Catalyst for ammonia gas selective catalytic reduction of NOx, and preparation method and application thereof

By developing the ZrCu-SAPO-18 molecular sieve catalyst, the synergistic effect of Zr and Cu, the problems of narrow temperature window of vanadium-based catalyst and Cu-CHA molecular sieve inactivation are solved, and efficient NOx removal and hydrothermal heat over a wide temperature range are achieved Stability, meet the requirements of diesel vehicle emission regulations.

CN118874533AActive Publication Date: 2024-11-01BEIJING UNIV OF CHEM TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410893760.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-04
Publication Date
2024-11-01
Estimated Expiration
2044-07-04

AI Technical Summary

Technical Problem

The existing vanadium-based catalyst has a narrow temperature window for NOx removal in diesel vehicle exhaust, and contains biotoxic components, making it difficult to achieve efficient removal. The Cu-CHA molecular sieve is inactivated at high temperatures, which cannot meet the strict requirements of diesel vehicle emission regulations. .

Method used

Develop a ZrCu-SAPO-18 molecular sieve catalyst to increase the active Cu2+ sites and acidic sites of the catalyst through the synergistic effect between Zr and Cu. The preparation method includes hydrothermal synthesis of SAPO-18, ammonium nitrate and copper nitrate ions Exchange, zirconium nitrate impregnation, forming the ZrCu-SAPO-18 catalyst, with a wide temperature window, excellent hydrothermal stability and anti-sulfur poisoning ability.

Benefits of technology

Highly efficient NOx removal is achieved within a wide temperature range, with NOx conversion rate reaching more than 90%. The activity of the catalyst is improved after high-temperature hydrothermal aging, and has excellent hydrothermal stability and anti-sulfur poisoning ability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874533A_ABST
    Figure CN118874533A_ABST
Patent Text Reader

Abstract

The invention relates to a catalyst for selective catalytic reduction of NOx by ammonia gas as well as a preparation method and application of the catalyst, and belongs to the technical field of environmental catalysis and air pollution control. The catalyst comprises a carrier, a main active component and a performance additive, the carrier is selected from SAPO-18 molecular sieves, the main active component is selected from Cu, and the performance additive is selected from Zr. According to the ZrCu-SAPO-18 molecular sieve catalyst, the conversion rate of NOx reaches 90% or above when the temperature of the ZrCu-SAPO-18 molecular sieve catalyst is 225-450 DEG C and the air speed is 88,000 h <-1 >; after hydrothermal treatment is carried out for 12 hours at 750 DEG C, the conversion rate of NOx is still 90% or above within the range of 175-400 DEG C. The catalyst disclosed by the invention can be used for efficiently removing NOx in diesel vehicle tail gas and stationary source flue gas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for selective catalytic reduction of NO by ammonia x The catalyst and its preparation method and application are suitable for NO in diesel vehicle exhaust and fixed source flue gas. x The catalytic removal belongs to the technical field of environmental catalysis and air pollution control. Background Art

[0002] NO x As a major air pollutant, NO has serious harm to environmental quality and human health. x Control has become a hot topic in the field of atmospheric environmental protection technology. At present, ammonia selective catalytic reduction technology (NH3-SCR) is a technology that can effectively reduce NO x For NH3-SCR denitrification technology, traditional vanadium-based catalysts are effective in removing NO from coal-fired power plants. x However, the catalyst has a narrow temperature window (300℃-400℃) and contains the biologically toxic active component V2O5. Given the low exhaust temperature of diesel vehicles and the large temperature fluctuation range, the narrow temperature window of vanadium-based catalysts cannot achieve the control of NO emissions from diesel vehicles. x Therefore, the development of SCR catalysts with a wider active temperature window is of great significance for the purification of diesel vehicle exhaust.

[0003] Molecular sieve catalysts have been discovered and gradually widely studied and applied due to their unique pore structure, wide reaction activity window and non-toxicity. In recent years, CHA-type molecular sieves (SSZ-13 and SAPO-34) have attracted much attention due to their excellent SCR activity and good hydrothermal stability. However, Cu-CHA molecular sieves still face the problem of deactivation at high temperatures (850°C). With the increasingly stringent emission regulations for diesel vehicles, researchers are committed to developing other types of molecular sieves, and AEI-configured molecular sieve catalysts (SAPO-18 and SSZ-39) that are very similar to CHA structures are increasingly attracting the attention of researchers.

[0004] The invention prepares a ZrCu-SAPO-18 molecular sieve catalyst which has good catalytic activity, excellent hydrothermal stability and sulfur poisoning resistance for NH3-SCR denitration in a wide temperature range. Summary of the invention

[0005] The present invention aims to provide a method for selective catalytic reduction of NO by ammonia. x The catalyst and its preparation method and application are simple in preparation method and have excellent performance for NH3-SCR denitration. Through the synergistic effect between Zr and Cu in the catalyst, not only the active Cu in the catalyst2+ The number of sites on the catalyst surface increases significantly, and the acid sites on the catalyst surface also increase significantly, so that the catalyst shows excellent NH3-SCR denitrification activity, hydrothermal stability and resistance to sulfur poisoning, thereby obtaining a highly efficient NO removal in a wide temperature window. x catalyst.

[0006] The objective of the present invention is achieved through the following technical solutions:

[0007] In a first aspect, the present invention provides a method for selective catalytic reduction of NO with ammonia. x The catalyst comprises a carrier, a main active component and a modification aid. The catalyst uses small pore molecular sieve SAPO-18 as a carrier, Cu as a main active component, and Zr as a modification aid. Its composition is expressed as ZrCu-SAPO-18. Taking the mass of the carrier as 100%, the mass percentage of Cu is 0.5-2%, and the mass percentage of Zr is 0.02-0.2%.

[0008] In a second aspect, the present invention provides a method for preparing the catalyst as described in the first aspect, the method comprising the following steps:

[0009] (1) NN diisopropylethylamine (C8H 19 N) is used as a template to prepare a synthetic solution, followed by hydrothermal reaction, solid-liquid separation, washing, drying, and calcination at 450-550° C. to obtain a small-pore molecular sieve SAPO-18;

[0010] (2) treating the small pore molecular sieve SAPO-18 prepared in step (1) with an ammonium nitrate solution to obtain NH4-SAPO-18;

[0011] (3) placing NH4-SAPO-18 in a copper nitrate solution for at least two ion exchanges, washing, drying, and calcining at 450-550° C. to obtain Cu-SAPO-18;

[0012] (4) Cu-SAPO-18 is immersed in a zirconium nitrate solution, dried, and calcined at 450-550° C. to obtain a ZrCu-SAPO-18 catalyst.

[0013] Preferably, the molar composition of the synthetic solution in step (1) is (1.4-1.8)NN diisopropylethylamine: 1Al2O3:

[0014] (0.85~0.95)P2O5:(0.95~1.05)SiO2:(40~60)H2O; For example: 1.6DIEA:1Al2O3:0.9P2O5:

[0015] 1.0SiO2:50H2O, etc.

[0016] Preferably, the number of solid-liquid separation and washing in step (1) is 5 to 8 times.

[0017] Preferably, the method for solid-liquid separation in step (1) is selected from centrifugation.

[0018] Preferably, the drying method in step (1) is drying at 90-110° C. for 12-24 hours.

[0019] Preferably, the calcination time in step (1) is 4 to 8 hours.

[0020] Preferably, the concentration of the ammonium nitrate solution in step (2) is 0.9 mol / L to 1.1 mol / L, for example 0.95 mol / L,

[0021] 1.0mol / L, 1.1mol / L, etc.

[0022] Preferably, the method of treating the small pore molecular sieve SAPO-18 with an ammonium nitrate solution in step (2) comprises: adding the small pore molecular sieve SAPO-18 to the ammonium nitrate solution, stirring at 60-80° C. for 5-10 hours, separating the product into a solid and a liquid, washing with water, and drying at 90-110° C. for 12-24 hours.

[0023] Preferably, the number of ion exchanges in step (3) is selected from 2 times.

[0024] Preferably, the duration of each ion exchange is selected from 6 h to 10 h.

[0025] Preferably, the ion exchange temperature is selected from 70°C to 85°C.

[0026] Preferably, the calcination time in step (3) is 4 to 8 hours.

[0027] Preferably, the concentration of the copper nitrate solution in step (3) is selected from 0.05 to 0.2 mol / L.

[0028] Preferably, the ion exchange method in step (3) comprises: adding the NH4-SAPO-18 obtained in step (2) to a copper nitrate solution to perform ion exchange, followed by solid-liquid separation, washing the product with water, and heating at 90 to 110°C.

[0029] The mixture is dried at room temperature for 12 to 24 hours, and then the second ion exchange is performed.

[0030] Preferably, the mass fraction of zirconium in the zirconium nitrate solution in step (4) is 0.02 to 0.2 wt%.

[0031] Preferably, the impregnation method in step (4) comprises: adding the Cu-SAPO-18 obtained in step (3) to a zirconium nitrate solution and stirring for 4 to 8 hours. The impregnation temperature is preferably room temperature, more preferably 20°C to 35°C.

[0032] Preferably, the drying temperature in step (4) is 110 to 130° C. and the drying time is 12 to 24 hours.

[0033] Preferably, the calcination time in step (4) is 4 to 8 hours.

[0034] Preferably,

[0035] The method comprises the following steps in sequence:

[0036] (a) Prepare 0.1 mol / L ammonium nitrate solution and 0.05-0.2 mol / L copper nitrate (copper acetate) solution;

[0037] (b) NN diisopropylethylamine (C8H 19 N) was used as template, and SAPO-18 molecular sieve was synthesized by hydrothermal method, and the molar composition of the synthetic solution was 1.6DIEA: 1Al2O3: 0.9P2O5: 1.0SiO2: 50H2O;

[0038] (c) taking the reaction solution obtained in step (2), washing it by centrifugation for 5 to 8 times, drying it at 100° C. for 12 to 24 hours, and then calcining it in a muffle furnace at 450 to 550° C. for 4 to 8 hours to obtain a SAPO-18 molecular sieve catalyst;

[0039] (d) adding the SAPO-18 molecular sieve obtained in step (3) to a 0.1 mol / L ammonium nitrate solution, stirring at 60-80° C. for 5-10 hours, filtering and washing the product with deionized water, and drying at 100° C. for 12-24 hours to obtain an NH4-SAPO-18 catalyst;

[0040] (e) adding the NH4-SAPO-18 catalyst sample obtained in step (4) to a 0.05-0.2 mol / L copper nitrate solution, performing ion exchange at 80°C for 8 hours, filtering and washing the product with deionized water, drying at 100°C for 12-24 hours, and then performing a second exchange at the same ratio, washing and drying. Placing the product in a muffle furnace and calcining it at 450-550°C for 4-8 hours to obtain a Cu-SAPO-18 catalyst;

[0041] (f) adding the sample obtained in step (5) to a zirconium nitrate solution having a zirconium mass fraction of 0.02 to 0.20 wt%, stirring at room temperature for 4 to 8 hours, drying the obtained slurry at 120° C. for 12 to 24 hours to obtain a dry sample; placing the sample in a muffle furnace and calcining it at 450 to 550° C. for 4 to 8 hours to obtain a ZrCu-SAPO-18 catalyst.

[0042] After the catalyst of the present invention is hydrothermally treated at 750°C for 12 hours, the NO x The conversion rate can still reach over 90%.

[0043] Compared with the prior art, the present invention has the following advantages and outstanding effects: Due to the synergistic effect between Cu and Zr, the ZrCu-SAPO-18 molecular sieve catalyst improves the denitration performance of the catalyst and broadens the active temperature window of the catalyst. In the range of 225 to 450° C., the purification efficiency of nitrogen oxides reaches more than 90%; at the same time, the ZrCu-SAPO-18 molecular sieve catalyst has excellent hydrothermal stability and resistance to sulfur poisoning. After high-temperature hydrothermal aging treatment, the activity of the ZrCu-SAPO-18 catalyst not only does not decrease, but is significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 The effect of SO2 on the activity of 0.64%Cu-SAPO-18 and 0.05%Zr-0.64%Cu-SAPO-18 catalysts.

[0045] Specific implementation method

[0046] The technical solution of the present invention is further described below in conjunction with embodiments:

[0047] Example 1: Preparation of 0.02% Zr-0.64% Cu-SAPO-18 catalyst

[0048] a) NN diisopropylethylamine (C8H 19 N) was used as a template and SAPO-18 molecular sieve was synthesized by hydrothermal method. The molar composition of the synthetic solution is 1.6DIEA: 1Al2O3: 0.9P2O5: 1.0SiO2: 50H2O; the specific steps of the hydrothermal synthesis method are: dissolving pseudo-boehmite in a certain amount of deionized water, then adding phosphoric acid dropwise, stirring for 1 hour, adding an appropriate amount of silica sol, and stirring for another 1 hour. Finally, the template C8H 19 N was added dropwise to the mixed solution and stirred for 1 hour. The mixed solution was transferred to a hydrothermal autoclave lined with polytetrafluoroethylene, crystallized at 180°C for 7 days, filtered after cooling, centrifuged and washed, dried at 100°C for 12 hours, and calcined at 550°C for 6 hours to obtain SAPO-18 molecular sieve.

[0049] b) Adding SAPO-18 molecular sieve into 0.1 mol / L ammonium nitrate solution (solid-liquid ratio of 1 / 50), stirring at 80° C. for 8 hours, filtering and washing the product with deionized water, and drying at 100° C. for 12 hours to obtain NH4-SAPO-18 catalyst.

[0050] c) The NH4-SAPO-18 catalyst sample was added to a 0.05 mol / L copper nitrate solution (solid-to-liquid ratio of 1 / 100), ion exchanged at 80°C for 8 hours, the product was filtered and washed with deionized water, dried at 100°C for 12 hours, and then exchanged for the second time with the same ratio, washed and dried. The product was placed in a muffle furnace and calcined at 550°C for 6 hours to obtain a 0.64% Cu-SAPO-18 catalyst.

[0051] d) Weigh 0.001 g of Zr(NO3)4·5H2O and dissolve it in 10 mL of deionized water, stir thoroughly, then add 1 g of 0.64% Cu-SAPO-18 powder prepared in step c), stir at room temperature for 4 hours, dry the prepared slurry at 120°C for 12 hours, and then calcine it in a muffle furnace at 550°C for 6 hours to obtain a 0.02% Zr-0.64% Cu-SAPO-18 catalyst.

[0052] Example 2: Preparation of 0.05% Zr-0.64% Cu-SAPO-18 Catalyst

[0053] a) NN diisopropylethylamine (C8H 19 N) was used as a template and SAPO-18 molecular sieve was synthesized by hydrothermal method. The molar composition of the synthetic solution is 1.6DIEA: 1Al2O3: 0.9P2O5: 1.0SiO2: 50H2O; the specific steps of the hydrothermal synthesis method are: dissolving pseudo-boehmite in a certain amount of deionized water, then adding phosphoric acid dropwise, stirring for 1 hour, adding an appropriate amount of silica sol, and stirring for another 1 hour. Finally, the template C8H 19 N was added dropwise to the mixed solution and stirred for 1 hour. The mixed solution was transferred to a hydrothermal autoclave lined with polytetrafluoroethylene, crystallized at 180°C for 7 days, filtered after cooling, centrifuged and washed, dried at 100°C for 12 hours, and calcined at 550°C for 6 hours to obtain SAPO-18 molecular sieve.

[0054] b) Adding SAPO-18 molecular sieve into 0.1 mol / L ammonium nitrate solution (solid-liquid ratio of 1 / 50), stirring at 80° C. for 8 hours, filtering and washing the product with deionized water, and drying at 100° C. for 12 hours to obtain NH4-SAPO-18 catalyst.

[0055] c) The NH4-SAPO-18 catalyst sample was added to a 0.05 mol / L copper nitrate solution (solid-to-liquid ratio of 1 / 100), ion exchanged at 80°C for 8 hours, the product was filtered and washed with deionized water, dried at 100°C for 12 hours, and then exchanged for the second time with the same ratio, washed and dried. The product was placed in a muffle furnace and calcined at 550°C for 6 hours to obtain a 0.64% Cu-SAPO-18 catalyst.

[0056] d) Weigh 0.0024 g Zr(NO3)4·5H2O and dissolve it in 10 mL deionized water, stir thoroughly, then add 1 g 0.64% Cu-SAPO-18 powder prepared in step c), stir at room temperature for 4 hours, dry the prepared slurry at 120°C for 12 hours, and then calcine it in a muffle furnace at 550°C for 6 hours to obtain 0.05% Zr-0.64% Cu-SAPO-18 catalyst.

[0057] Example 3: Preparation of 0.2% Zr-0.64% Cu-SAPO-18 Catalyst

[0058] a) NN diisopropylethylamine (C8H 19 N) was used as a template and SAPO-18 molecular sieve was synthesized by hydrothermal method. The molar composition of the synthetic solution is 1.6DIEA: 1Al2O3: 0.9P2O5: 1.0SiO2: 50H2O; the specific steps of the hydrothermal synthesis method are: dissolving pseudo-boehmite in a certain amount of deionized water, then adding phosphoric acid dropwise, stirring for 1 hour, adding an appropriate amount of silica sol, and stirring for another 1 hour. Finally, the template C8H 19 N was added dropwise to the mixed solution and stirred for 1 hour. The mixed solution was transferred to a hydrothermal autoclave lined with polytetrafluoroethylene, crystallized at 180°C for 7 days, filtered after cooling, centrifuged and washed, dried at 100°C for 12 hours, and calcined at 550°C for 6 hours to obtain SAPO-18 molecular sieve.

[0059] b) Adding SAPO-18 molecular sieve into 0.1 mol / L ammonium nitrate solution (solid-liquid ratio of 1 / 50), stirring at 80° C. for 8 hours, filtering and washing the product with deionized water, and drying at 100° C. for 12 hours to obtain NH4-SAPO-18 catalyst.

[0060] c) The NH4-SAPO-18 catalyst sample was added to a 0.05 mol / L copper nitrate solution (solid-to-liquid ratio of 1 / 100), ion exchanged at 80°C for 8 hours, the product was filtered and washed with deionized water, dried at 100°C for 12 hours, and then exchanged for the second time with the same ratio, washed and dried. The product was placed in a muffle furnace and calcined at 550°C for 6 hours to obtain a 0.64% Cu-SAPO-18 catalyst.

[0061] d) Weigh 0.0094 g Zr(NO3)4·5H2O and dissolve it in 10 mL deionized water, stir thoroughly, and then add 1 g Cu prepared in step c). 0.64 -SAPO-18 powder, stirred at room temperature for 4 hours, the obtained slurry was dried at 120°C for 12 hours, and then placed in a muffle furnace and calcined at 550°C for 6 hours to obtain 0.2% Zr-0.64% Cu-SAPO-18 catalyst.

[0062] Example 4: Preparation of 0.05% Zr-0.5% Cu-SAPO-18 catalyst

[0063] a) NN diisopropylethylamine (C8H 19 N) was used as a template and SAPO-18 molecular sieve was synthesized by hydrothermal method. The molar composition of the synthetic solution is 1.6DIEA: 1Al2O3: 0.9P2O5: 1.0SiO2: 50H2O; the specific steps of the hydrothermal synthesis method are: dissolving pseudo-boehmite in a certain amount of deionized water, then adding phosphoric acid dropwise, stirring for 1 hour, adding an appropriate amount of silica sol, and stirring for another 1 hour. Finally, the template C8H 19 N was added dropwise to the mixed solution and stirred for 1 hour. The mixed solution was transferred to a hydrothermal autoclave lined with polytetrafluoroethylene, crystallized at 180°C for 7 days, filtered after cooling, centrifuged and washed, dried at 100°C for 12 hours, and calcined at 550°C for 6 hours to obtain SAPO-18 molecular sieve.

[0064] b) Adding SAPO-18 molecular sieve into 0.1 mol / L ammonium nitrate solution (solid-liquid ratio of 1 / 50), stirring at 80° C. for 8 hours, filtering and washing the product with deionized water, and drying at 100° C. for 12 hours to obtain NH4-SAPO-18 catalyst.

[0065] c) The NH4-SAPO-18 catalyst sample was added to a 0.05 mol / L copper nitrate solution (solid-liquid ratio of 1 / 100), ion exchange was performed at 80°C for 8 hours, the product was filtered and washed with deionized water, and dried at 100°C for 12 hours. The product was placed in a muffle furnace and calcined at 550°C for 6 hours to obtain a 0.5% Cu-SAPO-18 catalyst.

[0066] d) Weigh 0.0024 g Zr(NO3)4·5H2O and dissolve it in 10 mL deionized water, stir thoroughly, and then add 1 g Cu prepared in step c). 0.5-SAPO-18 powder was stirred at room temperature for 4 hours, the obtained slurry was dried at 120°C for 12 hours, and then calcined in a muffle furnace at 550°C for 6 hours to obtain 0.05% Zr-0.5% Cu-SAPO-18 catalyst.

[0067] Example 5: Preparation of 0.05% Zr-2% Cu-SAPO-18 Catalyst

[0068] a) NN diisopropylethylamine (C8H 19 N) was used as a template and SAPO-18 molecular sieve was synthesized by hydrothermal method. The molar composition of the synthetic solution is 1.6DIEA: 1Al2O3: 0.9P2O5: 1.0SiO2: 50H2O; the specific steps of the hydrothermal synthesis method are: dissolving pseudo-boehmite in a certain amount of deionized water, then adding phosphoric acid dropwise, stirring for 1 hour, adding an appropriate amount of silica sol, and stirring for another 1 hour. Finally, the template C8H 19 N was added dropwise to the mixed solution and stirred for 1 hour. The mixed solution was transferred to a hydrothermal autoclave lined with polytetrafluoroethylene, crystallized at 180°C for 7 days, filtered after cooling, centrifuged and washed, dried at 100°C for 12 hours, and calcined at 550°C for 6 hours to obtain SAPO-18 molecular sieve.

[0069] b) Adding SAPO-18 molecular sieve into 0.1 mol / L ammonium nitrate solution (solid-liquid ratio of 1 / 50), stirring at 80° C. for 8 hours, filtering and washing the product with deionized water, and drying at 100° C. for 12 hours to obtain NH4-SAPO-18 catalyst.

[0070] c) The NH4-SAPO-18 catalyst sample was added to a 0.2 mol / L copper nitrate solution (solid-liquid ratio of 1 / 100), ion exchange was performed at 80°C for 8 hours, the product was filtered and washed with deionized water, and dried at 100°C for 12 hours. The product was placed in a muffle furnace and calcined at 550°C for 6 hours to obtain a 2% Cu-SAPO-18 catalyst.

[0071] d) Weigh 0.0024 g of Zr(NO3)4·5H2O and dissolve it in 10 mL of deionized water, stir thoroughly, then add 1 g of the 2% Cu-SAPO-18 powder prepared in step c), stir at room temperature for 4 hours, dry the obtained slurry at 120° C. for 12 hours, and then calcine it in a muffle furnace at 550° C. for 6 hours to obtain a 0.05% Zr-2% Cu-SAPO-18 catalyst.

[0072] Example 6 (reference): Preparation of 0.64% Cu-SAPO-18 catalyst

[0073] a) NN diisopropylethylamine (C8H19 N) was used as a template and SAPO-18 molecular sieve was synthesized by hydrothermal method. The molar composition of the synthetic solution is 1.6DIEA: 1Al2O3: 0.9P2O5: 1.0SiO2: 50H2O; the specific steps of the hydrothermal synthesis method are: dissolving pseudo-boehmite in a certain amount of deionized water, then adding phosphoric acid dropwise, stirring for 1 hour, adding an appropriate amount of silica sol, and stirring for another 1 hour. Finally, the template C8H 19 N was added dropwise to the mixed solution and stirred for 1 hour. The mixed solution was transferred to a hydrothermal autoclave lined with polytetrafluoroethylene, crystallized at 180°C for 7 days, filtered after cooling, centrifuged and washed, dried at 100°C for 12 hours, and calcined at 550°C for 6 hours to obtain SAPO-18 molecular sieve.

[0074] b) Adding SAPO-18 molecular sieve into 0.1 mol / L ammonium nitrate solution (solid-liquid ratio of 1 / 50), stirring at 80° C. for 8 hours, filtering and washing the product with deionized water, and drying at 100° C. for 12 hours to obtain NH4-SAPO-18 catalyst.

[0075] c) The NH4-SAPO-18 catalyst sample was added to a 0.05 mol / L copper nitrate solution (solid-to-liquid ratio of 1 / 100), ion exchanged at 80°C for 8 hours, the product was filtered and washed with deionized water, dried at 100°C for 12 hours, and then exchanged for the second time with the same ratio, washed and dried. The product was placed in a muffle furnace and calcined at 550°C for 6 hours to obtain a 0.64% Cu-SAPO-18 catalyst.

[0076] Example 7: The preparation method of the catalyst is the same as that of Example 1. 0.12 g of the catalyst is loaded into a fixed bed reactor. The reaction conditions are: 500 ppm NO, 500 ppm NH3, 5% O2, and N2 as the balance gas. The gas flow rate is 300 cm 3 ·min -1 , gas space velocity (GHSV) is 88,000h -1 The activity evaluation temperature range is 150~500℃, and NO x The conversion rates are shown in Table 1.

[0077] Example 8: The preparation method of the catalyst is the same as that of Example 2. 0.12 g of the catalyst is loaded into a fixed bed reactor. The reaction conditions are: 500 ppm NO, 500 ppm NH3, 5% O2, and N2 as the balance gas. The gas flow rate is 300 cm 3 ·min -1 , gas space velocity (GHSV) is 88,000h -1 The activity evaluation temperature range is 150~500℃, and NOx The conversion rates are shown in Table 1.

[0078] Example 9: The preparation method of the catalyst is the same as that of Example 3. 0.12 g of the catalyst is loaded into a fixed bed reactor. The reaction conditions are: 500 ppm NO, 500 ppm NH3, 5% O2, and N2 as the balance gas. The gas flow rate is 300 cm 3 ·min -1 , gas space velocity (GHSV) is 88,000h -1 The activity evaluation temperature range is 150~500℃, and NO x The conversion rates are shown in Table 1.

[0079] Example 10: The preparation method of the catalyst is the same as that of Example 4. 0.12 g of the catalyst is loaded into a fixed bed reactor. The reaction conditions are: 500 ppm NO, 500 ppm NH3, 5% O2, and N2 as the balance gas. The gas flow rate is 300 cm 3 ·min -1 , gas space velocity (GHSV) is 88,000h -1 The activity evaluation temperature range is 150~500℃, and NO x The conversion rates are shown in Table 1.

[0080] Example 11: The preparation method of the catalyst is the same as that of Example 5. 0.12 g of the catalyst is loaded into a fixed bed reactor. The reaction conditions are: 500 ppm NO, 500 ppm NH3, 5% O2, and N2 as the balance gas. The gas flow rate is 300 cm 3 ·min -1 , gas space velocity (GHSV) is 88,000h -1 The activity evaluation temperature range is 150~500℃, and NO x The conversion rates are shown in Table 1.

[0081] Table 1 Activity evaluation results of copper-zirconium bimetallic supported molecular sieves and reference catalysts

[0082]

[0083] Example 12: The preparation method of the catalyst is the same as that of Example 6. 0.12 g of the catalyst is loaded into a fixed bed reactor. The reaction conditions are: 500 ppm NO, 500 ppm NH3, 5% O2, and N2 as the balance gas. The gas flow rate is 300 cm 3 ·min -1 , gas space velocity (GHSV) is 88,000h -1 The activity evaluation temperature range is 150~500℃, and NOx The conversion rates are shown in Table 1.

[0084] Example 13: The preparation method of the catalyst is the same as that of Example 2. 0.12 g of the catalyst is loaded into a fixed bed reactor. The reaction conditions are: 500 ppm NO, 500 ppm NH3, 5% O2, 5 vol% H2O, and N2 as the balance gas. The gas flow rate is 300 cm 3 ·min -1 , gas space velocity (GHSV) is 88,000h -1 The catalyst was hydrothermally treated at 750℃ for 12h. The activity evaluation temperature range was 150~500℃. x The conversion rates are shown in Table 1.

[0085] Example 14: The preparation method of the catalyst is the same as that of Example 6. 0.12 g of the catalyst is loaded into a fixed bed reactor. The reaction conditions are: 500 ppm NO, 500 ppm NH3, 5% O2, 5 vol% H2O, and N2 as the balance gas. The gas flow rate is 300 cm 3 ·min -1 , gas space velocity (GHSV) is 88,000h -1 The catalyst was hydrothermally treated at 750℃ for 12h. The activity evaluation temperature range was 150~500℃. x The conversion rates are shown in Table 1.

[0086] Example 15: The preparation method of the catalyst is the same as that of Example 2. 0.12 g of the catalyst is loaded into a fixed bed reactor. The reaction conditions are: 500 ppm NO, 500 ppm NH3, 5% O2, 50 ppm SO2, and N2 as the balance gas. The gas flow rate is 300 cm 3 ·min -1 , gas space velocity (GHSV) is 88,000h -1 The activity evaluation temperature range is 150~500℃, and NO x The conversion rates are shown in Table 1.

[0087] Example 16: The preparation method of the catalyst is the same as that of Example 6. 0.12 g of the catalyst is loaded into a fixed bed reactor. The reaction conditions are: 500 ppm NO, 500 ppm NH3, 5% O2, 50 ppm SO2, and N2 as the balance gas. The gas flow rate is 300 cm 3 ·min -1 , gas space velocity (GHSV) is 88,000h -1 The activity evaluation temperature range is 150~500℃. Figure 1 shown.

Claims

1. A method for selective catalytic reduction of NO with ammonia x A catalyst characterized by: The catalyst comprises a carrier, a main active component and a modification aid. The carrier of the catalyst is a small-pore molecular sieve SAPO-18, Cu is the main active component, Zr is the modification aid, and its composition is expressed as ZrCu-SAPO-18. Taking the mass of the carrier as 100%, the mass percentage of Cu is 0.5-2%, and the mass percentage of Zr is 0.05-0.2%.

2. A method for preparing the catalyst according to claim 1, characterized in that: The method comprises the following steps: (1) NN diisopropylethylamine (C8H 19 N) is used as a template to prepare a synthetic solution, followed by hydrothermal reaction, solid-liquid separation, washing, drying, and calcination at 450-550° C. to obtain a small-pore molecular sieve SAPO-18; (2) treating the small pore molecular sieve SAPO-18 prepared in step (1) with an ammonium nitrate solution to obtain NH4-SAPO-18; (3) placing NH4-SAPO-18 in a copper nitrate solution for at least two ion exchanges, washing, drying, and calcining at 450-550° C. to obtain Cu-SAPO-18; (4) Cu-SAPO-18 is immersed in a zirconium nitrate solution, dried, and calcined at 450-550° C. to obtain a ZrCu-SAPO-18 catalyst.

3. The method according to claim 2, characterized in that: The molar composition of the synthetic solution in step (1) is (1.4-1.8)NN diisopropylethylamine: 1Al2O3: (0.85-0.95)P2O5: (0.95-1.05)SiO2: (40-60)H2O; Preferably, the number of solid-liquid separation and washing in step (1) is 5 to 8 times; Preferably, the method for solid-liquid separation in step (1) is selected from centrifugation; Preferably, the drying method in step (1) is drying at 90 to 110° C. for 12 to 24 hours; Preferably, the calcination time in step (1) is 4 to 8 hours.

4. The method according to claim 2, characterized in that: The concentration of the ammonium nitrate solution in step (2) is 0.9 mol / L to 1.1 mol / L; Preferably, the method of treating the small pore molecular sieve SAPO-18 with an ammonium nitrate solution in step (2) comprises: adding the small pore molecular sieve SAPO-18 to the ammonium nitrate solution, stirring at 60-80° C. for 5-10 hours, separating the product into a solid and a liquid, washing with water, and drying at 90-110° C. for 12-24 hours.

5. The method according to claim 2, characterized in that: The number of ion exchanges in step (3) is selected from 2 times; Preferably, the duration of each ion exchange is selected from 6h to 10h; Preferably, the temperature of ion exchange is selected from 70°C to 85°C; Preferably, the calcination time in step (3) is 4 to 8 hours. Preferably, the concentration of the copper nitrate solution in step (3) is selected from 0.05 to 0.2 mol / L.

6. The method according to claim 2, characterized in that: The ion exchange method in step (3) comprises: adding the NH4-SAPO-18 obtained in step (2) to a copper nitrate solution to perform ion exchange, then performing solid-liquid separation, washing the product with water, drying at 90 to 110° C. for 12 to 24 hours, and then performing a second ion exchange.

7. The method according to claim 2, characterized in that: The mass fraction of zirconium in the zirconium nitrate solution in step (4) is 0.02~0.2wt%.

8. The method according to claim 7, characterized in that The impregnation method in step (4) comprises: adding the Cu-SAPO-18 obtained in step (3) into a zirconium nitrate solution and stirring for 4 to 8 hours. The impregnation temperature is preferably room temperature, more preferably 20°C to 35°C.

9. The method according to claim 2, characterized in that: The drying temperature in step (4) is 110 to 130° C. and the drying time is 12 to 24 hours; Preferably, the calcination time in step (4) is 4 to 8 hours.

10. The use of the catalyst according to claim 1, characterized in that: The catalyst is suitable for NO in diesel vehicle exhaust and stationary source flue gas. x catalytic removal.

Citation Information

Patent Citations

  • Preparation method of SAPO-18-carried Cu-Fe catalyst for ammonia-selective catalytic elimination of NOx

    CN102626653A

  • Exhaust gas purifying catalyst

    CN104907092A

  • Preparation method for metal-modified SAPO molecular sieve

    CN105984876A

  • Preparation method and application of auxiliary metal-doped Cu-SAPO-18 catalyst

    CN107185589A

  • Preparation method and application of SAPO-18 doped Cu and Ce composite catalyst

    CN108187737A