Ce-doped cobalt-based perovskite catalyst material and preparation method and application thereof
By introducing Ce into the Co-based perovskite catalyst and using glucose as a complexing agent, Ce doped cobalt-based perovskite catalyst with high catalytic activity was prepared, and the Co-based perovskite oxide catalyst in the prior art was solved. The problem of insufficient activity has achieved efficient removal of soot particles.
Patent Information
- Application Number
- CN202410923338.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-01
AI Technical Summary
The existing Co-based perovskite oxide catalysts have low catalytic activity in soot combustion reactions and cannot meet actual needs.
Using the preparation method of Ce doped cobalt-based perovskite catalyst material, by introducing Ce element into cobalt-based perovskite and using glucose as a complexing agent, the structure and activity of the catalyst are optimized and its combustion reaction in soot particles is improved. performance in.
The high catalytic activity of completely removing soot particles below 400°C is achieved, the oxygen storage and discharge capacity of the catalyst and the contact efficiency of the active site are improved, and the catalytic performance is optimized.
Smart Images

Figure BDA0004937338450000071 
Figure BDA0004937338450000101 
Figure BDA0004937338450000111
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of catalyst material preparation, and in particular relates to a Ce-doped cobalt-based perovskite catalyst material and a preparation method and application thereof. Background Art
[0002] Perovskite or perovskite-like catalysts (ABO 3 ) refers to natural CaTiO 3 Oxides with the same structure. Due to its controllable structure, good thermal stability, high catalytic efficiency and low price, it has gradually become a hot topic in the field of modern industrial catalysis. In the early 1970s, Libby and Voorhoeve et al. initially studied the catalysis of cobalt or manganese perovskite catalysts in gasoline engine exhaust and found that perovskite-type structured catalysts have high activity. Studies have shown that perovskite catalysts are a very potential substitute for precious metal catalysts, with advantages that general catalysts do not have: 1) diverse constituent elements and chemical compositions; 2) stable particle volume and easy specific surface area evaluation; 3) a large range of stoichiometric coefficients, chemical valences, and vacancies, with great potential for changing catalytic performance. In perovskite oxide catalysts, both A and B positions can be partially replaced by other metal cations of the same or different valences. Researchers can use this feature to regulate the stability, redox properties, and texture properties of the catalyst. Over the years, perovskite oxide catalysts have been widely studied in catalyzing the combustion of diesel engine soot particles. The selection of metal cations at the A and B positions of perovskite catalysts, the morphology and specific surface area of the catalysts, and the redox performance have all become research areas of concern to researchers.
[0003] In recent years, perovskite catalysts with transition metal cations as active sites, such as Co-based, Mn-based, Fe-based, Ti-based and Ni-based perovskite catalysts, have been widely used in diesel engine catalytic soot particle combustion. Because the d orbital of the transition metal cations in them has the characteristics of easily gaining or losing electrons, these perovskite catalysts show high redox performance in the deep redox reaction of catalytic soot particle combustion. Among them, Co-based perovskite oxide catalysts often use rare earth cations as A-site ions, among which La 3+ Perovskite catalysts with A-site cations have the characteristics of low cost, good structural adjustability, and high thermal stability. Researchers have found that Co-based perovskite oxide catalysts often exhibit lattice oxygen defect states. In order to maintain the electrical neutrality of the crystal, this charge change is often caused by Co 2+ This reversible oxidation state is more conducive to the oxidation of NO in the soot particle combustion reaction atmosphere. Therefore, Co-based perovskite oxide catalysts are widely used in soot particle combustion reactions and have high catalytic activity. However, LaCoO 3The single component of the catalytic material has become an important factor affecting the intrinsic activity of the catalyst, and the catalytic activity of this perovskite oxide cannot meet the actual needs.
[0004] The object of the present invention is to provide a Ce-doped cobalt-based perovskite catalyst material and a preparation method and application thereof, so as to solve the technical problem that the catalytic activity of soot combustion catalysts in the prior art is low.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The present invention discloses a method for preparing a Ce-doped cobalt-based perovskite catalyst material, comprising the following steps:
[0007] The precursor metal salt, the complexing agent and water are mixed and stirred to obtain a mixed solution; the obtained mixed solution is dried once to obtain a dried product;
[0008] The dried product is subjected to secondary drying treatment, and then subjected to calcination treatment. After the calcination treatment is completed, a Ce-doped cobalt-based perovskite catalyst material is obtained.
[0009] Furthermore, the precursor metal salt is a mixture of lanthanum salt, cerium salt and cobalt salt.
[0010] Furthermore, the complexing agent is one of glucose and citric acid monohydrate.
[0011] Furthermore, the usage ratio of the precursor metal salt, the complexing agent and water is 0.2-10g:0.5-10g:10-50mL.
[0012] Furthermore, the mixing and stirring time is 1-4h.
[0013] Furthermore, the temperature of the primary drying treatment is 80-120° C. and the time is 12-24 hours.
[0014] Furthermore, the secondary drying treatment is performed at 80-100° C. for 12-24 hours.
[0015] Furthermore, the calcination treatment is carried out at a temperature of 450-1000°C and for a time of 2-10 hours.
[0016] The present invention also discloses a Ce-doped cobalt-based perovskite catalyst material prepared by the preparation method. The Ce-doped cobalt-based perovskite catalyst material is obtained by complexing the A position and the B position of the perovskite catalyst material.
[0017] The present invention also discloses the application of the Ce-doped cobalt-based perovskite catalyst material in the catalytic combustion reaction of carbon smoke particles.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The invention discloses a preparation method of a Ce-doped cobalt-based perovskite catalyst material. Precursor metal salt, a complexing agent and water are used as reaction raw materials, and a Ce element with oxygen storage and release capacity is used as an A-position doping element to obtain a Ce-doped cobalt-based perovskite catalyst material. The preparation method introduces Ce into the cobalt-based perovskite catalyst. Since the valence state of Ce can be changed between +3 and +4, the oxygen storage and release capacity of the catalyst is further improved. At the same time, the complexing agent selected by the invention improves the contact efficiency between carbon smoke particles and catalyst active sites and optimizes the catalytic activity thereof.
[0020] Furthermore, by using glucose as a complexing agent and also playing its role as a pore-forming agent, a Ce-doped Co-based perovskite oxide catalyst with a porous structure is prepared, thereby improving the contact efficiency between the soot particles and the active sites of the catalyst and optimizing its catalytic performance.
[0021] Furthermore, the use of a primary drying treatment and a secondary drying treatment can accelerate the drying process and make the precursor gel foam evenly, so as to obtain a Co-based perovskite catalyst with evenly dispersed active components.
[0022] The present invention also discloses the application of the Ce-doped cobalt-based perovskite catalyst material in the catalytic combustion reaction of soot particles. The catalyst has high catalytic activity. According to relevant experimental results, the soot particles can be completely removed at temperatures below 400°C. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 XRD patterns of Ce-doped cobalt-based perovskite catalyst materials under different glucose dosage conditions;
[0024] Figure 2 Scanning electron microscope photos of Ce-doped cobalt-based perovskite catalyst materials under different calcination temperature conditions;
[0025] Figure 3 XRD patterns of Ce-doped cobalt-based perovskite catalyst materials prepared under different calcination temperature conditions;
[0026] Figure 4 Nitrogen adsorption-desorption isotherms of Ce-doped cobalt-based perovskite catalyst materials;
[0027] Figure 5 This is the pore size distribution diagram of Ce-doped cobalt-based perovskite catalyst material. DETAILED DESCRIPTION
[0028] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0029] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0030] Herein, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are for simplicity and convenience only. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0031] In this document, unless otherwise specified, “includes,” “including,” “contains,” “has,” or similar terms cover the meanings of “consisting of” and “mainly consisting of,” for example, “A includes a” covers the meanings of “A includes a and other” and “A only includes a.”
[0032] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0033] The invention provides a Ce-doped cobalt-based perovskite catalyst material, which is a cobalt-based perovskite structural material doped with Ce element A-position.
[0034] The present invention also provides a method for preparing the above-mentioned Ce-doped cobalt-based perovskite catalyst material, using glucose as a complexing agent, which has the advantages of simple preparation process, easy availability of raw materials, low cost, strong practicality, and easy large-scale production.
[0035] The present invention also provides the Ce-doped cobalt-based perovskite catalyst material for use in the catalytic combustion reaction of soot particles. The catalyst has a high catalytic activity and can completely remove soot particles at temperatures below 400°C.
[0036] The preparation method of the Ce-doped cobalt-based perovskite catalyst material comprises the following steps:
[0037] Mix three raw materials, namely, precursor salt, complexing agent glucose and water, in a beaker and stir on a stirrer, wherein the stirring time is 1-4 hours, the amount of precursor metal salt is 0.2-10 g, the amount of water is 10-50 mL, and the amount of glucose is 0.5-10 g; place the stirred solution in a 60-80°C oven and dry it for 12-24 hours, then move the dried sample into an 80-100°C oven and continue drying it for 12-24 hours; place the dried sample in a muffle furnace and calcine it at 450-1000°C for 2-10 hours to obtain a Ce-doped cobalt-based perovskite catalyst material.
[0038] The catalytic material is a perovskite catalyst material doped with Ce element A-site, and the B-site of the perovskite oxide material is any one of transition metal elements iron, cobalt, manganese, and nickel; secondly, the preparation method mainly uses glucose as a complexing agent, which complexes the A-site and B-site ions in the perovskite to obtain a Ce-doped cobalt-based perovskite oxide material.
[0039] The present invention will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not intended to limit the scope of the present invention. In addition, it should be understood that after reading the content taught by the present invention, those skilled in the art can make various changes or modifications to the present invention, and these equivalent forms fall within the scope limited by the appended claims of the application equally.
[0040] The following examples use conventional instruments and equipment in the art. The experimental methods in the following examples where specific conditions are not specified are usually carried out under conventional conditions or under conditions recommended by the manufacturer. The various raw materials used in the following examples are conventional commercial products unless otherwise specified, and their specifications are conventional specifications in the art. In the specification of the present invention and the following examples, unless otherwise specified, "%" means weight percentage, "part" means weight part, and ratio means weight ratio.
[0041] Example 1
[0042] A method for preparing a Ce-doped cobalt-based perovskite catalyst material comprises the following steps:
[0043] 2.056 g of lanthanum nitrate, 0.108 g of cerium nitrate and 1.455 g of cobalt nitrate were weighed according to the stoichiometric ratio, placed in a beaker and dissolved in 30 mL of deionized water, followed by adding 0.49 g of glucose and stirring on a stirrer for 2 h to obtain a mixed solution; the mixed solution was placed in an oven at 100°C for 12 h, and then dried at 80°C for 12 h, and the dried sample was placed in a muffle furnace and calcined at 650°C for 4 h to obtain a Ce-doped cobalt-based perovskite catalyst material (0.25 / 1 glucose dosage - (molar ratio of glucose to precursor metal salt)).
[0044] Figure 1 This is the XRD diagram of the Ce-doped cobalt-based perovskite catalyst material with a glucose dosage of 0.25 / 1. It can be seen from the figure that the prepared catalyst is a cobalt-based perovskite structure.
[0045] Example 2
[0046] A method for preparing a Ce-doped cobalt-based perovskite catalyst material comprises the following steps:
[0047] 2.056 g of lanthanum nitrate, 0.108 g of cerium nitrate, and 1.455 g of cobalt nitrate were weighed in a stoichiometric ratio, placed in a beaker and dissolved in 30 mL of deionized water, followed by adding 0.99 g of glucose, and then stirred on a stirrer for 2 h to obtain a mixed solution; the mixed solution was placed in an oven at 100 ° C and dried for 24 h, and then dried at 80 ° C for 12 h. The dried sample was placed in a muffle furnace and calcined at 650 ° C for 4 h to obtain a Ce-doped cobalt-based perovskite catalyst material (0.5 / 1 glucose dosage).
[0048] Figure 1 This is the XRD diagram of the Ce-doped cobalt-based perovskite catalyst material with a glucose dosage of 0.5 / 1. It can be seen from the figure that the prepared catalyst is a cobalt-based perovskite structure.
[0049] Example 3
[0050] A method for preparing a Ce-doped cobalt-based perovskite catalyst material comprises the following steps:
[0051] 2.056 g of lanthanum nitrate, 0.108 g of cerium nitrate, and 1.455 g of cobalt nitrate were weighed in a stoichiometric ratio, placed in a beaker and dissolved in 30 mL of deionized water, followed by adding 1.98 g of glucose, and then stirred on a stirrer for 2 h to obtain a mixed solution; the mixed solution was placed in an oven at 100 ° C and dried for 12 h, and then dried at 80 ° C for 12 h. The dried sample was placed in a muffle furnace and calcined at 650 ° C for 4 h to obtain a Ce-doped cobalt-based perovskite catalyst material (1 / 1 glucose dosage).
[0052] Figure 1 This is the XRD pattern of Ce-doped cobalt-based perovskite catalyst material with 1 / 1 glucose dosage. It can be seen from the figure that the prepared catalyst is a cobalt-based perovskite structure.
[0053] Example 4
[0054] A method for preparing a Ce-doped cobalt-based perovskite catalyst material comprises the following steps:
[0055] 2.056 g of lanthanum nitrate, 0.108 g of cerium nitrate, and 1.455 g of cobalt nitrate were weighed in a stoichiometric ratio, placed in a beaker and dissolved in 30 mL of deionized water, followed by adding 2.97 g of glucose, and then stirred on a stirrer for 2 h to obtain a mixed solution; the mixed solution was placed in an oven at 100 ° C and dried for 12 h, and then dried at 80 ° C for 12 h. The dried sample was placed in a muffle furnace and calcined at 650 ° C for 4 h to obtain a Ce-doped cobalt-based perovskite catalyst material (1.5 / 1 glucose dosage).
[0056] Figure 1 This is the XRD diagram of the Ce-doped cobalt-based perovskite catalyst material with a glucose dosage of 1.5 / 1. It can be seen from the figure that the prepared catalyst is a cobalt-based perovskite structure.
[0057] Example 5
[0058] A method for preparing a Ce-doped cobalt-based perovskite catalyst material comprises the following steps:
[0059] 2.056 g of lanthanum nitrate, 0.108 g of cerium nitrate, and 1.455 g of cobalt nitrate were weighed in a stoichiometric ratio, placed in a beaker and dissolved in 30 mL of deionized water, followed by adding 3.96 g of glucose, and then stirred on a stirrer for 2 h to obtain a mixed solution; the mixed solution was placed in an oven at 100 ° C and dried for 12 h, and then dried at 80 ° C for 12 h. The dried sample was placed in a muffle furnace and calcined at 650 ° C for 4 h to obtain a Ce-doped cobalt-based perovskite catalyst material (2 / 1 glucose dosage).
[0060] Figure 1 This is the XRD diagram of the Ce-doped cobalt-based perovskite catalyst material with a 2 / 1 glucose dosage. It can be seen from the figure that the prepared catalyst is a cobalt-based perovskite structure.
[0061] Figure 1 The XRD graph of Ce-doped cobalt-based perovskite catalyst material under different glucose dosage conditions shows that the prepared catalysts are all perovskite catalysts. Table 1 shows the activity of Ce-doped cobalt-based perovskite catalyst material in catalytic combustion of soot particles under different glucose dosage conditions. When the molar ratio of metal ions to glucose dosage is 1:1, the catalyst obtained shows the best catalytic activity.
[0062] Table 1 Activity of Ce-doped cobalt-based perovskite catalyst materials in catalytic combustion of soot particles under different glucose dosage conditions
[0063]
[0064] Example 6
[0065] A method for preparing a Ce-doped cobalt-based perovskite catalyst material comprises the following steps:
[0066] 2.056 g of lanthanum nitrate, 0.108 g of cerium nitrate, and 1.455 g of cobalt nitrate were weighed according to the stoichiometric ratio, placed in a beaker and dissolved in 30 mL of deionized water, followed by adding 1.98 g of glucose, and then stirred on a stirrer for 2 hours to obtain a mixed solution; the mixed solution was placed in an oven at 100°C and dried for 12 hours, and then dried at 80°C for 12 hours. The dried sample was placed in a muffle furnace and calcined at 450°C for 4 hours to obtain a Ce-doped cobalt-based perovskite catalyst material.
[0067] Figure 3 This is the XRD pattern of the Ce-doped cobalt-based perovskite catalyst material prepared under a calcination temperature of 450°C. It can be observed from the figure that the catalyst obtained at a calcination temperature of 450°C did not form an obvious cobalt-based perovskite structure.
[0068] Example 7
[0069] A method for preparing a Ce-doped cobalt-based perovskite catalyst material comprises the following steps:
[0070] 2.056 g of lanthanum nitrate, 0.108 g of cerium nitrate, and 1.455 g of cobalt nitrate were weighed according to the stoichiometric ratio, placed in a beaker and dissolved in 30 mL of deionized water, followed by adding 1.98 g of glucose, and then stirred on a stirrer for 2 hours to obtain a mixed solution; the mixed solution was placed in an oven at 100°C and dried for 12 hours, and then dried at 80°C for 12 hours. The dried sample was placed in a muffle furnace and calcined at 550°C for 4 hours to obtain a Ce-doped cobalt-based perovskite catalyst material.
[0071] Figure 3 This is the XRD pattern of the Ce-doped cobalt-based perovskite catalyst material prepared under a calcination temperature of 550°C. It can be observed from the figure that the catalyst obtained at a calcination temperature of 550°C did not form an obvious cobalt-based perovskite structure.
[0072] Example 8
[0073] A method for preparing a Ce-doped cobalt-based perovskite catalyst material comprises the following steps:
[0074] 2.056 g of lanthanum nitrate, 0.108 g of cerium nitrate, and 1.455 g of cobalt nitrate were weighed according to the stoichiometric ratio, placed in a beaker and dissolved in 30 mL of deionized water, followed by adding 1.98 g of glucose, and then stirred on a stirrer for 2 hours to obtain a mixed solution; the mixed solution was placed in an oven at 100°C and dried for 12 hours, and then dried at 80°C for 12 hours. The dried sample was placed in a muffle furnace and calcined at 750°C for 4 hours to obtain a Ce-doped cobalt-based perovskite catalyst material.
[0075] Figure 3This is the XRD pattern of the Ce-doped cobalt-based perovskite catalyst material prepared under a calcination temperature of 750°C. It can be observed from the figure that the catalyst obtained at a calcination temperature of 750°C did not form an obvious cobalt-based perovskite structure.
[0076] Example 9
[0077] A method for preparing a Ce-doped cobalt-based perovskite catalyst material comprises the following steps:
[0078] 2.056 g of lanthanum nitrate, 0.108 g of cerium nitrate, and 1.455 g of cobalt nitrate were weighed in a stoichiometric ratio, placed in a beaker and dissolved in 30 mL of deionized water, followed by adding 1.98 g of glucose and stirring on a stirrer for 2 h to obtain a mixed solution; the mixed solution was placed in an oven at 100 °C and dried for 12 h, and then dried at 80 °C for 12 h. The dried sample was placed in a muffle furnace and calcined at 850 °C for 4 h to obtain a Ce-doped cobalt-based perovskite catalyst material.
[0079] Figure 3 This is the XRD pattern of the Ce-doped cobalt-based perovskite catalyst material prepared under a calcination temperature of 850°C. It can be observed from the figure that the catalyst obtained at a calcination temperature of 850°C did not form an obvious cobalt-based perovskite structure.
[0080] Figure 2 These are scanning electron microscope photos of Ce-doped cobalt-based perovskite catalyst materials under different calcination temperature conditions. It can be seen from the figure that the change of calcination temperature has a great influence on the morphology of the prepared catalyst. With the increase of calcination temperature, the pore structure of the catalyst collapses and the size of the nanoparticles increases significantly. Figure 3 Figure 2 shows the XRD patterns of Ce-doped cobalt-based perovskite catalyst materials prepared under different calcination temperature conditions. It can be observed from the figure that only the catalysts obtained at calcination temperatures of 650, 750 and 850°C are cobalt-based perovskite oxides, which further indicates that 650°C is the lowest temperature for forming the cobalt-based perovskite oxide crystal phase. Figure 4 The nitrogen adsorption-desorption isotherms of this series of catalysts are shown in the figure. As shown in the figure, the adsorption isotherms of the above catalysts are typical type IV isotherms with H3 type hysteresis loops. The nitrogen adsorption isotherms of various catalysts are similar in shape, but the sizes of hysteresis loops are quite different. This may be due to the difference in the number of stacked pores and the shape of pore size in the obtained catalysts due to the difference in calcination temperature. Figure 5is the pore size distribution diagram of this series of catalysts. The results show that the pore size distribution of the catalysts obtained under different calcination temperature conditions is quite different, which may be caused by the significant change in the catalyst morphology, further indicating that the calcination temperature is one of the factors that significantly affect its physical properties. Table 2 shows the activity of Ce-doped cobalt-based perovskite catalysts in catalytic combustion of soot particles under different calcination temperature conditions. Combined with Table 1, it shows that when the calcination temperature is 450°C, the T 10 , T 50 and T 90 are 286℃, 352℃ and 391℃ respectively. With the increase of calcination temperature, the T 10 , T 50 and T 90 The catalyst calcined at 650 °C showed the best catalytic activity. 10 , T 50 and T 90 They are 279℃, 336℃ and 375℃ respectively.
[0081] Table 2 Activity of Ce-doped cobalt-based perovskite catalysts in the combustion of soot particles under different calcination temperatures
[0082]
[0083] Example 10
[0084] 2.056 g of lanthanum nitrate, 0.108 g of cerium nitrate, and 1.455 g of cobalt nitrate were weighed according to the stoichiometric ratio, placed in a beaker and dissolved in 30 mL of deionized water, followed by adding 2.10 g of citric acid monohydrate, and then stirred on a stirrer for 2 hours to obtain a mixed solution; the mixed solution was placed in an oven at 100°C and dried for 12 hours, and then dried at 80°C for 12 hours. The dried sample was placed in a muffle furnace and calcined at 850°C for 4 hours to obtain a Ce-doped cobalt-based perovskite catalyst material.
[0085] Embodiment 11
[0086] 2.056 g of lanthanum nitrate, 0.108 g of cerium nitrate, and 2.02 g of ferric nitrate were weighed in a stoichiometric ratio, placed in a beaker and dissolved in 30 mL of deionized water, followed by adding 2.10 g of citric acid monohydrate, and then stirred on a stirrer for 2 hours to obtain a mixed solution; the mixed solution was placed in an oven at 100°C and dried for 12 hours, and then dried at 80°C for 12 hours. The dried sample was placed in a muffle furnace and calcined at 850°C for 4 hours to obtain a Ce-doped cobalt-based perovskite catalyst material.
[0087] Example 12
[0088] 2.056 g of lanthanum nitrate, 0.108 g of cerium nitrate, and 1.789 g of manganese nitrate were weighed according to the stoichiometric ratio, placed in a beaker and dissolved in 30 mL of deionized water, followed by adding 2.10 g of citric acid monohydrate, and then stirred on a stirrer for 2 hours to obtain a mixed solution; the mixed solution was placed in an oven at 100°C and dried for 12 hours, and then dried at 80°C for 12 hours. The dried sample was placed in a muffle furnace and calcined at 850°C for 4 hours to obtain a Ce-doped cobalt-based perovskite catalyst material.
[0089] Embodiment 13
[0090] 2.056 g of lanthanum nitrate, 0.108 g of cerium nitrate, and 1.454 g of nickel nitrate were weighed according to the stoichiometric ratio, placed in a beaker and dissolved in 30 mL of deionized water, followed by adding 2.10 g of citric acid monohydrate, and then stirred on a stirrer for 2 hours to obtain a mixed solution; the mixed solution was placed in an oven at 100°C and dried for 12 hours, and then dried at 80°C for 12 hours. The dried sample was placed in a muffle furnace and calcined at 850°C for 4 hours to obtain a Ce-doped cobalt-based perovskite catalyst material.
[0091] Catalyst activity evaluation method: using gas chromatography detection system, the catalyst adopts fixed bed method
[0092] Specific steps: weighed Ce-doped cobalt-based perovskite catalyst material and soot particles are placed on weighing paper, stirred evenly with a medicine spoon to make the catalyst and soot particles in loose contact, and loaded into a 6mm quartz reaction tube, wherein the gas flow rate is controlled to be 50mL / min, the volume content of NO in the gas is 2000ppm, and O 2 The volume content is 10%, and the balance is Ar; the heating rate is controlled at about 2℃ / min.
[0093] Evaluation method: The oxidation ability of the catalyst is expressed by the combustion temperature of the soot particles, where the ignition temperature of the soot particles (T 10 ), the temperature corresponding to the maximum burning rate (T 50 ) and burnout temperature (T 90 ), which represent the temperature points corresponding to 10%, 50% and 90% of the soot combustion, respectively. The calculation method is to calculate the CO generated by the combustion of soot in the programmed temperature oxidation reaction. 2 Integrate the curve with CO, CO 2 The temperature points corresponding to 10%, 50%, and 90% of the sum of the CO integral areas are T 10 、T 50 and T 90 . Where S CO2 m Indicates the CO corresponding to the catalyst when the soot combustion rate is the maximum2 The results of the catalytic combustion of pure soot particles are shown in Table 3. It can be seen from the table that in the absence of a catalyst, the combustion temperature of pure soot is higher, and its T 10 , T 50 and T 90 are 408℃, 539℃ and 584℃ respectively, and CO 2 The selectivity is only 49.2%, which indicates that the Ce-doped cobalt-based perovskite catalyst material prepared by the present invention has a high catalytic activity for the catalytic combustion of soot particles.
[0094] Table 3 Catalytic combustion activity of pure soot particles
[0095]
[0096] The preparation method of the present invention has the advantages of simple preparation process, strong practicability, easy large-scale production, high preparation success rate, and a yield close to 100%. In particular, no solid and liquid waste is generated during the preparation process, and the gas generated during the catalyst calcination process is mainly CO 2 , CO and NO x , the current exhaust after-treatment technology is fully capable of achieving clean emissions.
[0097] The present invention introduces Ce into the cobalt-based perovskite catalyst. Since the valence state of Ce can be changed between +3 and +4, cerium oxide has a strong oxygen storage and release capacity. At the same time, during the drying and high-temperature heat treatment of the perovskite catalyst, the surface area of the synthesized catalyst is relatively low due to shrinkage and particle agglomeration, thereby affecting the contact efficiency between the soot particles and the active sites of the catalyst. Therefore, the present invention selects glucose as a complexing agent and also exerts its function as a pore-forming agent to prepare a Ce-doped Co-based perovskite oxide catalyst with a porous structure, thereby optimizing its catalytic performance.
[0098] The above contents are only for explaining the technical idea of the present invention and cannot be used to limit the protection scope of the present invention. Any changes made on the basis of the technical solution in accordance with the technical idea proposed by the present invention shall fall within the protection scope of the claims of the present invention.
Claims
1. A method for preparing a Ce-doped cobalt-based perovskite catalyst material, characterized in that: The following steps are involved: The precursor metal salt, the complexing agent and water are mixed and stirred to obtain a mixed solution; the obtained mixed solution is dried once to obtain a dried product; The dried product is subjected to secondary drying treatment, and then subjected to calcination treatment. After the calcination treatment is completed, a Ce-doped cobalt-based perovskite catalyst material is obtained.
2. The method for preparing a Ce-doped cobalt-based perovskite catalyst material according to claim 1, characterized in that: The precursor metal salt is a mixture of lanthanum salt, cerium salt and cobalt salt.
3. The method for preparing a Ce-doped cobalt-based perovskite catalyst material according to claim 1, characterized in that: The complexing agent is one of glucose and citric acid monohydrate.
4. The method for preparing a Ce-doped cobalt-based perovskite catalyst material according to claim 1, characterized in that: The usage ratio of the precursor metal salt, the complexing agent and water is 0.2-10g:0.5-10g:10-50mL.
5. The method for preparing a Ce-doped cobalt-based perovskite catalyst material according to claim 1, characterized in that: The mixing and stirring time is 1-4h.
6. The method for preparing a Ce-doped cobalt-based perovskite catalyst material according to claim 1, characterized in that: The temperature of the primary drying treatment is 80-120° C. and the time is 12-24 hours.
7. The method for preparing a Ce-doped cobalt-based perovskite catalyst material according to claim 1, characterized in that: The secondary drying treatment is performed at 80-100°C for 12-24 hours.
8. The method for preparing a Ce-doped cobalt-based perovskite catalyst material according to claim 1, characterized in that: The calcination treatment is carried out at a temperature of 450-1000° C. and for a time of 2-10 hours.
9. A Ce-doped cobalt-based perovskite catalyst material, characterized in that: The material is prepared by the preparation method described in any one of claims 1 to 8; the Ce-doped cobalt-based perovskite catalyst material is obtained by complexation between the A site and the B site of the perovskite catalyst material.
10. Use of the Ce-doped cobalt-based perovskite catalyst material according to claim 9 in the catalytic combustion reaction of soot particles.
Citation Information
Patent Citations
Preparation method for hierarchical pore perovskite catalyst
CN107376924A
Large-pore structured lanthanum-based perovskite catalyst material as well as preparation method and application thereof
CN108126691A
Bimetallic element co-doped lanthanum-based perovskite oxide catalyst as well as preparation method and application thereof
CN115155603A
Method and device for catalytic oxidation and reduction of gases and vapours by crystalline compounds of heavy metals and rare earths
US20080085830A1
Perovskite catalyst and method of manufacturing the same
US20120129689A1