Supported complex catalyst as well as preparation method and application thereof
By using metal ions and polyethylene polyamine coordination compounds of chelated resin carriers, the problems of narrow pH application range and high cost of traditional Fenton oxidation method are solved, and more efficient organic pollutant degradation and lower operating costs are achieved. .
Patent Information
- Application Number
- CN202410917598.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-09
- Publication Date
- 2024-11-01
AI Technical Summary
The traditional Fenton oxidation method has defects in the narrow pH application range, high iron sludge yield, low hydrogen peroxide utilization rate, and high cost, which limits its engineering application in organic pollutant treatment.
The coordination compound formed by metal ions and polyethylene polyamines with chelating resin as the support is used as the hydrogen peroxide catalyst. By combining metal ions with polyethylene polyamines, a more stable coordination compound is formed, and catalytic activity is improved. A wider pH application range and better cycleability are obtained through simple preparation and low energy consumption.
It achieves higher catalytic activity and a wider pH application range, and can effectively catalyze and degrade a variety of organic pollutants. The product after degradation is green and environmentally friendly, pollution-free, and has high H2O2 utilization efficiency. The catalyst can be recycled many times and the efficiency is only reduced by about 100% 5%.
Smart Images

Figure CN118874547A_ABST
Abstract
Description
Technical Field
[0001] The present application belongs to the field of organic wastewater treatment, and in particular relates to a supported complex catalyst and a preparation method and application thereof. Background Art
[0002] With the expansion of industrialization and production scale, more and more organic pollutants are discharged into water bodies, which not only causes water pollution, but also brings a series of negative impacts to the aquatic ecosystem. Since most organic pollutants are biologically toxic, they seriously threaten humans and the ecological environment. Therefore, it is of great significance to explore effective methods to treat organic pollutants.
[0003] At present, treatment technologies such as adsorption, membrane filtration, chemical oxidation, photocatalysis, and biological methods have been widely used in the treatment of organic wastewater. Among them, catalytic oxidation technology is considered to be one of the effective and sustainable methods for water purification.
[0004] The traditional catalytic degradation of organic pollutants in water uses the Fenton oxidation method, the key of which is Fe 2+ and H2O2. 2+ The catalytic decomposition of H2O2 produces ·OH (hydroxyl radicals) with extremely strong oxidizing properties, which can oxidize refractory organic pollutants into small molecular organic matter, carbon dioxide and water, etc. The traditional Fenton reaction has good treatment effect, energy saving and environmental protection, but it also has defects such as narrow pH application range (mainly low pH range), high iron sludge production, low hydrogen peroxide utilization rate and high cost, which limits the promotion and use of this method in engineering applications.
[0005] Therefore, people have made improvements based on the traditional Fenton oxidation method. For example, they use iron-containing minerals and other transition metals to make heterogeneous catalysts to form Fenton-like systems, which can also catalyze the decomposition of H2O2 to produce highly oxidizing hydroxyl radicals (·OH) and other active oxidizing substances. One of the methods with excellent results is to load the Fenton-like catalytic active components on resins. For example, a metal-loaded (Fe) system with polyamide oxime chelate resin as a carrier III , Cu II and Zn II) catalyst, compared with the traditional Fenton reagent, not only has excellent catalytic performance, can catalyze H2O2 to quickly and effectively degrade the organic pollutant phenol in water, and due to the excellent stability of the chelating resin and the metal ions, the catalyst can be reused, effectively avoiding the secondary pollution caused by the leakage of the metal components of the catalyst. On this basis, the present application provides a hydrogen peroxide catalyst with a chelating resin as a carrier and a coordination compound formed by metal ions and polyethylene polyamine as an active component. The preparation process of the catalyst is simple, the energy consumption is low, the catalyst has higher catalytic activity, a wider pH range of application, better recyclability, and can effectively catalyze the degradation of various organic pollutants. Summary of the invention
[0006] In order to overcome the defects of the above-mentioned prior art, the present application provides a hydrogen peroxide catalyst with a chelating resin as a carrier and a coordination compound formed by metal ions and polyethylene polyamine as an active component. The preparation process of the catalyst is simple and the energy consumption is low. The catalyst has higher catalytic activity, a wider pH application range, better recyclability, and can effectively catalyze the degradation of various organic pollutants.
[0007] The first object of the present application is to provide a supported complex catalyst, which includes a chelating resin and metal ions supported thereon, wherein the metal ions are combined with polyethylene polyamines through coordination.
[0008] Furthermore, the metal ions include Cu 2+ 、Zn 2+ 、Ni 2+ or Co 2+ .
[0009] Further, the polyethylene polyamines include ethylenediamine, diethylenetriamine, triethylenetetramine and tetraethylenepentamine.
[0010] The second object of the present application is to provide a method for preparing a supported complex catalyst, comprising:
[0011] Add the chelating resin to the metal ion solution and stir at room temperature for 2-4 hours to obtain an intermediate resin;
[0012] Rinse the intermediate resin with distilled water until no metal ions overflow from the water;
[0013] Drying the rinsed intermediate resin to obtain a metal-loaded resin;
[0014] The metal-loaded resin is put into a polyethylene polyamine solution, stirred and reacted at 30-60° C. for 2-4 hours, then rinsed with distilled water and dried to obtain a loaded complex catalyst.
[0015] Further, before adding the chelating resin to the metal ion solution, the method comprises:
[0016] The chelating resin is repeatedly washed with distilled water to remove impurities and then dried.
[0017] Furthermore, before adding the chelating resin into the metal ion solution, the method further comprises:
[0018] The chelating resin is activated.
[0019] Furthermore, the chelating resin includes CH90 chelating resin.
[0020] Furthermore, the activation treatment includes: immersing the CH90 chelating resin in a 0.1 mol / L NaOH solution for activation for 2-4 hours, rinsing it with distilled water, then immersing it in a 0.1 mol / L hydrochloric acid solution for activation for 2-4 hours, rinsing it with distilled water, and then drying it.
[0021] Further, the rinsed intermediate resin is dried, including:
[0022] The rinsed intermediate resin is placed in an oven for drying at a drying temperature of 80-95°C.
[0023] The third object of the present application is to provide an application of a supported complex catalyst, wherein the catalyst is used to catalyze hydrogen peroxide oxidation to degrade organic pollutants.
[0024] Technical effects and advantages of this application:
[0025] 1. Traditional Fenton oxidation method (with Fe 2+ The application of metal (Fe) as the catalytic active component is limited, secondary pollution will occur, the catalytic utilization rate is low, and the cost is high. III , Cu II and Zn II ) catalyst, the supported complex catalyst used in the present application has higher catalytic activity: during the catalytic process, the metal ions on ordinary supported metal catalysts (such as CH90-Cu) can coordinate with water molecules in water, while the metal ions on the complex catalyst (such as CH90-Cu(Dien)) can form a more stable coordination compound with polyethylene polyamine; the electronegativity of nitrogen is weaker than that of oxygen, and the complex formed by metal ions and polyethylene polyamine has a higher electron cloud density than that of ordinary metal ions, which is conducive to the production of low-valent metal complex ions in the catalytic process, and can produce more hydroxyl free radicals, thereby ultimately improving the catalytic activity.
[0026] 2. The preparation method of the supported complex catalyst of the present application is simple, has low energy consumption, is reusable, and has controllable costs.
[0027] 3. The supported complex catalyst of the present application has better catalytic effect, and can catalytically degrade a variety of organic pollutants (including but not limited to dyes (rhodamine B, methylene blue, Congo red), antibiotics (amoxicillin, ciprofloxacin, tetracycline), aromatic pollutants (phenol, halogenated benzene, polycyclic aromatic hydrocarbons)). The degradation products are green, environmentally friendly and pollution-free (the final products are inorganic molecules such as carbon dioxide and water), the cost is controllable, the H2O2 utilization efficiency is high, and the catalyst still has a high catalytic activity after being used for 6 cycles, and the efficiency is only reduced by about 5%.
[0028] Other features and advantages of the present application will be described in the following description, and partly become apparent from the description, or be understood by practicing the present application. The purpose and other advantages of the present application can be realized and obtained by the structures indicated in the description, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 A flow chart of a method for preparing a supported complex catalyst of the present application;
[0030] Figure 2 This is a performance comparison chart of copper complex catalyst, copper-loaded resin and CH90 chelating resin in degrading dye (methylene blue). DETAILED DESCRIPTION
[0031] The following will be combined with the drawings in the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0032] In the first aspect, the present application provides a supported complex catalyst, the catalyst comprising a chelating resin and a metal ion supported thereon, the metal ion being combined with polyethylene polyamine by coordination, the metal ion comprising Cu 2+ 、Zn 2+ 、Ni 2+ or Co 2+ , polyethylene polyamines include ethylenediamine, diethylenetriamine, triethylenetetramine and tetraethylenepentamine.
[0033] It should be noted that the traditional Fenton oxidation method (based on Fe 2+ The application of metal (Fe) as the catalytic active component is limited, secondary pollution will occur, the catalytic utilization rate is low, and the cost is high. III , Cu II and Zn II) catalyst, the supported complex catalyst of the present application has higher catalytic activity, this is because in the catalytic process of ordinary metal-supported catalysts (such as CH90-Cu), the metal ions on it will coordinate with water molecules in water, while the metal ions on the complex catalyst can form a more stable coordination compound with polyethylene polyamine, the electronegativity of nitrogen is weaker than that of oxygen, and the complex formed by metal ions and polyethylene polyamine has a higher electron cloud density than that of ordinary metal ions, which is conducive to the generation of low-valent metal complex ions in the catalytic process, and can generate more hydroxyl radicals. Taking CH90-Cu (Dien) as an example, the specific reaction mechanism is as follows:
[0034] (1) Formation of copper peroxide intermediate
[0035]
[0036] (2) Formation of active oxidizing species
[0037]
[0038]
[0039] (3) Dye oxidation
[0040]
[0041] Wherein, Dye represents dye, including but not limited to rhodamine B, methylene blue, Congo red, etc.; Dien represents diethylenetriamine; k1, k2, k3, k4 represent the reaction rate constants of the corresponding steps, CH90 chelating resin The R in the above figure represents a carbon chain. The non-carbonyl oxygen and tertiary nitrogen in the two -COOH groups can react with Cu 2+ Forming a chelate structure.
[0042] Second, as Figure 1 As shown, the present application also provides a method for preparing a supported complex catalyst, comprising:
[0043] Adding the chelating resin to the metal ion solution, stirring at room temperature for 2-4 hours (e.g., 2 hours, 2.5 hours, 3 hours, 3.5 hours or 4 hours) to obtain an intermediate resin;
[0044] Rinse the intermediate resin with distilled water until no metal ions overflow from the water;
[0045] The rinsed intermediate resin is dried to obtain a metal-loaded resin;
[0046] The metal-loaded resin is put into a polyethylene polyamine solution, and the reaction is stirred at 30-60°C (e.g., 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C) for 2-4h (e.g., 2h, 2.5h, 3h, 3.5h or 4h), and then rinsed with distilled water and dried to obtain a supported complex catalyst.
[0047] In some embodiments of the present application, before adding the chelating resin to the metal ion solution, the steps include: repeatedly washing the chelating resin with distilled water to remove impurities, and then drying.
[0048] In some embodiments of the present application, before adding the chelating resin to the metal ion solution, the method further includes: activating the chelating resin, wherein the chelating resin includes CH90 chelating resin. Taking CH90 chelating resin as an example, activating the chelating resin includes: soaking the CH90 chelating resin in a 0.1mol / L NaOH solution for activation for 2-4h (e.g., 2h, 2.5h, 3h, 3.5h or 4h), rinsing with distilled water, and then soaking the CH90 chelating resin in a 0.1mol / L hydrochloric acid solution for activation for 2-4h (e.g., 2h, 2.5h, 3h, 3.5h or 4h) to improve the exchange capacity of the resin, and then rinsing with distilled water and drying.
[0049] In some embodiments of the present application, drying the rinsed intermediate resin comprises:
[0050] The rinsed intermediate resin is placed in an oven to dry at a drying temperature of 80-95° C. (eg, 80° C., 85° C., 90° C. or 95° C.).
[0051] In a third aspect, the present application discloses an application of a supported complex catalyst, in which the above-mentioned catalyst is used to catalyze the oxidation of hydrogen peroxide to degrade organic pollutants. The organic pollutants that can be catalytically degraded include but are not limited to dyes (rhodamine B, methylene blue, Congo red), antibiotics (amoxicillin, ciprofloxacin, tetracycline), and aromatic pollutants (phenol, halogenated benzene, polycyclic aromatic hydrocarbons). The degradation products are green, environmentally friendly and pollution-free (the final products are inorganic molecules such as carbon dioxide and water), the cost is controllable, the H2O2 utilization efficiency is high, and the catalyst still has a high catalytic activity after being used in a cycle for 6 times, and the efficiency is only reduced by about 5%.
[0052] In order to better illustrate the present solution, the following embodiments are also provided.
[0053] Example 1
[0054] The CH90 chelate resin was repeatedly washed with distilled water to remove impurities, and then dried. The dried CH90 chelate resin was immersed in a 0.1 mol / L NaOH solution for 2 hours, rinsed with distilled water, and then immersed in a 0.1 mol / L hydrochloric acid solution for 2 hours to improve the exchange capacity of the resin, rinsed with distilled water, and then dried.
[0055] Accurately weigh a certain amount of CuSO4 and dissolve it in distilled water to obtain 100mL of 0.5mol / L CuSO4 solution. Weigh 10g of dry activated CH90 chelating resin, add it to the CuSO4 solution, stir at room temperature for 3h, and rinse the obtained intermediate resin repeatedly with distilled water until no copper ions overflow from the water; then place the intermediate resin in an oven at 90℃ to dry to obtain a metal-loaded resin (i.e., CH90-Cu).
[0056] Weigh a certain amount of diethylenetriamine and dissolve it in distilled water to make a solution (10mmol / L); put 3g of CH90-Cu resin into 100mL of diethylenetriamine solution and stir at 45℃ for 3h. Rinse with distilled water and then dry to obtain a supported complex catalyst (CH90-Cu(Dien)).
[0057] Example 2
[0058] The CH90 chelate resin was repeatedly washed with distilled water to remove impurities, and then dried. The dried CH90 chelate resin was immersed in a 0.1 mol / L NaOH solution for 3 hours, rinsed with distilled water, and then immersed in a 0.1 mol / L hydrochloric acid solution for 3 hours to improve the exchange capacity of the resin, rinsed with distilled water, and then dried.
[0059] Accurately weigh a certain amount of CuSO4 and dissolve it in distilled water to obtain 100mL of 0.5mol / L CuSO4 solution. Weigh 10g of dry activated CH90 chelating resin, add it to the CuSO4 solution, stir at room temperature for 2.5h, and rinse the obtained intermediate resin repeatedly with distilled water until no copper ions overflow from the water; then place the intermediate resin in an oven at 88℃ to dry to obtain a metal-loaded resin (i.e., CH90-Cu).
[0060] Weigh a certain amount of diethylenetriamine and dissolve it in distilled water to prepare a solution (10mmol / L); put 3g of CH90-Cu resin into 100mL of diethylenetriamine solution and stir at 30℃ for 4h. Rinse with distilled water and then dry to obtain a supported complex catalyst (CH90-Cu(Dien)).
[0061] Example 3
[0062] The CH90 chelate resin was repeatedly washed with distilled water to remove impurities, and then dried. The dried CH90 chelate resin was immersed in a 0.1 mol / L NaOH solution for 2.5 hours, rinsed with distilled water, and then immersed in a 0.1 mol / L hydrochloric acid solution for 2.5 hours to improve the exchange capacity of the resin, rinsed with distilled water, and then dried.
[0063] Accurately weigh a certain amount of CuSO4 and dissolve it in distilled water to obtain 100mL of 0.5mol / L CuSO4 solution. Weigh 10g of dry activated CH90 chelating resin, add it to the CuSO4 solution, stir at room temperature for 3.5h, and rinse the obtained intermediate resin repeatedly with distilled water until no copper ions overflow from the water; then place the intermediate resin in an oven at 92℃ to dry to obtain a metal-loaded resin (i.e., CH90-Cu).
[0064] Weigh a certain amount of diethylenetriamine and dissolve it in distilled water to prepare a solution (10mmol / L); put 3g of CH90-Cu resin into 100mL of diethylenetriamine solution, stir and react at 60°C for 2h, rinse with distilled water and then dry to obtain a supported complex catalyst (CH90-Cu(Dien)).
[0065] Example 4
[0066] The CH90 chelate resin was repeatedly washed with distilled water to remove impurities, and then dried. The dried CH90 chelate resin was immersed in a 0.1 mol / L NaOH solution for 2 hours, rinsed with distilled water, and then immersed in a 0.1 mol / L hydrochloric acid solution for 2 hours to improve the exchange capacity of the resin, rinsed with distilled water, and then dried.
[0067] Accurately weigh a certain amount of ZnSO4 and dissolve it in distilled water to obtain 100mL of 0.5mol / L ZnSO4 solution. Weigh 10g of dry activated CH90 chelating resin, add it to the ZnSO4 solution, stir at room temperature for 3h, and rinse the obtained intermediate resin repeatedly with distilled water until there is no new water and zinc ions overflow; then place the intermediate resin in an oven at 90℃ to dry to obtain a metal-loaded resin (i.e., CH90-Zn).
[0068] Weigh a certain amount of ethylenediamine (EDA) and dissolve it in distilled water to prepare a solution (20mmol / L); put 3g of CH90-Zn resin into 100mL of ethylenediamine solution, stir and react at 45°C for 3h, rinse with distilled water and then dry to obtain a supported complex catalyst (CH90-Zn(EDA)).
[0069] Example 5
[0070] The CH90 chelate resin was repeatedly washed with distilled water to remove impurities, and then dried. The dried CH90 chelate resin was immersed in a 0.1 mol / L NaOH solution for 4 hours, rinsed with distilled water, and then immersed in a 0.1 mol / L hydrochloric acid solution for 4 hours to improve the exchange capacity of the resin, rinsed with distilled water, and then dried.
[0071] Accurately weigh a certain amount of NiSO4 and dissolve it in distilled water to obtain 100mL of 0.5mol / L NiSO4 solution. Weigh 10g of dry activated CH90 chelating resin, add it to the NiSO4 solution, stir at room temperature for 3.5h, and rinse the obtained intermediate resin repeatedly with distilled water until no Ni ions overflow from the water; then place the intermediate resin in an oven at 95℃ to dry to obtain a metal-loaded resin (i.e., CH90-Ni).
[0072] Weigh a certain amount of triethylenetetramine (TETA) and dissolve it in distilled water to prepare a solution (10 mmol / L); put 3 g of CH90-Ni resin into 100 mL of triethylenetetramine solution, stir and react at 50°C for 4 h, rinse with distilled water and then dry to obtain a supported complex catalyst (CH90-Ni (TETA)).
[0073] Example 6
[0074] The CH90 chelate resin was repeatedly washed with distilled water to remove impurities, and then dried. The dried CH90 chelate resin was immersed in a 0.1 mol / L NaOH solution for 3 hours, rinsed with distilled water, and then immersed in a 0.1 mol / L hydrochloric acid solution for 3 hours to improve the exchange capacity of the resin, rinsed with distilled water, and then dried.
[0075] Accurately weigh a certain amount of CoSO4 and dissolve it in distilled water to obtain 100mL of 0.5mol / L CoSO4 solution. Weigh 10g of dry activated CH90 chelating resin, add it to the CoSO4 solution, stir at room temperature for 3h, and rinse the intermediate resin repeatedly with distilled water until no Co ions overflow from the water; then place the intermediate resin in an oven at 90℃ to dry to obtain a metal-loaded resin (i.e., CH90-Co).
[0076] Weigh a certain amount of tetraethylenepentamine (TEPA) and dissolve it in distilled water to prepare a solution (10mmol / L); put 3g of CH90-Co resin into 100mL of tetraethylenepentamine solution, stir and react at 50°C for 2h, rinse with distilled water and then dry to obtain a supported complex catalyst (CH90-Co(TEPA)).
[0077] The activity evaluation test was carried out on the supported complex catalysts prepared in Examples 1, 2, 3, 4, 5 and 6. 100 mL of 5 mg / L rhodamine B, methylene blue and Congo red solutions were respectively prepared to simulate organic wastewater, 0.3 mL of 30% hydrogen peroxide and 0.05 g of supported complex catalyst were respectively added, and the concentration change of the dye was tested. After testing, the supported complex catalysts prepared in the six embodiments can degrade more than 92% of rhodamine B, more than 95% of methylene blue, and more than 90% of Congo red in the water after reacting for 1.5 h. The supported complex catalysts prepared in the six embodiments still have high catalytic activity after being recycled for 6 times, and the efficiency is only reduced by about 5%.
[0078] The performance of unloaded CH90 resin, copper-loaded resin CH90-Cu and the supported complex catalyst prepared in Example 1 in treating organic wastewater was tested using methylene blue to simulate organic wastewater. The results are as follows Figure 2 As shown, the horizontal axis is the time when unloaded CH90 resin, copper-loaded resin CH90-Cu and the supported complex catalyst prepared in Example 1 are added to methylene blue, and the vertical axis is the methylene blue test concentration (C t ) to the initial concentration (C0), among which, the concentration of methylene blue in the blank group decreased slightly after H2O2 was added at the 90th minute; the unloaded CH90 resin removed the dye in the water by adsorption, and the concentration of methylene blue did not change much after H2O2 was added at the 90th minute; the copper-loaded resin CH90-Cu and CH90-Cu(Dien) catalyst had a certain catalytic effect on hydrogen peroxide, but the catalytic effect of CH90-Cu(Dien) catalyst was significantly stronger than that of the copper-loaded resin CH90-Cu.
[0079] Finally, it should be noted that the above is only a preferred embodiment of the present application and is not intended to limit the present application. Although the present application has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present application shall be included in the protection scope of the present application.
Claims
1. A supported complex catalyst, It is characterized in that The catalyst comprises a chelating resin and metal ions loaded thereon, wherein the metal ions are combined with polyethylene polyamine through coordination.
2. A supported complex catalyst according to claim 1, It is characterized in that The metal ions include Cu 2 + 、Zn 2+ 、Ni 2+ or Co 2+ .
3. A supported complex catalyst according to claim 1, It is characterized in that The polyethylene polyamines include ethylenediamine, diethylenetriamine, triethylenetetramine and tetraethylenepentamine.
4. A method for preparing a supported complex catalyst, It is characterized in that include: Add the chelating resin to the metal ion solution and stir at room temperature for 2-4 hours to obtain an intermediate resin; Rinse the intermediate resin with distilled water until no metal ions overflow from the water; Drying the rinsed intermediate resin to obtain a metal-loaded resin; The metal-loaded resin is put into a polyethylene polyamine solution, stirred and reacted at 30-60° C. for 2-4 hours, then rinsed with distilled water and dried to obtain a supported complex catalyst.
5. A method for preparing a supported complex catalyst according to claim 4, It is characterized in that Before the chelating resin is added to the metal ion solution, the method comprises: The chelating resin is repeatedly washed with distilled water to remove impurities and then dried.
6. A method for preparing a supported complex catalyst according to claim 4, It is characterized in that Before the chelating resin is added to the metal ion solution, the method further comprises: The chelating resin is activated.
7. A method for preparing a supported complex catalyst according to claim 6, It is characterized in that The chelating resin includes CH90 chelating resin.
8. A method for preparing a supported complex catalyst according to claim 7, It is characterized in that The activation treatment comprises: soaking the CH90 chelating resin in a 0.1 mol / L NaOH solution for activation for 1-3 hours, rinsing with distilled water, then soaking in a 0.1 mol / L hydrochloric acid solution for activation for 1-3 hours, rinsing with distilled water and then drying.
9. A method for preparing a supported complex catalyst according to claim 4, It is characterized in that The step of drying the rinsed intermediate resin comprises: The rinsed intermediate resin is placed in an oven for drying at a drying temperature of 80-95°C.
10. Application of a supported complex catalyst, It is characterized in that The catalyst according to any one of claims 1 to 3, or the supported complex catalyst prepared by the method according to any one of claims 4 to 9, is used to catalyze hydrogen peroxide oxidation to degrade organic pollutants.
Citation Information
Patent Citations
Efficient metal complex molecular catalyst as well as preparation and application of catalyst
CN108772101A
Chelating resin-based electro-Fenton catalyst and preparation method and application thereof
CN109317209A