Anticorrosive coating as well as preparation method and application thereof
By adopting a multi-layer coating structure in the intertidal zone area, combining cyanide oligomers, epoxy resins and fluorocarbon topcoats and other materials, the lack of binding strength and salt spray resistance of anticorrosion coatings in the intertidal zone environment is solved. The problem has achieved efficient marine protection effect.
Patent Information
- Application Number
- CN202410948476.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-15
- Publication Date
- 2024-11-01
- Estimated Expiration
- 2044-07-15
AI Technical Summary
In the intertidal zone, existing anticorrosion coatings are difficult to meet the requirements of high bond strength, cathode peel resistance and salt spray resistance, especially in the ocean and land transition areas where dry and wet and dry alternating oxygen concentrations are large, so as to protect them. Not effective.
Using a multi-layer coating structure, including pretreatment liquid, first base coating, functional coating and topcoat, using cyanide oligomers, epoxy resins, asphalt, porous fillers, self-healing agents and fluorocarbon topcoats , improve the adhesion and weather resistance of the coating through moisture curing and optimization processes.
It realizes the high bonding strength, cathode peel resistance and salt spray resistance of the coating. It is suitable for marine anti-corrosion fields in the intertidal zone. The bonding strength of the coating can reach 28.5N/(mm2)-1, and the salt spray resistance can be Up to 5200/h.
Smart Images

Figure BDA0004946427110000101
Abstract
Description
Technical Field
[0001] The invention belongs to the field of anti-corrosion coatings, and specifically relates to an anti-corrosion coating and a preparation method and application thereof. Background Art
[0002] The intertidal zone is the transition area between the ocean and the land. It refers to the coast between the average highest tide level and the lowest tide level, that is, the range from the place submerged when the sea water rises to the highest to the place exposed to the water surface when the tide recedes to the lowest. Affected by the tide, the intertidal zone is submerged by sea water twice a day and exposed to the air twice. Therefore, the buildings and facilities in the intertidal zone are affected by the tide and have the characteristics of cyclic exposure. The environment temperature changes dramatically, the humidity and salinity change greatly, and it is severely eroded by waves and tides. It has the characteristics of alternating dry and wet, and large changes in oxygen concentration. On the road of marine corrosion protection, we have a long way to go.
[0003] Patent CN104073127B discloses a wet-curing epoxy asphalt anticorrosive coating and its preparation method. The invention can still be constructed normally when the ambient humidity is higher than 85%. The dehumidification process is eliminated during the construction process, which greatly saves energy consumption. Patent CN101638550A discloses a recoatable general epoxy antirust paint that can be constructed in all seasons with a single curing agent. The invention uses a low molecular weight bisphenol A epoxy resin as a base material and introduces an anticorrosive coating with a branched active diluent in the formula. The coating solves the problem of construction in all seasons. The product has good resistance to cathodic stripping, can be matched with various topcoats, and can improve the efficiency of ship coating. However, in the intertidal zone area of the transition zone between the ocean and the land, due to the environmental characteristics of alternating dry and wet and large changes in oxygen concentration, when the coating is used to protect the substrate, in order to achieve a better protection effect, there are certain requirements for the bonding strength, stripping resistance, and salt spray resistance of the coating. Therefore, developing a special anticorrosive coating and process suitable for intertidal zone protection is an important measure for marine protection. Summary of the invention
[0004] The main purpose of the present invention is to provide an anti-corrosion coating and a preparation method and application thereof, so as to overcome the deficiencies in the prior art.
[0005] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:
[0006] One aspect of the present invention provides a method for preparing an anti-corrosion coating, comprising:
[0007] Pre-treating the substrate with a previous treatment liquid;
[0008] Applying a first primer solution containing an adhesive, a cyanide oligomer and / or a cyanide monomer to the surface of the substrate to form a first primer layer;
[0009] Applying a second primer solution containing epoxy resin, cyanide oligomer and / or cyanide monomer to the surface of the first primer layer to form a second primer layer;
[0010] Applying a functional coating to the surface of the second primer to form a functional coating, wherein the functional coating comprises asphalt, porous filler, self-repairing agent, epoxy micaceous iron intermediate paint and branched reactive diluent;
[0011] A transition coating liquid containing a coupling agent is applied to the surface of the functional coating to form a transition layer; a fluorocarbon topcoat is applied to the surface of the transition layer to form a topcoat to obtain an anti-corrosion coating.
[0012] Another aspect of the present invention provides an anti-corrosion coating prepared by the aforementioned preparation method, which includes a first primer layer, a second primer layer, a functional coating, a transition layer and a top coating.
[0013] Another aspect of the present invention also provides the use of the aforementioned anti-corrosion coating in the field of anti-corrosion.
[0014] Compared with the prior art, the technical solution of the present invention has at least the following advantages:
[0015] The anticorrosion coating provided by the present invention has good bonding strength, cathode stripping resistance and salt spray resistance. According to tests, the bonding strength of the coating of the present invention can reach 28.5N / (mm 2 ) -1 The cathodic disbonding resistance can reach 1mm; the salt spray resistance can reach 5200 / h. It can be used in the field of marine corrosion protection, especially for the protection of substrates in the intertidal zone in the transition zone between the sea and the land. DETAILED DESCRIPTION
[0016] The present invention will be more fully understood by reading the following specific embodiments. However, it should be understood that the specific embodiments disclosed below are only exemplary of the present invention, and the present invention can be embodied in various forms. Therefore, the specific functional details disclosed herein should not be interpreted as limiting, but only as the basis for the claims and as a representative basis for teaching those skilled in the art to adopt the present invention in different ways in any appropriate detailed embodiment.
[0017] As one aspect of the technical solution of the present invention, a method for preparing an anti-corrosion coating includes:
[0018] Pre-treating the substrate with a previous treatment liquid;
[0019] Applying a first primer solution containing an adhesive, a cyanide oligomer and / or a cyanide monomer to the surface of the substrate to form a first primer layer;
[0020] Applying a second primer solution containing epoxy resin, cyanide oligomer and / or cyanide monomer to the surface of the first primer layer to form a second primer layer;
[0021] Applying a functional coating to the surface of the second primer layer to form a functional coating, wherein the functional coating comprises asphalt, a porous filler, a self-healing agent, and a branched active diluent;
[0022] applying a transition coating liquid containing a coupling agent to the surface of the functional coating to form a transition layer;
[0023] A fluorocarbon topcoat is applied to the surface of the transition layer to form a topcoat to obtain an anti-corrosion coating.
[0024] The present invention uses cyanide oligomers and / or monomers in the primer layer to achieve wet curing. At the same time, since such oligomer monomers can form good bonding force with the substrate during polymerization, the adhesion between the coating layers is effectively improved, and the coating peeling phenomenon caused by excessive coating thickness, impact or aging in the later stage is further effectively alleviated, so that the coating has excellent weather resistance and UV resistance, high and low temperature resistance and aging resistance; the binder enables the coating to have high bonding strength and good bonding to glass and aluminum alloy.
[0025] The use of the functional coating in the present invention can not only effectively block the penetration and diffusion of water in a wet environment, but also effectively alleviate and eliminate the continuous damage and coating peeling caused by impact force, thereby making the coating have the dual functions of both corrosion resistance and fatigue impact resistance.
[0026] The present invention uses fluorocarbon topcoat in the topcoat to achieve the functions of waterproofing, aging resistance and corrosion resistance.
[0027] Furthermore, the present invention uses oligomers / monomers with high-strength bonding force to more effectively improve the interlayer bonding force, so that an effective bond is formed inside the entire anti-corrosion coating system, further avoiding the peeling problem between layers, maximizing the coating effect, and achieving an effect of one plus one being greater than two, thereby effectively improving the overall anti-corrosion and corrosion resistance of the coating.
[0028] In some embodiments, the method for preparing the anti-corrosion coating comprises: applying a pretreatment liquid to a substrate, wherein the pretreatment liquid comprises a mixture of a quaternary ammonium salt corrosion inhibitor, an adhesion promoter, and a waterproofing agent.
[0029] Furthermore, the mass ratio of the quaternary ammonium salt corrosion inhibitor, the adhesion promoter and the waterproofing agent is 3:1:1-5:1:1.
[0030] Furthermore, the mass concentration of the mixture of the quaternary ammonium salt corrosion inhibitor, the adhesion promoter and the waterproofing agent in the pretreatment solution is 5-10%.
[0031] In some embodiments, the quaternary ammonium salt corrosion inhibitor includes, but is not limited to, any one or a combination of two or more of an imidazoline quaternary ammonium salt corrosion inhibitor, a polyethyleneimine quaternary ammonium salt corrosion inhibitor, and a pyridinium quaternary ammonium salt corrosion inhibitor.
[0032] In some embodiments, the adhesion promoter includes but is not limited to any one or a combination of two or more of phenoxydimethylsilane compound (HY-F4011), aminosilane compound (Adherant1121), and CatacureTIN-22. Among them, Adherant1121 can enhance salt spray resistance.
[0033] In some embodiments, the waterproofing agent includes but is not limited to any one of Degussa P750, sodium methyl silicate, and potassium methyl silicate, or a combination of two or more thereof.
[0034] In some embodiments, the mass ratio of the binder to the cyanide oligomer and / or cyanide monomer in the first primer solution is 1:1-1:3.
[0035] In some embodiments, the binder includes but is not limited to alkali metal silicates, preferably any one of lithium silicates, sodium silicates, and potassium silicates, or a combination of two or more thereof.
[0036] In some embodiments, the mass ratio of the epoxy resin to the cyanide oligomer and / or cyanide monomer in the second primer solution is 3:1-5:1.
[0037] In some embodiments, the epoxy resin includes but is not limited to any one or a combination of two or more of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol E epoxy resin, novolac epoxy resin, and aromatic heterocyclic resin.
[0038] In some embodiments, the cyanide oligomer and / or cyanide monomer includes, but is not limited to, any one or a combination of two or more of ethyl cyanoacrylate, triphenylmethane triisocyanate, and polyisocyanate.
[0039] Furthermore, the polyisocyanate includes, but is not limited to, any one or a combination of two or more of diisocyanate, triisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, polymethylene polyphenyl polyisocyanate, and isophorone polyisocyanate.
[0040] In some embodiments, the preparation method of the functional coating includes: first filling the self-healing agent into the porous filler, then coating the porous filler with asphalt, then adding the asphalt-coated porous self-healing material to the epoxy micaceous iron intermediate paint and mixing evenly, and then diluting with a branched active diluent to obtain the functional coating. The porous filler is coated with soft and elastic asphalt to form a soft shell, which overcomes the rigid effect of the coating, so that when the coating is hit by the tide, it can achieve the buffering and erosion effect of the impact force through its soft shell, so that the coating has the dual functions of both corrosion resistance and impact resistance.
[0041] In some embodiments, the asphalt includes but is not limited to any one or a combination of two or more of petroleum asphalt, shale asphalt, and coal tar asphalt. Since the functional coating contains asphalt or tar components, it has waterproof, moisture-proof and anti-corrosion effects, and can also increase the peeling resistance of the coating, which can effectively block the penetration and diffusion of moisture in a wet environment.
[0042] In some embodiments, the porous filler includes, but is not limited to, any one of zeolite, porous quartz powder, and porous silicon carbide, or a combination of two or more thereof.
[0043] In some preferred embodiments, the average particle size of the porous filler is 10-40 μm.
[0044] In some embodiments, the self-repairing agent includes but is not limited to any one of dicyclopentadiene, epoxy resin, isocyanate, polyurethane, siloxane, and tung oil, or a combination of two or more thereof. Introducing a chelating resin into asphalt can further hinder the penetration of harmful ions in environmental water, and through its chelating effect, the harmful ions are bound in a certain space, thereby achieving an effective anti-corrosion effect.
[0045] In some embodiments, the branched reactive diluent includes but is not limited to any one or a combination of two or more of ethylene glycol bisglycidyl ether, resorcinol bisglycidyl ether, and 1,6-hexanediol diacrylate (HDDA) containing two or more reactive groups.
[0046] In some embodiments, the functional coating is applied by methods including, but not limited to, spraying.
[0047] In some embodiments, the mass concentration of the coupling agent in the transition coating liquid is 30-50%.
[0048] In some embodiments, the coupling agent contains, but is not limited to, at least any two of amino, thiol, vinyl, epoxy, hydroxyl, and acyloxy groups.
[0049] Furthermore, the coupling agent includes but is not limited to a combination of any two of γ-(methacryloyloxy)propyltrimethoxysilane, 3-(triethoxysilyl)-1-propanethiol, γ-(methacryloyloxy)propyltriethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane, and γ-aminopropyltrimethoxysilane.
[0050] Furthermore, the mass ratio of the two coupling agents is 2:1-2:5.
[0051] In some preferred embodiments, the coupling agent includes a first coupling agent and a second coupling agent, wherein the molecules of the first coupling agent include but are not limited to any one of acyloxy, thiol, and epoxy groups, including but not limited to any one of γ-(methacryloyloxy)propyltrimethoxysilane, 3-(triethoxysilyl)-1-propanethiol, γ-(methacryloyloxy)propyltriethoxysilane, and γ-(2,3-epoxypropyloxy)propyltrimethoxysilane; the molecules of the second coupling agent include but are not limited to any one of thiol, halogen, and amino groups, including but not limited to any one of γ-mercaptopropyltrimethoxysilane and γ-aminopropyltrimethoxysilane.
[0052] In some embodiments, the mass content of the fluororesin in the fluorocarbon topcoat is 24-30%, and the solid content is 50-60%.
[0053] In some embodiments, the fluororesin includes but is not limited to any one of PPG2800 or KANPE FLON HD TOPCOAT tetrafluorocarbon coating or a combination of both.
[0054] In some embodiments, the first primer layer, the second primer layer, the transition layer, and the topcoat layer are applied in a manner including, but not limited to, at least one of spraying, brushing, and roller coating.
[0055] In some preferred embodiments, the first primer layer and the second primer layer are constructed using different processes. The first primer layer is roller coated to form a rougher surface, and the second primer layer is sprayed. On the one hand, it is beneficial for the coating layers to adhere more firmly. On the other hand, the coating can be embedded into the anchor points of the rough surface of the first primer layer through the construction pressure of the spraying, thereby strengthening the adhesion between the two coating layers.
[0056] In some more specific embodiments, the method for preparing the anti-corrosion coating comprises:
[0057] S1: First remove the debris and dust on the substrate, then rinse the substrate with a high-pressure water gun, and then brush it with a pre-treatment liquid; the mass concentration of the mixture of quaternary ammonium salt corrosion inhibitor, adhesion promoter and waterproofing agent in the pre-treatment liquid is 5-10%; the quaternary ammonium salt corrosion inhibitor, adhesion promoter and waterproofing agent are mixed in a mass ratio of 3:1:1-5:1:1;
[0058] S2: applying the first primer liquid to the surface of the substrate by spraying, brushing or roller coating to form a first primer layer; the mass ratio of the binder to the cyanide oligomer and / or cyanide monomer in the first primer liquid is 1:1-1:3;
[0059] S3: applying the second primer liquid to the surface of the first primer layer by spraying, brushing or roller coating to form the second primer layer; the mass ratio of the epoxy resin to the cyanide oligomer and / or cyanide monomer in the second primer liquid is 3:1-5:1;
[0060] S4: When the second primer layer has not yet been completely cured, a functional coating is applied to the surface of the second primer layer by spraying or the like to form a functional coating; the preparation method of the functional coating comprises: firstly filling a self-healing agent into a porous filler, then coating the porous filler with asphalt, then adding the asphalt-coated porous self-healing material into the epoxy micaceous iron intermediate paint and mixing them evenly, and then diluting the mixture with a branched active diluent to obtain the functional coating;
[0061] S5: When the functional coating is dry and non-sticky, a transition coating liquid containing a coupling agent at a mass concentration of 30-50% is applied to the surface of the functional coating by spraying, brushing or roller coating to form a transition layer;
[0062] S6: After the transition layer is dry, a fluorocarbon topcoat having a fluororesin mass content of 24-30% and a solid content of 50-60% is applied to the surface of the transition layer by spraying, brushing or roller coating to form a topcoat, thereby obtaining an anti-corrosion coating.
[0063] As another aspect of the technical solution of the present invention, it also relates to an anti-corrosion coating prepared by the aforementioned anti-corrosion coating preparation method, which includes a first primer layer, a second primer layer, a functional coating, a transition layer and a top coating.
[0064] Furthermore, the thickness of the first primer layer is 5-10 μm.
[0065] Furthermore, the thickness of the second primer layer is 10-30 μm.
[0066] Furthermore, the thickness of the functional coating is 150-300 μm.
[0067] Furthermore, the thickness of the transition layer is 5-15 μm.
[0068] Furthermore, the thickness of the top coating is 30-50 μm.
[0069] As another aspect of the technical solution of the present invention, it also involves the application of the aforementioned anti-corrosion coating in the field of anti-corrosion.
[0070] Furthermore, the application includes: application of the anti-corrosion coating in marine protection.
[0071] Furthermore, the application includes: application of the anti-corrosion coating in the protection of intertidal zones in the transition zone between ocean and land.
[0072] In summary, the intertidal zone anticorrosion coating process disclosed in the present invention is a coating process designed for the characteristics of intertidal zone structural facilities. Through a design concept of external protection and internal penetration, materials that are resistant to aging, waterproof and moisture-proof, corrosion-resistant, wet-cured, and strongly adherent are used, and then the coating optimization process is used to achieve an unexpected protective effect on the structure. The process has simple pre-treatment requirements for the substrate, can be wet-cured, the raw materials are easily available, the coating method is simple, and the requirements for the construction environment are low. Therefore, the intertidal zone anticorrosion coating prepared by the present invention and its coating process can be applied to the field of surface corrosion protection, especially marine protection, especially the intertidal zone area in the transition zone between the sea and the land, which is affected by the tide and has the characteristics of cyclic exposure, and has large changes in temperature and humidity, large changes in salinity, severe scouring by waves and tides to form dry and wet alternation, and large changes in oxygen concentration. Corrosion and protection of buildings or marine facilities.
[0073] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The reagents and raw materials used in the following examples are commercially available, and the experimental methods without specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturers.
[0074] Example 1
[0075] (1) Substrate surface treatment:
[0076] First, remove the debris and dust on the substrate, then rinse the substrate with a high-pressure water gun, and then apply the pretreatment liquid containing imidazoline quaternary ammonium salt corrosion inhibitor, Degussa P750 waterproofing agent and phenoxydimethylsilane compound (HY-F4011) adhesion promoter to the surface of the substrate; the quaternary ammonium salt corrosion inhibitor, waterproofing agent and adhesion promoter are mixed in a mass ratio of 3:1:1, and the mass concentration of the mixture in the pretreatment liquid is 5%.
[0077] (2) Primer coating:
[0078] First, the base is coated with a first coat of primer 1, the composition ratio of which is 1:1 between lithium silicate adhesive and ethyl cyanoacrylate. The coating thickness is 5 μm. Then, the base is coated with a second coat of primer 2, the composition ratio of which is 5:1 between bisphenol A epoxy resin and ethyl cyanoacrylate. The coating thickness is 30 μm. The coating method is spraying.
[0079] (3) Preparation and coating of functional coatings:
[0080] First, the self-healing agent dicyclopentadiene is filled into a zeolite material with an average particle size of 10-20 μm, and then the zeolite is coated with petroleum asphalt. Then, the asphalt-coated porous self-healing material is added to the epoxy micaceous iron intermediate paint and stirred evenly, and then diluted with ethylene glycol diglycidyl ether to obtain a functional coating, wherein the mass ratio of dicyclopentadiene, zeolite, petroleum asphalt, ethylene glycol diglycidyl ether and epoxy micaceous iron intermediate paint is 1:5:10:5:40, and then when the primer layer is not completely cured, the functional coating is applied on the primer surface by spraying, and the coating thickness is 150 μm.
[0081] (4) After the functional coating is applied and the coating is dry and not sticky, a transition layer is applied by brushing, and the coating thickness is 15 μm; the transition layer contains two coupling agents with a mass concentration of 30%, and the mass ratio of γ-(methacryloyloxy)propyltrimethoxysilane to γ-aminopropyltrimethoxysilane is 2:1.
[0082] (5) After the transition layer is applied and the surface is dried, a layer of PPG2800 fluorocarbon topcoat is applied on the surface by spraying, with a coating thickness of 50 μm. The fluorocarbon topcoat contains 24% fluororesin by mass and 60% solid content.
[0083] The coating was applied on the substrate surface according to the above process. After the coating was completely cured, the various properties of the anti-corrosion coating were tested for 7 days. The results are shown in Table 1.
[0084] Example 2
[0085] (1) Substrate surface treatment:
[0086] First, remove the debris and dust on the substrate, then rinse the substrate with a high-pressure water gun, and then apply the pretreatment solution containing polyethyleneimine quaternary ammonium salt corrosion inhibitor, sodium methyl silicate waterproofing agent and aminosilane compound (Adherant1 121) adhesion promoter to the surface of the substrate; the quaternary ammonium salt corrosion inhibitor, waterproofing agent and adhesion promoter are mixed in a mass ratio of 4:1:1, and the mass concentration of the mixture in the pretreatment solution is 7%.
[0087] (2) Primer coating:
[0088] First, the base is coated with a first coat of primer 1, the composition ratio of the primer 1 is a mass ratio of sodium silicate adhesive to triphenylmethane triisocyanate of 1:2. The coating thickness is 7 μm, and then the base is coated with a second coat of primer 2, the composition ratio of the primer 2 is a mass ratio of bisphenol F epoxy resin to triphenylmethane triisocyanate of 4:1. The coating thickness is 20 μm. The coating method is spraying.
[0089] (3) Preparation and coating of functional coatings:
[0090] First, the self-healing agent isocyanate is filled into the porous quartz powder material with an average particle size of 20-30μm, and then the porous quartz powder is coated with shale asphalt, and then the asphalt-coated porous self-healing material is added to the epoxy micaceous iron intermediate paint and stirred evenly, and then diluted with resorcinol diglycidyl ether to obtain a functional coating. The mass ratio of isocyanate, porous quartz powder, shale asphalt, resorcinol diglycidyl ether and epoxy micaceous iron intermediate paint is 2.5:6.5:14:6.5:48, and then when the base coating is not completely cured, the functional coating is applied on the base coating surface by spraying, and the coating thickness is 200μm.
[0091] (4) After the functional coating is applied and the coating is dry and not sticky, a transition layer is applied by brushing, and the coating thickness is 12 μm; the transition layer contains two coupling agents with a mass concentration of 38%, and the mass ratio of γ-(2,3-epoxypropoxy)propyltrimethoxysilane to γ-mercaptopropyltrimethoxysilane is 1:1.
[0092] (5) After the transition layer is applied and the surface is dried, a layer of KANPE FLON HDTOPCOAT tetrafluorocarbon topcoat is applied on the surface by brushing, with a coating thickness of 40 μm. The fluorocarbon topcoat contains 30% fluororesin by mass and 50% solid content.
[0093] The coating was applied on the substrate surface according to the above process. After the coating was completely cured, the various properties of the anti-corrosion coating were tested for 7 days. The results are shown in Table 1.
[0094] Example 3
[0095] (1) Substrate surface treatment:
[0096] First, remove the debris and dust on the substrate, then rinse the substrate with a high-pressure water gun, and then apply the pretreatment solution containing quaternary ammonium pyridine corrosion inhibitor, potassium methyl silicate waterproofing agent and Catacure TIN-22 adhesion promoter to the surface of the substrate; the quaternary ammonium corrosion inhibitor, waterproofing agent and adhesion promoter are mixed in a mass ratio of 5:1:1, and the mass concentration of the mixture in the pretreatment solution is 8%.
[0097] (2) Primer coating:
[0098] First, the base is coated with a first coat of primer 1, the composition ratio of the primer 1 is a mass ratio of potassium silicate adhesive to toluene diisocyanate of 1:3. The coating thickness is 10μm, and then the base is coated with a second coat of primer 2, the composition ratio of the primer 2 is a mass ratio of bisphenol E epoxy resin to diphenylmethane diisocyanate of 3:1. The coating thickness is 10μm. The coating method is spraying.
[0099] (3) Preparation and coating of functional coatings:
[0100] First, the self-healing agent epoxy resin is filled into the porous silicon carbide material with an average particle size of 30-40μm, and then the porous silicon carbide is coated with coal tar pitch, and then the asphalt-coated porous self-healing material is added to the epoxy micaceous iron intermediate paint and stirred evenly, and then diluted with 1,6-hexanediol diacrylate (HDDA) to obtain a functional coating. The mass ratio of epoxy resin, porous silicon carbide, coal tar pitch, 1,6-hexanediol diacrylate and epoxy micaceous iron intermediate paint is 3.5:8.5:17:8.5:55, and then the functional coating is applied to the surface of the primer by spraying when the primer is not completely cured, and the coating thickness is 250μm.
[0101] (4) After the functional coating is applied and the coating is dry and not sticky, a transition layer is applied by roller coating, and the coating thickness is 8 μm; the transition layer contains two coupling agents with a mass concentration of 42%, and the mass ratio of 3-(triethoxysilyl)-1-propanethiol to Y-aminopropyltrimethoxysilane is 1:2.
[0102] (5) After the transition layer is applied and the surface is dried, a layer of PPG2800 fluorocarbon topcoat is applied on the surface by roller coating, with a coating thickness of 35 μm. The fluorocarbon topcoat contains 26% fluororesin by mass and 57% solid content.
[0103] The coating was applied on the substrate surface according to the above process. After the coating was completely cured, the various properties of the anti-corrosion coating were tested for 7 days. The results are shown in Table 1.
[0104] Example 4
[0105] (1) Substrate surface treatment:
[0106] First, remove the debris and dust on the substrate, then rinse the substrate with a high-pressure water gun, and then apply the pretreatment liquid containing polyethyleneimine quaternary ammonium salt corrosion inhibitor, Degussa P750 waterproofing agent and Catacure TIN-22 adhesion promoter to the surface of the substrate; the quaternary ammonium salt corrosion inhibitor, waterproofing agent and adhesion promoter are mixed in a mass ratio of 4:1:1, and the mass concentration of the mixture in the pretreatment liquid is 10%.
[0107] (2) Primer coating:
[0108] First, the base is coated with the first coat of primer 1, the composition ratio of the primer 1 is a mass ratio of sodium silicate adhesive to triisocyanate of 1:2. The coating thickness is 8μm, and then the base is coated with the second coat of primer 2, the composition ratio of the primer 2 is a mass ratio of phenolic epoxy resin to triisocyanate of 4:1. The coating thickness is 15μm. The coating method is spraying.
[0109] (3) Preparation and coating of functional coatings
[0110] First, the self-repairing agent tung oil is filled into the porous silicon carbide material with an average particle size of 30-40 μm, and then the porous silicon carbide is coated with petroleum asphalt, and then the asphalt-coated porous self-repairing material is added to the epoxy micaceous iron intermediate paint and stirred evenly, and then diluted with resorcinol bisglycidyl ether to prepare a functional coating. The mass ratio of tung oil, porous silicon carbide, petroleum asphalt, resorcinol bisglycidyl ether and epoxy micaceous iron intermediate paint is 5:10:20:10:60, and then when the base coating is not completely cured, the functional coating is applied on the base coating surface by spraying, and the coating thickness is 300 μm.
[0111] (4) After the functional coating is applied and the coating is dry and not sticky, a transition layer is applied by spraying, and the coating thickness is 5 μm; the transition layer contains two coupling agents with a mass concentration of 50%, and the mass ratio of γ-(methacryloyloxy)propyltriethoxysilane to γ-mercaptopropyltrimethoxysilane is 2:5.
[0112] (5) After the transition layer is applied and the surface is dried, a layer of KANPE FLON HDTOPCOAT tetrafluorocarbon topcoat is applied on the surface by spraying, with a coating thickness of 30 μm. The mass content of fluororesin in the fluorocarbon topcoat is 28% and the solid content is 54%.
[0113] The coating was applied on the substrate surface according to the above process. After the coating was completely cured, the various properties of the anti-corrosion coating were tested for 7 days. The results are shown in Table 1.
[0114] Comparative Example 1
[0115] Different from Example 1, in this comparative example, no pretreatment liquid is applied after the substrate is treated in step (1). The subsequent coating steps are the same. After being completely cured, the performance test is performed after being left for 7 days. The results are shown in Table 1.
[0116] Comparative Example 2
[0117] Different from Example 2, in step (2), primer 1 was not used but primer 2 was used. The subsequent coating steps were the same. After being completely cured, the performance test was carried out after being left for 7 days. The results are shown in Table 1.
[0118] Comparative Example 3
[0119] Different from Example 2, in step (2), only primer 1 was used instead of primer 2. The subsequent coating steps were the same. After being completely cured, the performance test was carried out after being left for 7 days. The results are shown in Table 1.
[0120] Comparative Example 4
[0121] Different from Example 3, in this comparative example, the functional coating used in step (3) does not contain any porous filler coated with asphalt. The subsequent coating steps are the same. After the coating is completely cured and left for 7 days, performance testing is performed. The results are shown in Table 1.
[0122] Comparative Example 5
[0123] Different from Example 4, step (4) is omitted in this comparative example, and the fluorocarbon topcoat is directly applied without coating the transition layer. The subsequent coating steps are the same. After being completely cured, the performance test is carried out after being left for 7 days. The results are shown in Table 1.
[0124] Test items: Cathodic disbonding resistance GB / T7790-1996, salt spray resistance GB / T1771-2007, bonding strength GB / T5210-2006
[0125] Table 1 Test results of various properties of coatings in various embodiments and comparative examples
[0126]
[0127] From the data in Table 1, it can be seen that the bonding strength, salt spray resistance and cathodic stripping resistance of the coating are significantly better after using pretreatment liquid, primer 1, primer 2, adding asphalt-coated porous filler and applying a transition layer.
[0128] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.
[0129] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing an anti-corrosion coating, characterized in that: include: Pre-treating the substrate with a previous treatment liquid; Applying a first primer solution containing an adhesive, a cyanide oligomer and / or a cyanide monomer to the surface of the substrate to form a first primer layer; Applying a second primer solution containing epoxy resin, cyanide oligomer and / or cyanide monomer to the surface of the first primer layer to form a second primer layer; Applying a functional coating to the surface of the second primer to form a functional coating, wherein the functional coating comprises asphalt, porous filler, self-repairing agent, epoxy micaceous iron intermediate paint and branched reactive diluent; applying a transition coating liquid containing a coupling agent to the surface of the functional coating to form a transition layer; A fluorocarbon topcoat is applied to the surface of the transition layer to form a topcoat to obtain an anti-corrosion coating.
2. The preparation method according to claim 1, characterized in that: include: Applying a pretreatment liquid to the substrate, wherein the pretreatment liquid includes a mixture of a quaternary ammonium salt corrosion inhibitor, an adhesion promoter and a waterproofing agent; Preferably, the mass ratio of the quaternary ammonium salt corrosion inhibitor, the adhesion promoter and the waterproofing agent is 3:1:1-5:1:1; Preferably, the mass concentration of the mixture of the quaternary ammonium salt corrosion inhibitor, the adhesion promoter and the waterproofing agent in the pretreatment solution is 5-10%; Preferably, the quaternary ammonium salt corrosion inhibitor includes any one or a combination of two or more of an imidazoline quaternary ammonium salt corrosion inhibitor, a polyethyleneimine quaternary ammonium salt corrosion inhibitor, and a pyridine quaternary ammonium salt corrosion inhibitor; Preferably, the adhesion promoter includes any one or a combination of two or more of a phenoxydimethylsilane compound, an aminosilane compound, and CatacureTIN-22; Preferably, the waterproofing agent includes any one of Degussa P750, sodium methyl silicate, and potassium methyl silicate, or a combination of two or more thereof.
3. The preparation method according to claim 1, characterized in that: The mass ratio of the binder to the cyanide oligomer and / or cyanide monomer in the first primer solution is 1:1-1:3; And / or, the adhesive includes alkali metal silicate, preferably any one of lithium silicate, sodium silicate and potassium silicate or a combination of two or more thereof.
4. The preparation method according to claim 1, characterized in that: The mass ratio of epoxy resin to cyanide oligomer and / or cyanide monomer in the second primer solution is 3:1-5:1; And / or, the epoxy resin includes any one or a combination of two or more of bisphenol A epoxy resin, bisphenol F epoxy resin, bisphenol E epoxy resin, novolac epoxy resin, and aromatic heterocyclic resin.
5. The preparation method according to claim 1, characterized in that: The cyanide oligomer and / or cyanide monomer includes any one or a combination of two or more of ethyl cyanoacrylate, triphenylmethane triisocyanate, and polyisocyanate; Preferably, the polyisocyanate includes any one or a combination of two or more of diisocyanate, triisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, polymethylene polyphenyl polyisocyanate, and isophorone polyisocyanate.
6. The preparation method according to claim 1, characterized in that: The preparation method of the functional coating comprises: first filling a self-repairing agent into a porous filler, then coating the porous filler with asphalt, then adding the asphalt-coated porous self-repairing material into an epoxy micaceous iron intermediate paint and mixing them evenly, and then diluting the mixture with a branched active diluent to obtain the functional coating; Preferably, the asphalt includes any one or a combination of two or more of petroleum asphalt, shale asphalt, and coal tar asphalt; Preferably, the porous filler includes any one of zeolite, porous quartz powder, and porous silicon carbide, or a combination of two or more thereof; preferably, the average particle size of the porous filler is 10-40 μm; Preferably, the self-healing agent includes any one or a combination of two or more of dicyclopentadiene, epoxy resin, isocyanate, polyurethane, siloxane, and tung oil; Preferably, the branched reactive diluent includes any one or a combination of two or more of ethylene glycol diglycidyl ether, resorcinol diglycidyl ether, and 1,6-hexanediol diacrylate containing two or more reactive groups; Preferably, the mass ratio of the self-repairing agent, porous filler, asphalt, branched reactive diluent and epoxy micaceous iron intermediate paint is (1-5): (5-10): (10-20): (5-10): (40-60); Preferably, the functional coating is applied by spraying.
7. The preparation method according to claim 1, characterized in that: The mass concentration of the coupling agent in the transition coating liquid is 30-50%; Preferably, the coupling agent contains at least any two of amino, mercapto, vinyl, epoxy, hydroxyl and acyloxy groups; preferably, the coupling agent includes any two of γ-(methacryloyloxy)propyltrimethoxysilane, 3-(triethoxysilyl)-1-propanethiol, γ-(methacryloyloxy)propyltriethoxysilane, γ-(2,3-epoxypropyloxy)propyltrimethoxysilane, γ-mercaptopropyltrimethoxysilane and γ-aminopropyltrimethoxysilane; preferably, the mass ratio of the two coupling agents is 2:1-2:5; Particularly preferably, the coupling agent includes a first coupling agent and a second coupling agent, wherein the molecule of the first coupling agent contains any one of an acyloxy group, a thiol group, and an epoxy group, and preferably includes any one of γ-(methacryloyloxy)propyltrimethoxysilane, 3-(triethoxysilyl)-1-propanethiol, γ-(methacryloyloxy)propyltriethoxysilane, and γ-(2,3-epoxypropoxy)propyltrimethoxysilane; the molecule of the second coupling agent contains any one of a thiol group, a halogen group, and an amino group, and preferably includes any one of γ-mercaptopropyltrimethoxysilane and γ-aminopropyltrimethoxysilane.
8. The preparation method according to claim 1, characterized in that: The mass content of the fluororesin in the fluorocarbon topcoat is 24-30%, and the solid content is 50-60%; preferably, the fluororesin includes any one of PPG2800 or KANPE FLON HD TOPCOAT tetrafluorocarbon coating or a combination of the two; And / or, the first primer layer, the second primer layer, the transition layer, and the topcoat are applied by at least one of spraying, brushing, and roller coating.
9. The anticorrosion coating prepared by the preparation method according to any one of claims 1 to 8, comprising a first primer layer, a second primer layer, a functional coating layer, a transition layer and a top coating layer; Preferably, the thickness of the first primer layer is 5-10 μm; Preferably, the thickness of the second primer layer is 10-30 μm; Preferably, the thickness of the functional coating is 150-300 μm; Preferably, the thickness of the transition layer is 5-15 μm; Preferably, the thickness of the top coating is 30-50 μm.
10. Application of the anti-corrosion coating according to claim 9 in the field of anti-corrosion, preferably, the application includes: The anti-corrosion coating is used in marine protection, especially in the protection of intertidal zones in the transition zone between the sea and the land.
Citation Information
Patent Citations
Flexible epoxy asphalt corrosion-resistant coating as well as preparation and application thereof
CN116376441A
Preparation method of ceramic-based composite coating resistant to seawater cavitation
CN116463578A
Epoxy asphalt anticorrosive paint for steel structure and preparation method of epoxy asphalt anticorrosive paint
CN117586698A
Water-based anticorrosive coating method and coated body
JP5246977B1