyst activity was evaluated by referring to the method of Example 1, except that the reaction temperature was 823K.

[0081] Embodiment 15

[0082] A nickel-based intermetallic compound catalyst was prepared and the catalyst activity was evaluated by referring to the method of Example 1, except that the reaction temperature was 923K.

[0083] Example 16

[0084] The nickel-based intermetallic compound catalyst was prepared and the catalyst activity was evaluated according to the method of Example 1, except that the impregnation solution was a mixture of 10 μL of 0.1 g (Ni) / mL Ni (NO3) 2 · 6H2O aqueous solution and 19.6 μL of 0.1 g (In) / mL In (NO3) 3 aqueous solution. At this time, the Ni loading was 0.1%, recorded as 0.1NiIn / SiO2.

[0085] Embodiment 17

[0086] The nickel-based intermetallic compound catalyst was prepared and the catalyst activity was evaluated according to the method of Example 1, except that the impregnation solution was a mixture of 500 μL of 0.1 g (Ni) / mL Ni (NO3) 2 · 6H2O aqueous solution and 983.3 μL of 0.1 g (In) / mL In (NO3) 3 aqueous solution. At this time, the Ni loading was 5%, recorded as 5NiIn / SiO2.

[0087] Embodiment 18

[0088] The nickel-based intermetallic compound catalyst was prepared and the catalyst activity was evaluated according to the method of Example 1, except that the impregnation solution was a mixture of 1000 μL of 0.1 g (Ni) / mL Ni (NO3) 2·6H2O aqueous solution and 1966.7 μL of 0.1 g (In) / mL In (NO3) 3 aqueous solution. At this time, the Ni loading was 10%, recorded as 10NiIn / SiO2.

[0089] The test results of the above Examples 1-18 were compared to examine the effects of different parameters on the catalyst reaction performance.

[0090] (1) The effect of the introduction of In additive on the catalyst activity in Examples 1 and 2. For specific test results, see Table 1.

[0091] Table 1 Propane conversion and propylene selectivity over different nickel-based catalysts and commercial catalysts

[0092]

[0093] From Table 1 and Figure 1 It can be seen that compared with Ni / SiO2, the propane conversion rate of the NiIn / SiO2 catalyst of the present invention is 12.5% ​​initially and 6.5% after 24 hours at a reaction temperature of 873K; the propylene selectivity is maintained above 91% during the entire reaction process, showing excellent propane dehydrogenation to propylene performance and regeneration stability. This shows that the introduction of In into Ni / SiO2 to form a NiIn / SiO2 catalyst can significantly improve the propane dehydrogenation performance of the catalyst. Figure 2 As shown, it can be seen from the high-magnification transmission electron microscopy image that the characteristic lattice spacing (0.255nm) belonging to the body-centered cubic structure NiIn alloy appears on the NiIn / SiO2 catalyst, indicating that the body-centered cubic structure NiIn alloy exists in the catalyst.

[0094] (2) The effect of the amount of In additive introduced in Examples 1, 2, 3, and 4 on the catalyst activity. For specific test results, see Table 2.

[0095] Table 2 Propane conversion and propylene selectivity of Ni-In catalysts with different In contents

[0096]

[0097] From the comparison in Table 2, it can be seen that the propane dehydrogenation performance of NiIn catalysts with different molar ratios is better than that of Ni catalysts, and there is a volcanic peak relationship between the indium content in the Ni-In catalyst and the propylene yield. Specifically, when the In content is low (In:Ni=0.5:1), a lower propylene yield is shown; when In:Ni is increased to 1:1, the propylene yield will be improved to a certain extent; when In:Ni is further increased to 2:1, the propylene yield will be reduced to a certain extent. The above results show that the In content in the Ni-In catalyst directly affects the propane dehydrogenation performance of the catalyst, among which the propane dehydrogenation performance of the catalyst is optimal when In:Ni is 1:1.

[0098] (3) Effect of the change of the carrier in Examples 1, 2, and 5 on the catalyst activity. For specific test results, see Table 3.

[0099] Table 3 Propane conversion and propylene selectivity of Ni-In catalysts with different supports

[0100]

[0101] From the comparison in Table 3, it can be seen that when SiO2 or Al2O3 is used as the carrier of the nickel-indium alloy catalyst, a relatively good effect of selectively converting propane to propylene can be obtained. Among them, when Al2O3 is used as the carrier, the initial propylene selectivity of the NiIn / Al2O3 catalyst is 42.6%, which is much higher than the propylene selectivity of the Ni / SiO2 catalyst; when SiO2 is used as the carrier, the initial propylene selectivity of the NiIn / SiO2 catalyst is increased to 93.5%, which shows that the Ni-In catalyst is better when the carrier is SiO2.

[0102] (4) Effect of the modification elements (In, Ga, Zn, Cu or Mn) in Examples 1, 6, 7, 8 and 9 on the catalyst activity. For specific test results, see Table 4.

[0103] Table 4 Propane conversion and propylene selectivity of Ni-based catalysts modified with different elements

[0104]

[0105] From the comparison in Table 4, it can be seen that the propane dehydrogenation performance of the catalyst changes with the change of the second element. When In or Ga is used as the second element, both have a relatively good effect of selectively converting propane. When In is used as the modifying element, the comprehensive propane dehydrogenation performance of the catalyst is the best, which shows that In or Ga are both suitable second modifying elements, and In is the best second modifying element.

[0106] (5) Effect of changing the calcination temperature in reducing atmosphere on the catalyst activity of Examples 1, 10 and 11. For specific test results, see Table 5.

[0107] Table 5 Effect of calcination temperature on propane conversion and propylene selectivity of Ni-In catalyst

[0108]

[0109] From the comparison in Table 5, it can be seen that changing the calcination temperature has a certain effect on the propane dehydrogenation performance of the catalyst, but the overall performance is still better than that of the Ni / SiO2 catalyst. Among them, when the calcination temperature is 873K, the overall performance of the catalyst is better, indicating that the calcination temperature of 873K is the preferred option.

[0110] (6) Effect of changing the calcination time in reducing atmosphere on the catalyst activity of Examples 1, 12 and 13. For specific test results, see Table 6.

[0111] Table 6 Effect of calcination temperature on propane conversion and propylene selectivity of Ni-In catalyst

[0112]

[0113]

[0114] From the comparison in Table 6, it can be seen that changing the calcination time has a certain effect on the propane dehydrogenation performance of the catalyst, but the overall performance is still better than that of the Ni / SiO2 catalyst. Among them, when the calcination time is 1h, the propane dehydrogenation performance of the catalyst is better, indicating that the calcination temperature of 1h is the preferred option.

[0115] (7) Effect of the change of reaction temperature on the catalyst activity of Examples 1, 14 and 15. For specific test results, see Table 7.

[0116] Table 7 Effect of reaction temperature on propane conversion and propylene selectivity of Ni-In catalyst

[0117]

[0118] From the comparison in Table 7, it can be seen that changing the reaction temperature has a certain influence on the propane dehydrogenation performance of the catalyst, among which the propylene yield increases with the increase of the reaction temperature, and the propylene selectivity is always greater than 90%. When the reaction temperature is 873K, the propane dehydrogenation performance of the catalyst is optimal, which indicates that the reaction temperature of 873K is the preferred option.

[0119] (8) Effect of the change of nickel loading on the catalyst activity in Examples 1, 16, 17 and 18. For specific test results, see Table 8.

[0120] Table 8 Effect of nickel loading on propane conversion and propylene selectivity of Ni-In catalyst

[0121]

[0122] From the comparison in Table 8, it can be seen that the nickel loading has a certain influence on the propane dehydrogenation performance of the catalyst. The propane conversion rate increases with the increase of the nickel loading, and the propylene selectivity is ≥92.9%, indicating that they all have excellent ability to selectively convert propane into propylene. Among them, when the nickel loading is 3%, the catalyst maintains a high propane conversion rate while the propylene yield / nickel loading value is higher than that of the catalyst with a nickel loading of 5% and 10%, indicating that the utilization rate of active metal nickel is higher at this time. Therefore, a nickel loading of 3% is preferred.

[0123] In summary, the NiM / SiO2 catalyst of the present invention has the advantages of high selectivity for propylene and high stability, and is expected to replace existing industrial catalysts for the process of propane dehydrogenation to propylene, and has broad industrial application prospects.

[0124] The specific embodiments described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A nickel-based alloy catalyst, characterized in that: It includes active metal nickel and a second modifying element M, wherein the second modifying element M is at least one of In and Ga; the active metal nickel and the second modifying element M form a nickel-based metal alloy and are loaded on the surface of a carrier; the crystal structure of the nickel-based metal alloy is a body-centered cubic structure.

2. A nickel-based alloy catalyst according to claim 1, characterized in that: Based on the mass of the carrier, the mass percentage of the active metal Ni is 0.1%-10%.

3. A nickel-based alloy catalyst according to claim 1, characterized in that: The molar ratio of Ni to M is (0.5-2):

1.

4. A nickel-based alloy catalyst according to claim 3, characterized in that: The molar ratio of Ni to M is 1:

1.

5. A method for preparing the nickel-based alloy catalyst according to any one of claims 1 to 4, characterized in that: The process includes the following: (1) Immersing the support in a Ni and M precursor solution; (2) drying the impregnated product obtained in step (1); (3) calcining the dried product of step (2) in a reducing atmosphere to obtain a nickel-based intermetallic compound NiM catalyst.

6. The method for preparing a nickel-based alloy catalyst according to claim 5, characterized in that: In step (1), the precursors of Ni and M are both their nitrates, and the solvent is water.

7. The method for preparing a nickel-based alloy catalyst according to claim 5, characterized in that: The calcination temperature in step (3) is 773-973K and the calcination time is 0.5-3 hours.

8. Use of the nickel-based alloy catalyst according to any one of claims 1 to 4, characterized in that: Used for dehydrogenation of low-carbon alkanes to olefins.

9. The use of the nickel-based alloy catalyst according to claim 8, characterized in that: When used for propane dehydrogenation to produce propylene, the reaction temperature of the propane dehydrogenation reaction is 823-923K.

Citation Information

Patent Citations

  • Load type carbonized nickel indium alloy catalyst and its preparation method and application

    CN107649157A

  • Cobalt-nickel alloy modified platinum-based catalyst and preparation method thereof, and application of cobalt-nickel alloy modified platinum-based catalyst in CO oxidation

    CN111330592A

  • Synthesis and application method of supported nickel-gallium catalyst

    CN114471580A

  • Supported bimetallic alloy catalyst as well as preparation method and application thereof

    CN118022728A

  • High-entropy alloy catalyst as well as preparation method and application thereof

    CN118179522A