SSZ-39 zeolite supported catalyst as well as preparation method and application thereof
Through etching treatment and addition of metal oxides, the modified SSZ-39 zeolite-supported catalyst solved the problem of the reduction in the activity of In/H-Beta catalyst in the presence of high-temperature water vapor and SO2 and H2O, which significantly improved the NOx conversion rate and stability , achieving more efficient NOx removal effect.
Patent Information
- Application Number
- CN202410951842.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-16
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-16
AI Technical Summary
The existing In/H-Beta catalysts are sensitive to high-temperature water vapor in the CH4-SCR reaction, resulting in reduced activity or inactivation, and are insufficient in the presence of SO2 and H2O, making it difficult to effectively remove NOx.
Using SSZ-39 zeolite-supported catalyst, the addition of In and metal oxides (such as Co3O4) after etching treatment by etching agents to improve the denitrification activity and water resistance and SO2 resistance of the catalyst. The preparation method includes etching SSZ-39 zeolite and etching. The agent is reacted, dried, calcined, and In and metal oxides are added to form a modified catalyst.
The NOx conversion and stability of the catalyst in CH4-SCR reaction was significantly improved. Especially under the conditions containing SO2 and H2O, the NOx conversion increased by 33%, and good catalytic activity and selectivity were maintained.
Smart Images

Figure CN118874530A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of catalyst preparation and environmental pollution control, and in particular to an SSZ-39 zeolite-supported catalyst and a preparation method and application thereof. Background Art
[0002] Nitrogen oxides (NO x ) is mainly derived from industrial production and is considered a major air pollutant. x It is a toxic and harmful gas. Under certain conditions, it can combine with hydrocarbons to produce photochemical smog and other pollution, irritate the eyes, form acid rain to damage plants, reduce atmospheric visibility, and react with ozone in the air to cause ozone layer holes, deteriorating the environment on which humans depend for survival. x Emissions, reducing NO in the ambient atmosphere x Concentration has become an important target for environmental pollution control in my country.
[0003] Selective Catalytic Reduction of NO x SCR technology refers to the addition of additional reducing agents to reduce NO x The process of reducing and converting into N2. CH4-SCR is a very promising and effective NO removal x The technology has attracted close attention from scholars at home and abroad in recent years. x However, the hydrothermal stability (water resistance) of In / H-Beta catalysts needs to be improved, and the influence of high-temperature water vapor causes the catalyst activity to decrease or even lose its activity. In order to solve the problem of catalyst deactivation when encountering high-temperature water vapor in the CH4-SCR reaction, seeking a zeolite carrier with good hydrothermal stability is an effective way to solve H2O poisoning. Summary of the invention
[0004] In view of the above technical problems, the present invention discloses a SSZ-39 zeolite-supported catalyst and a preparation method and application thereof. The obtained catalyst has better denitrification activity for CH4-SCR and good resistance to H2O and SO2.
[0005] To this end, the technical solution adopted by the present invention is:
[0006] A method for preparing a SSZ-39 zeolite-supported catalyst comprises the following steps:
[0007] Step S1, dispersing SSZ-39 zeolite in water, adding an etchant to obtain a mixture, wherein the etchant is oxalic acid or citric acid, and the concentration of the etchant is 0.1-2.0 mol / L; reacting the mixture at a temperature of 70-85° C. for a reaction time of 2-10 h;
[0008] Step S2, after the reaction is completed, filtering and washing, drying the filter cake, grinding and calcining, the calcination temperature is 480-550°C, and the calcination time is more than 2 hours to obtain H-SSZ-39;
[0009] Step S3, dissolving In(NO3)3·xH2O in water, adding the H-SSZ-39 zeolite obtained in step S2, stirring at a constant temperature of 80-90°C for more than 6 hours, centrifuging, washing and drying, and then calcining at a calcination temperature of 480-550°C for at least 2 hours to obtain an In / H-SSZ-39 catalyst.
[0010] By adopting this technical solution, the denitrification activity of the SSZ-39 zeolite-supported In catalyst is significantly improved after being etched by the etchant.
[0011] As a further improvement of the present invention, in step S2, the calcination time is 3 hours or more.
[0012] As a further improvement of the present invention, in step S3, In(NO3)3·xH2O is dissolved in water, and the H-SSZ-39 zeolite obtained in step S2 is added, and the mixture is stirred at a constant temperature of 85°C for 8 hours.
[0013] As a further improvement of the present invention, in step S3, the calcination time is 3 hours or more.
[0014] As a further improvement of the present invention, the method for preparing the SSZ-39 zeolite-loaded catalyst further includes: in step S3, in addition to adding the H-SSZ-39 zeolite obtained in step S2, a metal oxide is also added, and the metal oxide is Co3O4, NiO or CeO2.
[0015] By adopting this technical solution, In / H-SSZ-39 is combined with metal oxides Co3O4, NiO or CeO2, which further improves the denitrification activity of the catalyst and improves the stability of the catalyst under conditions containing H2O and SO2.
[0016] As a further improvement of the present invention, the mass ratio of the metal oxide to the H-SSZ-39 zeolite is 1:20-50.
[0017] As a further improvement of the present invention, the metal oxide is Co3O4. This technical solution has better catalytic activity.
[0018] As a further improvement of the present invention, the mass ratio of the metal oxide to the H-SSZ-39 zeolite is 1:30-50.
[0019] As a further improvement of the present invention, in the mixture of step S1, the concentration of the etchant is 0.5-1.0 mol / L.
[0020] As a further improvement of the present invention, the solid-liquid ratio of the zeolite to the etchant aqueous solution is 1 g:15-30 mL. Furthermore, the solid-liquid ratio of the zeolite to the etchant aqueous solution is 1 g:20 mL.
[0021] As a further improvement of the present invention, the etchant is OA. By adopting this technical solution, the obtained catalyst has better catalytic activity.
[0022] As a further improvement of the present invention, in step S1, the mixture is reacted at a temperature of 75-80°C.
[0023] As a further improvement of the present invention, in step S2 and step S3, the heating rate of calcination is 3-6°C / min.
[0024] The present invention also discloses a SSZ-39 zeolite-supported catalyst, which is prepared by using any one of the above methods for preparing the SSZ-39 zeolite-supported catalyst.
[0025] The present invention also discloses the use of the SSZ-39 zeolite supported catalyst as described above, which is used for CH4-SCR denitration reaction. Further, it is used for CH4-SCR denitration under the condition of containing SO2 and H2O.
[0026] As a further improvement of the present invention, the conditions of the CH4-SCR denitrification reaction are: CH4 concentration 400-600ppm, CH4 concentration to NO concentration ratio of 1.5-2.0, O2 concentration 5-10vol%, SO2 concentration 0-50ppm, H2O concentration 5-10vol%, space velocity 11800-23600h -1 .
[0027] As a further improvement of the present invention, the conditions of the denitrification environment containing SO2 and H2O are: NO concentration 400ppm, CH4 concentration 600ppm, O2 concentration 10vol%, SO2 concentration 50ppm, H2O concentration 5vol%, space velocity 11800h -1 .
[0028] Compared with the prior art, the present invention has the following beneficial effects:
[0029] The technical solution of the present invention adopts acid-etched H-SSZ-39, and the obtained modified In / H-SSZ-39 zeolite catalyst has better denitrification activity for CH4-SCR. For example, the In / H-SSZ-39 (OA) catalyst modified by oxalic acid etching has better denitrification activity for NO under the condition of no SO2 and no H2O.x The highest conversion rate is 62.6%, which is 47.6% higher than that of the unmodified sample. Furthermore, the catalyst In-Co3O4 / H-SSZ-39(OA) modified by Co3O4 can convert NO x The conversion rate can reach up to 83.1%, which is 33% higher than that of the unmodified catalyst, and the stability is good. After acid etching and metal oxide modification, there are certain mesopores in the catalyst, the acidity and redox properties of medium-strong acids are enhanced, the proportion of surface adsorbed oxygen increases, and In-Co3O4 / H-SSZ-39(OA) can retain more stable N than In / H-SSZ-39(OA). x O y species for further reaction. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 The results of the comparison of CH4-SCR denitrification activity after modification with different etchants in the embodiments of the present invention are shown in FIG. 1 , where (a) is NO x (b) is the CH4 conversion rate, and (c) is the CH4 selectivity.
[0031] Figure 2 The results of the comparison of CH4-SCR denitrification activity after modification with different OA concentrations in Example 2 of the present invention are shown in FIG. 1 , where (a) is NO x (b) is the CH4 conversion rate, and (c) is the CH4 selectivity.
[0032] Figure 3 is the comparison result of CH4-SCR denitrification activity after modification with different CA concentrations in Example 4 of the present invention, where (a) is NO x (b) is the CH4 conversion rate, and (c) is the CH4 selectivity.
[0033] Figure 4 The results of the comparison of CH4-SCR denitrification activity after different etching times in Example 5 of the present invention are shown in FIG. 1 , where (a) is NO x (b) is the CH4 conversion rate, and (c) is the CH4 selectivity.
[0034] Figure 5 The results of the comparison of CH4-SCR denitrification activity after modification at different etching temperatures in Example 6 of the present invention are shown in FIG. 1 , where (a) is NO x (b) is the CH4 conversion rate, and (c) is the CH4 selectivity.
[0035] Figure 6 is the comparison result of CH4-SCR denitrification activity after modification with different solid-liquid ratios in Example 7 of the present invention, wherein (a) is NO x(b) is the CH4 conversion rate, and (c) is the CH4 selectivity.
[0036] Figure 7 The comparison results of CH4-SCR catalytic activity of the modified catalyst of Example 8 of the present invention at different water contents are shown in FIG. 1 , wherein (a) is NO x (b) is the CH4 conversion rate, and (c) is the CH4 selectivity.
[0037] Figure 8 In-MO modified by different metal oxides of the present invention x / H-SSZ-39 catalyst CH4-SCR denitrification activity results, where (a) is NO x (b) is the CH4 conversion rate, and (c) is the CH4 selectivity.
[0038] Fig. 9 The results of the effect of the amount of Co3O4 modification on the denitration performance of In-Co3O4 / H-SSZ-39(OA) in Example 11 of the present invention are shown in FIG. 11, wherein (a) is NO x (b) is the CH4 conversion rate, and (c) is the CH4 selectivity.
[0039] Fig.10 The results of the effect of O2 concentration on the denitration performance of In-Co3O4 / H-SSZ-39(OA) in Example 12 of the present invention are shown in FIG. 1, wherein (a) is NO x (b) is the CH4 conversion rate, and (c) is the CH4 selectivity.
[0040] Fig.11 The results of the effect of CH4 / NO on the denitration performance of In-Co3O4 / H-SSZ-39(OA) in Example 13 of the present invention, where (a) is NO x (b) is the CH4 conversion rate, and (c) is the CH4 selectivity.
[0041] Fig.12 The results of the effect of the space velocity on the denitration performance of In-Co3O4 / H-SSZ-39(OA) in Example 14 of the present invention are shown in FIG. 14, wherein (a) is NO x (b) is the CH4 conversion rate, and (c) is the CH4 selectivity.
[0042] Fig.13 The results of the effect of water vapor concentration on the denitration performance of In-Co3O4 / H-SSZ-39(OA) in Example 15 of the present invention are shown in FIG. 15 , where (a) is NO x (b) is the CH4 conversion rate, and (c) is the CH4 selectivity.
[0043] Fig.14 The results of the effect of SO2 concentration on the denitration performance of In-Co3O4 / H-SSZ-39(OA) in Example 16 of the present invention are shown in FIG. 16, where (a) is NO x (b) is the CH4 conversion rate, and (c) is the CH4 selectivity.
[0044] Fig.15 These are the experimental results of the H2O and SO2 resistance of In-Co3O4 / H-SSZ-39 (OA) in Example 17 of the present invention.
[0045] Fig.16 These are the experimental results of the stability of In-Co3O4 / H-SSZ-39 (OA) against H2O and SO2 of Example 18 of the present invention. DETAILED DESCRIPTION
[0046] The preferred embodiments of the present invention are described in further detail below.
[0047] Example 1
[0048] A method for preparing a SSZ-39 zeolite-supported catalyst comprises the following steps:
[0049] Step S1, 1 g of commercial H-SSZ-39 zeolite is ultrasonically dispersed in 20 mL of ultrapure water, and an etchant oxalic acid (OA) with a concentration of 0.1 mol / L (i.e., 0.1 M) is added thereto, the reaction temperature is selected to be 80°C, and the reaction time is 4-10 h from short to long.
[0050] Step S2, after the etching is completed, suction filtration is performed, and the mixture is washed with ultrapure water for multiple times until the pH is neutral (non-framework aluminum and residual etchant are washed away). The filter cake is taken out, placed in an oven with the oven temperature set at 80°C and dried for more than 12 hours, and after drying, the etched modified zeolite is ground and placed in a muffle furnace, gradually heated from room temperature to 500°C, with a heating rate of 5°C / min, and calcined for 3 hours to produce H-SSZ-39 (OA) zeolite.
[0051] Step S3, active metal In is introduced into zeolite by ion exchange method, the specific steps are: firstly, In(NO3)3·xH2O Prepare an aqueous solution of indium nitrate with ultrapure water to a concentration of 0.066M, take 1g of H-SSZ-39 (OA) zeolite and ultrasonically disperse it into 33.33mL In(NO3)3 aqueous solution was stirred at 85℃ for 8h. After ion exchange, the In-exchanged sample was collected by high-speed centrifugation, dried at 80℃ overnight, and then placed in a muffle furnace and gradually raised from room temperature to 500℃ at 5℃ / min and calcined for 3h to obtain In / H-SSZ-39(OA) catalyst.
[0052] By adopting this technical solution, the denitrification activity of the SSZ-39 zeolite-supported In catalyst is significantly improved after being etched by the etchant.
[0053] Example 2
[0054] Based on Example 1, the difference of this example is that citric acid (CA) is used as the etchant, and the rest is the same as Example 1.
[0055] Comparative Example 1
[0056] Based on Example 1, the difference of this comparative example is that EDTA is used as the etchant, and the other steps are the same as Example 1.
[0057] Comparative Example 2
[0058] This comparative example is a blank sample, that is, based on Example 1, this comparative example is different in that no etching is performed.
[0059] The In / H-SSZ-39 catalysts obtained in Example 1, Example 2, Comparative Example 1, and Comparative Example 2 were subjected to a denitration experiment in the absence of SO2 and H2O. The experimental conditions were [NO] = 400 ppm, [CH4] = 600 ppm, [O2] = 10 vol%, and a space velocity of 23600 h -1 The results are as follows Figure 1 As shown in the figure, it can be seen that the denitration efficiency of the In / H-SSZ-39 catalyst that has not been etched and modified in CH4-SCR does not reach 15%. Figure 1 As shown in (a), the denitrification performance of In / H-SSZ-39 zeolite catalyst after being etched by different types of etchants is significantly improved. x The removal effect is the best, and ~40% of NO can be achieved at 550°C x Conversion rate: After CA etching modification, its denitrification activity is slightly worse than that of OA at 550℃, with ~35% NO x Conversion rate: After EDTA etching modification, the In / H-SSZ-39 catalyst has the worst activity at the same temperature, with only ~30% of NO x Conversion rate.
[0060] like Figure 1 As shown in (b), the overall trends of CH4 conversion rates of In / H-SSZ-39 catalysts modified by OA, CA, EDTA and unetched are consistent and have good overlap. At 650℃, the CH4 conversion rates of In / H-SSZ-39 catalysts modified by three etchants are OA, CA, and EDTA from high to low. Figure 1 It can be seen from (c) that at 500°C, the CH4 selectivity of the catalyst that has not been modified with an etchant is as low as 32%; however, after being modified with an etchant, the CH4 selectivity is improved, and the CH4 selectivity of the catalysts modified with OA and CA is significantly improved.
[0061] Example 3
[0062] Based on Example 1, the difference of this example is that the concentration of the etchant OA is 0.5M, 1.0M, 1.5M, and 2.0M, the etching time is 4h, the etching temperature is 80°C, the solid-liquid ratio of zeolite to the etchant aqueous solution is 1g:20mL, and the reaction gas conditions of the denitrification experiment remain unchanged.
[0063] Example 4
[0064] Based on Example 2, the difference of this example is that the concentration of the etchant CA is 0.5M, 1.0M, 1.5M, and 2.0M, the etching time is 4h, the etching temperature is 80°C, the solid-liquid ratio of zeolite to the etchant aqueous solution is 1g:20mL, and the reaction gas conditions of the denitrification experiment remain unchanged.
[0065] The catalyst performances obtained in Examples 3 and 4 are as follows: Figure 2 As shown, Figure 2 (a) It can be seen that the In / H-SSZ-39 catalyst modified by 1.0M OA etching has the best activity in CH4-SCR, which can reach ~60% NO at 550℃. x conversion rate; when the concentration is 0.5M, the denitrification activity decreases slightly after etching modification (about 50%), which may be due to the low OA concentration and the insignificant zeolite effect; when the OA concentration is increased to 1.5M or 2.0M, it can be seen that the activity of In / H-SSZ-39 catalyst further decreases, and its denitrification activity drops below 50%.
[0066] Figure 2 (b) is the CH4 conversion rate curve of In / H-SSZ-39 in CH4-SCR reaction after etching with different concentrations of OA. The overall trend of CH4 conversion rate under the four concentrations is consistent, and the CH4 conversion rate increases with the increase of temperature. Since the catalyst modified by 1.0M OA etching has the best denitrification effect, its CH4 conversion rate is higher than that of the catalyst etched with other concentrations at the same temperature. The CH4 conversion rate reaches more than 80% at 650℃. The CH4 conversion rate after etching with other concentrations is slightly lower than that of 1.0M, but it also increases with the increase of activity. Figure 2 (c) is a bar graph of the CH4 selectivity of the catalysts after etching modification with different OA concentrations. The CH4 selectivity of the four concentrations decreases with increasing temperature, and the overall trend is consistent. The In / H-SSZ-39 catalyst modified with 1.0M OA has a maximum CH4 selectivity of 48% at 500°C. The In / H-SSZ-39 catalyst modified with 0.5M, 1.5M, and 2.0M OA has a CH4 selectivity slightly lower than 1.0M at 500°C, but is close to 45%.
[0067] Furthermore, in order to compare the CH4-SCR catalytic activity under the optimal etching conditions of OA and CA, the activity of In / H-SSZ-39 modified by etching with different CA concentrations (0.5M, 1.0M, 1.5M, 2.0M) was tested, and other etching conditions remained unchanged. The test results are shown in Figure 2. Figure 3 shown.
[0068] Figure 3 (a) The denitrification activity of In / H-SSZ-39 catalysts modified by CA etching at 0.5M, 1.0M, 1.5M, and 2.0M in CH4-SCR. The best denitrification effect was achieved after 1.0M CA etching, which could reach 55% denitrification activity at 550℃. However, the denitrification activity of In / H-SSZ-39 catalyst modified by OA at the same concentration could reach 60%. Therefore, the denitrification effect of In / H-SSZ-39 catalyst modified by OA was better than that of In / H-SSZ-39 catalyst modified by CA. When the CA concentration was reduced to 0.5M, NO x The conversion rate slightly decreased to 50%, which was caused by the decrease in etchant concentration. When the CA concentration was increased to 1.5M and 2.0M, it was found that the denitrification activity after CA etching modification was significantly reduced compared with that of 1.0M CA, which was consistent with the NO conversion of In / H-SSZ-39 catalyst after OA etching modification at different concentrations. x The trend of conversion rate change is consistent, which may be due to the excessively high concentration of the etchant, which leads to the amorphization of zeolite, a small specific surface area, and the active species InO + Due to the reduction of load.
[0069] Figure 3 (b) is the CH4 conversion rate curve of the catalyst after etching with CA at different concentrations. It can be seen that the CH4 conversion rate trend of the catalyst after etching with CA at several concentrations is consistent with the CH4 conversion rate after etching with OA. When the reaction temperature is 650°C, its CH4 conversion rate can reach 80%, which is about 5% lower than that of OA. At the same time, by comparing the CH4 conversion rates of the catalyst after etching with CA at different concentrations, it is found that its CH4 conversion rate is slightly lower than that of the catalyst after etching with OA. Figure 3 (c) is the CH4 selectivity curve of the catalysts modified by etching with CA at different concentrations. At 500℃, the CH4 selectivity of the catalyst modified by etching with 1.0M CA did not reach 45%, while the CH4 conversion rate of the catalyst modified by etching with 1.0M OA could reach more than 45% at 500℃. At other concentrations and temperatures, the CH4 selectivity of the catalyst modified by etching with OA was also higher than that of the catalyst modified by etching with CA. xThe results of conversion rate, CH4 conversion rate and CH4 selectivity indicate that the denitrification activity of the catalyst after OA etching modification is better than that after CA etching modification.
[0070] Example 5
[0071] On the basis of Example 1, the etchant OA was used, the etchant OA concentration was 1M, the solid-liquid ratio was 1g:20mL, the etching reaction temperature was 80°C, the etching time was changed, and the etching modification time was 2h, 4h, 6h, 8h, and 10h; the obtained catalyst denitrification reaction conditions were: [NO] = 400ppm, [CH4] = 600ppm, [O2] = 10vol%, and the others were the same as Example 1.
[0072] The denitrification activity of In / H-SSZ-39 catalysts with etching modification time of 2h, 4h, 6h, 8h and 10h is shown in Figure 4 shown.
[0073] Figure 4 (a) NO of In / H-SSZ-39 catalyst modified by different OA etching times x The conversion rate curve shows that when the etching time is 4 h, the catalyst has 60.8% NO at 550 °C. x The conversion rate decreased, while the denitrification activity dropped below 50% when the etching time was 2h, 6h, 8h, and 10h. According to literature reports, this may be due to the change in etching time, which led to a decrease in the pore volume of zeolite.
[0074] Figure 4 (b) is the CH4 conversion rate curve of the In / H-SSZ-39 catalyst after modification with different OA etching times. The trends of the CH4 conversion rate curves of the catalysts after these etching modification times are almost the same, and the CH4 conversion rate increases with increasing temperature. Among them, the CH4 conversion rate of the In / H-SSZ-39 catalyst modified by etching for 4h can reach as high as 90% at 650℃; and when the etching time is 2h, 6h, 8h, and 10h, its CH4 conversion rate is about 80%. Figure 4 (c) is a bar chart of the CH4 selectivity of the catalyst after modification with different OA etching times. When the etching time is 4h, the CH4 selectivity of the catalyst can reach 45% at 500℃; when the etching time is 2h and 6h, the CH4 selectivity of the catalyst is slightly lower, at 40%; when the etching time is increased to 8h and 10h, the CH4 selectivity of the catalyst drops to 35% and 30%.
[0075] By comparing the different OA etching modification time NO x The results of conversion rate, CH4 conversion rate and CH4 selectivity show that the denitrification effect is the best after 4h etching modification, and the CH4 selectivity is the highest.
[0076] Example 6
[0077] On the basis of Example 1, in this example, firstly, an aqueous solution of indium nitrate with a concentration of 0.066M was prepared with In(NO3)3·xH2O and ultrapure water, and 1g of H-SSZ-39(OA) zeolite was ultrasonically dispersed in 33.33mL of the aqueous solution of In(NO3)3; the concentration of the etchant was 1M, and the etching temperature was changed. OA etching modification was performed at 70°C, 75°C, 80°C, and 85°C, and the CH4-SCR activity test was performed. The rest was the same as in Example 1. The NO obtained after the catalyst test x Conversion rate, CH4 conversion rate, CH4 selectivity, etc. Figure 5 shown.
[0078] Figure 5 (a) NO of In / H-SSZ-39 catalyst after OA etching modification at different etching temperatures x The conversion rate curve shows that the NO x The overall trend of conversion rate is consistent. When the etching temperature is 80℃, NO x The highest conversion rate can reach 60.8%. The denitrification activity is slightly reduced after etching modification at other temperatures, and its denitrification activity drops below 60%.
[0079] Figure 5 (b) is the CH4 conversion rate curve of the catalyst after etching modification at different temperatures. It can be seen from the figure that when the etching modification temperature is 80℃, the CH4 conversion rate of the catalyst can reach 92%. When the etching temperature is 70℃, 75℃, and 85℃, the CH4 conversion rate is lower than 90%. Figure 5 (c) is the CH4 selectivity curve of the catalyst. It can be found that the CH4 selectivity of the catalyst after etching modification at 80℃ can reach 50%; the CH4 selectivity of the catalyst after etching modification at 70℃ and 75℃ is about 45%; and after etching modification at 85℃, its CH4 selectivity drops to below 40%.
[0080] Example 7
[0081] On the basis of Example 1, the solid-liquid ratio of the etching process was changed in this example, and OA etching modification treatment was performed under the conditions of solid-liquid ratio of 1g:15mL, 1g:20mL, 1g:25mL, and 1g:30mL, respectively. The denitration activity test results of the modified catalyst are as follows: Figure 6 shown.
[0082] Figure 6 (a) In / H-SSZ-39 catalyst NO after etching modification with different solid-liquid ratios xThe conversion rate curve shows that the denitrification activity is the highest at 62.6% when the solid-liquid ratio is 1g:25mL. When the solid-liquid ratio is 1g:20mL, the denitrification activity slightly decreases to 60.8%. When the solid-liquid ratio is 1g:15mL and 1g:30mL, the denitrification activity drops below 60%. At this time, NO x The conversion rates were 59.1% and 59.3%, respectively.
[0083] Figure 6 (b) is the CH4 conversion rate curve of In / H-SSZ-39 catalyst after etching modification with different solid-liquid ratios. It can be seen that the CH4 conversion rate curves of In / H-SSZ-39 catalyst after etching modification with several different solid-liquid ratios are almost identical, and the CH4 conversion rate increases with increasing temperature, indicating that the change in solid-liquid ratio has little effect on the CH4 conversion rate of the catalyst. The catalyst can achieve a CH4 conversion rate of 90% at 650°C.
[0084] Figure 6 (c) is the CH4 selectivity curve of the catalyst after etching modification with different solid-liquid ratios. When the solid-liquid ratio is 1g:25mL and 1g:30mL, the CH4 selectivity is 44.3% and 43.6% respectively. When the solid-liquid ratio is 1g:15mL and 1g:30mL, the CH4 selectivity is high. In summary, by comparing the CH4-SCR test results of the catalyst after etching with different solid-liquid ratios, it is found that the solid-liquid ratio has little effect on the denitration effect of the catalyst, and the solid-liquid ratio of 1g:25mL is the best.
[0085] Example 8
[0086] An application of SSZ-39 zeolite supported catalyst is used for SO2 and H2O resistance denitration in CH4-SCR. In this embodiment, the catalyst of Example 1 is used. Then, the CH4-SCR activity test is carried out under the conditions of water vapor concentration of 2.5 vol%, 5 vol%, 7.5 vol%, and 10 vol%, and compared with the CH4-SCR activity of the unetched In / H-SSZ-39 catalyst under 2.5 vol% H2O. The test results are as follows Figure 7 shown.
[0087] Figure 7 (a) NO after OA etching modification conditions are optimized x Conversion rate curve, compared with the anhydrous condition, with the increase of water vapor concentration, the denitrification activity of the catalyst decreases. When the reaction gas contains 2.5 vol% H2O, the catalyst NO x The conversion rate is 57.7%. When the water vapor content in the mixed gas increases to 5.0 vol%, 7.5 vol%, and 10 vol%, NO xThe conversion rates were 51.3%, 45.7%, and 42.2%, respectively. Compared with Beta zeolite, the denitrification activity was better at the same water vapor concentration, indicating that the In / H-SSZ-39 zeolite catalyst had a certain resistance to H2O compared with other types of zeolite catalysts, but it still needed to be further enhanced. The In / H-SSZ-39 catalyst that had not been modified by OA etching had a low NO conversion rate in the presence of 2.5 vol% H2O. x The highest conversion rate is only 10%. It was also found that when water vapor is contained in the reaction gas, the active temperature window of the catalyst becomes narrower, and the optimal active temperature moves from 550°C to 600°C.
[0088] Figure 7 (b) is the CH4 conversion rate curve of In / H-SSZ-39 catalyst when different concentrations of water vapor are introduced into the reaction gas. It can be found that when H2O is not added to the reaction gas, the CH4 conversion rate of the catalyst in different temperature ranges is higher than that under the condition of water vapor; at the same time, as the concentration of water vapor in the reaction gas continues to increase, the CH4 conversion rate of the catalyst gradually decreases. Figure 7 (c) is the CH4 selectivity curve of the catalyst activity test under water conditions. When no H2O is added to the reaction gas, the CH4 selectivity of the catalyst is 46% at 500°C; when the mixed gas contains 2.5 vol% H2O, the CH4 selectivity is slightly reduced to 44% compared with the dry condition. As the water vapor concentration in the reaction gas gradually increases, the CH4 selectivity of the catalyst gradually decreases, especially when it increases to 7.5 vol% H2O and 10 vol% H2O, the CH4 selectivity decreases to below 30%, which indicates that water vapor has a significant inhibitory effect on the CH4 selectivity of the catalyst.
[0089] Example 9
[0090] On the basis of Example 1, in step S3 of the preparation method of the SSZ-39 zeolite supported catalyst, in addition to adding the H-SSZ-39 (OA) zeolite obtained in step S2, a metal oxide is also added, and the metal oxide is Co3O4. The mass ratio of the metal oxide to H-SSZ-39 (OA) is 1:20.
[0091] Example 10
[0092] Based on Example 9, the difference of this example is that the metal oxide is NiO, and the rest is the same as Example 9.
[0093] Embodiment 11
[0094] Based on Example 9, the difference of this example is that the metal oxide is CeO2, and the rest is the same as Example 9.
[0095] Comparative Example 3
[0096] Based on Example 9, the difference of this comparative example is that the metal oxide is Fe2O3, and the rest is the same as Example 9.
[0097] Comparative Example 4
[0098] Based on Example 9, the difference of this comparative example is that the metal oxide is MnO2, and the rest is the same as Example 9.
[0099] Comparative Example 5
[0100] Based on Example 9, the difference of this comparative example is that the metal oxide is Cr2O3, and the rest is the same as Example 9.
[0101] The catalysts prepared in Examples 9-11 and Comparative Examples 3-5 were subjected to a denitration experiment. The reaction conditions were: [NO] = 400 ppm, [CH4] = 600 ppm, [O2] = 10 vol%, and a space velocity of 23600 h -1 , prepared In-MO modified with different metal oxides x / H-SSZ-39(OA) catalyst activity in CH4-SCR denitrification Figure 8 shown.
[0102] Figure 8 (a) is In-MO x / H-SSZ-39(OA) catalyst in CH4-SCR reaction x The conversion rate curve shows that after Co3O4 modification, the catalyst can reach 91.4% NO x conversion rate; at the same time, the modification of CeO2 and NiO also improved the denitrification activity of the catalyst, NO x The conversion rate can reach up to about 72% at 550℃, but the modification of Cr2O3, MnO2 and Fe2O3 does not significantly improve the activity of the catalyst. x The conversion rates are the highest at 550°C, which are 50.6%, 30.4% and 22.5% respectively.
[0103] Figure 8 (b) In-MO x From the CH4 conversion rate curve of In / H-SSZ-39(OA) catalyst in CH4-SCR reaction, it can be seen that the CH4 conversion rate of the catalyst after adding metal oxides is significantly improved compared with that of In / H-SSZ-39(OA) catalyst. At 650°C, the CH4 conversion rates of the six metal oxides modified are all above 97%. Figure 8 (c) In-MO xThe CH4 selectivity of / H-SSZ-39(OA) catalyst in the CH4-SCR reaction is the best due to the best catalytic activity after Co3O4 modification, so compared with other metal oxide modifications, its CH4 selectivity is also the best, reaching 52% at 500°C, while the CH4 selectivity of other oxides after modification is below 40%.
[0104] Example 12
[0105] Based on Example 9, the difference of this example is that the modification amount of the metal oxide is different. In step S3, the mass ratio of H-SSZ-39 (OA) zeolite to Co3O4 is 5g:1g, 10g:1g, 20g:1g, 30g:1g, 40g:1g, 50g:1g to prepare In-Co3O4 / H-SSZ-39 (OA) catalyst, and other conditions are the same as Example 9.
[0106] The obtained catalyst was subjected to a denitration experiment, and the reaction test conditions were: [NO] = 400 ppm, [CH4] = 600 ppm, [O2] = 10 vol%, and the air velocity was 23600 h -1 , the water vapor concentration is 5 vol%, and the catalyst is tested in CH4-SCR as shown in Fig. 9 shown.
[0107] from Fig. 9 As can be seen from (a), the In-Co3O4 / H-SSZ-39 catalysts prepared under different Co3O4 modification conditions showed different denitrification activities in CH4-SCR. The NO removal of In-Co3O4 / H-SSZ-39(OA) catalysts prepared when the Co3O4 modification amount and zeolite mass ratio were 1g:5g, 1g:10g, 1g:20g, 1g:30g, 1g:40g, and 1g:50g was significantly higher than that of In-Co3O4 / H-SSZ-39(OA) catalysts. x The highest conversion rates were 49.4%, 49.0%, 58.3%, 80.2%, 73.4%, and 70.9%, respectively. When the amount of Co3O4 modification increased, the denitration activity of the catalyst decreased. This may be because the increase in Co3O4 promoted the non-selective oxidation of CH4, resulting in reduced activity. At the same time, when the amount of Co3O4 modification was less than 1g:30g, the denitration activity of the catalyst would also decrease. This was because the fewer Co3O4 components reduced the participation of CH4 activation products in the process of NO reduction to N2, resulting in reduced activity.
[0108] from Fig. 9As can be seen in (b), the catalyst starts to convert CH4 at 400℃, and the CH4 conversion is more obvious at 500℃ and higher temperatures. It is completely converted at 650℃. The CH4 conversion rates of the six Co3O4 modification ratios at 650℃ all reach 99%, indicating that CH4 has been completely converted at this time. Compared with the CH4 conversion rate of In / H-SSZ-39(OA) catalyst at the same temperature, it shows that the addition of Co3O4 is indeed beneficial to CH4 conversion. Fig. 9 It can be seen from (c) that as the temperature increases, the CH4 selectivity decreases. When the Co3O4 modification amount is 1g:30g, the CH4 selectivity of the catalyst is as high as 54.2% at 500°C. Under other modification conditions, the CH4 selectivity decreases slightly, which is consistent with the change in catalyst activity during the reaction.
[0109] Embodiment 13
[0110] During the CH4-SCR reaction, the O2 concentration will affect the CH4 conversion and thus affect the denitrification activity of the catalyst. In this example, the effect of O2 concentration on the denitrification performance of the In-Co3O4 / H-SSZ-39 (OA) catalyst was investigated. Specifically, the activity of the catalyst of Example 9 was evaluated by changing the oxygen concentration in the reaction gas (3vol%, 5vol%, 8vol%, 10vol%, 15vol%, 20vol%). Other gas parameter conditions are: [NO] = 400ppm, [CH4] = 600ppm, space velocity of 23600h -1 、[H2O]=5vol%NO of In-Co3O4 / H-SSZ-39(OA) catalyst x The test results of conversion rate, CH4 conversion rate and CH4 selectivity are as follows: Fig.10 shown.
[0111] Fig.10 (a) NO2 degradation of In-Co3O4 / H-SSZ-39(OA) catalyst under different O2 concentrations x Conversion rate curve. It can be seen that as the O2 concentration increases, NO x The conversion rate increases because the increase in O2 concentration promotes CH4 activation. When the O2 concentration increases to 10 vol%, the catalyst can achieve 80.3% NO conversion at 600 °C. x As the O2 concentration further increases, the denitrification activity of the catalyst begins to decline. When the O2 concentration in the reaction gas is 15% and 20%, the In-Co3O4 / H-SSZ-39 (OA) catalyst has only 59.8% and 58.7% NO conversion at 600 °C. x Removal rate.
[0112] Fig.10(b) is the CH4 conversion curve of In-Co3O4 / H-SSZ-39(OA) catalyst under different O2 concentrations. It can be found that the CH4 conversion trends of the catalysts under several O2 concentrations are basically the same. At 600℃, the CH4 conversion rate is as high as 90.1% when the O2 content in the reaction gas is 10vol%; when the O2 concentration is increased to 15vol% and 20vol%, the CH4 conversion rate of the catalyst drops to 87.8% and 82.8%, respectively.
[0113] Fig.10 (c) is the CH4 selectivity bar graph of the catalyst In-Co3O4 / H-SSZ-39(OA). It can be found that the CH4 selectivity of the catalyst increases with the increase of O2 concentration. When the O2 concentration is 10 vol%, the CH4 selectivity is as high as 54.2%. When the O2 concentration is further increased, the CH4 selectivity of the catalyst decreases.
[0114] Embodiment 14
[0115] In the CH4-SCR reaction, CH4 / NO will affect the denitration activity of the catalyst. This example experiments on the CH4 / NO ratio. Specifically, based on Example 13, the catalyst of Example 9 was used to explore the effect of different CH4 / NO on the denitration performance of the In-Co3O4 / H-SSZ-39 (OA) catalyst. The denitration activity was tested under three reaction conditions of CH4 / NO of 1:1, 1.5:1, and 2:1. The results of the CH4-SCR test of the In-Co3O4 / H-SSZ-39 (OA) catalyst under 5 vol% H2O are as follows: Fig.11 shown.
[0116] Fig.11 (a) It can be found that under the three ratios, NO x The trend of the conversion rate curve is consistent as a whole. When CH4 / NO is 1.0, 1.5, and 2.0, the NO conversion rate of In-Co3O4 / H-SSZ-39(OA) catalyst at 600℃ is x The conversion rates were 65.0%, 80.3%, and 71.5%, respectively. x The removal rate results showed that the optimal reaction condition for CH4 / NO was 1.5. It was also found that the denitrification activity of the catalyst began to increase significantly at 500°C, indicating that the catalyst exhibited extremely high catalytic performance in the temperature range of 500-600°C, which may be related to the selective catalytic reduction of CH4 in this temperature range.
[0117] Fig.11(b) is the CH4 conversion rate curve of In-Co3O4 / H-SSZ-39(OA) catalyst under different CH4 / NO. It can be found that when the CH4 concentration of the reaction gas is 400ppm and 600ppm, the CH4 conversion rate is higher than that when the CH4 concentration is 800ppm. This may be because low-concentration CH4 can be fully utilized, and when the CH4 concentration is increased to 800ppm, it cannot be fully utilized, thus resulting in a slight decrease in the CH4 conversion rate.
[0118] Fig.11 (c) is a histogram of the CH4 selectivity of the In-Co3O4 / H-SSZ-39 catalyst. It can be found that when the CH4 concentration is 400ppm, 600ppm, and 800ppm, the CH4 selectivity of the In-Co3O4 / H-SSZ-39 (OA) catalyst at 500°C is 56.4%, 54.2%, and 42.9%, respectively. As the CH4 concentration increases, the selectivity decreases, which is consistent with the CH4 conversion rate at high CH4 concentrations.
[0119] Embodiment 15
[0120] In the CH4-SCR reaction, the space velocity affects the denitration activity of the catalyst. This example explores the effect of different space velocities on the denitration performance of the In-Co3O4 / H-SSZ-39 (OA) catalyst. Specifically, based on Example 13, the catalyst of Example 9 was used to perform the denitration reaction under the conditions of 11800h -1 、23600h -1 、35400h -1 、47200h -1 The CH4-SCR denitrification activity test under air velocity, the CH4-SCR test results of the catalyst In-Co3O4 / H-SSZ-39 (OA) under 5 vol% H2O test are as follows Fig.12 shown.
[0121] from Fig.12 It can be seen from (a) that as the airspeed decreases, NO x The conversion rate is improved. The air velocity is 11800h -1 The catalyst can achieve 86.7% NO at 600 °C. x Conversion rate, as the space velocity increases, the catalyst in CH4-SCR NO x The conversion rate decreased. When the air velocity was 23600h -1 、35400h -1 and 47200h -1 When the catalyst is at 600℃, NO xThe conversion rates dropped to 80.3%, 60.4% and 50.0% respectively. Therefore, in order to ensure that the catalyst has a high denitrification efficiency in the reaction, it is very important to select a suitable space velocity. In the subsequent cyclic test and stability test, the space velocity condition was selected to be 11800h -1 Conduct CH4-SCR denitrification activity test.
[0122] Fig.12 (b) is the CH4 conversion rate curve of In-Co3O4 / H-SSZ-39(OA) catalyst under different space velocity adaptability conditions. It can be seen that when the space velocity condition is 11800h -1 Under the condition of reaction temperature at 600℃, the CH4 conversion rate of catalyst can reach 98.6%, and the space velocity is 23600h -1 、35400h -1 and 47200h -1 When the temperature is 600℃, the CH4 conversion rates are 90.1%, 76.1% and 64.8% respectively; compared with the CH4 conversion rate results at high space velocity, at a space velocity of 11800h -1 When the space velocity is increased to 23600h / min, CH4 is almost completely converted over In-Co3O4 / H-SSZ-39(OA) catalyst at 600℃. -1 、35400h -1 and 47200h -1 When the reaction temperature was raised to 650°C, the CH4 conversion rate of the In-Co3O4 / H-SSZ-39(OA) catalyst reached 99%, and most of the CH4 was converted in the form of non-selective oxidation at high temperature.
[0123] Fig.12 (c) is the CH4 selectivity bar graph of In-Co3O4 / H-SSZ-39(OA) catalyst. It can be found that when the space velocity is 11800h -1 The catalyst CH4 selectivity can reach up to 58.8% when the space velocity is increased to 23600h -1 , 35400h -1 and 47200h -1 The CH4 selectivity of In-Co3O4 / H-SSZ-39(OA) catalyst began to decrease, and its CH4 selectivity reached the highest at 500℃, reaching 54.2%, 50.6% and 48.8%, respectively.
[0124] Example 16
[0125] In actual industrial flue gas, there is often a certain amount of water vapor. It is particularly important to test the effect of water vapor content on the denitration performance of the catalyst during the experimental test. This example explores the effect of different water vapor contents in the reaction gas on the denitration performance of the In-Co3O4 / H-SSZ-39 (OA) catalyst. The catalyst of Example 9 is used to perform CH4-SCR denitration evaluation tests on the In-Co3O4 / H-SSZ-39 (OA) catalyst under water vapor concentrations of 5 vol%, 7.5 vol%, 10 vol%, and 15 vol%. The experimental test results are shown in Figure 1. Fig.13 shown.
[0126] Fig.13 (a) It can be found that the In-Co3O4 / H-SSZ-39(OA) catalyst increases with the increase of water vapor concentration in the reaction gas. The activity of the catalyst begins to decline, and the active temperature window of the catalyst also narrows with the increase of water content. When the water content in the reaction gas is 5 vol%, the In-Co3O4 / H-SSZ-39 (OA) catalyst can achieve 80% NO at 600 °C. x However, when the water vapor concentration in the reaction gas was increased to 7.5 vol%, 10 vol%, and 15 vol%, respectively, the In-Co3O4 / H-SSZ-39 (OA) catalyst NO x The highest conversion rates are 70.1%, 67.5% and 58.6% respectively. It can be seen that the increase in water vapor concentration leads to an enhanced inhibitory effect on catalyst activity.
[0127] Fig.13 (b) is the CH4 conversion rate curve of In-Co3O4 / H-SSZ-39(OA) catalyst under different water vapor concentrations. It can be found that the CH4 conversion rate changes in the same trend under several water vapor concentrations. At 600°C, when the water vapor content in the reaction gas is 5vol%, 7.5vol%, 10vol%, and 15vol%, the catalyst CH4 conversion rates are 90.1%, 85.4%, 87.8%, and 83.3%, respectively. It can be seen that the increase in water vapor content will inhibit the selective conversion of CH4 over the In-Co3O4 / H-SSZ-39(OA) catalyst.
[0128] Fig.13 (c) is a histogram of the CH4 selectivity of the In-Co3O4 / H-SSZ-39 catalyst at different water vapor concentrations. It can be seen that the catalyst can achieve a CH4 selectivity of 55% at 500°C. As the water vapor concentration in the reaction gas increases, the CH4 selectivity begins to decrease. When the water vapor concentration increases to 7.5 vol% and 10 vol%, the CH4 selectivity drops to about 45%. When the water vapor content is further increased to 15 vol%, the CH4 selectivity of the catalyst drops to 40%.
[0129] Embodiment 17
[0130] This example explores the effect of SO2 concentration in CH4-SCR on the denitration performance of In-Co3O4 / H-SSZ-39 catalyst. The catalyst of Example 9 was used to test the denitration activity of CH4-SCR at 0ppm, 50ppm, and 100ppm SO2 concentrations. The test results are as follows: Fig.14 As shown in the figure, the NO x Conversion rate, CH4 conversion rate, CH4 selectivity, other test conditions are: [H2O] = 5vol%, [CH4] = 600ppm, [NO] = 400ppm, [O2] = 10vol%, space velocity 23600h -1 .
[0131] Fig.14 (a) NO2 degradation of In-Co3O4 / H-SSZ-39(OA) catalyst under different SO2 concentrations x Conversion rate curve. When the reaction gas contains only 5 vol% H2O, the catalyst has a maximum of 80% NO x Conversion rate: When 50 ppm SO2 is introduced into the reaction gas, the catalyst activity is highest at 600°C. x The highest conversion rate is 60%. When the SO2 concentration in the reaction gas is increased to 100ppm, it can be seen that the catalyst is seriously poisoned by SO2, and only about 20% of NO is converted at 600℃. x Conversion rate. The actual industrial flue gas can reach this concentration very rarely, so the subsequent cyclicity experiment and stability experiment will be tested at 50ppm SO2 concentration.
[0132] Fig.14 (b) is the CH4 conversion rate curve of In-Co3O4 / H-SSZ-39(OA) catalyst under different SO2 concentrations. It can be seen that when no SO2 is added to the reaction gas, the CH4 conversion rate of the catalyst can reach 90.1% at 600℃. Add in reaction gas 50ppm and 100ppm After SO2, the CH4 conversion rate of the catalyst at 600℃ dropped to 83.4% and 58.9%, which shows that SO2 not only reduces the NO x conversion rate, and also inhibit CH4 conversion.
[0133] Fig.14(c) is a histogram of the CH4 selectivity of the In-Co3O4 / H-SSZ-39(OA) catalyst at different SO2 concentrations. It can be seen that when no SO2 is added to the reaction gas, the CH4 selectivity of the catalyst can reach 55% at 500°C. When 50ppm and 100ppm SO2 are added to the reaction gas, the CH4 selectivity of the catalyst at the same temperature drops to 38.3% and 33.2%, respectively. Therefore, the increase in the SO2 concentration in the reaction gas will reduce the CH4 selectivity of the catalyst.
[0134] Embodiment 17
[0135] This example investigates the cyclic performance of the In-Co3O4 / H-SSZ-39 (OA) catalyst under operating conditions. The catalyst of Example 9 is used to conduct a cyclic test experiment under the following conditions: [NO] = 400 ppm, [CH4] = 600 ppm, [O2] = 10 vol%, [H2O] = 5 vol%, [SO2] = 50 ppm, and the space velocity is 11800 h -1 , heating rate 10℃ / min, catalyst in CH4-SCR NO x The curve of conversion rate changing with time is as follows Fig.15 As shown. It can be seen that at an airspeed of 11800h -1 Under the condition of 100℃, the catalyst was tested once with H2O and SO2. The catalyst showed NO x The highest conversion rate can reach 57.1%, and the denitrification activity of the catalyst in other temperature ranges (500℃ and 650℃) is also slightly lower than the first time. From the results of the second cycle test of the catalyst, it can be seen that compared with the first cycle test, the activity of each temperature range has a downward trend, and the best denitrification activity of the catalyst at 600℃ is 51.3%. When the catalyst goes through the third cycle, NO x The degree of decrease in conversion rate is not as obvious as that in the first two cycles. The reason for this is that after the catalyst has undergone the first two SO2 poisoning reactions, the subsequent cycle experiments are less affected by the SO2 poisoning effect. Therefore, the catalyst has better cyclability under reaction conditions containing H2O and SO2.
[0136] Embodiment 18
[0137] This example investigates the denitration stability of the In-Co3O4 / H-SSZ-39 (OA) catalyst under operating conditions. The catalyst of Example 9 is used for stability testing. The experimental conditions are: [NO] = 400 ppm, [CH4] = 600 ppm, [O2] = 10 vol%, [H2O] = 5 vol%, [SO2] = 50 ppm, and the space velocity is 11800 h -1 , the catalyst in CH 4 -NO in SCR xThe curve of conversion rate changing with time is as follows Fig.16 As shown. It can be seen that at an airspeed of 11800h -1 The catalyst still had 68.1% NO at the beginning of the reaction under 5 vol% H2O and 50 ppm SO2. x The conversion rate, as the reaction time gradually increased, the catalyst denitrification performance began to steadily decline. After 7h stability test, NO x The conversion rate gradually decreased from 68.1% to 55.3%, indicating that the catalyst has good stability.
[0138] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. A method for preparing a SSZ-39 zeolite supported catalyst, characterized in that: The steps include: Step S1, ultrasonically dispersing H-SSZ-39 zeolite in water, adding an etchant to obtain a mixture, wherein the etchant is oxalic acid or citric acid, and the concentration of the etchant is 0.1-2.0 mol / L; reacting the mixture at a temperature of 70-85° C. for a reaction time of 2-10 h; Step S2, after the reaction is completed, the filter cake is filtered and washed, and then dried, ground and calcined at a temperature of 480-550°C for more than 2 hours to obtain etched H-SSZ-39 zeolite; Step S3, dissolving In(NO3)3·xH2O in water, adding the H-SSZ-39 zeolite obtained in step S2, stirring at a constant temperature of 80-90°C for more than 6 hours, centrifuging, washing and drying, and then calcining at a calcination temperature of 480-550°C for at least 2 hours to obtain an In / H-SSZ-39 catalyst.
2. The method for preparing the SSZ-39 zeolite supported catalyst according to claim 1, characterized in that: It also includes: in step S3, in addition to adding the H-SSZ-39 zeolite obtained in step S2, a metal oxide is also added, and the metal oxide is Co3O4, NiO or CeO2; the mass ratio of the metal oxide to the H-SSZ-39 zeolite is 1:20-50.
3. The method for preparing the SSZ-39 zeolite supported catalyst according to claim 2, characterized in that: The metal oxide is Co3O4, and the mass ratio of the metal oxide to the H-SSZ-39 zeolite is 1:30-50.
4. The method for preparing the SSZ-39 zeolite supported catalyst according to any one of claims 1 to 3, characterized in that: In the mixture of step S1, the concentration of the etchant is 0.5-1.0 mol / L; the solid-to-liquid ratio of the zeolite to the etchant aqueous solution is 1 g:15-30 mL.
5. The method for preparing the SSZ-39 zeolite supported catalyst according to claim 4, characterized in that: The etchant is oxalic acid.
6. The method for preparing the SSZ-39 zeolite supported catalyst according to claim 4, characterized in that: In step S1, the mixture is reacted at a temperature of 75-80°C.
7. The method for preparing the SSZ-39 zeolite supported catalyst according to claim 4, characterized in that: In step S2 and step S3, the heating rate of calcination is 3-6°C / min.
8. A SSZ-39 zeolite supported catalyst, characterized in that: The catalyst is prepared by the method for preparing the SSZ-39 zeolite-supported catalyst as described in any one of claims 1 to 7.
9. The use of the SSZ-39 zeolite supported catalyst as claimed in claim 8, characterized in that: Used for CH4-SCR denitrification reaction.
10. The use of the SSZ-39 zeolite supported catalyst according to claim 9, characterized in that: The conditions of the CH4-SCR denitrification reaction are: CH4 concentration 400-600ppm, CH4 concentration to NO concentration ratio 1.5-2.0, O2 concentration 5-10vol%, SO2 concentration 0-50ppm, H2O concentration 5-10vol%, space velocity 11800-23600h -1 .
Citation Information
Patent Citations
Cu-SSZ-39 molecular sieve, preparation method thereof and DeNOx catalyst
CN114870887A
Preparation method and application of In-H-SSZ-13 denitration catalyst for adjusting improvement of acid sites
CN117619427A
Co-SSZ-39 catalyst for selective catalytic reduction denitration of methane and preparation method of Co-SSZ-39 catalyst
CN118059936A
Method for preparing molecular sieve-multielement oxide composite integrally extruded denitration catalyst