Bi2-xEuxWO6 / Nb2C MXene photo-thermal material as well as preparation method and application thereof

Through the preparation of Bi2-xEuxWO6/Nb2C MXene photothermal materials, a heterojunction structure is formed by combining rare earth elements Eu doping and Nb2C MXene, which solves the problem of low photocatalytic performance of Bi2WO6 and achieves efficient CO2 reduction reaction, especially Methane selectivity reaches 100% and maintains good cycle stability.

CN118874506AActive Publication Date: 2024-11-01SHAANXI UNIV OF SCI & TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410916283.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-09
Publication Date
2024-11-01
Estimated Expiration
2044-07-09

AI Technical Summary

Technical Problem

The photocatalytic performance of pure phase Bi2WO6 is low, mainly due to its low photoelectron separation efficiency and poor surface activation energy, resulting in insufficient catalytic activity and selectivity in CO2 photoreduction reaction.

Method used

Bi2-xEuxWO6/Nb2C MXene photothermal material is used to form a heterojunction structure through the combination of rare earth element Eu doping and Nb2C MXene, and is prepared by ultraviolet irradiation method to form a built-in electric field and LSPR effect to enhance photothermal catalytic activity.

Benefits of technology

The activity and selectivity of CO2 reduction reaction are significantly improved, the methane selectivity reaches 100%, and the material maintains good stability during recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004935186200000011
    Figure HDA0004935186200000011
  • Figure HDA0004935186200000012
    Figure HDA0004935186200000012
  • Figure HDA0004935186200000013
    Figure HDA0004935186200000013
Patent Text Reader

Abstract

The invention provides a Bi (2-x) EuxWO6 / Nb2C MXene photo-thermal material and a preparation method and application thereof.The preparation method comprises the steps that Bi (NO3) 3, Eu (NO3) 3 and Na2WO4 are dissolved in ethylene glycol, then a reaction precursor solution is obtained, a hydrothermal reaction is conducted, and Bi (2-x) EuxWO6 is obtained; the preparation method comprises the following steps: dispersing Nb2C MXene powder in ethanol to obtain a turbid liquid A; the preparation method comprises the following steps: dispersing Bi (2-x) EuxWO6 in ethanol to obtain a turbid liquid B; the turbid liquid A and the turbid liquid B are subjected to ultraviolet irradiation respectively, then the turbid liquid A is slowly added into the turbid liquid B, the obtained mixed turbid liquid is subjected to ultraviolet irradiation, and the Bi2-xEuxWO6 / Nb2C MXene photo-thermal material is obtained. According to the Bi2-xEuxWO6 / Nb2C MXene photo-thermal material disclosed by the invention, the photo-thermal catalytic CO2 reduction activity and the methane selectivity are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of composite materials for environmental protection and solar energy utilization, and is specifically a Bi 2-x Eu x WO6 / Nb2C MXene photothermal material and its preparation method and application. Background Art

[0002] The resource utilization of CO2 is an effective way to develop clean energy. Currently, there are many commercial carbon fixation methods, such as biological carbon fixation and thermal catalytic CO2 methanation. Among them, photothermal catalytic CO2 reduction reaction has significant advantages and can convert CO2 into clean energy or high-value chemicals such as CO, CH4, CH3OH, C2H4, etc.

[0003] Bi2WO6 is made of perovskite (Bi2O2) 2+ and fluorite (WO4) 2- The alternating layers not only provide a large number of low-coordinated atoms as catalytic sites, but also shorten the carrier transport distance. In addition, the redox potential of Bi2WO6 is suitable for all CO2 photoreduction reactions. However, due to its low photoelectron separation efficiency and poor surface activation energy, the photocatalytic performance of pure phase Bi2WO6 is low. Summary of the invention

[0004] In order to solve the above-mentioned problems of the prior art, the present invention provides a Bi 2-x Eu x WO6 / Nb2C MXene photothermal materials, their preparation methods and applications promote the photothermal catalytic CO2 reduction activity and selectivity of Bi2WO6.

[0005] The present invention is achieved through the following technical solutions:

[0006] The present invention provides a Bi 2-x Eu x The preparation method of WO6 / Nb2C MXene photothermal material comprises the following steps:

[0007] Step 1, dissolving Bi(NO3)3, Eu(NO3)3 and Na2WO4 in ethylene glycol, stirring, and obtaining a reaction precursor solution; subjecting the reaction precursor solution to a hydrothermal reaction to obtain Bi 2-x Eu x WO6;

[0008] Step 2: Add Nb2C MXene powder to ethanol and disperse it by ultrasonic to obtain suspension A; 2-x Eu x WO6 was added to ethanol and ultrasonically dispersed to obtain suspension B;

[0009] Step 3, irradiating suspension A and suspension B with ultraviolet light respectively, then slowly adding suspension A into suspension B, irradiating the obtained mixed suspension with ultraviolet light, washing and drying the product, and obtaining Bi 2-x Eu x WO6 / Nb2C MXene photothermal materials.

[0010] Preferably, in step 1, the molar ratio of Eu(NO3)3 to Bi(NO3)3 is (0.002-0.010):1.

[0011] Preferably, in step 1, the hydrothermal reaction temperature is 150-180° C. and the time is 9-12 h.

[0012] Preferably, in step 2, Bi 2-x Eu x The molar ratio of WO6 and Nb2C MXene is (0.5-1):1.

[0013] Preferably, in step 2, the preparation method of Nb2C MXene powder is: adding Nb2AlC precursor powder to HF solution, and then stirring the obtained mixture solution in a water bath to react, and after the reaction is completed, washing and drying the obtained product to obtain Nb2C MXene.

[0014] Preferably, in step 3, the suspension A and the suspension B are respectively irradiated with ultraviolet light for 30-60 minutes.

[0015] Preferably, in step 3, the mixed suspension is irradiated with ultraviolet light for 3-6 hours.

[0016] The present invention provides Bi obtained by the preparation method as described above 2-x Eu x WO6 / Nb2C MXene photothermal materials.

[0017] Preferably, the Bi 2-x Eu x Bi in WO6 / Nb2C MXene photothermal materials 2-x Eu x The morphology of WO6 is nano-flower-shaped. 2-x Eu x WO6 is distributed on the surface of Nb2C MXene.

[0018] The present invention also provides the Bi 2-x Eu x Application of WO6 / Nb2C MXene photothermal materials in photothermal catalytic reduction of CO2 to produce methane.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention successfully uses ultraviolet irradiation to dope Bi with rare earth element Eu. 2-x Eu x WO6 and Nb2C MXene were composited to successfully prepare Bi 2-x Eu x WO6 / Nb2C MXene heterojunction photothermal materials. Nb2C MXene and Bi 2-x Eu x The electron concentration difference of WO6 causes the electrons to move from Bi 2-x Eu x WO6 transfer to Nb2C MXene accompanied by Bi 2-x Eu x Bi in WO6 / Nb2C MXene 5+ The reduction of Bi 2-x Eu x WO6 points to the built-in electric field of Nb2C MXene.

[0021] The Bi prepared by the present invention 2-x Eu x When WO6 / Nb2C MXene heterojunction photothermal materials are used in the photothermal reduction of CO2, the structure of Bi2WO6 is adjusted by doping with rare earth elements to generate more electrons to participate in the CO2 reduction reaction; 2- x Eu x The built-in electric field of the WO6 / Nb2C MXene heterojunction, the LSPR effect of Nb2C MXene, and the upconversion effect of the rare earth element Eu jointly replenish the electrons required in the photothermal reduction of CO2 reaction, thereby improving the photothermal catalytic CO2 reduction activity and selectivity, significantly enhancing the degree of product methanation, and achieving a methane selectivity of 100%. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0023] Figure 1 The XRD pattern of the photothermal material prepared in the present invention;

[0024] Figure 2 This is a SEM image of the Nb2C MXene photothermal material prepared in Comparative Example 1 of the present invention;

[0025] Figure 3 This is a SEM image of the Bi2WO6 / Nb2C MXene photothermal material prepared in Comparative Example 2 of the present invention;

[0026] Figure 4 This is a SEM image of the photothermal material prepared in Example 2 of the present invention;

[0027] Figure 5 TEM image of the photothermal material prepared in Example 2 of the present invention;

[0028] Figure 6 HRTEM image of the photothermal material prepared in Example 2 of the present invention;

[0029] Figure 7 MB absorbance curve of Nb2C MXene prepared in comparative example 1 of the present invention under dark conditions;

[0030] Figure 8 MB absorbance curve of Bi2WO6 / Nb2C MXene prepared in comparative example 2 of the present invention under dark conditions;

[0031] Fig. 9 MB absorbance curve of the photothermal material prepared in Example 2 of the present invention under dark conditions;

[0032] Fig.10 The hole EPR spectrum of the photothermal material prepared in Example 2 of the present invention under dark conditions;

[0033] Fig.11 For the present invention Bi 2-x Eu x WO6 / Nb2C MXene formation process;

[0034] Fig.12 UV-Vis-NIR DRS spectra of the photothermal materials of Comparative Example 3 and Examples 1-4 prepared in the present invention;

[0035] Fig.13 Bi prepared in the present invention 2-x Eu x WO6 / Nb2C MXene photothermal catalytic reduction of CO2 conversion rate diagram;

[0036] Fig.14 Bi prepared in the present invention 2-x Eu x WO6 / Nb2C MXene photothermal catalytic reduction of CO2 cycle diagram;

[0037] Fig.15 This is a graph showing the change in surface temperature of the photothermal material prepared in Example 2 of the present invention over time;

[0038] Fig.16 This is a graph of the CO2 photocatalytic conversion rate of the photothermal materials prepared in Comparative Example 3 and Example 2 of the present invention under a single-wavelength light source. DETAILED DESCRIPTION

[0039] The following describes the embodiments of the present invention through specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention.

[0040] It should be noted that the process equipment or devices not specifically specified in the following embodiments are all conventional equipment or devices in the art.

[0041] It should be noted that the terms "include" and "have" and any variations thereof are intended to cover non-exclusive inclusions. For example, a process, method, system, product or device that includes a series of steps or units is not necessarily limited to those steps or units clearly listed, but may include other steps or units that are not clearly listed or inherent to these processes, methods, products or devices. Moreover, unless otherwise specified, the numbering of each method step is only a convenient tool for identifying each method step, and is not intended to limit the order of arrangement of each method step or to define the scope of the present invention. Changes or adjustments in their relative relationships should also be regarded as the scope of the present invention without substantially changing the technical content.

[0042] In the following embodiments, Bi 2-x Eu x WO6 was prepared according to the method of Comparative Example 3, except that the amount of Eu(NO3)3 was adjusted according to the value of x.

[0043] Comparative Example 1

[0044] Step 1: Add Nb2AlC powder to HF solution of >40% to form a mixed solution; wherein the concentration of Nb2AlC is 0.05 g / mL.

[0045] Step 2: Place the mixed solution in a water bath, heat to 55°C, and stir at a stirring rate of 600 r / min for 96 h.

[0046] Step 3: The mixed solution obtained in step 2 was centrifuged, and the obtained product was washed with deionized water until the pH of the supernatant reached about 6 to 7, and then vacuum dried at 60°C for 12 h to obtain Nb2C MXene.

[0047] Comparative Example 2

[0048] Step 1: Dissolve 1mmol Bi(NO3)3 and 0.5mmol Na2WO4 in 30ml ethylene glycol, stir magnetically for 30min to obtain a reaction precursor solution, then transfer the reaction precursor solution to a 50ml hydrothermal autoclave, perform a hydrothermal reaction at 160℃ for 12h, cool to room temperature with the furnace, wash the resulting precipitate with deionized water and anhydrous ethanol for 3 times respectively, and dry at 70℃ for 12h to obtain Bi2WO6.

[0049] Step 2: Add 1 mmol of Nb2C MXene powder into 20 ml of ethanol and disperse it by ultrasonic for 30 min to obtain suspension A.

[0050] Step 3: Add 1 mmol Bi2WO6 into 20 ml ethanol and disperse by ultrasonic for 30 min to obtain suspension B.

[0051] Step 4: Suspension A and suspension B were irradiated with ultraviolet light for 30 minutes under magnetic stirring conditions, and then suspension A was slowly added to suspension B. The molar ratio of Bi2WO6 and Nb2C MXene was 1:1. The obtained mixed suspension was irradiated with ultraviolet light for 3 hours. The product was first washed with deionized water 3 times, then washed with anhydrous ethanol 3 times, and dried at 70°C for 12 hours to obtain a Bi2WO6 / Nb2C MXene heterojunction photocatalyst.

[0052] Comparative Example 3

[0053] Step 1: Dissolve 1 mmol of Bi(NO3)3, 0.005 mmol of Eu(NO3)3 and 0.5 mmol of Na2WO4 in 30 ml of ethylene glycol and stir magnetically for 30 min to obtain a reaction precursor solution.

[0054] Step 2: Transfer the reaction precursor solution to a 50 ml hydrothermal reactor, react at 160 ° C for 12 hours, cool to room temperature with the furnace, wash the resulting precipitate with deionized water and anhydrous ethanol three times respectively, and dry at 70 ° C for 12 hours to obtain Bi 1.995 Eu 0.005 WO6.

[0055] Embodiment 1:

[0056] Step 1: Add 1 mmol of Nb2C MXene powder into 20 ml of ethanol and disperse it by ultrasonic for 30 min to obtain suspension A.

[0057] Step 2: 1 mmol Bi 1.998 Eu 0.002 WO6 was added to 20 ml of ethanol and ultrasonically dispersed for 30 min to obtain suspension B.

[0058] Step 3, irradiate suspension A and suspension B with ultraviolet light for 30 min under magnetic stirring, then slowly add suspension A to suspension B. 1.998 Eu 0.002 The molar ratio of WO6 and Nb2C MXene was 1:1. The obtained mixed suspension was irradiated with UV light for 3 h. The product was washed 3 times with deionized water and then 3 times with anhydrous ethanol, and dried at 70 °C for 12 h to obtain Bi 1.998 Eu 0.002 WO6 / Nb2C MXene heterojunction photocatalyst.

[0059] Embodiment 2:

[0060] Step 1: Add 1 mmol of Nb2C MXene powder into 20 ml of ethanol and disperse it by ultrasonic for 30 min to obtain suspension A.

[0061] Step 2: 1mmolBi 1.995 Eu 0.005 WO6 was added to 20 ml of ethanol and ultrasonically dispersed for 30 min to obtain suspension B.

[0062] Step 3, irradiate suspension A and suspension B with ultraviolet light for 30 min under magnetic stirring, then slowly add suspension A to suspension B. 1.995 Eu 0.005 The molar ratio of WO6 and Nb2C MXene was 1:1. The obtained mixed suspension was irradiated with UV light for 3 h. The product was washed 3 times with deionized water and then 3 times with anhydrous ethanol, and dried at 70 °C for 12 h to obtain Bi 1.995 Eu 0.005 WO6 / Nb2C MXene heterojunction photocatalyst.

[0063] Embodiment 3:

[0064] Step 1: Add 1 mmol of Nb2C MXene powder into 20 ml of ethanol and disperse it by ultrasonic for 30 min to obtain suspension A.

[0065] Step 2: 1mmolBi 1.9925 Eu 0.0075 WO6 was added to 20 ml of ethanol and ultrasonically dispersed for 30 min to obtain suspension B.

[0066] Step 3, irradiate suspension A and suspension B with ultraviolet light for 30 min under magnetic stirring, then slowly add suspension A to suspension B. 1.9925 Eu 0.0075The molar ratio of WO6 and Nb2C MXene was 1:1. The obtained mixed suspension was irradiated with UV light for 3 h. The product was washed 3 times with deionized water and then 3 times with anhydrous ethanol, and dried at 70 °C for 12 h to obtain Bi 1.9925 Eu 0.0075 WO6 / Nb2C MXene heterojunction photocatalyst.

[0067] Embodiment 4:

[0068] Step 1: Add 1 mmol of Nb2C MXene powder into 20 ml of ethanol and disperse it by ultrasonic for 30 min to obtain suspension A.

[0069] Step 2: 1mmolBi 1.990 Eu 0.010 WO6 was added to 20 ml of ethanol and ultrasonically dispersed for 30 min to obtain suspension B.

[0070] Step 3, irradiate suspension A and suspension B with ultraviolet light for 30 min under magnetic stirring, then slowly add suspension A to suspension B. 1.990 Eu 0.010 The molar ratio of WO6 and Nb2C MXene was 1:1. The obtained mixed suspension was irradiated with UV light for 3 h. The product was washed 3 times with deionized water and then 3 times with anhydrous ethanol, and dried at 70 °C for 12 h to obtain Bi 1.990 Eu 0.010 WO6 / Nb2C MXene heterojunction photocatalyst.

[0071] Embodiment 5:

[0072] Step 1: Add 1 mmol of Nb2C MXene powder into 20 ml of ethanol and disperse it by ultrasonic for 30 min to obtain suspension A.

[0073] Step 2: 1 mmol Bi 1.995 Eu 0.005 WO6 was added to 20 ml of ethanol and ultrasonically dispersed for 30 min to obtain suspension B.

[0074] Step 3, irradiate suspension A and suspension B with ultraviolet light for 30 min under magnetic stirring, then slowly add suspension A to suspension B. 1.995 Eu 0.005 The molar ratio of WO6 and Nb2C MXene was 1:1. The obtained mixed suspension was irradiated with UV light for 4 h. The product was washed 3 times with deionized water and then 3 times with anhydrous ethanol, and dried at 70 °C for 12 h to obtain Bi 1.995 Eu 0.005WO6 / Nb2C MXene heterojunction photocatalyst.

[0075] Embodiment 6:

[0076] Step 1: Add 1 mmol of Nb2C MXene powder into 20 ml of ethanol and disperse it by ultrasonic for 30 min to obtain suspension A.

[0077] Step 2: 1 mmol Bi 1.995 Eu 0.005 WO6 was added to 20 ml of ethanol and ultrasonically dispersed for 30 min to obtain suspension B.

[0078] Step 3, irradiate suspension A and suspension B with ultraviolet light for 30 min under magnetic stirring, then slowly add suspension A to suspension B. 1.995 Eu 0.005 The molar ratio of WO6 and Nb2C MXene was 1:1. The obtained mixed suspension was irradiated with UV light for 5 h. The product was washed 3 times with deionized water and then 3 times with anhydrous ethanol, and dried at 70 °C for 12 h to obtain Bi 1.995 Eu 0.005 WO6 / Nb2C MXene heterojunction photocatalyst.

[0079] Embodiment 7:

[0080] Step 1: Add 1 mmol of Nb2C MXene powder into 20 ml of ethanol and disperse it by ultrasonic for 30 min to obtain suspension A.

[0081] Step 2: 1 mmol Bi 1.995 Eu 0.005 WO6 was added to 20 ml of ethanol and ultrasonically dispersed for 30 min to obtain suspension B.

[0082] Step 3, irradiate suspension A and suspension B with ultraviolet light for 30 min under magnetic stirring, then slowly add suspension A to suspension B. 1.995 Eu 0.005 The molar ratio of WO6 and Nb2C MXene was 1:1. The obtained mixed suspension was irradiated with UV light for 6 h. The product was washed 3 times with deionized water and then 3 times with anhydrous ethanol, and dried at 70 °C for 12 h to obtain Bi 1.995 Eu 0.005 WO6 / Nb2C MXene heterojunction photocatalyst.

[0083] Embodiment 8:

[0084] Step 1: Add 1 mmol of Nb2C MXene powder into 20 ml of ethanol and disperse it by ultrasonic for 30 min to obtain suspension A.

[0085] Step 2: 1 mmol Bi 1.995 Eu 0.005 WO6 was added to 20 ml of ethanol and ultrasonically dispersed for 30 min to obtain suspension B.

[0086] Step 3, irradiate suspension A and suspension B with ultraviolet light for 30 min under magnetic stirring, then slowly add suspension A to suspension B. 1.995 Eu 0.005 The molar ratio of WO6 and Nb2C MXene was 0.5:1. The obtained mixed suspension was irradiated with UV light for 3 h. The product was washed 3 times with deionized water and then 3 times with anhydrous ethanol, and dried at 70 °C for 12 h to obtain Bi 1.995 Eu 0.005 WO6 / Nb2C MXene heterojunction photocatalyst.

[0087] Embodiment 9:

[0088] Step 1: Add 1 mmol of Nb2C MXene powder into 20 ml of ethanol and disperse it by ultrasonic for 30 min to obtain suspension A.

[0089] Step 2: 1 mmol Bi 1.995 Eu 0.005 WO6 was added to 20 ml of ethanol and ultrasonically dispersed for 30 min to obtain suspension B.

[0090] Step 3, irradiate suspension A and suspension B with ultraviolet light for 30 min under magnetic stirring, then slowly add suspension A to suspension B. 1.995 Eu 0.005 The molar ratio of WO6 and Nb2C MXene was 0.7:1. The obtained mixed suspension was irradiated with UV light for 3 h. The product was washed 3 times with deionized water and then 3 times with anhydrous ethanol, and dried at 70 °C for 12 h to obtain Bi 1.995 Eu 0.005 WO6 / Nb2C MXene heterojunction photocatalyst.

[0091] Embodiment 10:

[0092] Step 1: Add 1 mmol of Nb2C MXene powder into 20 ml of ethanol and disperse it by ultrasonic for 30 min to obtain suspension A.

[0093] Step 2: 1 mmol Bi 1.995 Eu0.005 WO6 was added to 20 ml of ethanol and ultrasonically dispersed for 30 min to obtain suspension B.

[0094] Step 3, irradiate suspension A and suspension B with ultraviolet light for 30 min under magnetic stirring, then slowly add suspension A to suspension B. 1.995 Eu 0.005 The molar ratio of WO6 and Nb2C MXene was 0.8:1. The obtained mixed suspension was irradiated with UV light for 3 h. The product was washed 3 times with deionized water and then 3 times with anhydrous ethanol, and dried at 70 °C for 12 h to obtain Bi 1.995 Eu 0.005 WO6 / Nb2C MXene heterojunction photocatalyst.

[0095] Embodiment 11:

[0096] Step 1: Add 1 mmol of Nb2C MXene powder into 20 ml of ethanol and disperse it by ultrasonic for 30 min to obtain suspension A.

[0097] Step 2: 1 mmol Bi 1.995 Eu 0.005 WO6 was added to 20 ml of ethanol and ultrasonically dispersed for 30 min to obtain suspension B.

[0098] Step 3, irradiate suspension A and suspension B with ultraviolet light for 30 min under magnetic stirring, then slowly add suspension A to suspension B. 1.995 Eu 0.005 The molar ratio of WO6 and Nb2C MXene was 0.9:1. The obtained mixed suspension was irradiated with UV light for 3 h. The product was washed 3 times with deionized water and then 3 times with anhydrous ethanol, and dried at 70 °C for 12 h to obtain Bi 1.995 Eu 0.005 WO6 / Nb2C MXene heterojunction photocatalyst.

[0099] Photothermal catalytic carbon dioxide reduction reaction test:

[0100] 60 mg of the material prepared by the present invention was added to a culture dish, water was added and stirred, and then the culture dish was placed in a vacuum oven and vacuum dried at 65°C. The culture dish was placed in a normal-pressure photothermal catalytic device at 250°C, and an inert gas was continuously passed at a flow rate of 2 mL / min for 10 minutes. Close the inlet and outlet valves, and fill the normal-pressure photothermal catalytic device with 20 mL of carbon dioxide gas and 60 mL of hydrogen. The pressure after inflation was 0.12 MPa, and the reaction was carried out for 3 hours. 1 mL was sampled every hour for gas chromatography analysis to detect the carbon monoxide and methane content. The light source used was a 300W xenon lamp, and the auxiliary heat temperature was 250°C.

[0101] Figure 1 for Bi 2-x Eu x XRD diagram of WO6 / Nb2C MXene heterojunction. For the Nb2C MXene nanosheets in Comparative Example 1, a clear characteristic diffraction peak can be found at 9.8°, which is attributed to the layered stacking structure of Nb2C MXene. 1.995 Eu 0.005 The XRD spectrum of WO6 shows obvious diffraction peaks at 28.4°, 32.8°, 47.2°, 56.0° and 59.6°, corresponding to the (131), (200), (260), (331) and (262) crystal planes of Bi2WO6 (PDFNo.79-2381). In the XRD spectra of Example 1, Example 2, Example 3 and Example 4 compared with Comparative Example 2, it can be observed that the (131) and (260) crystal planes are broadened and shifted by 0.3° and 0.2° respectively, which proves that the Eu element is successfully doped into the Bi2WO6 lattice. In addition, the samples of Comparative Example 2, Example 1 to Example 4 have characteristic peaks of Nb2C MXene and Bi2WO6 at the same time, indicating that Bi 2-x Eu x WO6 / Nb2CMXene photothermal material. In addition, it can be observed that the characteristic peaks at 9.8° in Comparative Example 2 and Examples 1 to 4 weakened after compounding, which is presumably due to Bi2WO6 or Bi 2-x Eu x WO6 grows on the surface of Nb2C MXene, which weakens the diffraction peak.

[0102] Figure 2 This is the SEM image of Nb2C MXene in Comparative Example 1. From the image, we can see a layered structure with uniform thickness and interlayer spacing. Figure 3 In the SEM image of Comparative Example 2Bi2WO6 / Nb2C MXene, it can be seen that flake Bi2WO6 grows on the surface of layered Nb2C MXene. Figure 4 In the SEM image of the heterojunction of Example 2, Bi 1.995 Eu 0.005 WO6 (Eu-Bi2WO6) grows on the surface of Nb2C MXene in the form of nanoflowers. Figure 5 In the TEM of the heterojunction of Example 2, nanoflower balls exist between the Nb2C MXene layers. Figure 6 The interplanar spacing in the HRTEM image of the heterojunction in Example 2 is 0.32 nm, corresponding to the (014) plane of Bi2WO6, and the lattice fringes with an interplanar spacing of 0.28 nm correspond to Nb2C MXene, confirming that the preparation of Bi 2-xEu x WO6 / Nb2C MXene heterojunction.

[0103] Figure 7 , Figure 8 , Fig. 9 They are Comparative Example 1 Nb2C MXene, Comparative Example 2 Bi2WO6 / Nb2C MXene and Example 2 Bi 1.995 Eu 0.005 The electron concentration diagram of WO6 storage is 31.9 μmol·g -1 , 26.8 μmol·g -1 and 42.8 μmol·g -1 . Explanation of the Bi of the present invention 2-x Eu x The electron concentration of the WO6 / Nb2C MXene heterojunction is higher than that of Nb2C MXene and Bi2WO6 / Nb2C MXene. The hole concentration stored in the heterojunction of Example 2 is estimated to be 173 μmol·g by EPR quantum spin number test under dark conditions. -1 ( Fig.10 ).

[0104] from Fig.11 It can be seen that UV light forms Bi 2-x Eu x In the WO6 / Nb2C MXene process, the electrons of Bi2WO6 tend to move from E fWO E flowing to Nb2C MXene crystals fNC ( Fig.11 (a) green and blue dashed lines), causing electrons to accumulate in the Nb2C MXene crystal. This electron flow trend will cause the E fBWO until the Fermi levels of the two are in equilibrium ( Fig.11 The red dashed line E in (b) f(E-BWO-NC) ), Bi 2-x Eu x The work function of WO6 / Nb2CMXene is 4.73eV ( Fig.11 (c)) At the interface where Nb2C MXene and Bi2WO6 contact, Bi2WO6 is positively charged and Nb2C MXene is negatively charged. A built-in electric field is formed at the interface between Nb2C MXene and Bi2WO6, with the direction pointing from Bi2WO6 to the Nb2C MXene interface. At the same time, the conduction band and valence band of Nb2C MXene at the heterojunction interface are bent upward to -0.43 / 0.69 eV, respectively. Therefore, Bi2WO6 is formed by ultraviolet light irradiation. 2-x Eu xWO6 / Nb2C MXene heterojunction.

[0105] Fig.12 The UV-vis-NIR DRS diagrams of the catalysts of Comparative Example 1, Comparative Example 3 and Examples 1 to 4 show that all materials have light absorption in the ultraviolet-visible-near infrared spectrum range of 200 to 2200 nm. Fig.12 The illustration in the figure proves that comparative example 3 has absorption peaks at 762nm and 795nm due to the upconversion effect after Eu doping.

[0106] Fig.13 The photothermal catalytic reduction of CO2 conversion rate of the catalysts in comparative example 3 and examples 1 to 4 is shown in Figure 3. Under simulated sunlight for 3 hours, the catalyst in comparative example 3 enhances light absorption, resulting in the presence of free electrons. After illumination, hot electrons are excited to participate in the reduction reaction of CO2, and the CH4 yield reaches 155.6 μmol·g -1 ·h -1 After UV irradiation and recombination, the CH4 yields of the catalysts of Examples 1 to 4 reached 218.8 μmol·g -1 ·h -1 、304.7μmol·g -1 ·h -1 、183.7μmol·g -1 ·h -1 、157.7μmol·g -1 ·h -1 . This shows that after introducing different proportions of Eu into Bi2WO6, due to Bi 2-x Eu x The WO6 upconversion effect enhances light absorption, generating more electrons to participate in the CO2 reduction reaction, making Bi 2-x Eu x The degree of methanation of CO2 products reduced by WO6 / Nb2C MXene heterojunction is significantly enhanced, and the methane selectivity reaches 100%. For the Nb2C MXene in Comparative Example 1, the photothermal catalytic reduction product of CO2 is only CO, while the selectivity of the CO2 product reduced by the catalyst in Comparative Example 3 to CH4 can reach 100%. Moreover, the selectivity of the CO2 product reduced by the catalysts in Examples 1-4 to CH4 all reaches 100%, and the yield of methane in the CO2 product is significantly enhanced compared with that in Comparative Example 2. This shows that in Bi 2-x Eu x The built-in electric field of the WO6 / Nb2C MXene heterojunction, the LSPR effect of Nb2C MXene, and the upconversion effect of the rare earth element Eu jointly replenish the electrons required in the photothermal reduction of CO2 reaction, thereby improving the photothermal catalytic CO2 reduction activity and selectivity. Fig.14After 6 complete cycles of photothermal catalytic reduction of CO2, the activity of the catalyst in Example 2 was still 296.3 μmol·g -1 ·h -1 , proving that the prepared Bi 2-x Eu x WO6 / Nb2C MXene photothermal material has good cycle stability.

[0107] Fig.15 The graphs of the catalyst surface temperature of Example 2 with time when the internal temperature of the reactor is room temperature and 250°C show that after 15 minutes of simulated sunlight irradiation, the catalyst surface temperature increases to 196°C and 329°C respectively compared with the ambient temperature, indicating that Bi 2-x Eu x WO6 / Nb2C MXene heterojunction has good photothermal conversion performance.

[0108] Fig.16 After being irradiated with light of 740, 800, 940, and 1100 nm wavelengths, the photocatalytic reduction activity of CO2 in Comparative Example 3 was 2.3 μmol·g -1 ·h -1 , 3.2 μmol·g -1 ·h -1 , 3.2 μmol·g -1 ·h -1 , 5.3 μmol·g -1 ·h -1 , the photocatalytic reduction CO2 activity of Example 2 was 5.2 μmol·g -1 ·h -1 , 6.1 μmol·g -1 ·h -1 , 7.3 μmol·g -1 ·h -1 , 1.2 μmol·g -1 ·h -1 Example 2 has the strongest photocatalytic activity in reducing CO2 after irradiation with light at a wavelength of 940 nm. 2-x Eu x The upconversion effect of Eu in WO6 / Nb2C MXene is mainly to convert 940nm to 762nm and 795nm to enhance light absorption, which further proves that the upconversion effect produces more photogenerated electrons and promotes the catalytic conversion of CO2.

[0109] The above is only one embodiment of the present invention, not all or the only embodiment. Any equivalent changes made to the technical solution of the present invention by ordinary technicians in this field after reading the specification of the present invention are covered by the claims of the present invention.

Claims

1. A Bi 2-x Eu x The preparation method of WO6 / Nb2C MXene photothermal material is characterized in that: The steps include: Step 1, dissolving Bi(NO3)3, Eu(NO3)3 and Na2WO4 in ethylene glycol, stirring, and obtaining a reaction precursor solution; subjecting the reaction precursor solution to a hydrothermal reaction to obtain Bi 2-x Eu x WO6; Step 2: Add Nb2C MXene powder to ethanol and disperse it by ultrasonic to obtain suspension A; 2-x Eu x WO6 was added to ethanol and ultrasonically dispersed to obtain suspension B; Step 3, irradiating suspension A and suspension B with ultraviolet light respectively, then slowly adding suspension A into suspension B, irradiating the obtained mixed suspension with ultraviolet light, washing and drying the product, and obtaining Bi 2-x Eu x WO6 / Nb2C MXene photothermal materials.

2. Bi according to claim 1 2-x Eu x The preparation method of WO6 / Nb2C MXene photothermal material is characterized in that: In step 1, the molar ratio of Eu(NO3)3 to Bi(NO3)3 is (0.002-0.010):

1.

3. Bi according to claim 1 2-x Eu x The preparation method of WO6 / Nb2C MXene photothermal material is characterized in that: In step 1, the hydrothermal reaction temperature is 150-180° C. and the time is 9-12 h.

4. Bi according to claim 1 2-x Eu x The preparation method of WO6 / Nb2C MXene photothermal material is characterized in that: In step 2, Bi 2-x Eu x The molar ratio of WO6 and Nb2C MXene is (0.5-1):

1.

5. Bi according to claim 1 2-x Eu x The preparation method of WO6 / Nb2C MXene photothermal material is characterized in that: In step 2, the preparation method of Nb2C MXene powder is: adding Nb2AlC precursor powder to HF solution, and then stirring the obtained mixture solution in a water bath to react. After the reaction is completed, the obtained product is washed and dried to obtain Nb2C MXene.

6. Bi according to claim 1 2-x Eu x The preparation method of WO6 / Nb2C MXene photothermal material is characterized in that: In step 3, the suspension A and the suspension B are respectively irradiated with ultraviolet light for 30-60 minutes.

7. Bi according to claim 1 2-x Eu x The preparation method of WO6 / Nb2C MXene photothermal material is characterized in that: In step 3, the mixed suspension is irradiated with ultraviolet light for 3-6 hours.

8. Bi obtained by the preparation method according to any one of claims 1 to 7 2-x Eu x WO6 / Nb2CMXene photothermal material.

9. Bi according to claim 8 2-x Eu x WO6 / Nb2C MXene photothermal material, characterized in that: The Bi 2- x Eu x Bi in WO6 / Nb2C MXene photothermal materials 2-x Eu x The morphology of WO6 is nano-flower-shaped. 2-x Eu x WO6 is distributed on the surface of Nb2CMXene.

10. Bi according to claim 8 2-x Eu xApplication of WO6 / Nb2C MXene photothermal materials in photothermal catalytic reduction of CO2 to produce methane.

Citation Information

Patent Citations

  • Eu-loaded Bi2WO6 porous microspheres with good dispersion, as well as preparation method and application thereof

    CN103623810A

  • V4C3 MXene-coated BiVO4 photo-thermal catalytic material as well as preparation method and application thereof

    CN116899601A

  • Energy storage Nb2AlC / Nb2C MXene heterojunction photocatalyst as well as preparation method and application thereof

    CN116943696A

  • Method for preparing methanol by reducing CO2 through photo-thermal catalysis and photo-thermal catalyst thereof

    CN118146069A

  • KR20200145819A