Sulfur-tolerant shift catalyst and preparation method thereof

The porosity of the catalyst is improved by step-by-step mixing and kneading preparation method, and the problem of strong exotherm of methanation side reaction caused by high CO content in pulverized coal gasification technology is solved, and the effect of reducing the reaction temperature and methane generation is achieved, ensuring the device Safe and stable operation.

CN118874480APending Publication Date: 2024-11-01QINGDAO LIANXIN CATALYTIC MATERIALS CO LTD

Patent Information

Application Number
CN202410915058.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01

AI Technical Summary

Technical Problem

The strong exothermic problem of methanation side reaction caused by high CO content in pulverized coal gasification technology leads to catalyst sintering and equipment overtemperature, making it difficult to ensure the safe and stable operation of the device.

Method used

The carrier preparation method is adopted by step-by-step mixing and kneading to prepare the skeleton material and roast it through the mixing and kneading method to increase the porosity of the catalyst, prevent the sintering between the carrier particles, improve the pore structure of the catalyst, and increase the macroporous fraction to reduce the reaction temperature.

Benefits of technology

The methane generation amount is significantly reduced, prevents the temperature of the furnace from flying, and improves the durability of the catalyst and the stability of the device.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004934850780000071
    Figure BDA0004934850780000071
Patent Text Reader

Abstract

The invention discloses a sulfur-tolerant shift catalyst with high porosity and a preparation method thereof. The catalyst comprises a catalyst carrier and effective components loaded on the catalyst carrier, the catalyst carrier is prepared from a framework material, a carrier raw material and sesbania powder; the framework material is prepared from a framework material raw material and a binder; the effective components comprise cobalt and molybdenum. The catalyst disclosed by the invention has relatively high porosity and macroporous distribution, and can be beneficial to rapid transfer of shift reaction heat and reduction of the hot-spot temperature of the reaction, so that the catalyst has a function of inhibiting methane side reaction, temperature runaway of a shift converter due to methanation side reaction can be prevented, and shift operation is stabilized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of catalysts, and specifically relates to a sulfur-resistant shift catalyst and a preparation method thereof, and particularly relates to a sulfur-resistant shift catalyst capable of reducing or inhibiting a strongly exothermic methanation side reaction and a preparation method thereof. Background Art

[0002] In recent years, with the rapid development of my country's coal chemical industry, new coal gasification technologies have been continuously introduced and emerged, forming my country's unique and diverse coal gasification technologies. Pulverized coal gasification technology is very popular among coal chemical users due to its low coal quality requirements, high content of effective components (CO+H2 89%) in process gas, low consumption of raw coal and oxygen, and low environmental pollution. In less than ten years, my country has successively introduced dozens of such pulverized coal gasification processes and used this technology for synthetic ammonia, methanol or coal-to-liquid projects. However, the CO content in the raw gas produced by pulverized coal gasification technology is as high as 60%. How to avoid the methanogenic side reaction in the first reactor, prevent the overheating of the conversion furnace, stabilize the operation of the device and obtain the desired gas composition is the key issue in the production of high CO raw gas devices.

[0003] Methanation is a method of producing methane by hydrogenating CO or CO2 under the action of a catalyst, but it is one of the side reactions of the CO conversion process. The specific reaction equation is as follows:

[0004] CO + 3H2→CH4 + H2O ΔH298 K = -206.28 kJ / mol (1)

[0005] CO2 + 4H2→CH4 + 2H2O ΔH298 K = -165 kJ / mol (2)

[0006] Because the reaction is a highly exothermic reaction, every 1% of CH4 generated will cause the bed to generate a temperature rise of about 60-70℃, burning the catalyst and equipment! And the higher the CO content and the lower the water / gas ratio, the easier it is for the methanogenic side reaction to occur. Since the CO content in the pulverized coal gasification feed gas is high and the water / gas ratio is low, the problem of preventing the methanogenic side reaction is more prominent. The catalyst's ability to resist the methanogenic side reaction must be improved to ensure the safe, stable and long-term implementation of the pulverized coal gasification process gas in the coal chemical plant. Summary of the invention

[0007] Since the methanation reaction is a highly exothermic reaction, a large amount of reaction heat will be generated inside the reactor, and high temperature will cause the catalyst particles to sinter and deactivate. Therefore, lowering the reaction temperature is the key to reducing methane generation. The present invention finds that by improving the pore structure of the catalyst and increasing the macropore fraction of the catalyst, the developed catalyst has a higher porosity, which is conducive to the rapid transfer and removal of reaction heat, thereby reducing the reaction temperature and achieving the purpose of inhibiting the methane side reaction.

[0008] When preparing the carrier of traditional sulfur-resistant shift catalysts, the raw materials are directly mixed and prepared. The carrier raw material particles are easily sintered to form small holes or dead holes. The prepared catalyst has a small porosity, which is not conducive to the rapid removal of heat and easily induces methanation side reactions.

[0009] The present invention adopts a carrier preparation method using step-by-step kneading, firstly adopts a kneading method to prepare a carrier skeleton material, then crushes the skeleton material to 180-300 meshes, kneads it with the carrier raw material, extrudes it into strips and bakes it to prepare a catalyst carrier. The skeleton material added in the present invention has a certain strength and particle size due to kneading, high-temperature baking and crushing, and can play a role in skeleton isolation between carrier particles, can prevent sintering between carrier particles, and make the carrier have a higher porosity, so as to achieve the purpose of improving the pore structure of the catalyst carrier and increasing the macropore fraction of the catalyst.

[0010] The catalyst prepared by this method has large porosity (pores larger than 150 nm are distributed at more than 40%, much higher than the 13.92% of the comparative sample) and high water absorption rate, and the methane generation is significantly reduced.

[0011] The first aspect of the present invention is to disclose a sulfur-resistant shift catalyst with high porosity, characterized in that it comprises a catalyst carrier and an effective component supported on the catalyst carrier;

[0012] The catalyst carrier is made of skeleton material, carrier raw material and sesbania powder; the skeleton material is made of skeleton material raw material and a binder;

[0013] The active ingredients include cobalt and molybdenum.

[0014] In some embodiments of the present invention, the carrier raw material is at least one of alumina, aluminum hydroxide and pseudo-boehmite.

[0015] In some embodiments of the present invention, the skeleton material raw material is at least one of oxides or carbonates of Mg, Zr, Ca, Ti, Fe, Ba and Al;

[0016] And / or, the binder is at least one of nitrates or sulfates of Mg, Al and Ca, preferably nitrates of Mg and Al.

[0017] In some embodiments of the present invention, the weight content of cobalt as an effective ingredient in the catalyst is 0.2-20% in terms of CoO; the weight content of molybdenum as an effective ingredient in the catalyst is 1-20% in terms of MoO3.

[0018] In some embodiments of the present invention, it is characterized in that the distribution of pores larger than 150 nm of the catalyst is larger than 40%.

[0019] In some embodiments of the present invention, the particle size of the skeleton material is 180-300 mesh.

[0020] The second aspect of the present invention is to disclose a method for preparing the sulfur-resistant shift catalyst with high porosity as described in the first aspect, comprising the following steps:

[0021] S01, kneading, drying, roasting and crushing the skeleton material raw material and the binder to obtain the skeleton material;

[0022] S02, kneading the skeleton material obtained in S01 with a carrier raw material, extruding and calcining to obtain a catalyst carrier;

[0023] S03, impregnating the catalyst carrier obtained in S02 with active components to obtain a catalyst.

[0024] In some embodiments of the present invention, the weight ratio of the skeleton material raw material to the binder is 100:(10-1).

[0025] In some embodiments of the present invention, in S01, the particles are crushed to a size of 180-300 mesh.

[0026] In some embodiments of the present invention, in S02, the calcination temperature is 450-700°C, preferably 500-600°C.

[0027] Beneficial effects of the present invention:

[0028] Traditional sulfur-resistant carriers are mostly prepared by directly mixing raw materials. The raw material particles of the carrier are easily sintered to form small holes or dead holes. The prepared catalyst has a small porosity, which is not conducive to the rapid removal of reaction heat. The present invention adopts a step-by-step kneading method for preparing the carrier, that is, firstly a kneading method is used to prepare a carrier skeleton material. The skeleton material has a certain strength and particle size, which can play a skeleton isolation role between the carrier particles, prevent the sintering between the carrier particles, and make the carrier have a higher porosity, thereby achieving the purpose of improving the pore structure of the catalyst carrier and increasing the macropore fraction of the catalyst.

[0029] The catalyst of the present invention has a high porosity and macropore distribution, which can be beneficial to the rapid transfer of heat of the conversion reaction, reduce the hot spot temperature of the reaction, and thus has the function of inhibiting the methane side reaction, which can prevent the conversion furnace from "overheating" due to the methanogenic side reaction and stabilize the conversion operation.

[0030] The catalyst prepared by the preparation method of the present invention has large porosity (pores larger than 150 nm are distributed at more than 40%, much higher than 13.92% of the comparative sample), high water absorption rate, and significantly reduced methane production. The comparative evaluation results are shown in Table 1. DETAILED DESCRIPTION

[0031] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0032] Unless otherwise specified, the embodiments and comparative examples are parallel tests with the same components, component contents, preparation steps and preparation parameters. The magnesium oxide (industrial pure), calcium oxide (industrial pure), titanium oxide (industrial pure), sesbania powder (industrial pure) and pseudo-boehmite (industrial pure, produced by Zibo Zhangdian Aluminum Plant or Shanxi Aluminum Plant) are commercially available products. Unless otherwise specified, the percentage of the solution is w / v percentage.

[0033] Example 1

[0034] Take 50 grams of magnesium oxide and 120 grams of pseudo-boehmite, add 30 mL of 10% aluminum nitrate solution and knead for 10 minutes, dry at 120°C for 2 hours, roast at 600°C for 2 hours and crush to 180 mesh to obtain a skeleton material.

[0035] Take 200 grams of pseudo-boehmite, add 100 grams of skeleton material, add 10 grams of sesbania powder and mix well.

[0036] 120 mL of 10% magnesium nitrate and 6 g of citric acid were added and stirred evenly. The evenly stirred solution was added to the above materials and kneaded for 30 minutes. The strips were extruded and calcined at 550° C. for 2 hours to obtain a carrier.

[0037] Take 100 grams of the carrier, add 12 grams of tetramolybdate ammonia, 8 grams of cobalt nitrate into 30 mL of ammonia water to prepare a co-impregnation solution, impregnate the carrier with equal volume of solution for 1 hour, dry at 120°C for 2 hours, and calcine at 550°C to obtain the catalyst. The catalyst number is C-1. Its test results are shown in Table 1.

[0038] Example 2

[0039] The preparation method is the same as that of Example 1, except that 50 grams of magnesium oxide is replaced by 50 grams of calcium oxide. The catalyst is numbered C-2. The performance comparison is shown in Table 1.

[0040] Example 3

[0041] The preparation method is the same as that of Example 1, except that 50 grams of magnesium oxide is replaced by 20 grams of titanium oxide and 30 grams of magnesium oxide. The catalyst is numbered C-3. The performance comparison is shown in Table 1.

[0042] Example 4

[0043] The preparation method is the same as that of Example 1, except that 180 g of pseudo-boehmite is added with 120 g of the skeleton material, and kneaded with 6% magnesium nitrate and 1% citric acid solution to obtain a carrier. The catalyst number is C-4. The performance comparison is shown in Table 1.

[0044] Comparative Example 1

[0045] The difference from Example 1 is that no aggregate material is added.

[0046] Comparative Example 2

[0047] The difference from Example 3 is that no aggregate material is added.

[0048] Table 1 Comparison of performance of different catalysts

[0049]

[0050] Experimental conditions: pressure 4.0Mpa, airspeed 2000h -1 , water vapor 0.4, reaction temperature 450℃.

[0051] Raw gas composition (volume ratio): CO 62.95%, CO2 3.56%, H2 balance.

[0052] The preferred specific implementation modes and embodiments of the present invention are described in detail above, but the present invention is not limited to the above implementation modes and embodiments, and various changes can be made within the knowledge scope of those skilled in the art without departing from the concept of the present invention.

Claims

1. A sulfur-resistant shift catalyst with high porosity, It is characterized in that It comprises a catalyst carrier and an effective component loaded on the catalyst carrier; The catalyst carrier is made of skeleton material, carrier raw material and sesbania powder; the skeleton material is made of skeleton material raw material and a binder; The active ingredients include cobalt and molybdenum.

2. The sulfur-resistant shift catalyst with high porosity according to claim 1, It is characterized in that The carrier raw material is at least one of aluminum oxide, aluminum hydroxide and pseudo-boehmite.

3. The sulfur-resistant shift catalyst with high porosity according to claim 1 or 2, It is characterized in that The raw material of the skeleton material is at least one of oxides or carbonates of Mg, Zr, Ca, Ti, Fe, Ba and Al.

4. The sulfur-resistant shift catalyst with high porosity according to any one of claims 1 to 3, It is characterized in that The binder is at least one of nitrates or sulfates of Mg, Al and Ca, preferably nitrates of Mg and Al.

5. The sulfur-resistant shift catalyst with high porosity according to any one of claims 1 to 4, It is characterized in that The weight content of the active ingredient cobalt in the catalyst is 0.2-20% in terms of CoO; 3 The weight content of molybdenum, an effective ingredient in the catalyst, is 1-20%.

6. The sulfur-resistant shift catalyst with high porosity according to any one of claims 1 to 5, It is characterized in that The catalyst has a distribution of pores larger than 150 nm of greater than 40%.

7. The sulfur-resistant shift catalyst with high porosity according to any one of claims 1 to 6, It is characterized in that The particle size of the skeleton material is 180-300 meshes.

8. A method for preparing a sulfur-resistant shift catalyst with high porosity according to any one of claims 1 to 7, It is characterized in that The following steps are involved: S01, kneading, drying, roasting and crushing the skeleton material raw material and the binder to obtain the skeleton material; S02, kneading the skeleton material obtained in S01 with a carrier raw material, extruding and calcining to obtain a catalyst carrier; S03, impregnating the catalyst carrier obtained in S02 with active components to obtain a catalyst.

9. The preparation method according to claim 8, It is characterized in that The weight ratio of the skeleton material raw material to the binder is 100:(10-1); And / or, the skeleton material raw material, calculated as oxide, is 5-60% (weight percentage) of the catalyst carrier raw material, and more preferably 20-40% (weight percentage).

10. The preparation method according to claims 8 and 9, It is characterized in that In S02, the calcination temperature is 450-700°C, preferably 500-600°C.

Citation Information

Patent Citations

  • Sulfur-tolerant methanation catalyst and preparation method thereof

    CN103495421A

  • Sulfur-tolerant shift catalyst with high porosity and preparation method thereof

    CN110841652A

  • Cobalt-molybdenum CO sulfur-tolerant shift catalyst and preparation method thereof

    CN112403482A

  • Sulfur transform resistant macroreticular catalyst and its preparing process

    CN1283524A

  • Water-gas shift catalyst

    US20140158942A1

Cited By

  • High-pressure sulfur-tolerant shift catalyst promoter compound and catalyst thereof

    CN120519204A

  • A high-pressure sulfur-tolerant shift catalyst promoter complex and catalyst thereof

    CN120519204B