Diatom pair photocatalyst, preparation method thereof and application of diatom pair photocatalyst in tetracycline degradation

By introducing highly dispersed diatom pairs and covalent organic framework structures into the photocatalyst, the problem of unclear synergistic mechanism of bimetallic sites is solved, and the pollutant degradation efficiency of photocatalysts is significantly improved.

CN118874545AInactive Publication Date: 2024-11-01TAIYUAN UNIVERSITY OF TECHNOLOGY
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410908526.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-01
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing bimetallic inorganic supported semiconductor materials have problems such as uneven distribution of active sites and difficult to determine the binding method in the degradation of photocatalytic water pollutants, resulting in unclear synergistic mechanisms between bimetallic sites and low catalyst efficiency.

Method used

Using diatom pair photocatalysts, metals such as Co, Ni, Cu, Fe, Mn, Pt are introduced through covalent organic frame structure to form highly dispersed M1-M2 diatom pairs, which are uniformly fixed on the one-dimensional pore walls, and the catalyst is improved. The contact efficiency of the site and the contaminant molecules is achieved through the electrochemical reaction preparation process to achieve uniform distribution of metal diatom pairs.

Benefits of technology

The pollutant degradation efficiency of photocatalysts is improved, the contact efficiency between catalyst sites and pollutant molecules in water bodies is enhanced, and the pollutant degradation rate is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118874545A_ABST
    Figure CN118874545A_ABST
Patent Text Reader

Abstract

The invention provides a diatom pair photocatalyst and a preparation method and application thereof.The diatom pair photocatalyst comprises M1-M2-COF, the diatom pair photocatalyst is prepared through a solvothermal method, an impregnation method and an electrochemical reduction method, M1-M2 diatom pairs are evenly fixed to one-dimensional hole walls of a covalent organic framework, and the covalent organic framework is formed. When the photocatalyst is used for catalyzing pollutant degradation, the contact efficiency of a catalyst site and pollutant molecules in a water body can be improved, and the photocatalytic pollutant degradation efficiency is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of catalysts, and in particular, to a diatomic pair photocatalyst, a preparation method thereof, and an application thereof in tetracycline degradation. Background Art

[0002] In recent years, driven by the goal of "reducing pollution and reducing carbon emissions", photocatalytic technology has shown great potential for pollutant removal. Currently, many bimetallic inorganic supported semiconductor materials have been applied to the research of photocatalytic water pollutant degradation technology, but they generally face problems such as uneven distribution of active sites and difficulty in determining the binding mode, resulting in the synergistic mechanism between bimetallic sites is still unclear. Therefore, the current photocatalysts need to be further improved. Summary of the invention

[0003] The present application aims to solve one of the technical problems in the related art at least to some extent.

[0004] In one aspect, the present application provides a diatomic pair photocatalyst, including a structure shown in Formula 1: Wherein M1 and M2 independently include at least one of Co, Ni, Cu, Fe, Mn, and Pt. Therefore, in the diatomic pair photocatalyst proposed in the present application, M1-M2 exists in the form of highly dispersed atomic pairs, which optimizes the electron distribution of the active site, and the M1-M2 diatomic pairs are uniformly fixed on the one-dimensional pore wall of the covalent organic framework. When it is used to catalyze the degradation of pollutants, it can improve the contact efficiency between the catalyst site and the pollutant molecules in the water body, and improve the photocatalytic degradation efficiency of pollutants.

[0005] According to some embodiments of the present application, M1 includes at least one of Co, Ni, and Cu, and M2 includes at least one of Fe, Mn, and Pt. Thus, Fe-Co exists in the form of highly dispersed atomic pairs, optimizing the electron distribution of active sites, and the Fe-Co diatomic pairs are uniformly fixed on the one-dimensional pore walls of the covalent organic framework. When used to catalyze the degradation of pollutants, the contact efficiency between the catalyst sites and the pollutant molecules in the water body can be improved, thereby improving the efficiency of photocatalytic pollutant degradation.

[0006] Another aspect of the present application proposes a method for preparing the diatomic pair photocatalyst proposed in the first aspect of the present application, comprising: mixing 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and 2,2'-bipyridine-5,5'-dicarboxaldehyde with a first solvent, heating under vacuum conditions, filtering to obtain a solid powder; performing Soxhlet extraction on the solid powder, drying to obtain a COF precursor; mixing the COF precursor, M1 source, and a second solvent, stirring, and drying to obtain M1-COF; adding an M2 source to the electrolyte, forming the M1-COF on the surface of a conductive glass as a working electrode, and obtaining the diatomic pair photocatalyst through an electrochemical reaction. As a result, the method is process controllable and easy to repeat, and the metal diatomic pairs are uniformly fixed on the one-dimensional pore wall of the covalent organic framework, which can increase the degradation rate of pollutants by the photocatalyst.

[0007] The method proposed in this application also has the following additional technical features:

[0008] According to some embodiments of the present application, the potential of the electrochemical reaction is 1.4V-1.8V.

[0009] According to some embodiments of the present application, the electrochemical reaction time is 0.5h-3h.

[0010] According to some embodiments of the present application, the molar concentration of the M2 source in the electrolyte is 0.5 mol / L-2 mol / L.

[0011] According to some embodiments of the present application, the molar ratio of the 2,4,6-tris(4-aminophenyl)-1,3,5-triazine to the 2,2'-bipyridine-5,5'-dicarbaldehyde is 1:(1-2).

[0012] According to some embodiments of the present application, the mass ratio of the COF precursor to the M1 source is 1:(0.5-2).

[0013] According to some embodiments of the present application, the method satisfies at least one of the following conditions: the M1 source includes M1 salt, the M2 source includes M2 salt; the first solvent includes at least one of 1,4-dioxane, mesitylene, and acetic acid; the second solvent includes at least one of o-dichlorobenzene, n-butanol, and trifluoromethanesulfonic acid.

[0014] On the other hand, the present application also proposes the application of diatomic pair photocatalyst in the degradation of tetracycline. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] The above and / or additional aspects and advantages of the present application will become apparent and easily understood from the description of the embodiments in conjunction with the following drawings, in which:

[0016] Figure 1 A schematic flow chart of a method for preparing a diatomic pair photocatalyst according to an embodiment of the present application is shown.

[0017] Figure 2 The infrared test spectrum of the COF precursor in Example 1 of the present application is shown.

[0018] Figure 3 The ultraviolet absorption spectra of Co-Fe-COF in Example 2 of the present application and Co-COF in Comparative Example 1 are shown.

[0019] Figure 4 The scanning electron microscope and transmission images of Co-Fe-COF in Example 3 of the present application and Co-COF in Comparative Example 1 are shown.

[0020] Figure 5 A graph showing the synchrotron radiation test results of Co-Fe-COF in Example 3 of the present application is shown.

[0021] Figure 6 The graph shows the band gap position test results of Co-Fe-COF in Example 3 of the present application and Co-COF in Comparative Example 1.

[0022] Figure 7 The photocurrent analysis test result graph of Co-Fe-COF in Example 3 of the present application and Co-COF in Comparative Example 1 is shown.

[0023] Figure 8 The degradation effects of Co-Fe-COF in Example 3 of the present application and Co-COF in Comparative Example 1 on tetracycline are shown. DETAILED DESCRIPTION

[0024] The embodiments of the present application are described in detail below. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific technology or conditions are indicated in the embodiments, the technology or conditions described in the document in this area or the product specification are used. The reagents used or the instruments that do not indicate the manufacturer are all conventional products that can be obtained commercially.

[0025] In a first aspect, the present application provides a diatomic pair photocatalyst, characterized in that it includes a structure shown in Formula 1, Wherein, M1 and M2 independently include at least one of Co, Ni, Cu, Fe, Mn, and Pt. Therefore, the diatomic pair photocatalyst proposed in this application, by taking advantage of the rich and adjustable structural advantages of the covalent organic framework, constructs a N-rich covalent organic framework substrate structure, coordinates the introduction of M1 and M2 active single atomic sites, and M1-M2 exists in the form of highly dispersed atomic pairs, optimizing the electronic distribution of active sites. The M1-M2 diatomic pairs are uniformly fixed on the one-dimensional pore wall of the covalent organic framework. When it is used to catalyze the degradation of pollutants, it can improve the contact efficiency between the catalyst site and the pollutant molecules in the water body, and improve the efficiency of photocatalytic pollutant degradation.

[0026] According to some embodiments of the present application, M1 includes at least one of Co, Ni, and Cu, and M2 includes at least one of Fe, Mn, and Pt. Therefore, the diatomic pair photocatalyst proposed in the present application, by taking advantage of the rich and adjustable structural advantages of the covalent organic framework, constructs a N-rich covalent organic framework substrate structure, coordinates the introduction of M1 and M2 active single atomic sites, and M1-M2 exists in the form of highly dispersed atomic pairs, which optimizes the electronic distribution of active sites. The M1-M2 diatomic pairs are uniformly fixed on the one-dimensional pore wall of the covalent organic framework. When it is used to catalyze the degradation of pollutants, it can improve the contact efficiency between the catalyst site and the pollutant molecules in the water body, and improve the efficiency of photocatalytic pollutant degradation.

[0027] According to some embodiments of the present application, M1 includes Co, and M2 includes Fe. Therefore, the diatomic pair photocatalyst proposed in the present application, by taking advantage of the rich and adjustable structural advantages of the covalent organic framework, constructs a N-rich covalent organic framework substrate structure, coordinates the introduction of Co and Fe active single atomic sites, and Co-Fe exists in the form of highly dispersed atomic pairs, which optimizes the electron distribution of the active sites. The Co-Fe diatomic pairs are uniformly fixed on the one-dimensional pore wall of the covalent organic framework. When it is used to catalyze the degradation of pollutants, it can improve the contact efficiency between the catalyst site and the pollutant molecules in the water body, and improve the efficiency of photocatalytic pollutant degradation.

[0028] Another aspect of the present application provides a method for preparing the diatomic pair photocatalyst provided in the first aspect of the present application, comprising: mixing 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and 2,2'-bipyridine-5,5'-dicarbaldehyde with a first solvent, heating under vacuum conditions, and filtering to obtain a solid powder; performing Soxhlet extraction on the solid powder and drying to obtain a COF precursor; mixing the COF precursor, an M1 source, and a second solvent, stirring, and drying to obtain M1-COF; adding an M2 source to an electrolyte, forming the M1-COF on the surface of a conductive glass as a working electrode, and obtaining the diatomic pair photocatalyst through an electrochemical reaction. Therefore, the present application prepares diatomic pair photocatalysts through continuous solvent thermal, impregnation method and in-situ electrochemistry. The preparation process is simple. In the prepared diatomic pair photocatalyst, M1-M2 exists in the form of highly dispersed atomic pairs, which optimizes the electron distribution of active sites. The M1-M2 diatomic pairs are uniformly fixed on the one-dimensional pore walls of the covalent organic framework. When it is used to catalyze the degradation of pollutants, it can improve the contact efficiency between the catalyst sites and the pollutant molecules in the water body, thereby improving the photocatalytic pollutant degradation efficiency.

[0029] The following is a detailed description of each step of the method. Figure 1 , the method comprising:

[0030] S10: Mix 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and 2,2'-bipyridine-5,5'-dicarbaldehyde with the first solvent, heat, and filter to obtain a solid powder.

[0031] According to some embodiments of the present application, 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and 2,2'-bipyridine-5,5'-dicarbaldehyde are added to a heat-resistant glass tube, and a mixed solvent of 1,4-dioxane, mesitylene and acetic acid is added to the heat-resistant glass tube; the air in the heat-resistant glass tube is removed, and the glass tube is sealed and placed in an oven for heating and allowed to stand for 3 days; the heat-resistant glass tube is taken out, and after it is cooled to room temperature, the product in the glass tube is taken out, filtered, washed, and dried to obtain a solid powder.

[0032] According to some embodiments of the present application, the molar ratio of the 2,4,6-tris(4-aminophenyl)-1,3,5-triazine to the 2,2'-bipyridine-5,5'-dicarbaldehyde may be 1:(1-2). For example, it may be 1:1, 1:1.2, 1:1.4, 1:1.6, 1:1.8 or 1:2, etc., or may be a range of any of the above values. Thus, the orderliness of the crystal structure is improved, and the transmission capacity of the photogenerated electrons in the framework structure is improved.

[0033] The molecular structure of the 2,4,6-tris(4-aminophenyl)-1,3,5-triazine is as follows:

[0034]

[0035] The structural formula of the 2,2'-bipyridine-5,5'-dicarboxaldehyde is as follows:

[0036]

[0037] According to some embodiments of the present application, the heating temperature in the oven may be 100°C-140°C, for example, 100°C, 110°C, 120°C, 130°C or 140°C, or a range of any of the above values. Thus, while increasing the crystallization rate, the risk of the framework structure being damaged due to excessive temperature is reduced.

[0038] According to some embodiments of the present application, the volume ratio of 1,4-dioxane, mesitylene and acetic acid in the mixed solvent may be 5:5:1.

[0039] S20: subjecting the solid powder to Soxhlet extraction and drying to obtain a COF precursor

[0040] According to some embodiments of the present application, the solid powder is placed in a Soxhlet extraction device for heating, and when the extraction solution is colorless and transparent, the product is taken out and placed in a vacuum oven for drying to obtain a COF precursor.

[0041] According to some embodiments of the present application, the temperature at which the solid powder is heated in a Soxhlet extraction apparatus is 95°C-110°C, for example, 95°C, 100°C, 105°C or 110°C, etc., or can be a range consisting of any of the above numerical values.

[0042] S30: Mix the COF precursor, M1 source, and the second solvent, stir, and dry to obtain M1-COF

[0043] According to some embodiments of the present application, an M1 source is mixed with a second solvent to form an M1 source solution, the M1 source solution is mixed with a COF precursor, and stirred under inert gas protection, and the product is taken out, filtered, and dried to obtain M1-COF.

[0044] According to some embodiments of the present application, the mass ratio of the COF precursor to the M1 source is 1:(0.5-2). For example, it can be 1:0.5, 1:1, 1:1.5 or 1:2, etc., or can be a range of any of the above values. Thus, while the metal is fully coordinated, the risk of excessive metal blocking the COF pores is reduced.

[0045] According to some embodiments of the present application, the second solvent includes at least one of o-dichlorobenzene, n-butanol, and trifluoromethanesulfonic acid.

[0046] According to some embodiments of the present application, drying can be performed in a vacuum drying oven at a temperature of 40° C.-70° C. for a time of 10 h-14 h.

[0047] According to some embodiments of the present application, the M1 source includes an M1 salt.

[0048] S40: Adding M2 source to the electrolyte, forming the M1-COF on the surface of the conductive glass as a working electrode, and obtaining the diatomic photocatalyst through electrochemical reaction

[0049] According to some embodiments of the present application, an M2 source is added to the electrolyte, and the M1-COF is formed on the surface of a conductive glass as a working electrode, with Ag / AgCl as a reference electrode and a Pt electrode as a counter electrode. A certain potential is continuously applied, and after the reaction is completed, the material on the surface of the conductive glass is collected and dried to obtain a diatomic photocatalyst.

[0050] According to some embodiments of the present application, the potential of the in-situ electrochemical reaction is 1.4V-1.8V. For example, it can be 1.4V, 1.5V, 1.6V, 1.7V or 1.8V, or can be a range of any of the above values. Thus, the risk of M2 being oxidized to other valence states is reduced, and the reduction ability of M2 is improved.

[0051] According to some embodiments of the present application, the time of the in-situ electrochemical reaction is 0.5h-3h. For example, it can be 0.5h, 1h, 1.5h, 2h, 2.5h or 3h, or can be a range of any of the above values. Thus, M2 is fully coordinated with M1, and at the same time, the risk of M2 being oxidized is reduced.

[0052] According to some embodiments of the present application, the molar concentration of the M2 source in the electrolyte is 0.5mol / L-2mol / L. For example, it can be 0.5mol / L, 0.8mol / L, 1mol / L, 1.2mol / L, 1.4mol / L, 1.6mol / L, 1.8mol / L or 2mol / L, etc., or it can be a range composed of any of the above values. Thus, while the metal is fully coordinated, the risk of excessive metal blocking the COF pores is reduced.

[0053] According to some embodiments of the present application, the M2 source includes M2 salt.

[0054] In another aspect, the present application proposes the use of a diatomic pair photocatalyst in the degradation of tetracycline.

[0055] The embodiments of the present application are described in detail below. The embodiments described below are exemplary and are only used to explain the present application, and should not be construed as limiting the present application. If no specific technology or conditions are indicated in the embodiments, the technology or conditions described in the document in this area or the product specification are used. The reagents used or the instruments that do not indicate the manufacturer are all conventional products that can be obtained commercially.

[0056] Example 1

[0057] (1) 0.03 mmol of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and 0.03 mmol of 2,2'-bipyridine-5,5'-dicarboxaldehyde were added to a heat-resistant glass tube, and then a mixed solution of 1,4-dioxane, mesitylene and acetic acid in a volume ratio of 5:5:1 was added to a total volume of 2.2 mL;

[0058] (2) Freeze-thaw degassing: Use a common oil pump to remove air from the glass tube, seal the glass tube, place it in a 120°C oven, and leave it for 3 days;

[0059] (3) After the glass tube is removed and cooled to room temperature, the product is taken out, filtered, washed with acetone, and dried to obtain a solid powder;

[0060] (4) placing the solid powder in a Soxhlet extraction device, heating it to 100°C, and taking out the product when the extraction solution is colorless and transparent; placing it in a vacuum oven and drying it at 100°C to obtain a COF precursor;

[0061] (5) Place 5 mg of COF precursor in a beaker, add DMF, and disperse by ultrasonication for later use;

[0062] (6) 5 mg of COF precursor and cobalt acetate solution were mixed and stirred with a magnetic stirrer under argon protection for 1 day;

[0063] (7) taking out the product, filtering it, repeatedly washing it with deionized water, and draining it to obtain a solid powder;

[0064] (8) The washed and filtered product was placed in a watch glass, and dried in a vacuum drying oven at 60° C. for 12 h to obtain Co-COF;

[0065] (9) Weigh a certain mass of Co-COF material, ultrasonically disperse it into 5 mL of deionized water to obtain a yellow dispersion, and spin-coat the yellow dispersion on a 2 cm*2 cm FTO surface as an electrode material for standby use;

[0066] (10) Weigh a certain amount of ferric acetate and ultrasonically disperse it into 30 mL of deionized water to obtain an electrolyte solution, wherein the molar concentration of ferric acetate is 1.2 mol / L. The electrode material obtained in step 9 is used as a working electrode, Ag / AgCl is used as a reference electrode, and a Pt electrode is used as a counter electrode. A potential of 1.4 V (V vs RHE) is continuously applied for 2 h. After the reaction is completed, the FTO surface material is collected, washed, and the product after suction filtration is placed in a vacuum drying oven at 60 ° C for drying for 12 h to obtain Co-Fe-COF.

[0067] Example 2

[0068] The preparation method of Co-Fe-COF is the same as that of Example 1, except that the potential applied for the in-situ electrochemical reaction is 1.5 V (V vs RHE).

[0069] Example 3

[0070] The preparation method of Co-Fe-COF is the same as that of Example 1, except that the potential applied for the in-situ electrochemical reaction is 1.6 V (V vs RHE).

[0071] Example 4

[0072] Take the photocatalyst obtained in Example 3, weigh 5mg ultrasonic dispersion in 50mL of 50mg / L tetracycline molecule aqueous solution. Configure a 300W xenon lamp with a wavelength cut-off filter (λ≥420nm) as a light source, and before light radiation, stir the suspension in the dark for 1h to reach adsorption saturation between the catalyst and the tetracycline molecule. Then turn on the xenon lamp, and the photocatalytic reaction process begins. Press the time interval during the degradation process, take out a small amount of suspension, and immediately filter and separate by Millipore filter to remove the catalyst. Use the residual concentration of tetracycline molecules in the UV-visible spectrophotometer analysis reaction system.

[0073] Comparative Example 1

[0074] (1) 0.03 mmol of 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and 0.03 mmol of 2,2'-bipyridine-5,5'-dicarboxaldehyde were added to a heat-resistant glass tube, and then a mixed solution of 1,4-dioxane, mesitylene and acetic acid in a volume ratio of 5:5:1 was added to a total volume of 2.2 mL;

[0075] (2) Freeze-thaw degassing: Use a common oil pump to remove air from the glass tube, seal the glass tube, place it in a 120°C oven, and leave it for 3 days;

[0076] (3) After the glass tube is removed and cooled to room temperature, the product is taken out, filtered, washed with acetone, and dried to obtain a solid powder;

[0077] (4) placing the solid powder in a Soxhlet extraction device, heating it to 100°C, and taking out the product when the extraction solution is colorless and transparent; placing it in a vacuum oven and drying it at 100°C to obtain a COF precursor;

[0078] (5) Place 5 mg of COF precursor in a beaker, add DMF, and disperse by ultrasonication for later use;

[0079] (6) 5 mg of COF precursor and cobalt acetate solution were mixed and stirred with a magnetic stirrer under argon protection for 1 day;

[0080] (7) taking out the product, filtering it, repeatedly washing it with deionized water, and draining it to obtain a solid powder;

[0081] (8) The washed and filtered product was placed in a watch dish and dried in a vacuum drying oven at 60° C. for 12 h to obtain Co-COF.

[0082] Test Method

[0083] 1. Infrared test: The FT-IR test of the embodiment was recorded on a Bruker INVENIOS using a KBr disk, with a test range of 500 cm -1 -4000cm -1

[0084] 2. Ultraviolet-visible diffuse reflectance spectroscopy (UV-MiSDRS): It was carried out on a Lambda 850+ series UV-visible spectrophotometer of PerkimElms, USA, using BaSO4 as a control, and the test range was 250nm-800nm.

[0085] 3. Synchrotron radiation testing: The X-ray absorption spectrum (XAS) of the sample includes X-ray absorption near-edge structure (XANES) and extended X-ray absorption fine structure (EXAFS), which are collected at the Instrument Analysis Center of Taiyuan University of Technology.

[0086] 4. Band gap position test: Calculated by Tauc Plot formula based on UV-Mis DRS data.

[0087] 5. Photocurrent characterization analysis: It was carried out on a CHI 760E electrochemical workstation and a standard three-electrode system. The Pt sheet was used as the counter electrode (1cm*1cm), Ag / AgCl was used as the reference electrode, a 3mm diameter platinum carbon electrode was used as the working electrode, the electrolyte was a 0.5M Na2SO4 aqueous solution, the test range was -1V to 1V, and the test frequencies were 200Hz, 500Hz, and 1000Hz.

[0088] in conclusion:

[0089] By the attached Figure 2 It can be seen that compared with the monomer, the NH (3320 cm -1 ) and C=O(1670cm -1 ) disappeared, and the stretching peak at 1618cm -1 、1510cm -1 The existence of hydrazone bond formation at the site demonstrates the successful synthesis of the covalent organic framework base material.

[0090] By the attached Figure 3 It can be seen that the UV-visible DRS of Co-Fe-COF shows stronger absorption in the visible light range than Co-COF, proving that Co-Fe-COF has better light absorption ability, which is more conducive to the generation of photogenerated electrons. In addition, based on this data, the band gaps of Co-COF and Co-Fe-COF were calculated by the Tauc Plot formula to be 2.22eV and 2.03eV, respectively.

[0091] By the attached Figure 4 It can be seen that the scanning electron microscope photos show that the prepared products exhibit the morphology of irregular nanosynaptic aggregates; the atomic resolution spherical aberration corrected transmission electron microscope photos show that Co-COF can be observed as uniformly monodispersed bright spots, that is, Co single atoms, while Co-Fe-COF can be observed as paired bright spots (usually circled), that is, Co-Fe diatomic pairs.

[0092] By the attached Figure 5 It can be seen that the near-edge absorption of Co-Fe-COF is close to the Co-k-edge absorption, and the absorption position is located between Co3O4 and Co foil, indicating that the valence state of the Co element is between 0 and +2.7. The EXAFS spectrum shows the formation of local Co-Fe diatomic coordination at the Co metal site.

[0093] By the attached Figure 6 It can be seen from the band gap structure analysis that the VB and CB potential positions of Co-Fe-COF and Co-COF can drive the corresponding - O2 / H2O2 and H2O2 / ·OH react, but Co-Fe-COF has a narrower band gap than Co-COF, indicating that Co-Fe-COF is more easily excited by light to produce photogenerated electrons, thereby driving the O2+H2O→H2O2→·OH efficient hydroxyl radical generation reaction.

[0094] By the attached Figure 7 It can be seen that the transient photocurrent response results show that among the prepared photocatalysts, the photocurrent density of Co-Fe-COF is higher than that of Co-COF, proving that it has better photoelectric conversion efficiency.

[0095] By the attached Figure 8 It can be seen that compared with Co-Fe-COF, the photocatalytic degradation efficiency of Co-Fe-COF on pollutant antibiotic molecules in the water environment reaches nearly 80% within 60 minutes, while Co-COF only reaches nearly 30% within 60 minutes, proving that the synergistic effect of bimetallic compounds can greatly improve the degradation effect.

[0096] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present application. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0097] Although the embodiments of the present application have been shown and described above, it can be understood that the above embodiments are exemplary and cannot be understood as limitations on the present application. Ordinary technicians in this field can change, modify, replace and modify the above embodiments within the scope of the present application.

Claims

1. A diatomic pair photocatalyst, characterized in that: Including the structure shown in Formula 1, Wherein M1 and M2 independently include at least one of Co, Ni, Cu, Fe, Mn and Pt.

2. The diatomic pair photocatalyst according to claim 1, characterized in that M1 includes at least one of Co, Ni, and Cu, and M2 includes at least one of Fe, Mn, and Pt.

3. A method for preparing the diatomic pair photocatalyst according to claim 1 or 2, characterized in that: include: Mixing 2,4,6-tris(4-aminophenyl)-1,3,5-triazine and 2,2'-bipyridine-5,5'-dicarbaldehyde with a first solvent, heating under vacuum conditions, and filtering to obtain a solid powder; The solid powder is subjected to Soxhlet extraction and dried to obtain a COF precursor; The COF precursor, the M1 source, and the second solvent are mixed, stirred, and dried to obtain M1-COF; An M2 source is added to the electrolyte, the M1-COF is formed on the surface of the conductive glass as a working electrode, and the diatomic pair photocatalyst is obtained through an electrochemical reaction.

4. The method according to claim 3, characterized in that The potential of the electrochemical reaction is 1.4V-1.8V.

5. The method according to claim 4, characterized in that The electrochemical reaction time is 0.5h-3h.

6. The method according to claim 5, characterized in that The molar concentration of the M2 source in the electrolyte is 0.5 mol / L-2 mol / L.

7. The method according to any one of claims 3 to 6, characterized in that: The molar ratio of the 2,4,6-tris(4-aminophenyl)-1,3,5-triazine to the 2,2'-bipyridine-5,5'-dicarbaldehyde is 1:(1-2).

8. The method according to claim 7, characterized in that The mass ratio of the COF precursor to the M1 source is 1:(0.5-2).

9. The method according to claim 7, characterized in that: The method satisfies at least one of the following conditions: The M1 source includes M1 salt; The M2 source includes M2 salt; The first solvent includes at least one of 1,4-dioxane, mesitylene, and acetic acid; The second solvent includes at least one of o-dichlorobenzene, n-butanol, and trifluoromethanesulfonic acid.

10. Application of a diatomic pair photocatalyst in tetracycline degradation.

Citation Information

Patent Citations

  • Single-site transition metal covalent organic framework photocatalyst and preparation method thereof

    CN111921559A

  • M1M2-bidentate ligand / COF-5 diatomic catalyst for efficiently catalyzing CO2 reduction and preparation method thereof

    CN113751075A

  • Preparation method and application of MnTi-MOFs derivative denitration catalyst

    CN114505071A

  • Fe-Co / COF photocatalyst and preparation method thereof

    CN118022836A