Porphyrin-loaded Ir metal Ir-N-C monatomic catalyst as well as preparation method and application thereof
By designing the Ir-N-C single-atom catalyst with porphyrin-supported Ir metal, the problems of high reaction temperature and low yield in indole synthesis are solved, and efficient and green indole derivative preparation is achieved, reducing pollution and production costs are reduced. .
Patent Information
- Application Number
- CN202410907949.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-01
AI Technical Summary
The prior art has problems such as high reaction temperature, low yield and complex catalytic system in the synthesis of indole and its derivatives, and lacks efficient, simple, gentle and sustainable bio-based preparation methods.
A single-atom catalyst of Ir metal supported by porphyrin is designed, by 5,10,15,20-tetrakis(4-methoxyphenyl)-21H,23H-porphyrin, chloroiridium acid and acetone, etc. The components are processed under specific conditions to prepare a highly dispersed Ir metal catalyst for catalyzing the one-step synthesis of indoles and their derivatives such as ethylene glycol and aniline.
It realizes efficient and green indole derivative preparation, reduces the use of precious metals, and the by-products are water and hydrogen, reduces pollution, improves the activity and selectivity of the catalyst, and reduces production costs.
Smart Images

Figure CN118874512A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of bioenergy, and in particular to an Ir-NC single-atom catalyst of porphyrin-loaded Ir metal, and a preparation method and application thereof. Background Art
[0002] With the reduction of petroleum resources and the increase of environmental pollution problems, the use of biomass to replace non-renewable energy sources to provide industrial materials and fine chemicals has attracted widespread attention. In this context, lignocellulosic biomass stands out as a promising renewable carbon source in the chemical industry due to its abundant reserves, eco-friendliness and wide global distribution. Cellulose is the most abundant source of biomass and is currently considered a promising alternative to fossil fuels because it cannot be digested by humans, so its use, unlike corn and starch, does not have a negative impact on food supply. One of the most attractive pathways for cellulose utilization reactions is its direct conversion into useful organic compounds. Lignocellulose mainly consists of cellulose, hemicellulose and lignin, and the conversion of these three biopolymers into value-added chemicals and biofuels is currently the subject of biomass stabilization. Technically, the conversion of the three biopolymers into small organic intermediates, i.e., platform molecules, is a key step in the synthesis of fine chemicals, biofuels and biodegradable materials. The hydrolysis of cellulose to glucose and then its conversion into high-value-added fine chemicals is an effective way to utilize cellulose. Cellulose can be converted into isosorbide, levulinic acid, glycerol, ethylene glycol and 1,2-propylene glycol. Using tungsten-based catalysts under acidic conditions, lignocellulose can be effectively converted into ethylene glycol with a reaction yield of 68.8%. As a downstream product of ethylene glycol, indole has important applications in biological systems and drug research. Some indole derivatives play an important role in the life activities of humans and animals, such as tryptophan, tryptamine, serotonin and melatonin. In addition, indole and its derivatives are encountered in many drugs and agricultural chemical preparations. For example, the natural drug vinpocetine is isolated from Vinca minor, belongs to the indole alkaloids, and is a conventional drug for the treatment of cardiovascular and cerebrovascular diseases.
[0003] In recent years, chemical catalysis has the advantages of simple operation, short reaction time, and high yield. The method has become one of the main methods for obtaining the indole skeleton structure by directional synthesis of indole and indole derivatives. ("A Continuous-Flow Fischer Indole Synthesis of 3-Methylindole in an Ionic Liquid", Jiangang Yu et al., JFlow Chem, 33-36, February 2017) A continuous flow reactor (Corning G1 reactor) was introduced to synthesize 3-methylindole from Fischer indole by the reaction of phenylhydrazine and propionaldehyde. ("Titanium-Catalyzed Multicomponent Couplings: Efficient One-Pot Syntheses of Nitrogen Heterocycles", Odom et al., Acc. Chem. Res, 2822-2833, August 2015) A multi-titanium coupling agent was used to generate indole heterocycles in a one-pot reaction with a yield of up to 42%. (“Study on the one-step synthesis of indole from aniline and ethylene glycol on Cu / SiO2 catalyst”, Sun Junming et al., Molecular Catalysis, 229-233; 2002) studied the catalytic effect of a series of supported Cu catalysts in the one-step synthesis of indole from ethylene glycol and aniline, and optimized the catalyst carrier, loading amount and reaction conditions. In the experiment, the catalyst was prepared by impregnation method, the reaction temperature was 325℃, the conversion rate of ethylene glycol was 100%, and the selectivity of indole was 84%. (“Study on the effect of magnesium oxide additive on the performance of Cu / SiO2 catalyst for one-step synthesis of indole”, Ren Shibin, Journal of Shanxi Normal University (Natural Science Edition), 60-62, 2005) et al. discussed the effect of MgO on the performance of supported catalyst Cu / SiO2 catalytic synthesis of indole. The Cu / SiO2-MgO catalyst was prepared by impregnation method, and the amount of additive MgO was optimized. The results show that when the molar ratio of Mg to Cu is 0.25, the activity and selectivity of the supported catalyst are the highest, and the selectivity of the catalyst is improved after the addition of the additive MgO. ("Straight Access to Indoles from Anilines and Ethylene Glycol by Heterogeneous Acceptorless Dehydrogenative Condensation" Juan, J. Org. Chem., 521-526, 2018) et al. studied the process of synthesizing indole from aniline and ethylene glycol in one step using Pt / Al2O3 as the main catalyst and ZnO as the co-catalyst. The most suitable reaction temperature of this method is 175°C, which is lower than the reaction temperature of the traditional method.The main features of the above research are to load the main catalysts such as copper, platinum, and iridium on carriers such as silica, and then add other co-catalysts to achieve the synthesis of indole. However, there are problems such as high reaction temperature (about 350°C), special reactor (fixed bed or fluidized bed), and low yield. Indole and its derivatives are important organic raw materials and chemical products. The synthesis of indole and its derivatives from aniline and aniline with different substituents and ethylenediamine is the most economical method for synthesizing indole and its derivatives in recent years. The catalytic systems in the existing methods for synthesizing indole and its derivatives are all multi-catalytic systems, and the main catalyst structure is complex. The one-step catalytic synthesis of indole and its derivatives by aniline and ethylene glycol system has attracted much attention because of its low cost of reaction raw materials, few reaction steps, harmless by-products and easy separation (by-products are water and hydrogen). Therefore, it is of great significance to develop a more efficient, simple, mild, sustainable and green bio-based indole preparation method.
[0004] The present invention proposes to design and synthesize a single-atom Ir-NC catalyst for a multi-step coupling reaction process to realize the one-pot directed preparation of indole derivatives from biomass platform compounds, thereby achieving precise construction of CN bonds and achieving the goal of efficient, green and sustainable production of indole derivatives. Summary of the invention
[0005] The technical problem to be solved by the present invention is to provide a porphyrin-loaded Ir metal Ir-NC single-atom catalyst and a preparation method and application thereof in view of the deficiencies of the above-mentioned prior art. Single-atom Ir-NC is used as a catalyst, and the single-atom catalyst has the characteristics of a single active site of a homogeneous catalyst and stability, easy separation and reusability of a heterogeneous catalyst, thereby improving the atomic utilization rate, and providing a new green and efficient way for the directional preparation of indole and its derivatives from ethylene glycol and aniline and its derivatives.
[0006] The invention provides a porphyrin-loaded Ir metal Ir-NC single-atom catalyst. The porphyrin-loaded Ir metal Ir-NC single-atom catalyst uses non-zero-valent noble metal Ir as an active site, the Ir content is 6% of the total weight, and the noble metal Ir is highly dispersed on a carrier.
[0007] The present invention also provides a method for preparing the above-mentioned porphyrin-loaded Ir metal Ir-NC single-atom catalyst, comprising the following steps:
[0008] S1. Add 5,10,15,20-tetrakis(4-methoxyphenyl)-21H,23H-porphyrin, chloroiridic acid and acetone into a pressure-resistant tube to obtain a mixed solution;
[0009] S2, heating the mixed solution prepared in S1 to obtain a suspension, centrifuging the suspension, washing it thoroughly, and then drying it to obtain a solid;
[0010] S3. Put the solid prepared in S2 into a tubular furnace, calcine it under a protective gas atmosphere, and naturally cool it to room temperature to obtain the porphyrin-loaded Ir metal Ir-NC single atom catalyst.
[0011] According to the preparation method of the Ir-NC single-atom catalyst of porphyrin loaded with Ir metal provided by the present invention, the porphyrin described in S1 is 5,10,15,20-tetrakis(4-methoxyphenyl)-21H,23H-porphyrin, the mass and volume ratio of the porphyrin, chloroiridic acid and acetone is 0.0735g:0.65mL:10mL, and the Ir content in the chloroiridic acid is 7.4mg / mL.
[0012] According to the preparation method of porphyrin-loaded Ir metal Ir-NC single-atom catalyst provided by the present invention, the heating in S2 is heating at 60°C for 24 hours, the washing solvent is acetone and deionized water, and the drying is vacuum drying at 60°C for 6 hours.
[0013] According to the preparation method of porphyrin-loaded Ir metal Ir-NC single-atom catalyst provided by the present invention, the protective gas atmosphere in S3 is N2, the flow rate of the protective gas atmosphere is 40 mL / min, the calcination is calcined at 200-400°C for 2h, and the calcination heating rate is 5°C / min.
[0014] The present invention also provides an application of the porphyrin-loaded Ir metal Ir-NC single-atom catalyst. The porphyrin-loaded Ir metal Ir-NC single-atom catalyst can catalyze ethylene glycol and aniline and its derivatives to generate indole and its derivatives in one step.
[0015] Compared with the prior art, the present invention has the following advantages:
[0016] (1) The raw material cellulose of the present invention is a natural renewable aromatic compound resource that is abundant in nature, with a wide range of sources and low cost. Compared with the existing petroleum-based industrial synthesis route for preparing aromatic compounds, the present invention does not consume petroleum resources, has the characteristics of renewable raw materials, and meets the requirements of sustainable development.
[0017] (2) The catalyst of the present invention has the characteristic of highly dispersed active components, which is beneficial to improving the activity and selectivity of the catalyst. At the same time, it can improve the atomic utilization rate of the catalyst, reduce the content of precious metals and thus reduce the cost of the catalyst.
[0018] (3) The present invention provides a new way to convert cellulose into high value-added compounds, reducing the pollution caused by biomass combustion emissions.
[0019] (4) In the one-step reaction of ethylene glycol and aniline and its derivatives to generate indole and its derivatives, the catalyst has the precious metal Ir as the active center, showing high activity and selectivity, and the by-products of the reaction are only water and hydrogen, which does not pollute the environment. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is a high-magnification transmission electron microscope image of the Ir-NC-200 single-atom catalyst prepared in Example 2;
[0021] Figure 2 This is an image of the Ir-NC-200 single atom catalyst prepared in Example 2 under a high-angle annular dark-field scanning transmission electron microscope. DETAILED DESCRIPTION
[0022] Example 1
[0023] This embodiment provides a method for preparing a porphyrin-supported Ir metal Ir-NC single-atom catalyst, and the specific steps are as follows:
[0024] S1. Add 0.0735 g of 5,10,15,20-tetrakis(4-methoxyphenyl)-21H,23H-porphyrin, 0.65 mL of chloroiridic acid and 10 mL of acetone into a 25 mL pressure tube to obtain a dark green solution.
[0025] Among them, the Ir content in chloroiridic acid is 7.4 mg / mL.
[0026] S2. Heat the dark green solution prepared in S1 to 60° C. and react for 24 h to obtain a suspension. Centrifuge the suspension, wash it thoroughly with acetone and deionized water, and then vacuum dry it at 60° C. for 6 h to obtain a dark green solid. After naturally cooling to room temperature, obtain the porphyrin-loaded Ir metal Ir-NC single atom catalyst.
[0027] In this embodiment, the theoretical loading amount of the Ir-NC single-atom catalyst of porphyrin-loaded Ir metal is 6%.
[0028] Example 2
[0029] This embodiment provides a method for preparing a porphyrin-loaded Ir metal Ir-NC-200 single-atom catalyst, and the specific steps are as follows:
[0030] S1. Add 0.0735 g of 5,10,15,20-tetrakis(4-methoxyphenyl)-21H,23H-porphyrin, 0.65 mL of chloroiridic acid and 10 mL of acetone into a 25 mL pressure tube to obtain a dark green solution.
[0031] Among them, the Ir content in chloroiridic acid is 7.4 mg / mL.
[0032] S2, heating the dark green solution prepared in S1 to 60°C and reacting for 24 hours to obtain a suspension, centrifuging the suspension, washing it with acetone and deionized water, and vacuum drying it at 60°C for 6 hours to obtain a dark green solid;
[0033] S3. The dark green solid prepared in S2 is placed in a tubular furnace and calcined at 200°C for 2 h under a N2 protective gas atmosphere at a heating rate of 5°C / min. After naturally cooling to room temperature, the porphyrin-loaded Ir metal Ir-NC-200 single atom catalyst is obtained.
[0034] In this embodiment, the theoretical loading amount of the Ir-NC-200 single-atom catalyst in which porphyrin is loaded with Ir metal is 6%.
[0035] At the same time, according to the above method provided in this embodiment, 0.0390g of chloroplatinic acid, 0.01345g of copper chloride, 0.0238g of cobalt chloride, 0.0130g of nickel chloride, 0.02047g of ruthenium chloride, and 0.0596g of palladium chloride were loaded on 0.0735g of 5,10,15,20-tetrakis(4-methoxyphenyl)-21H,23H-porphyrin, and the temperature was programmed to 200°C and calcined for 2h under nitrogen protection to obtain a series of catalysts such as Pt-NC-200, Cu-NC-200, Co-NC-200, Ni-NC-200, Ru-NC-200, and Pd-NC-200, with a theoretical loading of 6%.
[0036] Example 3
[0037] This embodiment provides a method for preparing a porphyrin-loaded Ir metal Ir-NC-300 single-atom catalyst, and the specific steps are as follows:
[0038] S1. Add 0.0735 g of 5,10,15,20-tetrakis(4-methoxyphenyl)-21H,23H-porphyrin, 0.65 mL of chloroiridic acid and 10 mL of acetone into a 25 mL pressure tube to obtain a dark green solution.
[0039] Among them, the Ir content in chloroiridic acid is 7.4 mg / mL.
[0040] S2, heating the dark green solution prepared in S1 to 60°C and reacting for 24 hours to obtain a suspension, centrifuging the suspension, washing it with acetone and deionized water, and vacuum drying it at 60°C for 6 hours to obtain a dark green solid;
[0041] S3. The dark green solid prepared in S2 is placed in a tubular furnace and calcined at 300°C for 2 h under a N2 protective gas atmosphere at a heating rate of 5°C / min. After naturally cooling to room temperature, the porphyrin-loaded Ir metal Ir-NC-300 single atom catalyst is obtained.
[0042] The theoretical loading amount of the Ir-NC-300 single-atom catalyst of porphyrin-loaded Ir metal in this embodiment is 6%.
[0043] Example 4
[0044] This embodiment provides a method for preparing a porphyrin-loaded Ir metal Ir-NC-400 single-atom catalyst, and the specific steps are as follows:
[0045] S1. Add 0.0735 g of 5,10,15,20-tetrakis(4-methoxyphenyl)-21H,23H-porphyrin, 0.65 mL of chloroiridic acid and 10 mL of acetone into a 25 mL pressure tube to obtain a dark green solution.
[0046] Among them, the Ir content in chloroiridic acid is 7.4 mg / mL.
[0047] S2, heating the dark green solution prepared in S1 to 60°C and reacting for 24 hours to obtain a suspension, centrifuging the suspension, washing it with acetone and deionized water, and vacuum drying it at 60°C for 6 hours to obtain a dark green solid;
[0048] S3. The dark green solid prepared in S2 is placed in a tubular furnace and calcined at 400°C for 2 h under a N2 protective gas atmosphere at a heating rate of 5°C / min. After naturally cooling to room temperature, the porphyrin-loaded Ir metal Ir-NC-400 single atom catalyst is obtained.
[0049] The theoretical loading amount of the Ir-NC-400 single-atom catalyst of porphyrin-loaded Ir metal in this embodiment is 6%.
[0050] Example 5
[0051] This embodiment provides a method for preparing a porphyrin-supported Ir metal Ir-NC single-atom catalyst, and the specific steps are as follows:
[0052] S1. Add 0.0181 g of 1,10-phenanthroline, 0.155 mL of chloroiridic acid and 10 mL of acetone into a 25 mL pressure tube to obtain an orange-yellow solution.
[0053] Among them, the Ir content in chloroiridic acid is 7.4 mg / mL.
[0054] S2, heating the orange-yellow solution prepared in S1 to 60° C. and reacting for 24 hours to obtain a suspension, centrifuging the suspension, and washing it thoroughly with acetone and deionized water until the ligand 1,10-phenanthroline on the catalyst surface is washed away, and then vacuum drying it at 60° C. for 6 hours to obtain an orange-red solid;
[0055] S3. The orange-red solid prepared in S2 is placed in a tubular furnace and calcined at 200°C for 2 h under a N2 protective gas atmosphere at a heating rate of 5°C / min. After naturally cooling to room temperature, a porphyrin-loaded Ir metal Ir-NC single-atom catalyst is obtained.
[0056] In this embodiment, the theoretical loading amount of the Ir-NC single-atom catalyst of porphyrin-loaded Ir metal is 6%.
[0057] Example 6
[0058] This embodiment provides a method for preparing a porphyrin-supported Ir metal Ir-NC single-atom catalyst, and the specific steps are as follows:
[0059] S1. Add 0.0283 g of DPPZ, 0.245 mL of chloroiridic acid and 10 mL of acetone into a 25 mL pressure tube to obtain a gray mixed solution;
[0060] Among them, the Ir content in chloroiridic acid is 7.4 mg / mL.
[0061] S2, heating the gray mixed solution prepared in S1 to 60° C. and reacting for 24 hours to obtain a suspension, centrifuging the suspension, washing it thoroughly with acetone and deionized water until the ligand DPPZ on the catalyst surface is washed away, and then vacuum drying it at 60° C. for 6 hours to obtain a gray-brown solid;
[0062] S3. The gray-brown solid prepared in S2 is placed in a tubular furnace and calcined at 200° C. for 2 h under a N2 protective gas atmosphere at a heating rate of 5° C. / min. After naturally cooling to room temperature, a porphyrin-loaded Ir metal Ir-NC single-atom catalyst is obtained.
[0063] In this embodiment, the theoretical loading amount of the Ir-NC single-atom catalyst of porphyrin-loaded Ir metal is 6%.
[0064] Example 7
[0065] This embodiment provides a method for preparing a porphyrin-supported Ir metal Ir-AC single-atom catalyst, and the specific steps are as follows:
[0066] 1 g of activated carbon and 4.18 mL of chloroiridic acid were added to a 5 mL beaker, stirred overnight and then vacuum dried at 60 ° C for 6 h. Then, the mixture was placed in a tubular furnace and calcined at 450 ° C for 3 h under N2 atmosphere at a heating rate of 5 ° C / min to obtain porphyrin-loaded Ir metal Ir-AC single atom catalyst.
[0067] Among them, the Ir content in chloroiridic acid is 7.4 mg / mL.
[0068] In this embodiment, the theoretical loading amount of the Ir-AC single-atom catalyst of porphyrin-loaded Ir metal is 6%.
[0069] Example 8
[0070] This embodiment provides a method for preparing a porphyrin-supported Ir metal Ir-NC single-atom catalyst, and the specific steps are as follows:
[0071] S1. Add 1.486 g of 1,10-phenanthroline, 1.624 mL of chloroiridic acid and 50 mL of ethanol into a 250 mL round-bottom flask, and after ultrasonic dispersion for 20 min, add 3.2 g of magnesium oxide and continue ultrasonication for 20 min, and reflux at 60 ° C overnight to obtain a yellow solution;
[0072] Among them, the Ir content in chloroiridic acid is 7.4 mg / mL.
[0073] S2. Remove excess ethanol from the yellow solution prepared in S1 to obtain a yellow solid, place the yellow solid in a tubular furnace, raise the temperature at a rate of 2°C / min, and calcine at 400°C for 2h under a N2 protective gas atmosphere to obtain a black powder solid, then add it to 200mL of a 0.5mol / L sulfuric acid solution, reflux overnight at 80°C for acid washing to remove magnesium oxide, centrifuge, wash with deionized water until neutral, and vacuum dry at 60°C for 4h to obtain an Ir-NC catalyst with a theoretical loading of 6%.
[0074] In this embodiment, the theoretical loading amount of the Ir-NC single-atom catalyst of porphyrin-loaded Ir metal is 6%.
[0075] Examples 9 to 18
[0076] In order to evaluate the catalytic performance of the porphyrin-loaded Ir metal Ir-NC-200 single atom catalyst prepared in Example 2, the catalyst was tested for its activity in the synthesis of 5-methylindole from ethylene glycol and p-toluidine using a microreactor evaluation device.
[0077] The test conditions are as follows: using a high temperature and high pressure reactor, 107.2 mg of p-toluidine and 3.4 mL of ethylene glycol are dissolved in p-xylene, and the amount of catalyst used is 10 mg.
[0078] The reactor was sealed and programmed to heat to 150-190°C, and the reaction was stirred at 600 rad / min for 12-24 h. After the reaction was completed, it was cooled to room temperature and the volume was made up to 50 mL with N,N-dimethylformamide. The supernatant was filtered and sampled for analysis.
[0079] The qualitative analysis of the product was achieved by GC-MS coupling technology and standard sample comparison, and the quantitative analysis was achieved by liquid chromatography external standard method. The reaction results are shown in Table 1.
[0080] Table 1 Synthesis of 5-methylindole from ethylene glycol and p-toluidine catalyzed by single atom catalyst Ir-NC under different conditions
[0081]
[0082] As can be seen from Table 1, under different conditions, the catalytic activity and selectivity of the porphyrin-loaded Ir metal Ir-NC-200 single atom catalyst are different. When the reaction temperature is 190°C, the reaction time is 24h, and the solvent is p-xylene, the catalyst shows a very high activity of 97.5% and a selectivity of 97.0%.
[0083] Examples 19 to 33
[0084] 107.2 mg of p-toluidine and 3.4 mL of ethylene glycol were dissolved in p-xylene, and 10 mg of the catalyst prepared in Examples 1 to 8 were added respectively.
[0085] The reactor was sealed and programmed to heat to 150-190°C, and the reaction was stirred at 600 rad / min for 12-24 h. After the reaction was completed, it was cooled to room temperature and the volume was made up to 50 mL with N,N-dimethylformamide. The supernatant was filtered and sampled for analysis.
[0086] The qualitative analysis of the product was carried out by GC-MS coupling technology and standard sample comparison, and the quantitative analysis was achieved by liquid chromatography external standard method. The reaction results are shown in Table 2.
[0087] Table 2 Synthesis of 5-methylindole from ethylene glycol and p-toluidine catalyzed by single-atom catalysts on different supports
[0088]
[0089]
[0090] The subscript [a] indicates the Ir-NC catalyst prepared by the method shown in Example 1, the subscript [b] indicates the Ir-NC catalyst prepared by the method shown in Example 5, and the subscript [c] indicates the Ir-NC catalyst prepared by the method shown in Example 8.
[0091] As can be seen from Table 2, compared with the individual ligands porphyrin and chloroiridic acid, the catalyst loaded with metal Ir can greatly improve the reaction activity and selectivity.
[0092] Under the same conditions, the Ir-doped catalyst showed a conversion rate of 97.5% and a 5-methylindole yield of 97.0%, which was more active than other metal-doped catalysts. Although other metal-doped catalysts also had a conversion rate of more than 70%, their selectivity for 5-methylindole was very low, indicating that the Ir-NC catalyst is specific for indole synthesis.
[0093] In addition, the catalytic activity of Ir-NC at different calcination temperatures was compared. The results showed that a calcination temperature of 200°C was more effective. As the calcination temperature increased, the yield of 5-methylindole decreased.
[0094] GC-MS confirmed the presence of by-products such as 1,2-di-p-tolylethane, 2,2'-(p-toluenepropylazanediyl)bis(ethyl-1-ol), 2-(5-methyl-1H-indol-3-yl)ethane-1-ol, and 1-methyl-4-vinylbenzene in the reaction products.
[0095] The above is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent change made to the above embodiment according to the technical essence of the invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A porphyrin-supported Ir metal Ir-NC single-atom catalyst, characterized in that: The porphyrin-loaded Ir metal Ir-NC single-atom catalyst uses non-zero-valent noble metal Ir as an active site, the Ir content in the porphyrin-loaded Ir metal Ir-NC single-atom catalyst is 6% of the total weight, and the noble metal Ir in the porphyrin-loaded Ir metal Ir-NC single-atom catalyst is highly dispersed on the carrier.
2. A method for preparing the porphyrin-supported Ir metal Ir-NC single-atom catalyst as claimed in claim 1, characterized in that: The following steps are involved: S1, adding porphyrin, chloroiridic acid and acetone into a pressure-resistant tube to obtain a mixed solution; S2, heating the mixed solution prepared in S1 to obtain a suspension, centrifuging the suspension, washing it thoroughly, and then drying it to obtain a solid; S3. Put the solid prepared in S2 into a tubular furnace, calcine it under a protective gas atmosphere, and naturally cool it to room temperature to obtain the porphyrin-loaded Ir metal Ir-NC single atom catalyst.
3. The method for preparing the porphyrin-supported Ir metal Ir-NC single-atom catalyst according to claim 2, characterized in that: The porphyrin described in S1 is 5,10,15,20-tetrakis(4-methoxyphenyl)-21H,23H-porphyrin, and the mass-volume ratio of the porphyrin, chloroiridic acid and acetone is 0.0735 g:0.65 mL:10 mL. The Ir content in the chloroiridic acid is 7.4 mg / mL.
4. The method for preparing the porphyrin-supported Ir metal Ir-NC single-atom catalyst according to claim 2, characterized in that: The heating in S2 is heating at 60° C. for 24 h, the washing solvents are acetone and deionized water, and the drying is vacuum drying at 60° C. for 6 h.
5. The method for preparing the porphyrin-supported Ir metal Ir-NC single-atom catalyst according to claim 2, characterized in that: The protective gas atmosphere in S3 is N2, the flow rate of the protective gas atmosphere is 40 mL / min, the calcination is performed at 200-400°C for 2h, and the heating rate of the calcination is 5°C / min.
6. An application of the porphyrin-supported Ir metal Ir-NC single-atom catalyst according to any one of claims 1 to 5, characterized in that: The porphyrin-loaded Ir metal Ir-NC single-atom catalyst can catalyze ethylene glycol and aniline and its derivatives to generate indole and its derivatives in one step.